A method for preparing zinc alloy negative electrode material for aqueous zinc ion battery

Through the preparation method of zinc alloy anode materials, the problem of industrial production difficulties in the preparation process of zinc alloy anode materials in aqueous zinc-ion batteries has been solved, zinc dendrite suppression and battery cycle life improvement have been achieved, and the performance is stable and reliable.

CN118039780BActive Publication Date: 2024-10-01JIANGSU JIARU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410311723.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-10-01
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

The preparation process of zinc alloy anode materials in existing aqueous zinc-ion batteries has the problem of difficulty in large-scale industrial production, which leads to problems such as zinc dendrite growth, hydrogen evolution and corrosion, affecting the capacity, Coulombic efficiency and cycle stability of the battery.

Method used

The preparation method of zinc alloy anode material is adopted, including batching, smelting, continuous casting, multi-pass rolling and coiling. Zinc alloy plates are prepared through medium frequency induction melting furnace and casting and rolling process. The process parameters are controlled to thinning and annealing to form Stable zinc alloy sheet used as anode material for aqueous zinc-ion batteries.

Benefits of technology

It achieves a simple and environmentally friendly preparation of zinc alloy anode materials, inhibits the growth of zinc dendrites, reduces hydrogen evolution and corrosion, improves the reversibility and charge-discharge cycle life of the battery, and achieves stable and reliable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118039780B_ABST
    Figure CN118039780B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery, comprising: S1, batching: taking the required batching of the zinc alloy negative electrode material; S2, smelting: adding the required batching of the zinc alloy negative electrode material into a medium frequency induction smelting furnace in batches, heating to melt, cleaning the oxide scale and scum on the surface of the melt after the melt is completely melted, obtaining a zinc alloy melt, and keeping it at a temperature of more than 580°C for casting; S3, continuous casting; S4, multi-pass rolling; S5, coiling. Compared with the prior art, the invention solves the problem that the existing preparation process of zinc alloy negative electrode materials in aqueous zinc ion batteries is difficult to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aqueous zinc ion batteries, and in particular relates to a method for preparing a zinc alloy negative electrode material for aqueous zinc ion batteries. Background Art

[0002] With the development of human society and the urgent need for clean energy, people are forced to accelerate the establishment of low-cost, environmentally friendly, and highly stable energy storage systems to meet the application of large-scale grid power. At present, the scale of high-energy-density lithium-ion batteries has been unprecedentedly developed, but the limited reserves of lithium resources, high costs, uneven distribution, and unsafe organic system electrolytes have restricted their further development.

[0003] Compared with lithium-ion batteries using organic electrolytes, secondary aqueous zinc-ion batteries are more cost-effective, environmentally friendly, highly reliable, have low electrochemical potential (-0.762 V relative to standard hydrogen electrode), and have high theoretical mass specific capacity (820 mAh g -1 ) and volumetric capacity (5854 mAh cm -3 ) and its good stability in the environment have attracted widespread attention.

[0004] At present, there are many types of electrolytes available for zinc-ion battery electrolytes, among which ZnSO 4 The weakly acidic electrolyte used as the electrolyte is low-cost and has excellent comprehensive performance. However, when zinc metal is used as the negative electrode material of zinc-ion batteries, it faces problems such as hydrogen evolution, corrosion, passivation and zinc dendrite growth, which seriously affect the battery's capacity, coulombic efficiency and cycle stability, thus restricting the development and practical application of zinc-based aqueous batteries.

[0005] In order to solve these problems, the current main methods are to improve the reversibility and efficiency of zinc deposition / stripping by modifying the zinc negative electrode itself, optimizing the electrolyte composition, modifying the diaphragm, etc., thereby extending the cycle life of the electrode.

[0006] Among them, modification of zinc negative electrode is an effective strategy, which has attracted widespread attention from researchers. For example: CN117039205A discloses an electrochromic battery based on a hydrophobic alloy negative electrode. The method for preparing the negative electrode is mainly to prepare a hydrophobic alloy negative electrode by an electrochemical deposition method. The hydrophobic alloy negative electrode comprises a metal substrate and an alloy coating. The alloy coating can effectively inhibit the uncontrollable dendrite growth of the zinc metal negative electrode and effectively improve the electrochemical reversibility and cycle stability. However, the method has high cost for preparing the alloy coating and is difficult to produce on a large scale.

[0007] In addition, CN114927632B invented a method of using metal vapor vacuum ion source ion implantation technology to dope pure zinc or zinc alloy with metal ions to obtain a modified zinc metal negative electrode. The modified zinc metal sheet can form a stable and gentle electrode / electrolyte interface on the surface of the zinc electrode, guide the uniform deposition of zinc during the electrochemical reaction, inhibit the growth of zinc dendrites, reduce the occurrence of side reactions such as hydrogen evolution and corrosion, and improve the cycle life of aqueous zinc batteries. However, this method also faces the problems of cost and industrialization difficulties.

[0008] Therefore, there is an urgent need to develop a method for preparing zinc-based negative electrode materials that is simple, easy to operate, has excellent performance and is easy to industrialize. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery, so as to solve the problem that the existing preparation process of the zinc alloy negative electrode material in the aqueous zinc ion battery is difficult to industrialize.

[0010] In order to achieve the above object, the present invention discloses a method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery, comprising the following steps:

[0011] S1. Ingredients: Take the ingredients required for the zinc alloy negative electrode material, wherein the zinc alloy negative electrode material includes the following components in mass percentage: copper 0.08-2.0, titanium: 0.06-0.40, manganese: 0.02-0.05, and the balance is zinc;

[0012] S2. Melting: Add the ingredients required for the zinc alloy negative electrode material into a medium frequency induction melting furnace in batches, heat until it is melted, and after the melt is completely melted, clean the oxide scale and slag on the surface of the melt to obtain a zinc alloy melt, and keep it at a temperature above 580°C for casting;

[0013] S3, continuous casting: the zinc alloy melt is continuously cast to obtain a slab, the prepared slab is cut and trimmed, and then coiled into a coil;

[0014] S4, multi-pass rolling: the slab is thinned to the required finished product thickness of 0.2 mm to 2.0 mm after multi-pass rolling to obtain a zinc alloy sheet;

[0015] S5, Coiling: The sheet is coiled into finished coils through hydraulic cutting and constant tension coiling.

[0016] As a further description of the above technical solution:

[0017] In step S1, when mixing the ingredients, industrial pure zinc is added as zinc, oxygen-free copper is added as copper, and one or more of zinc-titanium master alloy, copper-titanium master alloy, and zinc-copper-titanium master alloy are added as titanium.

[0018] As a further description of the above technical solution:

[0019] In step S3, the zinc alloy melt is used to prepare a slab by a casting and rolling process, and the melt after being molten is introduced into an inclined twin-roll casting and rolling mill to prepare a cast-rolled slab with a thickness of 3 mm to 5 mm.

[0020] As a further description of the above technical solution:

[0021] In step S4, the 3 mm to 5 mm thick slab prepared by the casting and rolling process is thinned by continuous rolling for 2 to 10 passes to a desired finished product thickness of 0.2 mm to 2.0 mm.

[0022] As a further description of the above technical solution:

[0023] In step S3, the zinc alloy melt is prepared into slabs by horizontal continuous casting process. The melted molten metal is introduced into a water-cooled strip crystallizer to rapidly solidify into a shell. The slabs are then pulled out by a horizontal ingot casting machine to gradually cast the desired slabs to prepare continuous casting slabs with a thickness of 8 mm to 12 mm.

[0024] As a further description of the above technical solution:

[0025] In step S4, the 8mm-12mm thick slab prepared by the horizontal continuous casting process is firstly thinned to about 3.0mm by 3-5 continuous rough rolling passes, and then thinned to a finished product thickness of 0.2mm-2.0mm by 2-8 continuous finish rolling passes.

[0026] As a further description of the above technical solution:

[0027] In step S4, intermediate annealing is performed during the rolling process. The intermediate annealing temperature is 130° C. to 250° C., the annealing time is 2 h to 6 h, and the cooling method is air cooling after the furnace is taken out.

[0028] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0029] 1. In the present invention, the preparation process of the zinc alloy negative electrode material in the aqueous zinc ion battery is simple and environmentally friendly, and the process parameters are easy to control, so that the prepared zinc alloy negative electrode has no obvious interface stratification phenomenon and has stable and reliable performance.

[0030] 2. In the present invention, metals such as Cu and Ti in the zinc alloy can increase the deposition sites of zinc during the electrochemical reaction, induce uniform deposition of zinc, inhibit the growth of zinc dendrites, reduce the occurrence of side reactions such as hydrogen evolution and corrosion, and improve their reaction kinetics, thereby achieving the reversibility and charge-discharge cycle life of the aqueous zinc ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 The pure zinc sheet and the zinc alloy sheet prepared in Example 1 of the present application were heated to 1M Na 2 SO 4 Linear scan curve in electrolyte.

[0033] Figure 2 This is a time-voltage comparison chart of a symmetrical battery assembled with a pure zinc negative electrode and a symmetrical battery assembled with a zinc alloy negative electrode prepared in Example 1 of the present application.

[0034] Figure 3 This is a time-voltage long cycle diagram of a symmetrical battery assembled with the zinc alloy negative electrode prepared in Example 1 of the present application.

[0035] Figure 4 This is a cycle life diagram of an aqueous zinc ion battery assembled with the zinc alloy prepared in Example 1 of the present application as the negative electrode and manganese dioxide as the positive electrode. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0037] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0039] In the description of the embodiments of the present invention, it should be noted that the terms "upper", "inner", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, or are directions or positional relationships in which the inventive product is usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.

[0040] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0041] Example 1

[0042] See also Figure 1-4 On the one hand, the present application discloses a method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery, comprising the following steps:

[0043] S1. Ingredients: Take the ingredients required for the zinc alloy negative electrode material, wherein the zinc alloy negative electrode material includes the following components in mass percentage: copper 0.08-2.0, titanium: 0.06-0.40, manganese: 0.02-0.05, and the balance is zinc;

[0044] S2. Melting: Add the ingredients required for the zinc alloy negative electrode material into a medium frequency induction melting furnace in batches, heat until it is melted, and after the melt is completely melted, clean the oxide scale and slag on the surface of the melt to obtain a zinc alloy melt, and keep it at a temperature above 580°C for casting;

[0045] S3, continuous casting: the zinc alloy melt is continuously cast to obtain a slab, the prepared slab is cut and trimmed, and then coiled into a coil;

[0046] S4, multi-pass rolling: the slab is thinned to the required finished product thickness of 0.2 mm to 2.0 mm after multi-pass rolling to obtain a zinc alloy sheet;

[0047] S5, Coiling: The sheet is coiled into finished coils through hydraulic cutting and constant tension coiling.

[0048] In step S1, when mixing the ingredients, industrial pure zinc is added, oxygen-free copper is added, and one or more of zinc-titanium master alloy, copper-titanium master alloy, and zinc-copper-titanium master alloy are added. Among them, the mass percentage of titanium in the zinc-titanium master alloy is 3-5, and the balance is zinc; the mass percentage of titanium in the copper-titanium master alloy is 20-50, and the balance is zinc; the mass percentage of copper in the zinc-copper-titanium master alloy is 10-30, the mass percentage of titanium is 4-16, and the balance is zinc.

[0049] In step S3, the zinc alloy melt is prepared into slabs by a casting and rolling process. The melt after molten clean is introduced into an inclined twin-roll casting and rolling machine. The melt is cast, solidified, rolled and deformed in a narrow casting and rolling zone formed by a feed nozzle, an upper roll, a forming casting and rolling roll and a lower solidifying casting and rolling roll. The casting and rolling slabs with a thickness of 3 mm to 5 mm are prepared by adjusting the gap between the casting and rolling rolls and the length of the casting and rolling zone.

[0050] In step S4, the 3 mm to 5 mm thick slab prepared by the casting and rolling process is thinned by continuous rolling for 2 to 10 passes to a desired finished product thickness of 0.2 mm to 2.0 mm.

[0051] In step S4, intermediate annealing is performed during the rolling process, the intermediate annealing temperature is 130℃~250℃, the annealing time is 2h~6h, and the cooling method is air cooling after the furnace. Specifically, in order to prevent the plate from edge cracking, plate surface buckling and other rolling defects during the rolling process, it is necessary to reasonably arrange the rolling passes, pass reduction and reduction rate. If the cumulative reduction rate is large, intermediate annealing is required. In order to prevent the plate from edge cracking or to restore its plasticity to facilitate rolling deformation during the rolling process, intermediate annealing needs to be performed in time. According to the different composition of the plate and the cumulative reduction rate, the intermediate annealing temperature is: 130℃~250℃, the annealing time is: 2h~6h, and the cooling method is air cooling after the furnace.

[0052] On the other hand, the present application also discloses an application of the zinc alloy negative electrode material prepared by the above preparation method in the negative electrode material of an aqueous zinc ion battery. In the aqueous zinc ion battery, the zinc alloy is the negative electrode and the manganese dioxide is the positive electrode.

[0053] Example 2

[0054] On the one hand, the present application discloses a method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery, comprising the following steps:

[0055] S1. Ingredients: Take the ingredients required for the zinc alloy negative electrode material, wherein the zinc alloy negative electrode material includes the following components in mass percentage: copper 0.08-2.0, titanium: 0.06-0.40, manganese: 0.02-0.05, and the balance is zinc;

[0056] S2. Melting: Add the ingredients required for the zinc alloy negative electrode material into a medium frequency induction melting furnace in batches, heat until it is melted, and after the melt is completely melted, clean the oxide scale and slag on the surface of the melt to obtain a zinc alloy melt, and keep it at a temperature above 580°C for casting;

[0057] S3, continuous casting: the zinc alloy melt is continuously cast to obtain a slab, the prepared slab is cut and trimmed, and then coiled into a coil;

[0058] S4, multi-pass rolling: the slab is thinned to the required finished product thickness of 0.2 mm to 2.0 mm after multi-pass rolling to obtain a zinc alloy sheet;

[0059] S5, Coiling: The sheet is coiled into finished coils through hydraulic cutting and constant tension coiling.

[0060] In step S1, when mixing the ingredients, industrial pure zinc is added, oxygen-free copper is added, and one or more of zinc-titanium master alloy, copper-titanium master alloy, and zinc-copper-titanium master alloy are added. Among them, the mass percentage of titanium in the zinc-titanium master alloy is 3-5, and the balance is zinc; the mass percentage of titanium in the copper-titanium master alloy is 20-50, and the balance is zinc; the mass percentage of copper in the zinc-copper-titanium master alloy is 10-30, the mass percentage of titanium is 4-16, and the balance is zinc.

[0061] In step S3, the zinc alloy melt is prepared into slabs by a horizontal continuous casting process. The melt after being molten is introduced into a water-cooled plate and strip crystallizer to quickly solidify into a shell, and the slab is pulled out by the ingot head of a horizontal ingot casting machine to gradually cast the required slabs. By replacing slab crystallizers of different sizes, continuous casting slabs with a thickness of 8 mm to 12 mm are prepared.

[0062] In step S4, the 8mm-12mm thick slab prepared by the horizontal continuous casting process is firstly thinned to about 3.0mm by 3-5 continuous rough rolling passes, and then thinned to a finished product thickness of 0.2mm-2.0mm by 2-8 continuous finish rolling passes.

[0063] In step S4, intermediate annealing is performed during the rolling process, the intermediate annealing temperature is 130℃~250℃, the annealing time is 2h~6h, and the cooling method is air cooling after the furnace. Specifically, in order to prevent the plate from edge cracking, plate surface buckling and other rolling defects during the rolling process, it is necessary to reasonably arrange the rolling passes, pass reduction and reduction rate. If the cumulative reduction rate is large, intermediate annealing is required. In order to prevent the plate from edge cracking or to restore its plasticity to facilitate rolling deformation during the rolling process, intermediate annealing needs to be performed in time. According to the different composition of the plate and the cumulative reduction rate, the intermediate annealing temperature is: 130℃~250℃, the annealing time is: 2h~6h, and the cooling method is air cooling after the furnace.

[0064] On the other hand, the present application also discloses an application of the zinc alloy negative electrode material prepared by the above preparation method in the negative electrode material of an aqueous zinc ion battery. In the aqueous zinc ion battery, the zinc alloy is the negative electrode and the manganese dioxide is the positive electrode.

[0065] Working principle: The preparation process of zinc alloy negative electrode materials in aqueous zinc ion batteries is simple and environmentally friendly, and the process parameters are easy to control, so that the prepared zinc alloy negative electrode has no obvious interface stratification phenomenon and stable and reliable performance. Metals such as Cu and Ti in zinc alloys can increase the deposition sites of zinc during the electrochemical reaction, induce uniform deposition of zinc, inhibit the growth of zinc dendrites, reduce the occurrence of side reactions such as hydrogen evolution and corrosion, and improve their reaction kinetics, thereby achieving the reversibility and charge and discharge cycle life of aqueous zinc ion batteries.

[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery, characterized in that: The following steps are involved: S1. Ingredients: Take the ingredients required for the zinc alloy negative electrode material, wherein the zinc alloy negative electrode material includes the following components in mass percentage: copper 0.08-2.0, titanium: 0.06-0.40, manganese: 0.02-0.05, and the balance is zinc; S2. Melting: Add the ingredients required for the zinc alloy negative electrode material into a medium frequency induction melting furnace in batches, heat until it is melted, and after the melt is completely melted, clean the oxide scale and slag on the surface of the melt to obtain a zinc alloy melt, and keep it at a temperature above 580°C for casting; S3, continuous casting: the zinc alloy melt is continuously cast to obtain a slab, and the prepared slab is cut and trimmed, and then coiled into a coil; the zinc alloy melt is prepared by a horizontal continuous casting process, the melt after being molten is introduced into a water-cooled plate and strip crystallizer to be rapidly solidified into a shell, and the slab is pulled out by a horizontal ingot casting machine, and the required slab is gradually cast to prepare a continuous casting slab with a thickness of 8 mm to 12 mm, or the zinc alloy melt is prepared by a casting and rolling process, the melt after being molten is introduced into an inclined twin-roll casting and rolling mill, and a cast-rolled slab with a thickness of 3 mm to 5 mm is prepared; S4, multi-pass rolling: intermediate annealing is performed during the rolling process, the intermediate annealing temperature is 130 ℃ ~ 250 ℃, the annealing time is 2 h ~ 6 h, and the cooling method is air cooling after leaving the furnace; for the 8 mm ~ 12 mm thick slab prepared by the horizontal continuous casting process, it is necessary to first undergo 3 ~ 5 passes of continuous rough rolling to be thinned to about 3.0 mm, and then undergo 2 ~ 8 passes of continuous finishing rolling to be thinned to a finished product thickness of 0.2 mm ~ 2.0 mm; for the 3 mm ~ 5 mm thick slab prepared by the casting and rolling process, it is thinned by 2 ~ 10 passes of continuous rolling to the required finished product thickness of 0.2 mm ~ 2.0 mm; S5, Coiling: The sheet is coiled into finished coils through hydraulic cutting and constant tension coiling.

2. The method for preparing a zinc alloy negative electrode material for an aqueous zinc ion battery according to claim 1, wherein: In step S1, when mixing the ingredients, industrial pure zinc is added as zinc, oxygen-free copper is added as copper, and one or more of zinc-titanium master alloy, copper-titanium master alloy, and zinc-copper-titanium master alloy are added as titanium.