A pore-expanding solution for magnesium alloy surface treatment

By combining liquids A, B, C, and D to form a pore-expanding solution, the problem of excessive application of existing magnesium alloy pore-expanding solutions affecting the effect was solved, and the formation of nanoscale pores on the magnesium alloy surface and the controllability of pore-expanding efficiency were achieved.

CN118086905BActive Publication Date: 2026-11-17重庆博昶电子科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410126065.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2026-11-17
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

Existing magnesium alloy expansion solutions are mostly mixtures of acids or bases, which are prone to excessive application, affecting the expansion effect, and lack catalysts, resulting in slow expansion efficiency.

Method used

A pore-expanding solution is composed of solution A, solution B, solution C and solution D. Solution A contains water, sodium gluconate and porphyrin-modified glucose, solution B contains water, sodium chloride and sodium hypochlorite, solution C contains water, sodium hydroxide and hydrogen peroxide, and solution D contains water, sodium lactate and citric acid. The pore-expanding efficiency is controlled by mixing and under light conditions.

Benefits of technology

It achieves the formation of nanoscale pores on the surface of magnesium alloys, with good hole expansion effect, and the hole expansion efficiency can be adjusted as needed to avoid damage to the workpiece due to excessive chemical solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118086905B_ABST
    Figure CN118086905B_ABST
Patent Text Reader

Abstract

This invention relates to the field of magnesium alloy surface treatment technology, and discloses a pore-expanding solution for magnesium alloy surface treatment. The pore-expanding solution is composed of solution A, solution B, solution C, and solution D. Solution A includes water, sodium gluconate, and porphyrin-modified glucose; solution B includes water, sodium chloride, and sodium hypochlorite; solution C includes water, sodium hydroxide, and hydrogen peroxide; and solution D includes water, sodium lactate, and citric acid. Preferably, the mass ratio of solution A, solution B, solution C, and solution D is (5-6):(2-3):(1-2):(5-9). The pore-expanding solution of this invention, composed of solutions A, B, C, and D, can be used for pore-expanding treatment of magnesium alloy surfaces. After treatment, many nanoscale pores are formed on the magnesium alloy surface, exhibiting excellent pore-expanding effect. By using or stopping light exposure, the pore-expanding efficiency can be controlled, and damage to the workpiece due to excessive solution or excessively rapid pore-expanding efficiency can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of magnesium alloy surface treatment technology, specifically to a pore-expanding solution for magnesium alloy surface treatment. Background Technology

[0002] Surface treatment of magnesium alloys can improve their corrosion resistance, increase adhesion, and enhance their aesthetics. Below are some common surface treatment methods for magnesium alloys:

[0003] Electrolytic treatment: Electrolytic treatment is one of the commonly used methods for treating the surface of magnesium alloys. By performing anodizing or anodizing in a specific electrolyte, a dense oxide film or other chemical film can be formed, which improves the corrosion resistance and wear resistance of magnesium alloys.

[0004] Chemical treatment: Chemical treatment can employ methods such as pickling and acid-base polishing to remove oxides, impurities, and corrosion products from the magnesium alloy surface, resulting in a cleaner surface. Additionally, surface activation treatment using chemical solutions can increase the adhesion between the magnesium alloy and coatings or paints.

[0005] Mechanical treatment: Magnesium alloy surfaces can be treated by mechanical methods such as sandblasting, grinding, and polishing to remove surface dirt and oxide layers and obtain a smooth surface.

[0006] Coating treatment: Chromium, nickel, zinc, and other coatings can be applied to the surface of magnesium alloys to form a protective layer, improving the corrosion resistance and hardness of the magnesium alloys.

[0007] In the process of magnesium alloy surface treatment, pore-expanding solutions are often used to expand the pores on the surface of magnesium alloys. Most of the existing magnesium alloy pore-expanding solutions are mixtures of acids or bases. When expanding pores, these solutions are easy to be overused, which will affect the pore-expanding effect. Moreover, the mixtures of acids and bases lack catalysts, resulting in slow pore-expanding efficiency. Summary of the Invention

[0008] The purpose of this invention is to provide a pore-expanding solution for magnesium alloy surface treatment, in order to solve the problem that most existing magnesium alloy pore-expanding solutions are mixtures of acids or bases. When expanding pores, such solutions are prone to excessive dosage, which affects the pore-expanding effect. Moreover, the mixtures of acids and bases lack catalysts, resulting in slow pore-expanding efficiency.

[0009] To achieve the above objectives, the present invention provides the following technical solution: a pore-expanding solution for magnesium alloy surface treatment, wherein the pore-expanding solution is composed of solution A, solution B, solution C and solution D;

[0010] Solution A comprises water, sodium gluconate, and porphyrin-modified glucose;

[0011] Solution B includes water, sodium chloride, and sodium hypochlorite;

[0012] The C solution includes water, sodium hydroxide, and hydrogen peroxide;

[0013] The D solution comprises water, sodium lactate, and citric acid.

[0014] Preferably, the mass content ratio of liquid A, liquid B, liquid C and liquid D is (5-6):(2-3):(1-2):(5-9).

[0015] Preferably, the contents of each component in liquid A, by mass parts, are as follows:

[0016] 14-18 parts water, 2-5 parts sodium gluconate, and 4-6 parts porphyrin-modified glucose.

[0017] Preferably, the contents of each component in liquid B, by mass parts, are as follows:

[0018] 12-16 parts water, 2-4 parts sodium chloride, and 2-4 parts sodium hypochlorite.

[0019] Preferably, the content ratio of sodium chloride to sodium hypochlorite is 1:1.

[0020] Preferably, the contents of each component in liquid C, by mass parts, are as follows:

[0021] 9-12 parts water, 3-4 parts sodium hydroxide, and 1-2 parts hydrogen peroxide.

[0022] Preferably, the contents of each component in liquid D, by mass parts, are as follows:

[0023] 15-20 parts water, 4-5 parts sodium lactate, and 3-5 parts citric acid.

[0024] Preferably, the steps for modifying glucose with porphyrin are as follows:

[0025] Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde.

[0026] Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

[0027] Preferably, the preparation method of the pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 5 to 8 hours; then add solution D and mix and stir for 0.5 to 1.5 hours, and set aside.

[0028] The present invention has at least the following beneficial effects:

[0029] (1) The present invention provides a pore-expanding solution for magnesium alloy surface treatment. The pore-expanding solution is composed of liquid A, liquid B, liquid C and liquid D. It can be used for pore-expanding treatment of magnesium alloy surface. After treatment, many nano-sized pores are formed on the magnesium alloy surface, which has a good pore-expanding effect.

[0030] (2) The present invention provides a pore-expanding solution for magnesium alloy surface treatment. By modifying glucose with porphyrin, the pore-expanding efficiency can be controlled by using or stopping the light irradiation. In addition, it can avoid damage to the workpiece caused by excessive solution or excessively fast pore-expanding efficiency. Attached Figure Description

[0031] Figure 1 SEM scan of the surface of a magnesium alloy part before hole enlargement treatment;

[0032] Figure 2 This is a SEM scan image of the surface of a magnesium alloy part after hole enlargement treatment. Detailed Implementation

[0033] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] Example 1

[0035] A pore-expanding solution for surface treatment of magnesium alloys, comprising solution A, solution B, solution C and solution D;

[0036] Solution A consists of water, sodium gluconate, and porphyrin-modified glucose. By mass, the contents of each component in Solution A are as follows: 14 parts water, 2 parts sodium gluconate, and 4 parts porphyrin-modified glucose.

[0037] Solution B consists of water, sodium chloride, and sodium hypochlorite. By mass, the contents of each component in Solution B are as follows: water 12 parts, sodium chloride 2 parts, sodium hypochlorite 2 parts; the ratio of sodium chloride to sodium hypochlorite is 1:1.

[0038] Solution C consists of water, sodium hydroxide, and hydrogen peroxide; by mass, the content of each component in solution C is as follows: 9 parts water, 3 parts sodium hydroxide, and 1 part hydrogen peroxide.

[0039] Solution D contains water, sodium lactate, and citric acid. By mass, the content of each component in solution D is as follows: 15 parts water, 4 parts sodium lactate, and 3 parts citric acid.

[0040] The mass content ratio of liquid A, liquid B, liquid C and liquid D is 5:2:1:5.

[0041] The steps for porphyrin-modified glucose are as follows:

[0042] Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde.

[0043] Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

[0044] The preparation method of the above pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 5 hours; then add solution D and mix and stir for 0.5 hours, and set aside.

[0045] Example 2

[0046] A pore-expanding solution for surface treatment of magnesium alloys, comprising solution A, solution B, solution C and solution D;

[0047] Solution A consists of water, sodium gluconate, and porphyrin-modified glucose. By mass, the content of each component in Solution A is as follows: 15 parts water, 3 parts sodium gluconate, and 4.5 parts porphyrin-modified glucose.

[0048] Solution B consists of water, sodium chloride, and sodium hypochlorite. By mass, the content of each component in Solution B is as follows: water 13 parts, sodium chloride 2.5 parts, sodium hypochlorite 2.5 parts; the ratio of sodium chloride to sodium hypochlorite is 1:1.

[0049] Solution C consists of water, sodium hydroxide, and hydrogen peroxide; by mass, the content of each component in solution C is as follows: water 10 parts, sodium hydroxide 3.2 parts, hydrogen peroxide 1.4 parts;

[0050] Solution D consists of water, sodium lactate, and citric acid. By mass, the content of each component in solution D is as follows: water 16 parts, sodium lactate 4.2 parts, and citric acid 3.5 parts.

[0051] The mass content ratio of liquid A, liquid B, liquid C and liquid D is 5.2:2.1:1.4:6.

[0052] The steps for porphyrin-modified glucose are as follows:

[0053] Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde.

[0054] Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

[0055] The preparation method of the above pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 7 hours; then add solution D and mix and stir for 0.75 hours, and set aside.

[0056] Example 3

[0057] A pore-expanding solution for surface treatment of magnesium alloys, comprising solution A, solution B, solution C and solution D;

[0058] Solution A consists of water, sodium gluconate, and porphyrin-modified glucose. By mass, the contents of each component in Solution A are as follows: 15 parts water, 3.5 parts sodium gluconate, and 5 parts porphyrin-modified glucose.

[0059] Solution B consists of water, sodium chloride, and sodium hypochlorite. By mass, the contents of each component in Solution B are as follows: water 15 parts, sodium chloride 3 parts, sodium hypochlorite 3 parts; the ratio of sodium chloride to sodium hypochlorite is 1:1.

[0060] Solution C consists of water, sodium hydroxide, and hydrogen peroxide; by mass, the content of each component in solution C is as follows: water 11 parts, sodium hydroxide 3.6 parts, hydrogen peroxide 1.3 parts;

[0061] Solution D consists of water, sodium lactate, and citric acid. By mass, the content of each component in solution D is as follows: water 17 parts, sodium lactate 4.4 parts, and citric acid 3.9 parts.

[0062] The mass content ratio of liquid A, liquid B, liquid C and liquid D is 5.3:2.5:1.6:7.

[0063] The steps for porphyrin-modified glucose are as follows:

[0064] Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde.

[0065] Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

[0066] The preparation method of the above pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 6 hours; then add solution D and mix and stir for 1 hour, then set aside.

[0067] Example 4

[0068] A pore-expanding solution for surface treatment of magnesium alloys, comprising solution A, solution B, solution C and solution D;

[0069] Solution A consists of water, sodium gluconate, and porphyrin-modified glucose. By mass, the contents of each component in Solution A are as follows: water 17 parts, sodium gluconate 4 parts, and porphyrin-modified glucose 5.5 parts.

[0070] Solution B consists of water, sodium chloride, and sodium hypochlorite. By mass, the content of each component in Solution B is as follows: water 15 parts, sodium chloride 3.2 parts, sodium hypochlorite 3.2 parts; the ratio of sodium chloride to sodium hypochlorite is 1:1.

[0071] Solution C consists of water, sodium hydroxide, and hydrogen peroxide; by mass, the content of each component in solution C is as follows: water 11 parts, sodium hydroxide 3.5 parts, hydrogen peroxide 1.8 parts;

[0072] Solution D consists of water, sodium lactate, and citric acid. By mass, the content of each component in solution D is as follows: water 18 parts, sodium lactate 4.6 parts, and citric acid 4.5 parts.

[0073] The mass content ratio of liquid A, liquid B, liquid C and liquid D is 5.7:2.2:1.6:8.

[0074] The steps for porphyrin-modified glucose are as follows:

[0075] Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde.

[0076] Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

[0077] The preparation method of the above pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 7.5 hours; then add solution D and mix and stir for 1.25 hours, and set aside.

[0078] Example 5

[0079] A pore-expanding solution for surface treatment of magnesium alloys, comprising solution A, solution B, solution C and solution D;

[0080] Solution A consists of water, sodium gluconate, and porphyrin-modified glucose. By mass, the contents of each component in Solution A are as follows: 18 parts water, 5 parts sodium gluconate, and 6 parts porphyrin-modified glucose.

[0081] Solution B consists of water, sodium chloride, and sodium hypochlorite. By mass, the contents of each component in Solution B are as follows: 16 parts water, 4 parts sodium chloride, and 4 parts sodium hypochlorite; the ratio of sodium chloride to sodium hypochlorite is 1:1.

[0082] Solution C consists of water, sodium hydroxide, and hydrogen peroxide; by mass, the content of each component in solution C is as follows: water 12 parts, sodium hydroxide 4 parts, hydrogen peroxide 2 parts;

[0083] Solution D contains water, sodium lactate, and citric acid. By mass, the content of each component in solution D is as follows: 20 parts water, 5 parts sodium lactate, and 5 parts citric acid.

[0084] The mass content ratio of liquid A, liquid B, liquid C and liquid D is 6:3:2:9.

[0085] The steps for porphyrin-modified glucose are as follows:

[0086] Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde.

[0087] Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

[0088] The preparation method of the above pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 8 hours; then add solution D and mix and stir for 1.5 hours, and set aside.

[0089] In this invention, by mixing solutions A, B, and C, porphyrin-modified glucose in an environment of sodium hydroxide, sodium chloride, and sodium hypochlorite will form porphyrin-modified sodium gluconate. When mixed with solution D, it can be used for pore enlargement. The pore enlargement tank can be irradiated as needed. Under irradiation, porphyrin-modified sodium gluconate will increase the acidity of the solution, thereby improving the pore enlargement efficiency. Moreover, porphyrin combined with hydrogen peroxide has a catalytic effect, which can further improve the pore enlargement efficiency. When the pore enlargement process is nearing completion, the irradiation can be stopped. Under no-light conditions, porphyrin-modified sodium gluconate tends to a stable state. At this time, the acidity of the solution decreases, the pore enlargement efficiency decreases, and thus no excessive damage is caused to the magnesium alloy.

[0090] The product prepared in Example 5 above was used in a magnesium alloy hole expansion test, and the results were as follows: Figure 1-2 As shown, it can be clearly seen that many nanoscale pores are formed on the surface of the magnesium alloy after treatment. The product of this invention has a very good pore-expanding effect on the surface treatment of magnesium alloy.

[0091] In summary, the hole-expanding solution provided by this invention can be used for hole-expanding treatment on magnesium alloy surfaces and has a good hole-expanding effect. In addition, the hole-expanding efficiency can be adjusted according to the use or cessation of light irradiation, and the workpiece can be avoided from being damaged by excessive solution or excessively fast hole-expanding efficiency.

[0092] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or basic characteristics. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

[0093] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A pore-expanding solution for surface treatment of magnesium alloys, characterized in that, The pore-expanding solution consists of solution A, solution B, solution C, and solution D; Solution A comprises water, sodium gluconate, and porphyrin-modified glucose; Solution B includes water, sodium chloride, and sodium hypochlorite; The C solution includes water, sodium hydroxide, and hydrogen peroxide; The D solution includes water, sodium lactate, and citric acid; The mass content ratio of the solutions A, B, C, and D is (5-6):(2-3):(1-2):(5-9); The contents of each component in solution A, by mass parts, are as follows: 14-18 parts water, 2-5 parts sodium gluconate, 4-6 parts porphyrin-modified glucose; The contents of each component in solution B, by mass parts, are as follows: 12-16 parts water, 2-4 parts sodium chloride, and 2-4 parts sodium hypochlorite; the ratio of sodium chloride to sodium hypochlorite is 1:

1. The contents of each component in liquid C, by mass parts, are as follows: 9-12 parts water, 3-4 parts sodium hydroxide, 1-2 parts hydrogen peroxide; The contents of each component in liquid D, by mass parts, are as follows: 15-20 parts water, 4-5 parts sodium lactate, and 3-5 parts citric acid.

2. The pore-expanding solution for magnesium alloy surface treatment according to claim 1, characterized in that, The steps for modifying glucose with porphyrin are as follows: Step (1): Take β-D-pentaacetyl glucose and carry out bromination reaction; then react it with p-hydroxybenzaldehyde. Step (2) involves reacting the reactants from step (1) with pyrrole, and then with glucose, benzaldehyde, and methylene dipyrrole to obtain porphyrin-modified glucose.

3. The pore-expanding solution for magnesium alloy surface treatment according to claim 1, characterized in that, The preparation method of the pore-expanding solution is as follows: first, mix solution A, solution B and solution C and stir for 5 to 8 hours; then add solution D and mix and stir for 0.5 to 1.5 hours, and set aside.

Citation Information

Patent Citations

  • Method for improving corrosion resistance of aluminum alloy part in grain machinery

    CN112176332A

  • Magnesium alloy with porous surface and preparation method of magnesium alloy

    CN112877697A