A Fe-Mn-Si based memory alloy material and preparation method and application thereof
By introducing Cu element into Fe-Mn-Si-based shape memory alloy and using MA+SPS technology, the problems of composition inhomogeneity and insufficient corrosion resistance of Fe-Mn-Si-based alloy in traditional metallurgical processes are solved, significantly improving Its shape memory performance and corrosion resistance are improved.
Patent Information
- Application Number
- CN202410536726.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-30
AI Technical Summary
Fe-Mn-Si-based shape memory alloys have problems with composition inhomogeneity, element loss, cracks and insufficient corrosion resistance in traditional metallurgical processes, which limits their wide application.
Cu element is introduced, and mechanical alloying (MA) and spark plasma sintering (SPS) technologies are used to prepare Fe-Mn-Si-based memory alloy materials. Through ball milling and pre-pressing molding, a high-density structure is formed to improve shape memory performance and durability. corrosive.
The shape memory performance, hardness and superelasticity of the Fe-Mn-Si based memory alloy are significantly improved, and its corrosion resistance is enhanced, solving the problems of insufficient composition uniformity and corrosion resistance in the traditional process.
Smart Images

Figure BDA0004819813340000011 
Figure BDA0004819813340000021 
Figure BDA0004819813340000041
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal materials, and in particular to a Fe-Mn-Si based memory alloy material and a preparation method and application thereof. Background Art
[0002] With the advancement of science and technology, the research and application of structural materials and functional materials have received increasing attention, and shape memory alloys are considered to be one of the most functional materials. Shape memory alloy (SMA) has shape memory effect (SME) and superelasticity (SE). It is an intelligent functional material with wide applications in driving, energy conversion, aerospace, robotics, civil construction, damping and micro-electromechanical systems, biomedicine and other fields. Ni-Ti-based SMAs have excellent SME, that is, a large recovery strain of about 8%, but their poor cold working performance and high processing cost limit their wide application. Fe-Mn-Si-based SMAs have the advantages of low cost, good mechanical properties, excellent processing performance, and high corrosion resistance, and have become a perfect substitute for Ni-Ti-based SMAs to a certain extent. The memory effect of Fe-Mn-Si-based SMAs is achieved through stress-induced martensitic phase transformation and its reverse phase transformation.
[0003] Generally speaking, Fe-Mn-Si based SMAs are produced by melting and casting in a high vacuum (or air) environment and then using thermomechanical processing. However, this process method is difficult to maintain the uniformity of the various components in Fe-Mn-Si based SMAs, and some elements are easily lost during heat treatment or smelting, cracks are easily generated during solidification or quenching, and some elements are incompletely dissolved in the melt, etc., which are inherent defects of the traditional steel ingot metallurgical route. Summary of the invention
[0004] In view of the above problems, the present invention provides a Fe-Mn-Si based memory alloy material. The Fe-Mn-Si based memory alloy material introduces Cu into the formula and adopts the MA+SPS preparation method to make it have good shape memory performance and high corrosion resistance, as well as better hardness and superelasticity.
[0005] In order to achieve the above object, the present invention provides a Fe-Mn-Si based memory alloy material, which is mainly prepared from the following raw materials in parts by weight:
[0006]
[0007] The preparation method of the Fe-Mn-Si based memory alloy material comprises the following steps: mixing raw materials, ball milling to obtain mixed powder, pre-pressing the mixed powder into a shape, and performing spark plasma sintering to obtain the material.
[0008] Since iron-based SMAs are widely used in disposable connectors, such as pipe joints or rail connection plates, and their working environment is exposed to air or humid conditions for a long time, corrosion resistance can also become an important indicator to measure whether the performance of this material is excellent. In Fe-Mn-Si-based SMAs, the type and ratio of alloying elements have an important influence on their shape memory properties, mechanical properties and corrosion resistance. In previous studies, it was found that when 0.047% N was added, the SME of Fe-30Mn-6Si alloy was slightly improved, but when 0.26% N was added to the SME of Fe-18Mn-13Cr-2Ni-5Si alloy, the SME was reduced by 80%. At the same time, the addition of Mn elements can significantly reduce the stacking fault energy of the alloy, strengthen the intergranular bonding of the alloy, and thus improve the strength of the alloy. However, when excessive Mn elements are added, banded structures will appear in the alloy, reducing its mechanical properties and shape memory properties; the addition of Si elements can regulate the segregation of Mn elements in the alloy and improve the memory properties of the alloy. In the early stage, some researchers added Cu element to Fe-Mn-Si based SMAs and found that it can reduce the Cl -The corrosion rate in solution is increased, but the effect on SME of Fe-Mn-Si based alloys is not obvious. For this, the inventor speculates that it should be because the electronegativity of the Cu element is higher than that of the Fe / Mn / Si / Cr element, and the ability of the Cu atom to attract electrons in the compound is stronger than that of the Fe / Mn / Si / Cr, and oxidation reaction is more likely to occur in electrochemical corrosion. Therefore, after adding the Cu element to the Ni element with equivalent electronegativity, the alloy is more likely to undergo oxidation reaction in the NaCl electrolyte to produce Cu2O and Cu2(OH)3Cl, forming a passivation film on the surface of the alloy to hinder further corrosion of the alloy. Based on this, the inventor further studied the addition of Cu to the Fe-Mn-Si based memory alloy material, and proposed the above raw material formula and preparation method to be used in combination. In the case of iron, manganese, silicon, chromium, nickel and copper as raw materials, mechanical alloying + spark plasma sintering (MA+SPS) is used to prepare the memory alloy material. Compared with the traditional sintering method, spark plasma sintering (SPS) can consolidate the metal powder at a relatively low temperature and in a shorter time to form a high-density organization with finer grains. Mechanical alloying (MA) can effectively reduce the particle size of the powder mixture, so that the alloy powder can be synthesized into a saturated solid solution before sintering, so as to promote the diffusion and phase change of elements in the subsequent sintering process, which is beneficial to the shape recovery performance of the alloy. At the same time, mechanical alloying can reduce the probability of pores in the alloy, improve the density of the alloy, and increase the hardness and yield strength of the alloy.
[0009] In one embodiment, the Fe-Mn-Si based memory alloy material is mainly prepared from the following raw materials in parts by weight:
[0010]
[0011] In one embodiment, the raw material is a single metal powder, the particle size of manganese is ≤45 μm, and the particle size of iron, silicon, chromium, nickel, and copper is ≤30 μm.
[0012] Compared with Fe-Mn-Si SMAs prepared by vacuum melting, Fe-Mn-Si SMAs prepared by powder metallurgy (PM) using single metal powder as raw material solves the disadvantage of incomplete solid solution of Mn and Si elements.
[0013] The invention also provides a method for preparing the Fe-Mn-Si based memory alloy material, comprising the following steps: mixing raw materials, ball milling to obtain mixed powder, pre-pressing the mixed powder into a shape, and performing spark plasma sintering to obtain the material.
[0014] In one embodiment, the ball-to-material mass ratio of the ball mill is (8-12):1, the rotation speed of the ball mill is 400-600 r / min, and the ball milling time is 45-55 h.
[0015] In one embodiment, the ball milling step further includes adding a process control agent every 8-12 hours, and the amount of the process control agent is: 0.1-0.25 mL of the process control agent is added for every 10 g of the total mass of the raw materials.
[0016] In one embodiment, the process control agent includes ethanol.
[0017] In one embodiment, the spark plasma sintering includes: heating from an initial temperature to an intermediate temperature, keeping the temperature, injecting a protective gas, heating to a target sintering temperature at a heating rate of 30-80° C. / min, and keeping the temperature.
[0018] In one embodiment, the pre-pressing pressure is 280-320MPa; the sintering pressure of the spark plasma sintering is 45-55MPa, the initial temperature is 25-27°C, the mid-term temperature is 550-650°C, the insulation time of the mid-term temperature is 10-30min, the target sintering temperature is 950-1050°C, and the insulation time of the target sintering temperature is 10-60min.
[0019] The present invention also provides a connecting piece, which is prepared by adopting the Fe-Mn-Si based memory alloy material.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The invention discloses an Fe-Mn-Si based memory alloy material, a preparation method and an application thereof. The Fe-Mn-Si based memory alloy material introduces Cu into a formula and adopts an MA+SPS preparation method, so that the Fe-Mn-Si based memory alloy material has good shape memory performance and high corrosion resistance, and also has better hardness and superelasticity. DETAILED DESCRIPTION
[0022] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0024] source:
[0025] Unless otherwise specified, the reagents, materials, and equipment used in this example are all commercially available; the experimental methods are all conventional experimental methods in the art unless otherwise specified.
[0026] Example 1
[0027] By mass percentage, iron powder is 60wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 5wt.%, and copper powder is 1wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 60:20:6:8:5:1). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition cabin of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the tank is taken out and placed in the ball mill under the argon gas environment. The ball milling speed is 500r / min, and the machine is stopped for 30 minutes for 1 hour. A process control agent is dripped every 10 hours. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.2ml / 10g powder. After 50 hours of ball milling, all the powder is taken out.
[0028] The mechanically alloyed memory alloy powder is loaded into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 300MPa, and the holding time is 60s. The obtained prefabricated sample is placed in a spark plasma sintering for sintering experiments. The sintering pressure is set to 50MPa, and the target sintering temperature is 950℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) for 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then increase the heating rate to close to the target sintering temperature at a rate of 50℃ / min, keep warm and pressurize for 30min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0029] The prepared memory alloy block material was polished and then subjected to microstructure and performance testing, and its mechanical properties were characterized. The mechanical properties test method was based on GB / T4340-2009, GB / T 3850-2015, GB / T 6525-2019 and YS / T1307.2-2019. The obtained technical parameters are shown in the following table:
[0030] Table 1 Performance test results of the memory alloy block material of this embodiment
[0031]
[0032] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0033] Example 2
[0034] By mass percentage, iron powder is 58wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 5wt.%, and copper powder is 3wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 58:20:6:8:5:3). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition cabin of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the tank is taken out and placed in the ball mill under the argon gas environment. The ball milling speed is 400r / min, and the machine is stopped for 30 minutes for 1 hour. A process control agent is dripped every 10 hours. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.2ml / 10g powder. After 55h of ball milling, all the powder is taken out.
[0035] The mechanically alloyed memory alloy powder is loaded into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 300MPa. The holding time is 60s, and the obtained prefabricated sample is placed in the spark plasma sintering for sintering experiments. The sintering pressure is set to 45MPa, and the target sintering temperature is 950℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) after 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then increase the heating rate to close to the target sintering temperature at a rate of 30℃ / min, keep warm and hold pressure for 30min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0036] The obtained memory alloy block material was polished and then subjected to the same method as in Example 1 for organization and performance testing. The obtained technical parameters are as follows:
[0037] Table 2 Performance test results of the memory alloy block material of this embodiment
[0038]
[0039] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0040] Example 3
[0041] By mass percentage, iron powder is 56wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 5wt.%, and copper powder is 5wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 56:20:6:8:5:5). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition chamber of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the tank is taken out and placed in the ball mill under the argon gas environment. The ball milling speed is 500r / min, and the machine is stopped for 30min for 1h. A process control agent is dripped every 10h. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.1ml / 10g powder. After 50h of ball milling, all the powder is taken out.
[0042] The mechanically alloyed memory alloy powder is loaded into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 320MPa for 60s. The obtained prefabricated sample is placed in a spark plasma sintering for sintering experiments. The sintering pressure is set to 55MPa, and the target sintering temperature is 950℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) for 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then increase the heating rate to close to the target sintering temperature at a rate of 50℃ / min, keep warm and pressurize for 30min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0043] The obtained memory alloy block material was polished and then subjected to the same method as in Example 1 for organization and performance testing. The obtained technical parameters are as follows:
[0044] Table 3 Performance test results of the memory alloy block material of this embodiment
[0045]
[0046] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0047] Example 4
[0048] By mass percentage, iron powder is 58wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 3wt.%, and copper powder is 3wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 58:20:6:8:3:3). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition cabin of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the tank is taken out and placed in the ball mill under the argon gas environment. The ball milling speed is 600r / min, and the machine is stopped for 30 minutes for 1 hour. A process control agent is dripped every 8 hours. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.15ml / 10g powder. After 55h of ball milling, all the powder is taken out.
[0049] The mechanically alloyed memory alloy powder is filled into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 280MPa, and the holding time is 60s. The obtained prefabricated sample is placed in a spark plasma sintering for sintering experiments. The sintering pressure is set to 45MPa, and the target sintering temperature is 1000℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) for 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then increase the heating rate to close to the target sintering temperature at a rate of 40℃ / min, keep warm and pressurize for 30min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0050] The obtained memory alloy block material was polished and then subjected to the same method as in Example 1 for organization and performance testing. The obtained technical parameters are as follows:
[0051] Table 4 Performance test results of the memory alloy block material of this embodiment
[0052]
[0053] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0054] Example 5
[0055] By mass percentage, iron powder is 58wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 5wt.%, and copper powder is 3wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 58:20:6:8:5:3). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition chamber of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the tank is taken out and placed in the ball mill under the argon gas environment. The ball milling speed is 400r / min, and the machine is stopped for 30 minutes for 1 hour. A process control agent is dripped every 10 hours. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.25ml / 10g powder. After 50 hours of ball milling, all the powder is taken out.
[0056] The mechanically alloyed memory alloy powder is filled into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 310MPa for 60s. The obtained prefabricated sample is placed in a spark plasma sintering for sintering experiments. The sintering pressure is set to 50MPa, and the target sintering temperature is 1050℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) for 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then heat up to a temperature close to the target sintering temperature at a heating rate of 50℃ / min, keep warm and pressurize for 30min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0057] The obtained memory alloy block material was polished and then subjected to the same method as in Example 1 for organization and performance testing. The obtained technical parameters are as follows:
[0058] Table 5 Performance test results of the memory alloy block material of this embodiment
[0059]
[0060] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0061] Example 6
[0062] By mass percentage, iron powder is 58wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 5wt.%, and copper powder is 3wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 58:20:6:8:5:3). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition cabin of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the tank is taken out and placed in the ball mill under the argon gas environment. The ball milling speed is 500r / min, and the machine is stopped for 30min for 1h. A process control agent is dripped every 12h. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.2ml / 10g powder. After 50h of ball milling, all the powder is taken out.
[0063] The mechanically alloyed memory alloy powder is filled into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 300MPa, and the holding time is 60s. The obtained prefabricated sample is placed in a spark plasma sintering for sintering experiments. The sintering pressure is set to 50MPa, and the target sintering temperature is 1000℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) for 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then increase the heating rate to close to the target sintering temperature at 80℃ / min, keep warm and hold pressure for 10min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0064] The obtained memory alloy block material was polished and then subjected to the same method as in Example 1 for organization and performance testing. The obtained technical parameters are as follows:
[0065] Table 6 Performance test results of the memory alloy block material of this embodiment
[0066]
[0067] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0068] Example 7
[0069] By mass percentage, iron powder is 58wt.%, manganese powder is 20wt.%, silicon powder is 6wt.%, chromium powder is 8wt.%, nickel powder is 5wt.%, and copper powder is 3wt.% (i.e., in this embodiment, the weight ratio of iron powder, manganese powder, silicon powder, chromium powder, nickel powder, and copper powder is 58:20:6:8:5:3). Put it into a stainless steel alloy can, the purity of all metal powders is 99%, the mesh number is 200 mesh, the particle size of manganese powder is ≤45μm, and the particle size of iron powder, silicon powder, chromium powder, nickel powder, and copper powder is ≤30μm. The ball-to-material ratio is 10:1, and the ball milling medium is a stainless steel alloy ball. After repeated gas washing (argon gas) in the transition chamber of the glove box, the ball is placed in the operating chamber and covered with a sealing cover to ensure that the argon gas environment in the tank is taken out and placed in the ball mill. The ball milling speed is 450r / min, and the machine is stopped for 30 minutes for 1 hour. A process control agent is dripped every 11 hours. In this embodiment, the process control agent is industrial ethanol (analytical grade ≥99.7%), and the dripping amount is 0.13ml / 10g powder. After 45 hours of ball milling, all the powder is taken out.
[0070] The mechanically alloyed memory alloy powder is filled into a graphite mold pre-installed with graphite pad paper, and pre-pressed with a hydraulic press at a pressure of 320MPa for 30s. The obtained prefabricated sample is placed in a spark plasma sintering for sintering experiments. The sintering pressure is set to 55MPa, and the target sintering temperature is 1000℃. The vacuum degree is 20Pa before the furnace temperature reaches 600℃. The furnace temperature is heated from room temperature (25-27℃, initial temperature) to 600℃ (mid-term temperature) for 5min, and then a protective Ar atmosphere is introduced. The heating system is: keep warm at 600℃ for 10min, then heat up to a temperature close to the target sintering temperature at a heating rate of 70℃ / min, keep warm and pressurize for 60min, then unload the pressure and slowly cool down to room temperature to obtain a memory alloy block material.
[0071] The obtained memory alloy block material was polished and then subjected to the same method as in Example 1 for organization and performance testing. The obtained technical parameters are as follows:
[0072] Table 7 Performance test results of the memory alloy block material of this embodiment
[0073]
[0074] The prepared memory alloy has good high-temperature stability, and its hardness and superelasticity have great advantages over traditional metals.
[0075] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A Fe-Mn-Si based memory alloy material, characterized in that: The Fe-Mn-Si based memory alloy material is mainly prepared from the following raw materials in parts by weight: The preparation method of the Fe-Mn-Si based memory alloy material comprises the following steps: mixing raw materials, ball milling to obtain mixed powder, pre-pressing the mixed powder into a shape, and performing spark plasma sintering to obtain the material.
2. The Fe-Mn-Si based memory alloy material according to claim 1, characterized in that: The Fe-Mn-Si based memory alloy material is mainly prepared from the following raw materials in parts by weight:
3. The Fe-Mn-Si based memory alloy material according to claim 1, characterized in that: The raw material is a single metal powder, the particle size of the manganese is ≤45 μm, and the particle sizes of the iron, silicon, chromium, nickel and copper are ≤30 μm.
4. The method for preparing the Fe-Mn-Si based memory alloy material according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: mixing raw materials, ball milling to obtain mixed powder, pre-pressing the mixed powder into a shape, and performing spark plasma sintering to obtain the mixed powder.
5. The preparation method according to claim 4, characterized in that: The ball-to-material mass ratio of the ball mill is (8-12):1, the rotation speed of the ball mill is 400-600r / min, and the ball milling time is 45-55h.
6. The preparation method according to claim 5, characterized in that: The ball milling step further includes adding a process control agent every 8-12 hours, and the amount of the process control agent is: 0.1-0.25 mL of the process control agent is added for every 10 g of the total mass of the raw materials.
7. The preparation method according to claim 6, characterized in that: The process control agent includes ethanol.
8. The preparation method according to claim 4, characterized in that: The spark plasma sintering includes: heating from an initial temperature to an intermediate temperature, keeping the temperature, filling with a protective gas, heating to a target sintering temperature at a heating rate of 30-80° C. / min, and keeping the temperature.
9. The preparation method according to claim 8, characterized in that: The pre-pressing pressure is 280-320 MPa; The sintering pressure of the spark plasma sintering is 45-55MPa, the initial temperature is 25-27°C, the intermediate temperature is 550-650°C, the insulation time of the intermediate temperature is 10-30min, the target sintering temperature is 950-1050°C, and the insulation time of the target sintering temperature is 10-60min.
10. A connecting piece, characterized in that: The alloy is prepared by using the Fe-Mn-Si based memory alloy material described in any one of claims 1 to 3.
Citation Information
Patent Citations
Shape memory alloy particular enhanced copper-based composite material and preparation method
CN109822095A
Fe-Mn-Si-Cr-Ni based shape memory alloy and preparation method thereof
CN110983152A
Corrosion-resistant Fe-Mn-Si-Cr-Ni-Ti shape memory alloy and preparation method thereof
CN111926267A
Method for producing tough iron-base shape memory alloy
JP2004292896A