A method for preparing large-particle basic cobalt carbonate
By using a magnetic diaphragm pump and ammonium fluoroborate in the preparation process of cobalt carbonate to control the reaction conditions, the problem of loose accumulation caused by the small particle size of cobalt carbonate was solved, the preparation of large particle size and dense cobalt carbonate was achieved, and the stability of the product was improved. sex and consistency.
Patent Information
- Application Number
- CN202410327187.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-21
AI Technical Summary
The existing cobalt carbonate has a small particle size, which results in loose accumulation, increases processing difficulty, and affects the consistency and stability of the product.
Using a large particle size basic cobalt carbonate preparation method, a solution containing cobalt and ammonium bicarbonate is prepared, and a magnetic diaphragm pump is used to transport the solution into the reaction kettle in parallel flow. The reaction is controlled at a temperature, and ammonium fluoroborate is added to promote particle chimerization and Crystal growth, control the stirring speed and pH value, and obtain large particle size and dense cobalt carbonate.
The preparation of cobalt carbonate with large particle size and excellent tap density is achieved, which improves the dense accumulation and purity of the product, reduces the entry of impurities, and improves the stability and consistency of the preparation process.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery materials, and particularly relates to a method for preparing large-particle-size basic cobalt carbonate. Background Art
[0002] With the rapid development of the 3C market, the demand and quality requirements of cobalt tetroxide, as one of the key materials, are also rising. In this context, cobalt carbonate, as an important precursor of cobalt tetroxide, plays a vital role in the performance of cobalt tetroxide in terms of its properties and indicators. Cobalt carbonate is usually manufactured by a two-stage calcination method, which has defects such as low equipment utilization and increased labor costs, and the particle size of the cobalt carbonate obtained is small. When the particle size of cobalt carbonate is less than 10μm, the particles cannot be effectively stacked, resulting in loose stacking. This loose stacking state easily leads to slippage, dispersion and diffusion between particles, which increases the difficulty of processing and challenges the consistency and stability of the product. Summary of the invention
[0003] The invention discloses a method for preparing large-particle basic cobalt carbonate, which belongs to the technical field of lithium ion battery materials. The preparation of the large-particle basic cobalt carbonate comprises the following steps: preparing a cobalt-containing solution A; preparing a solution B containing ammonium bicarbonate; preparing a base liquid; using a magnetic diaphragm pump to transport solution A and solution B to a reactor for temperature control reaction under stirring to obtain material C; adding ammonium fluoroborate to the reactor under stirring to obtain material D; continuing to use a magnetic diaphragm pump to transport solution A and solution B to the reactor under stirring, keeping the pH in the reactor at 7.2-7.3, and reacting at a controlled temperature until the average particle size of the slurry in the reactor is 10-12 μm; controlling the stirring speed of the slurry in the reactor to reduce by 10-15 rpm per hour until the reaction is completed, filtering, washing the solid phase, and drying to obtain basic cobalt carbonate with excellent tap density and large particle size.
[0004] The technical problem to be solved by the present invention is to produce basic cobalt carbonate with excellent tap density and large particle size.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing large-particle-size basic cobalt carbonate, the preparation of the large-particle-size basic cobalt carbonate comprising the following steps:
[0007] S1. preparing a cobalt-containing solution A;
[0008] S2, preparing solution B containing ammonium bicarbonate;
[0009] S3, adding deionized water and solution B into the reaction kettle, mixing, and obtaining a base solution;
[0010] S4, maintaining uniform stirring, using a magnetic diaphragm pump to transport solution A and solution B in parallel to a reactor containing the base liquid for temperature-controlled reaction, to obtain material C;
[0011] S5, keeping the stirring speed in step S4 unchanged, adding ammonium fluoroborate to the reactor containing material C, mixing and stirring evenly to obtain material D;
[0012] S6, keeping the stirring speed in step S4 unchanged, continue to use the magnetic diaphragm pump to transport solution A and solution B in parallel to the reactor containing the material D, keep the pH in the reactor at 7.2-7.3, and control the temperature to react until the average particle size of the slurry in the reactor is greater than 10 μm;
[0013] S7, then controlling the stirring speed of the slurry in the reactor to decrease by 10-15 rpm per hour until the reaction is completed, filtering, washing and drying the solid phase to obtain the large-particle-size basic cobalt carbonate.
[0014] As a preferred technical solution of the present invention, in step S1, the cobalt content in the solution A is 108-112 g / L.
[0015] As a preferred technical solution of the present invention, in step S2, the mass fraction of ammonium bicarbonate in the solution B is 18-22%.
[0016] As a preferred technical solution of the present invention, in step S3, the volume ratio of the deionized water to the solution B is 80-100:5-8.
[0017] As a preferred technical solution of the present invention, in step S4, the rotation speed of the uniform stirring is 1200-1500 rpm.
[0018] As a preferred technical solution of the present invention, in step S4, the feeding rate of solution A is 250-260 mL / h, the feeding rate of solution B is 700-720 mL / h, and the feeding time is 70-90 h.
[0019] As a preferred technical solution of the present invention, in step S4, the reaction temperature of the temperature-controlled reaction is 45-55°C.
[0020] As a preferred technical solution of the present invention, in step S5, the mass ratio of the material C to ammonium fluoroborate is 1.2-1.5:4-6.
[0021] As a preferred technical solution of the present invention, in step S6, the reaction temperature of the temperature-controlled reaction is 60-70°C.
[0022] As a preferred technical solution of the present invention, in step S7, the time from when the stirring speed starts to decrease to when the reaction ends is 45-55 hours.
[0023] Beneficial effects of the present invention:
[0024] The invention discloses a method for preparing large-particle-size basic cobalt carbonate. In the initial growth stage of cobalt carbonate crystals, ammonium fluoroborate is added to be adsorbed on the cobalt carbonate crystal surface to form an intercalation site matching the cobalt carbonate crystal surface lattice, thereby promoting the particles to be intercalated in the crystal to form dense stacking, and guiding the crystal growth direction at the same time, so that the particles are arranged in order in the crystal and connected to each other to form cobalt carbonate with a large particle size and a dense stacking structure; in addition, the dense stacking can also limit the entry of other impurity molecules, reduce adverse effects in the crystal growth process, facilitate the formation of pure cobalt carbonate crystals, and improve the tap density of the prepared cobalt carbonate crystals. DETAILED DESCRIPTION
[0025] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0026] Example 1
[0027] A method for preparing large-particle-size basic cobalt carbonate comprises the following steps:
[0028] S1. Dissolve 1030.3 g of cobalt sulfate (heptahydrate) in deionized water and adjust the volume to 2000 mL to obtain a solution A with a cobalt content of 108 g / L;
[0029] S2, dissolving 1053.7 g of ammonium bicarbonate in 4800 mL of deionized water to obtain a solution B having a mass fraction of ammonium bicarbonate of 18%;
[0030] S3, add 800 mL of deionized water and 50 mL of solution B into the reactor, mix well, and obtain a base solution;
[0031] S4, keep the stirring paddle in the reactor stirring at a speed of 1200rpm, use a magnetic diaphragm pump to deliver solution A and solution B to the reactor containing the bottom liquid in parallel, the feeding rate of solution A is 250mL / h, the feeding rate of solution B is 700mL / h, the reaction is carried out at 45°C, the feeding time is 70h, and the feeding is completed to obtain material C;
[0032] S5, keeping the stirring speed in step S4 unchanged, adding ammonium fluoroborate to the reactor containing material C, mixing and stirring evenly to obtain material D, wherein the mass ratio of material C to ammonium fluoroborate is 1.2:4;
[0033] S6, keeping the stirring speed in step S4 unchanged, continue to use the magnetic diaphragm pump to deliver solution A and solution B to the reactor containing the material D in parallel, adjust the feeding speed of solution A and solution B so that the pH in the reactor is 7.2, and react at 60° C. until the average particle size of the slurry in the reactor is 12 μm;
[0034] S7, then control the stirring speed of the slurry in the reactor to decrease by 10 rpm per hour until the reaction is completed when the stirring speed reaches 750 rpm, filter, take the solid phase for washing, and dry to obtain a solid with an average particle size of 22 μm and a tap density of 2.83 g / cm 3 of basic cobalt carbonate.
[0035] Example 2
[0036] A method for preparing large-particle-size basic cobalt carbonate comprises the following steps:
[0037] S1. Dissolve 1048.6 g of cobalt sulfate (heptahydrate) in deionized water and adjust the volume to 2000 mL to obtain a solution A with a cobalt content of 110 g / L;
[0038] S2, dissolving 1200 g of ammonium bicarbonate in 4800 mL of deionized water to obtain a solution B having a mass fraction of ammonium bicarbonate of 20%;
[0039] S3, add 900 mL of deionized water and 65 mL of solution B into the reactor, mix well, and obtain a base solution;
[0040] S4, keep the stirring paddle in the reactor stirring at a speed of 1350rpm, use a magnetic diaphragm pump to deliver solution A and solution B to the reactor containing the bottom liquid in parallel, the feeding rate of solution A is 255mL / h, the feeding rate of solution B is 710mL / h, the reaction is carried out at 50°C, the feeding time is 80h, and the feeding is completed to obtain material C;
[0041] S5, keeping the stirring speed in step S4 unchanged, adding ammonium fluoroborate to the reactor containing material C, mixing and stirring evenly to obtain material D, wherein the mass ratio of material C to ammonium fluoroborate is 1.35:5;
[0042] S6, keeping the stirring speed in step S4 unchanged, continue to use the magnetic diaphragm pump to deliver solution A and solution B to the reactor containing the material D in parallel, adjust the feeding speed of solution A and solution B so that the pH in the reactor is 7.25, and react at 65° C. until the average particle size of the slurry in the reactor is 13 μm;
[0043] S7, then control the stirring speed of the slurry in the reactor to decrease by 12 rpm per hour until the reaction is completed when the stirring speed reaches 738 rpm, filter, take the solid phase for washing, and dry to obtain a slurry with an average particle size of 24 μm and a tap density of 2.85 g / cm 3 of basic cobalt carbonate.
[0044] Example 3
[0045] A method for preparing large-particle-size basic cobalt carbonate comprises the following steps:
[0046] S1. Dissolve 1068.4 g of cobalt sulfate (heptahydrate) in deionized water and adjust the volume to 2000 mL to obtain a solution A having a cobalt content of 112 g / L;
[0047] S2, dissolving 1353.8 g of ammonium bicarbonate in 4800 mL of deionized water to obtain a solution B having a mass fraction of 22% ammonium bicarbonate;
[0048] S3, add 1000mL of deionized water and 80mL of solution B into the reactor, mix well, and obtain a base solution;
[0049] S4, keep the stirring paddle in the reactor stirring at a speed of 1500rpm, use a magnetic diaphragm pump to deliver solution A and solution B to the reactor containing the bottom liquid in parallel, the feeding rate of solution A is 260mL / h, the feeding rate of solution B is 720mL / h, the reaction is carried out at 55°C, the feeding time is 90h, and the feeding is completed to obtain material C;
[0050] S5, keeping the stirring speed in step S4 unchanged, adding ammonium fluoroborate to the reactor containing material C, mixing and stirring evenly to obtain material D, wherein the mass ratio of material C to ammonium fluoroborate is 1.5:6;
[0051] S6, keeping the stirring speed in step S4 unchanged, continue to use the magnetic diaphragm pump to deliver solution A and solution B to the reactor containing the material D in parallel, adjust the feeding speed of solution A and solution B so that the pH in the reactor is 7.3, and react at 70° C. until the average particle size of the slurry in the reactor is 14 μm;
[0052] S7, then control the stirring speed of the slurry in the reactor to decrease by 15 rpm per hour until the reaction is completed when the stirring speed reaches 675 rpm, filter, take the solid phase for washing, and dry to obtain a solid with an average particle size of 26 μm and a tap density of 2.86 g / cm 3 of basic cobalt carbonate.
[0053] Comparative Example 1
[0054] The difference from Example 1 is that ammonium fluoroborate is not added in step S5, and the other operations remain unchanged, and the average particle size is 20.8 μm and the tap density is 2.18 g / cm 3 of basic cobalt carbonate.
[0055] Comparative Example 2
[0056] The difference from Example 1 is that in step S7, the stirring speed of the slurry in the reactor is controlled to decrease from 1200 rpm to 750 rpm within 10 s, and the stirring is continued for 45 h until the reaction is completed. The other operations remain unchanged, and the average particle size is 20.2 μm and the tap density is 2.55 g / cm 3 of basic cobalt carbonate.
[0057] Comparative Example 3
[0058] The difference from Example 1 is that the reaction temperature in step S6 is 35°C, and the other operations remain unchanged, and the average particle size is 12.3 μm and the tap density is 2.78 g / cm 3 of basic cobalt carbonate.
[0059] Comparative Example 4
[0060] The difference from Example 1 is that the reaction temperature in step S6 is 45°C, and the other operations remain unchanged, and the average particle size is 13.5 μm and the tap density is 2.79 g / cm 3 of basic cobalt carbonate.
[0061] Comparative Example 5
[0062] The difference from Example 1 is that the reaction temperature in step S6 is 55°C, and the other operations remain unchanged, and the average particle size is 14.4 μm and the tap density is 2.81 g / cm 3 of basic cobalt carbonate.
[0063] Comparative Example 6
[0064] The difference from Example 1 is that the reaction temperature in step S6 is 75°C, and the other operations remain unchanged, and the average particle size is 28.2 μm and the tap density is 2.26 g / cm 3 of basic cobalt carbonate.
[0065] Comparative Example 7
[0066] The difference from Example 1 is that the reaction temperature in step S6 is 80°C, and the other operations remain unchanged, and the average particle size is 29.3 μm and the tap density is 2.21 g / cm 3 of basic cobalt carbonate.
[0067] Comparative Example 8
[0068] The difference from Example 1 is that the reaction temperature in step S6 is 85°C, and the other operations remain unchanged, and the average particle size is 30.2 μm and the tap density is 2.19 g / cm 3 of basic cobalt carbonate.
[0069] Comparative Example 9
[0070] The difference from Example 1 is that the reaction temperature in step S4 is 35°C, and the other operations remain unchanged, and the average particle size is 12.5 μm and the tap density is 2.04 g / cm 3 of basic cobalt carbonate.
[0071] Comparative Example 10
[0072] The difference from Example 1 is that the reaction temperature in step S4 is 40°C, and the other operations remain unchanged, and the average particle size is 16.7 μm and the tap density is 2.43 g / cm 3 of basic cobalt carbonate.
[0073] Comparative Example 11
[0074] The difference from Example 1 is that the reaction temperature in step S4 is 60°C, and the other operations remain unchanged, and the average particle size is 18.1 μm and the tap density is 2.48 g / cm 3 of basic cobalt carbonate.
[0075] Comparative Example 12
[0076] The difference from Example 1 is that the reaction temperature in step S4 is 65°C, and the other operations remain unchanged, and the average particle size is 17.3 μm and the tap density is 2.46 g / cm 3 of basic cobalt carbonate.
[0077] Comparative Example 13
[0078] The difference from Example 1 is that in step S6, the average particle size of the slurry in the reactor is 8 μm, and the other operations remain unchanged, and the average particle size is 10.5 μm and the tap density is 1.93 g / cm 3 of basic cobalt carbonate.
[0079] Comparative Example 14
[0080] The difference from Example 1 is that in step S6, the average particle size of the slurry in the reactor is 6 μm, and the other operations remain unchanged, and the average particle size is 9.4 μm and the tap density is 1.88 g / cm 3 of basic cobalt carbonate.
[0081] Results and Discussion
[0082] The basic cobalt carbonate prepared in Examples 1-3 has a larger particle size and excellent tap density;
[0083] In the preparation process of the basic cobalt carbonate prepared in Comparative Example 1, the cobalt carbonate crystals prepared in the primary reaction were used as a substrate without the addition of ammonium fluoroborate, resulting in the inability of the particles in the system to be effectively embedded and accumulated on the cobalt carbonate crystal substrate during the secondary reaction, resulting in a significant decrease in the tap density of the basic cobalt carbonate prepared;
[0084] In the preparation process of the basic cobalt carbonate prepared in Comparative Example 2, the stirring speed was not adjusted step by step, resulting in a decrease in the tap density of the basic cobalt carbonate prepared;
[0085] In the preparation process of the basic cobalt carbonate prepared in Comparative Examples 3-8, the temperature of the secondary reaction is too low, which is not conducive to the growth of cobalt carbonate crystals. Although the temperature of the secondary reaction is too high, it will promote the growth of cobalt carbonate crystals and increase the average particle size. However, the high temperature will make ammonium fluoroborate unable to stably and firmly adhere to the surface of the cobalt carbonate crystal substrate, resulting in a significant decrease in the tap density of the basic cobalt carbonate prepared;
[0086] In the preparation process of the basic cobalt carbonate prepared in Comparative Examples 9-12, if the reaction temperature is too low or too high during the initial reaction to obtain the cobalt carbonate crystals, the cobalt carbonate crystals will grow slowly and have a low tap density;
[0087] During the preparation process of the basic cobalt carbonate prepared in Comparative Examples 13-14, the cobalt carbonate crystals obtained by the initial reaction have low crystallinity, which leads to slow crystal growth, small and irregular particle size, and low tap density.
[0088] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing large-particle basic cobalt carbonate, characterized in that: The preparation of the large-particle-size basic cobalt carbonate comprises the following steps: S1. preparing a cobalt-containing solution A; S2, preparing solution B containing ammonium bicarbonate; S3, adding deionized water and solution B into the reaction kettle, mixing, and obtaining a base solution; S4, maintaining uniform stirring, using a magnetic diaphragm pump to transport solution A and solution B in parallel to a reactor containing the base liquid for temperature-controlled reaction, to obtain material C; S5, keeping the stirring speed in step S4 unchanged, adding ammonium fluoroborate to the reactor containing material C, mixing and stirring evenly to obtain material D; S6, keeping the stirring speed in step S4 unchanged, continue to use the magnetic diaphragm pump to transport solution A and solution B in parallel to the reactor containing the material D, keep the pH in the reactor at 7.2-7.3, and control the temperature to react until the average particle size of the slurry in the reactor is greater than 10 μm; S7, then controlling the stirring speed of the slurry in the reactor to decrease by 10-15 rpm per hour until the reaction is completed, filtering, washing and drying the solid phase to obtain the large-particle basic cobalt carbonate; In step S2, the mass fraction of ammonium bicarbonate in the solution B is 18-22%; In step S5, the mass ratio of material C to ammonium fluoroborate is 1.2-1.5:4-6.
2. The method for preparing large-particle-size basic cobalt carbonate according to claim 1, characterized in that: In step S1, the cobalt content in the solution A is 108-112 g / L.
3. The method for preparing large-particle-size basic cobalt carbonate according to claim 1, characterized in that: In step S3, the volume ratio of the deionized water to the solution B is 80-100:5-8.
4. The method for preparing large-particle-size basic cobalt carbonate according to claim 1, characterized in that: In step S4, the rotation speed of the uniform stirring is 1200-1500 rpm.
5. The method for preparing large-particle-size basic cobalt carbonate according to claim 1, characterized in that: In step S4, the feeding rate of solution A is 250-260 mL / h, the feeding rate of solution B is 700-720 mL / h, and the feeding time is 70-90 h.
6. The method for preparing large-particle-size basic cobalt carbonate according to claim 1, characterized in that: In step S4, the reaction temperature of the temperature-controlled reaction is 45-55°C.
7. The method for preparing large-particle basic cobalt carbonate according to claim 1, characterized in that: In step S6, the reaction temperature of the temperature-controlled reaction is 60-70°C.
8. The method for preparing large-particle-size basic cobalt carbonate according to claim 1, characterized in that: In step S7, the time from when the stirring speed starts to decrease to when the reaction ends is 45-55 hours.
Citation Information
Patent Citations
Method for preparing low-anion residual basic cobalt carbonate
CN103351030A
Preparation method of nano cobaltosic oxide / nitrogen-doped three-dimensional porous carbon skeleton composite material for supercapacitor
CN111261431A
Preparation method of magnesium-aluminum co-doped lithium cobalt oxide precursor
CN114349066A