A kind of automobile nano waterproof film and its preparation process

By preparing a combined coating of modified polydopamine and nanofiller layers on the surface of automobile glass, the problems of visual blind spots and insufficient waterproof performance of existing automobile waterproof films are solved, achieving more efficient waterproofing and water-resistant performance, and improving the performance of automobiles in rainwater. Safety from the weather.

CN118047970BActive Publication Date: 2024-10-15TAIZHOU HONGTENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410173527.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-07
Publication Date
2024-10-15
Estimated Expiration
2044-02-07

AI Technical Summary

Technical Problem

Existing automobile waterproofing membranes have blind spots under rainy weather conditions, which affects driving safety, and their waterproofing performance is insufficient, making it difficult to meet the needs of modern automobiles for being more environmentally friendly, safer, and more comfortable.

Method used

Using PET film as the base material, a modified polydopamine coating and a nanofiller layer are prepared on its surface, and materials such as alkenyl monomers, terpyridine derivatives, dopamine and silica sol are used to form a nanocoating with excellent waterproof properties . The modified polydopamine coating forms a rough hydrophobic film layer through the reaction of dopamine, methacryloyl chloride, pyridinedicarboxylic acid, 4-amino-2,2,6,2-terpyridine, and zinc nitrate, and the nanofiller layer is formed by UV light and heat treatment of vinylbenzene, dodecafluoroheptyl methacrylate, and vinyl-modified silica sol enhance the hydrophobic ability of the film layer.

Benefits of technology

Significantly improves the waterproof performance and water resistance of the car glass surface, enhances adhesion and mechanical properties, improves the visual effect, and enhances the driving safety of the car in rainy weather conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004701578150000101
    Figure BDA0004701578150000101
  • Figure BDA0004701578150000111
    Figure BDA0004701578150000111
Patent Text Reader

Abstract

The invention discloses a kind of automobile nano waterproof film and its preparation process, including PET film and nano coating coated on the surface of PET film, the nano coating including modified polydopamine coating and nano filler layer. The present invention prepares modified polydopamine on the surface of PET film by components dopamine, methacryloyl chloride, pyridine dicarboxylic acid, 4-amino-2,2,6,2-terpyridine, zinc nitrate, utilizes the coordination of terpyridine, amine group and zinc ion, intermolecular interaction, realizes the assembly of terpyridine structure, obtains rough hydrophobic film layer; Then divinylbenzene, dodecafluoroheptyl methacrylate, vinyl modified silica sol are successively polymerized under ultraviolet light and thermal initiation, prepare nano filler coating, load nano structure on the rough surface of modified polydopamine coating, further improve the hydrophobic ability of film layer, obtain nano coating with excellent adhesion, water resistance, waterproof and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof films, in particular to an automobile nano waterproof film and a preparation process thereof. Background Art

[0002] As one of the important industries for economic development, the automobile industry has great market potential, high industrial correlation, wide employment, strong capital accumulation capacity, and can promote the rapid development of the national economy and make significant contributions. At present, automobile technology is developing in the direction of being more environmentally friendly, safer, more comfortable, and more personalized. Composite materials are developed in modern science and technology, and are composed of two or more different materials; their materials have synergistic effects in performance. Nanomaterials can show special physical and chemical properties due to their size and structural characteristics. When used in the automotive field, they have an effective role in improving the performance of automotive parts. Nanocomposite film is an organic-inorganic nanocomposite film that combines nanomaterials with polymers. It has broad application prospects in the surface protection and modification of materials; when applied to automotive glass and surface films, it can make the glass surface hydrophobic, eliminate the visual blind spots of the car in rainy weather, and improve the safety of car driving. Therefore, we propose an automotive nano waterproof film and its preparation process. Summary of the invention

[0003] The object of the present invention is to provide an automobile nano waterproof film and a preparation process thereof to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: an automobile nano waterproof film, comprising a PET film and a nano coating coated on the surface of the PET film, wherein the nano coating comprises a modified polydopamine coating and a nano filler layer, and the modified polydopamine coating is located between the PET film and the nano filler layer.

[0005] Furthermore, the thickness of the PET film is 0.1 to 0.5 mm.

[0006] Furthermore, the modified polydopamine coating is prepared from olefinic monomers, terpyridine derivatives, dopamine and zinc nitrate;

[0007] The vinyl monomer is prepared by the reaction of dopamine and methacryloyl chloride;

[0008] The terpyridine derivative is prepared by reacting pyridinedicarboxylic acid, 4-amino-2,2,6,2-terpyridine and dopamine.

[0009] Furthermore, the nano filler layer is made of silica sol, dodecafluoroheptyl methacrylate and divinylbenzene.

[0010] A preparation process of an automobile nano waterproof film, comprising the following processes:

[0011] Step (1), preparation of modified polydopamine coating:

[0012] The terpyridine derivative and zinc nitrate are mixed in chloroform and methanol, and stirred at 45-55°C for 8-12 hours; salt is replaced, centrifuged, the precipitate is washed, and dried to obtain a coordination compound; the terpyridine derivative and zinc nitrate are mixed in N,N-dimethylformamide and buffer solution, and cooled to room temperature to obtain a first slurry;

[0013] The PET film is placed in the first slurry and immersed for 8 to 12 hours; taken out and dried at 60° C. for 24 hours to form a modified polydopamine coating to obtain a modified PET film;

[0014] Step (2) Preparation of nanofiller layer:

[0015] Mixing silica sol, dodecafluoroheptyl methacrylate and divinylbenzene in N,N-dimethylacetamide, adding an initiator, and obtaining a second slurry;

[0016] The second slurry was coated on the surface of the modified polydopamine coating and irradiated with ultraviolet light for 150 to 180 minutes under nitrogen atmosphere with a light intensity of 500 μW / cm 2 , heat treatment at 80-90℃ for 6-8h to form a nano filler layer to obtain a nano waterproof membrane.

[0017] Further, in step (1), the first slurry includes the following mass components: 1.2-1.8 g / L olefinic monomer, 0.7-1.0 g / L terpyridine derivative, 0.4-0.6 g / L dopamine, and 0.3-0.5 g / L zinc nitrate;

[0018] The ratio of terpyridine derivative, chloroform, and methanol is 10 g:100 mL:300 mL;

[0019] The ratio of N,N-dimethylformamide to buffer is 30 mL:100 mL; the buffer is 10 mM Tris buffer, pH 8.5.

[0020] Further, in step (2), the second slurry includes the following mass components: 18-33 g / L silica sol, 5.0-7.5 g / L dodecafluoroheptyl methacrylate, 50-75 g / L divinylbenzene, and 0.9-1.4 g / L initiator;

[0021] The initiator is 2,2'-azobisisobutyronitrile.

[0022] Further, the olefinic monomer is prepared by the following process:

[0023] Mix sodium borate and deionized water, stir and add dopamine under nitrogen atmosphere, and continue stirring for 12 to 18 minutes; add sodium carbonate, add methacryloyl chloride at 0 to 5°C, and stir for 10 to 15 minutes; heat to 25 to 30°C, and keep warm for 8 to 12 hours; add concentrated hydrochloric acid to adjust the pH to 1 to 2, extract with ethyl acetate, dry the organic phase with anhydrous magnesium sulfate, filter, spin dry, and vacuum dry to obtain an olefin monomer.

[0024] Further, the ratio of sodium borate to deionized water is 3.8 g / 100 mL;

[0025] The molar ratio of dopamine, methacryloyl chloride, sodium carbonate and sodium borate is 1:(1.0-1.1):(1.0-1.1):(1.0-1.1).

[0026] Further, the terpyridine derivative is prepared by the following process:

[0027] Mix anhydrous tetrahydrofuran and pyridine dicarboxylic acid, add N,N-dimethylformamide, slowly add thionyl chloride at 0-5°C, and add it within 15 minutes; heat to reflux temperature and react for 30-35 minutes; remove the solvent by distillation under reduced pressure to obtain pyridine dicarboxylic acid chloride;

[0028] Mix pyridine dichloride, toluene and sodium carbonate, slowly add 4-amino-2,2,6,2-terpyridine at a temperature of 0 to 5°C, and add it within 60 minutes; heat to 25 to 30°C, and react at a constant temperature for 100 to 150 minutes; add dopamine, stir for 10 to 15 minutes; continue to react for 8 to 12 hours; separate the liquid to remove toluene, extract, add 2M hydrochloric acid to adjust the pH of the system to 1.8 to 2.1, stir at a temperature of 0 to 5°C, filter, wash the precipitate with water, and dry to obtain a terpyridine derivative.

[0029] Further, the molar ratio of pyridine dicarboxylic acid to thionyl chloride is 1:(2.7-3.0);

[0030] The ratio of pyridinedicarboxylic acid, anhydrous tetrahydrofuran, and N,N-dimethylformamide is 5.6g:100mL:0.10mL.

[0031] Further, the mass ratio of pyridine dichloride, toluene, and sodium carbonate is 10 g:100 mL:40 g;

[0032] The mass ratio of pyridine dichloride, 4-amino-2,2,6,2-terpyridine and dopamine is 10:(12.1-12.2):(9.3-10.1).

[0033] Further, the pyridinedicarboxylic acid is one of pyridine-2,6-dicarboxylic acid, 3,5-pyridinedicarboxylic acid, and 3,4-pyridinedicarboxylic acid;

[0034] The dopamine raw material is dopamine hydrochloride.

[0035] In the above technical scheme, the amino group in dopamine reacts with the acyl chloride in methacryloyl chloride to generate an acrylamide group to obtain a dopamine derivative with an alkenyl group, which is recorded as an alkenyl monomer; the dihydroxyphenyl structure is retained and can participate in the polymerization process of dopamine. After copolymerization with a terpyridine derivative and dopamine to generate a modified polydopamine coating, the functionalized surface containing vinyl can react with the unsaturated bonds in the second slurry in the preparation process of the nanofiller layer, thereby enhancing the bonding strength between the modified polydopamine coating and the nanofiller layer, avoiding the peeling of the coating and the nanofiller, and improving the water resistance of the prepared nano waterproof film.

[0036] The two carboxyl groups in pyridine dicarboxylic acid are chlorinated and reacted with the amino groups in 4-amino-2,2,6,2-terpyridine and dopamine, respectively, to obtain derivatives with dihydroxyphenyl and terpyridine, which are recorded as terpyridine derivatives, and then mixed with zinc nitrate to generate coordination compounds formed by the assembly of terpyridine, amide group and zinc ion; then, by utilizing the characteristic that dopamine will undergo oxidative self-polymerization in a weak alkaline environment, the PET film is immersed in the first slurry, so that dopamine and its dopamine derivatives (terpyridine derivatives, olefin monomers) adhere to the surface of the PET film through oxidative self-polymerization, thereby obtaining a functionalized surface. After the terpyridine derivatives are copolymerized with the olefin monomer and dopamine, modified polydopamine is generated, and the terpyridine derivatives and their coordination compounds can be assembled through π-π interactions, electrostatic interactions, etc., to achieve surface roughening of the prepared modified polydopamine coating, forming a coating with a micro-nano structure, which helps to increase the contact angle of the film layer and improve the waterproof performance of the nano coating. The polydopamine molecular chain and terpyridine structure synergistically promote the adsorption of the modified polydopamine coating on the surface of the PET film, improve the adsorption strength between the modified polydopamine coating and the PET film layer, and help improve its waterproof, water-resistant and mechanical properties.

[0037] Furthermore, the silica sol is modified, and the modification process is as follows:

[0038] The silica sol is mixed with γ-methacryloxypropyltrimethoxysilane, stirred for 6 to 8 hours, heated to 80 to 90°C, and kept warm for 100 to 150 minutes; centrifuged, and dried to obtain a modified silica sol;

[0039] Further, silica sol: GT-30, solid content 30 wt%, sourced from Guangzhou Gutie New Materials Co., Ltd.;

[0040] The mass ratio of silica sol to γ-methacryloxypropyltrimethoxysilane is 10:(3.3-5.0).

[0041] In the above technical scheme, divinylbenzene and dodecafluoroheptyl methacrylate are used as monomers, and 2,2'-azobisisobutyronitrile is used as a photoinitiator. Under the action of ultraviolet radiation, graft precipitation copolymerization occurs, and in-situ polymerization undergoes microphase separation and re-fusion, so that divinylbenzene self-assembles to form spherical nano-micelles, which cooperate with nano-silica in silica sol and are deposited on the micro-nanostructure surface of the modified polydopamine coating to construct a super-hydrophobic surface. After γ-methacryloxypropyltrimethoxysilane, the silica sol introduces vinyl groups on the surface of nano-silica, which can participate in the polymerization reaction in the second slurry, increase the cross-linking density of the prepared nano-filler layer, improve the strength and barrier capacity of the film layer, and further improve the waterproof and water-resistant properties of the PET film. Heat treatment can decompose the residual ammonium persulfate in the system, promote the increase of cross-linking density, and refine the size of divinylbenzene polymerized micelles, further improving the hydrophobic, water-resistant and mechanical properties of the film layer.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The invention discloses a process for preparing a nano waterproof film for automobiles. The process comprises the following steps: preparing modified polydopamine on the surface of a PET film by using components such as dopamine, methacryloyl chloride, pyridinedicarboxylic acid, 4-amino-2,2,6,2-terpyridine and zinc nitrate; utilizing the coordination of terpyridine, amine groups and zinc ions and the interaction between molecules to realize the assembly of the terpyridine structure and obtain a rough hydrophobic film layer; then polymerizing divinylbenzene, dodecafluoroheptyl methacrylate and vinyl-modified silica sol in sequence under the action of ultraviolet light and heat initiation to prepare a nano filler coating; loading the nano structure on the rough surface of the modified polydopamine coating to further improve the hydrophobicity of the film layer and obtain a nano coating with excellent adhesion, water resistance, waterproofness and mechanical properties. DETAILED DESCRIPTION

[0044] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] In the following specific implementations,

[0046] The thickness of the PET film is 0.2 mm and is sourced from Wuxi Xingyue Plastic Industry Co., Ltd.;

[0047] Silica sol: GT-30, solid content 30wt%, from Guangzhou Gutie New Materials Co., Ltd.;

[0048] The wet film thickness of the second slurry applied on the surface of the modified polydopamine coating / polydopamine coating is 10 μm.

[0049] Embodiment 1: A process for preparing a nano-waterproof film for automobiles, comprising the following processes:

[0050] Step (1), preparation of modified polydopamine coating:

[0051] 1.1. Sodium borate and deionized water were mixed, stirred under nitrogen atmosphere, and dopamine hydrochloride was added, and stirring was continued for 12 minutes; sodium carbonate was added, and methacryloyl chloride was added at 0°C, and stirring was continued for 10 minutes; the temperature was raised to 25°C, and the reaction was kept warm for 12 hours; concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was extracted with ethyl acetate, and the organic phase was dried over anhydrous magnesium sulfate, filtered, spin-dried, and vacuum-dried to obtain an olefin monomer; the ratio of sodium borate to deionized water was 3.8 g / 100 mL; the molar ratio of dopamine hydrochloride, methacryloyl chloride, sodium carbonate, and sodium borate was 1:1:1:1;

[0052] 1.2. Mix anhydrous tetrahydrofuran and pyridine-2,6-dicarboxylic acid, add N,N-dimethylformamide, slowly add thionyl chloride at 0°C, and add it within 15 minutes; heat to reflux temperature and react for 30 minutes; remove the solvent by vacuum distillation to obtain pyridine dicarboxylic acid chloride; the molar ratio of pyridine-2,6-dicarboxylic acid to thionyl chloride is 1:2.7; the ratio of pyridine dicarboxylic acid, anhydrous tetrahydrofuran, and N,N-dimethylformamide is 5.6g:100mL:0.10mL;

[0053] Mix pyridine dichloride, toluene and sodium carbonate, and slowly add 4-amino-2,2,6,2-terpyridine at 0°C within 60 minutes; heat to 25°C and react at constant temperature for 100 minutes; the mass ratio of pyridine dichloride, toluene and sodium carbonate is 10g:100mL:40g;

[0054] The temperature was lowered to 0°C, dopamine hydrochloride was added, and the mixture was stirred for 10 minutes; the temperature was raised to 25°C, and the mixture was kept warm for 8 hours; the toluene was removed by separation, and the mixture was extracted. 2M hydrochloric acid was added to adjust the pH of the mixture to 2.1, and the mixture was stirred at 0°C, filtered, and the precipitate was washed with water and dried to obtain a terpyridine derivative; the mass ratio of pyridine dichloride, 4-amino-2,2,6,2-terpyridine, and dopamine hydrochloride was 10:12.1:9.3;

[0055] 1.3. Mix the terpyridine derivative and zinc nitrate in chloroform and methanol, and stir at 45°C for 12 hours; change the salt, centrifuge, wash the precipitate, and dry it to obtain a coordination compound; mix it with the olefin monomer and dopamine hydrochloride in N,N-dimethylformamide and buffer, and cool it to room temperature to obtain a first slurry; the ratio of the terpyridine derivative, chloroform, and methanol is 10g:100mL:300mL; the ratio of N,N-dimethylformamide and buffer is 30mL:100mL; the buffer is 10mM Tris buffer, pH 8.5; the first slurry includes the following mass components: 1.2g / L olefin monomer, 0.7g / L terpyridine derivative, 0.4g / L dopamine hydrochloride, 0.3g / L zinc nitrate;

[0056] The PET film is placed in the first slurry and immersed for 8 hours; taken out and dried at 60° C. for 24 hours to form a modified polydopamine coating to obtain a modified PET film;

[0057] Step (2) Preparation of nanofiller layer:

[0058] 2.1. Mix silica sol and γ-methacryloxypropyltrimethoxysilane, stir for 6 hours, heat to 80°C, and keep warm for 100 minutes; centrifuge and dry to obtain modified silica sol; the mass ratio of silica sol to γ-methacryloxypropyltrimethoxysilane is 10:3.3;

[0059] 2.2. The modified silica sol, dodecafluoroheptyl methacrylate, and divinylbenzene are mixed in N,N-dimethylacetamide, and an initiator is added to obtain a second slurry; the second slurry includes the following mass components: 18 g / L silica sol, 5.0 g / L dodecafluoroheptyl methacrylate, 50 g / L divinylbenzene, and 0.9 g / L initiator 2,2'-azobisisobutyronitrile;

[0060] The second slurry was coated on the surface of the modified polydopamine coating and irradiated with ultraviolet light for 150 min under nitrogen atmosphere with a light intensity of 500 W / cm 2 , heat treated at 80℃ for 6h to form a nano filler layer, obtain a nano coating, and obtain a nano waterproof membrane.

[0061] Embodiment 2: A process for preparing a nano-waterproof film for automobiles, comprising the following processes:

[0062] Step (1), preparation of modified polydopamine coating:

[0063] 1.1. Sodium borate and deionized water were mixed, stirred under nitrogen atmosphere, and dopamine hydrochloride was added, and stirring was continued for 15 minutes; sodium carbonate was added, and methacryloyl chloride was added at 2°C, and stirring was continued for 12 minutes; the temperature was raised to 27°C, and the reaction was kept warm for 10 hours; concentrated hydrochloric acid was added to adjust the pH to 1.5, and ethyl acetate was used for extraction, and the organic phase was dried over anhydrous magnesium sulfate, filtered, spin-dried, and vacuum-dried to obtain an olefin monomer; the ratio of sodium borate to deionized water was 3.8 g / 100 mL; the molar ratio of dopamine hydrochloride, methacryloyl chloride, sodium carbonate, and sodium borate was 1:1.05:1.05:1.05;

[0064] 1.2. Mix anhydrous tetrahydrofuran and pyridine-2,6-dicarboxylic acid, add N,N-dimethylformamide, slowly add thionyl chloride at 2°C, and add it within 15 minutes; heat to reflux temperature and react for 32 minutes; remove the solvent by vacuum distillation to obtain pyridine dicarboxylic acid chloride; the molar ratio of pyridine-2,6-dicarboxylic acid to thionyl chloride is 1:2.8; the ratio of pyridine dicarboxylic acid, anhydrous tetrahydrofuran, and N,N-dimethylformamide is 5.6g:100mL:0.10mL;

[0065] Mix pyridine dichloride, toluene and sodium carbonate, and slowly add 4-amino-2,2,6,2-terpyridine at 2°C within 60 minutes; heat to 27°C and react at constant temperature for 120 minutes; the mass ratio of pyridine dichloride, toluene and sodium carbonate is 10g:100mL:40g;

[0066] The temperature was lowered to 2°C, dopamine hydrochloride was added, and the mixture was stirred for 12 minutes; the temperature was raised to 27°C, and the mixture was kept warm for 10 hours; the toluene was removed by separation, and the mixture was extracted. 2M hydrochloric acid was added to adjust the pH of the mixture to 2.0, and the mixture was stirred at 2°C, filtered, and the precipitate was washed with water and dried to obtain a terpyridine derivative; the mass ratio of pyridine dichloride, 4-amino-2,2,6,2-terpyridine, and dopamine hydrochloride was 10:12.1:9.7;

[0067] 1.3. Mix the terpyridine derivative and zinc nitrate in chloroform and methanol, and stir at 50°C for 10 hours; change the salt, centrifuge, wash the precipitate, and dry it to obtain a coordination compound; mix it with the olefin monomer and dopamine hydrochloride in N,N-dimethylformamide and buffer, and cool it to room temperature to obtain a first slurry; the ratio of the terpyridine derivative, chloroform, and methanol is 10g:100mL:300mL; the ratio of N,N-dimethylformamide and buffer is 30mL:100mL; the buffer is 10mM Tris buffer, pH 8.5; the first slurry includes the following mass components: 1.25g / L olefin monomer, 0.8g / L terpyridine derivative, 0.5g / L dopamine hydrochloride, 0.4g / L zinc nitrate;

[0068] The PET film is placed in the first slurry and immersed for 10 hours; taken out and dried at 60° C. for 24 hours to form a modified polydopamine coating to obtain a modified PET film;

[0069] Step (2) Preparation of nanofiller layer:

[0070] 2.1. Mix silica sol and γ-methacryloxypropyltrimethoxysilane, stir for 7 hours, heat to 85°C, and keep warm for 120 minutes; centrifuge and dry to obtain modified silica sol; the mass ratio of silica sol to γ-methacryloxypropyltrimethoxysilane is 10:4.1;

[0071] 2.2. The modified silica sol, dodecafluoroheptyl methacrylate, and divinylbenzene are mixed in N,N-dimethylacetamide, and an initiator is added to obtain a second slurry; the second slurry includes the following mass components: 25 g / L silica sol, 6.3 g / L dodecafluoroheptyl methacrylate, 63 g / L divinylbenzene, and 1.2 g / L initiator 2,2'-azobisisobutyronitrile;

[0072] The second slurry was coated on the surface of the modified polydopamine coating and irradiated with ultraviolet light for 165 min under nitrogen atmosphere with a light intensity of 500 W / cm 2 , heat treated at 85℃ for 7h to form a nano filler layer, obtain a nano coating, and obtain a nano waterproof membrane.

[0073] Embodiment 3: A process for preparing a nano-waterproof film for automobiles, comprising the following processes:

[0074] Step (1), preparation of modified polydopamine coating:

[0075] 1.1. Sodium borate and deionized water were mixed, stirred under nitrogen atmosphere, and dopamine hydrochloride was added, and stirring was continued for 18 minutes; sodium carbonate was added, and methacryloyl chloride was added at 5°C and stirred for 10 minutes; the temperature was raised to 30°C and the reaction was kept warm for 8 hours; concentrated hydrochloric acid was added to adjust the pH to 1, extracted with ethyl acetate, and the organic phase was dried over anhydrous magnesium sulfate, filtered, spin-dried, and vacuum dried to obtain an olefin monomer; the ratio of sodium borate to deionized water was 3.8 g / 100 mL; the molar ratio of dopamine hydrochloride, methacryloyl chloride, sodium carbonate, and sodium borate was 1:1.1:1.1:1.1;

[0076] 1.2. Mix anhydrous tetrahydrofuran and pyridine-2,6-dicarboxylic acid, add N,N-dimethylformamide, slowly add thionyl chloride at 5°C, and add it within 15 minutes; heat to reflux temperature and react for 35 minutes; remove the solvent by vacuum distillation to obtain pyridine dicarboxylic acid chloride; the molar ratio of pyridine-2,6-dicarboxylic acid to thionyl chloride is 1:3.0; the ratio of pyridine dicarboxylic acid, anhydrous tetrahydrofuran, and N,N-dimethylformamide is 5.6g:100mL:0.10mL;

[0077] Mix pyridine dichloride, toluene and sodium carbonate, and slowly add 4-amino-2,2,6,2-terpyridine at 5°C within 60 minutes; heat to 30°C and react at constant temperature for 100 minutes; the mass ratio of pyridine dichloride, toluene and sodium carbonate is 10g:100mL:40g;

[0078] The temperature was lowered to 5°C, dopamine hydrochloride was added, and the mixture was stirred for 10 minutes; the temperature was raised to 30°C, and the mixture was kept warm for 8 hours; the toluene was removed by separation, and the mixture was extracted. 2M hydrochloric acid was added to adjust the pH of the mixture to 1.8, and the mixture was stirred at 5°C, filtered, and the precipitate was washed with water and dried to obtain a terpyridine derivative; the mass ratio of pyridine dichloride, 4-amino-2,2,6,2-terpyridine, and dopamine hydrochloride was 10:12.2:10.1;

[0079] 1.3. Mix the terpyridine derivative and zinc nitrate in chloroform and methanol, and stir at 55°C for 8h; change the salt, centrifuge, wash the precipitate, and dry it to obtain a coordination compound; mix it with the olefin monomer and dopamine hydrochloride in N,N-dimethylformamide and buffer, and cool it to room temperature to obtain a first slurry; the ratio of the terpyridine derivative, chloroform, and methanol is 10g:100mL:300mL; the ratio of N,N-dimethylformamide and buffer is 30mL:100mL; the buffer is 10mM Tris buffer, pH 8.5; the first slurry includes the following mass components: 1.8g / L olefin monomer, 1.0g / L terpyridine derivative, 0.6g / L dopamine hydrochloride, 0.5g / L zinc nitrate;

[0080] The PET film is placed in the first slurry and immersed for 12 hours; taken out and dried at 60° C. for 24 hours to form a modified polydopamine coating to obtain a modified PET film;

[0081] Step (2) Preparation of nanofiller layer:

[0082] 2.1. Mix silica sol and γ-methacryloxypropyltrimethoxysilane, stir for 8 hours, heat to 90°C, and keep warm for 100 minutes; centrifuge and dry to obtain modified silica sol; the mass ratio of silica sol to γ-methacryloxypropyltrimethoxysilane is 10:5;

[0083] 2.2. The modified silica sol, dodecafluoroheptyl methacrylate, and divinylbenzene are mixed in N,N-dimethylacetamide, and an initiator is added to obtain a second slurry; the second slurry includes the following mass components: 33 g / L silica sol, 7.5 g / L dodecafluoroheptyl methacrylate, 75 g / L divinylbenzene, and 1.4 g / L initiator 2,2'-azobisisobutyronitrile;

[0084] The second slurry was coated on the surface of the modified polydopamine coating and irradiated with ultraviolet light for 180 min under nitrogen atmosphere with a light intensity of 500 W / cm 2 , heat treated at 90℃ for 6h to form a nano filler layer, obtain a nano coating, and obtain a nano waterproof membrane.

[0085] Comparative Example 1: A process for preparing a nano-waterproof film for automobiles, comprising the following process: Step (1) is the same as in Example 1, forming a modified polydopamine coating to obtain a modified PET film;

[0086] Step (2) Preparation of nanofiller layer:

[0087] 2.1. Mix silica sol and γ-methacryloxypropyltrimethoxysilane, stir for 6 hours, heat to 80°C, and keep warm for 100 minutes; centrifuge and dry to obtain modified silica sol; the mass ratio of silica sol to γ-methacryloxypropyltrimethoxysilane is 10:3.3;

[0088] 2.2. The modified silica sol, dodecafluoroheptyl methacrylate, and methyl methacrylate were mixed in N,N-dimethylacetamide, and an initiator was added to obtain a second slurry; the second slurry included the following mass components: 18 g / L silica sol, 5.0 g / L dodecafluoroheptyl methacrylate, 50 g / L methyl methacrylate, and 0.9 g / L initiator 2,2'-azobisisobutyronitrile;

[0089] The second slurry was coated on the surface of the modified polydopamine coating and irradiated with ultraviolet light for 150 min under nitrogen atmosphere with a light intensity of 500 W / cm 2 , heat treated at 80℃ for 6h to form a nano filler layer, obtain a nano coating, and obtain a nano waterproof membrane.

[0090] Comparative Example 2: A preparation process of a nano-waterproof film for automobiles, comprising the following processes:

[0091] Step (1), preparation of modified polydopamine coating:

[0092] 1.1. Sodium borate and deionized water were mixed, stirred under nitrogen atmosphere, and dopamine hydrochloride was added, and stirring was continued for 12 minutes; sodium carbonate was added, and methacryloyl chloride was added at 0°C, and stirring was continued for 10 minutes; the temperature was raised to 25°C, and the reaction was kept warm for 12 hours; concentrated hydrochloric acid was added to adjust the pH to 2, and the mixture was extracted with ethyl acetate, and the organic phase was dried over anhydrous magnesium sulfate, filtered, spin-dried, and vacuum-dried to obtain an olefin monomer; the ratio of sodium borate to deionized water was 3.8 g / 100 mL; the molar ratio of dopamine hydrochloride, methacryloyl chloride, sodium carbonate, and sodium borate was 1:1:1:1;

[0093] 1.2. The olefin monomer and dopamine hydrochloride are mixed in a buffer solution, zinc nitrate is added, and the mixture is stirred at 45°C for 12 hours; the mixture is cooled to room temperature to obtain a first slurry; the buffer solution is 10 mM Tris buffer solution, and the pH value is 8.5; the first slurry comprises the following mass components: 1.2 g / L olefin monomer, 0.4 g / L dopamine hydrochloride, and 0.3 g / L zinc nitrate;

[0094] The PET film is placed in the first slurry and immersed for 8 hours; taken out and dried at 60° C. for 24 hours to form a modified polydopamine coating to obtain a modified PET film;

[0095] Step (2) is the same as that in comparative example 1, forming a nano filler layer, obtaining a nano coating, and obtaining a nano waterproof membrane.

[0096] Comparative Example 3: A preparation process of a nano-waterproof film for automobiles, comprising the following processes:

[0097] Step (1), preparation of polydopamine coating:

[0098] 1.2. Mix dopamine hydrochloride and buffer to obtain a first slurry; the buffer is 10 mM Tris buffer, pH 8.5; the first slurry is 0.4 g / L dopamine hydrochloride;

[0099] The PET film is placed in the first slurry and immersed for 8 hours; taken out and dried at 60° C. for 24 hours to form a modified polydopamine coating to obtain a modified PET film;

[0100] Step (2) is the same as that in comparative example 1, forming a nano filler layer, obtaining a nano coating, and obtaining a nano waterproof membrane.

[0101] Experiment: Take the nano waterproof membranes obtained in Examples 1-3 and Comparative Examples 1-3, prepare samples, test their properties respectively and record the test results:

[0102] Waterproof performance test: Use a contact angle meter to measure the static contact angle of water on the nano waterproof membrane sample, with a water drop volume of 2μL;

[0103] The surface roughness of the samples was measured using an atomic force microscope.

[0104] Water resistance test: Soak the sample in distilled water for 14 days, take it out, dry the water, record the mass change of the sample before and after the experiment, and calculate its mass change rate as performance data;

[0105] Adhesion test: Using GB / T 9286 as the reference standard, the sample is gridded and the tape peeling test is performed to record the adhesion of the nano coating in the sample;

[0106] Mechanical properties test: Taking GB / T 1043 as the reference standard, a universal testing machine was used to test the tensile properties of the nano coating sample at a tensile rate of 10 mm / min, a test temperature of 15°C, and a relative humidity of 80%.

[0107]

[0108]

[0109] According to the data in the above table, we can clearly draw the following conclusions:

[0110] The nano waterproof membranes obtained in Examples 1-3 are compared with the nano waterproof membranes obtained in Comparative Examples 1-3. The test results show that:

[0111] Compared with the comparative example, the nano waterproof membrane obtained in Examples 1-3 has more excellent water static contact angle, roughness, tensile strength and adhesion grade data, and lower mass change rate data. This fully demonstrates that the present invention achieves the improvement of the hydrophobicity and water resistance of the nano waterproof membrane and the mechanical properties and adhesion of the nano coating.

[0112] Compared with Example 1, the second slurry of Comparative Example 1 replaces divinylbenzene with methyl methacrylate; compared with Comparative Example 1, the first slurry of Comparative Example 2 does not contain the terpyridine derivative component; the first slurry in Comparative Example 3 is a dopamine hydrochloride solution; the water static contact angle, roughness, tensile strength and adhesion grade data are reduced, and the quality change rate data is increased. It can be seen that the setting of the nano waterproof film preparation process and the components used in this application can promote the improvement of the hydrophobicity and water resistance of the nano waterproof film and the mechanical properties and adhesion of the nano coating.

[0113] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0114] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing a nano-waterproof film for automobiles, characterized in that: Including the following processes: Step (1), preparation of modified polydopamine coating: The terpyridine derivative and zinc nitrate are mixed in chloroform and methanol, and stirred at 45 to 55° C. for 8 to 12 hours to obtain a coordination compound; the terpyridine derivative and zinc nitrate are mixed in N,N-dimethylformamide and a buffer solution, and cooled to room temperature to obtain a first slurry; placing a PET film in the first slurry and immersing it for 8 to 12 hours; taking it out and drying it to form a modified polydopamine coating to obtain a modified PET film; Step (2) Preparation of nanofiller layer: Mixing silica sol, dodecafluoroheptyl methacrylate and divinylbenzene in N,N-dimethylacetamide, adding an initiator, and obtaining a second slurry; The second slurry is coated on the surface of the modified polydopamine coating, and under the protection of a nitrogen atmosphere, ultraviolet light is irradiated for 150 to 180 minutes with a light intensity of 500 μW / cm2, and heat-treated at 80 to 90°C for 6 to 8 hours to form a nanofiller layer to obtain a nano waterproof film.

2. The process for preparing a nano-waterproof film for automobiles according to claim 1, characterized in that: In the step (1), the first slurry includes the following mass components: 1.2-1.8 g / L olefinic monomer, 0.7-1.0 g / L terpyridine derivative, 0.4-0.6 g / L dopamine, and 0.3-0.5 g / L zinc nitrate.

3. The process for preparing a nano-waterproof film for automobiles according to claim 1, characterized in that: In the step (2), the second slurry includes the following components by mass: 18-33 g / L silica sol, 5.0-7.5 g / L dodecafluoroheptyl methacrylate, 50-75 g / L divinylbenzene, and 0.9-1.4 g / L initiator.

4. The process for preparing a nano-waterproof film for automobiles according to claim 2, characterized in that: The olefinic monomer is prepared by the following process: Mix sodium borate and deionized water, stir and add dopamine under nitrogen atmosphere, and continue stirring for 12 to 18 minutes; add sodium carbonate, add methacryloyl chloride at 0 to 5°C, and stir for 10 to 15 minutes; heat to 25 to 30°C, and keep warm for 8 to 12 hours; add concentrated hydrochloric acid to adjust the pH to 1 to 2, extract with ethyl acetate, dry the organic phase with anhydrous magnesium sulfate, filter, spin dry, and vacuum dry to obtain an olefin monomer.

5. The process for preparing a nano-waterproof film for automobiles according to claim 2, characterized in that: The terpyridine derivative is prepared by the following process: Mix anhydrous tetrahydrofuran and pyridine dicarboxylic acid, add N,N-dimethylformamide, slowly add thionyl chloride at 0-5°C, and add it within 15 minutes; heat to reflux temperature and react for 30-35 minutes; remove the solvent by distillation under reduced pressure to obtain pyridine dicarboxylic acid chloride; Mix pyridine dichloride, toluene and sodium carbonate, slowly add 4-amino-2,2,6,2-terpyridine at a temperature of 0 to 5°C, and add it within 60 minutes; heat to 25 to 30°C, and react at a constant temperature for 100 to 150 minutes; add dopamine, stir for 10 to 15 minutes; continue to react for 8 to 12 hours; separate the liquid to remove toluene, extract, add 2M hydrochloric acid to adjust the pH of the system to 1.8 to 2.1, stir at a temperature of 0 to 5°C, filter, wash the precipitate with water, and dry to obtain a terpyridine derivative.

6. The process for preparing a nano-waterproof film for automobiles according to claim 3, characterized in that: The silica sol is modified, and the modification process is as follows: The silica sol is mixed with γ-methacryloxypropyltrimethoxysilane, stirred for 6-8 hours, heated to 80-90° C., and kept warm for reaction for 100-150 minutes; centrifuged, and dried to obtain the modified silica sol.

7. The process for preparing a nano-waterproof film for automobiles according to claim 5, characterized in that: The molar ratio of the pyridine dicarboxylic acid to thionyl chloride is 1:(2.7-3.0).

8. The process for preparing a nano-waterproof film for automobiles according to claim 5, characterized in that: The mass ratio of the pyridine dichloride, 4-amino-2,2,6,2-terpyridine and dopamine is 10:(12.1-12.2):(9.3-10.1).

9. The process for preparing a nano-waterproof film for automobiles according to claim 4, characterized in that: The molar ratio of dopamine, methacryloyl chloride, sodium carbonate and sodium borate is 1:(1.0-1.1):(1.0-1.1):(1.0-1.1).