An AlN template and its preparation method
By alternately growing AlN layers in an AlN template using magnetron sputtering and MOCVD, and utilizing high-concentration carbon impurities to form CAl point defects, the problem of oxygen impurity diffusion during the thermal annealing of AlN templates was solved, thus improving the performance of AlGaN materials and devices.
Patent Information
- Application Number
- CN202410546264.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-06
AI Technical Summary
Existing AlN templates have excessively high oxygen concentrations during thermal annealing, which leads to reduced doping efficiency, decreased carrier mobility, and low luminous efficiency in AlGaN materials, thus affecting device performance.
AlN layers were grown alternately using magnetron sputtering and MOCVD. By introducing a high concentration of carbon impurities into the second AlN layer, CAl point defects were formed to prevent the formation of oxygen impurities and VAl-ON complexes, thereby inhibiting the diffusion of oxygen impurities during thermal annealing.
It effectively reduces the concentration of oxygen impurity points in AlN templates, improves the quality of subsequent epitaxial AlGaN materials and device performance, and enhances the performance of optoelectronic and electronic devices.
Smart Images

Figure CN118241173B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor material growth technology, and in particular to an AlN template and its preparation method. Background Technology
[0002] AlGaN, a direct bandgap semiconductor with a continuously tunable bandgap of 3.4-6.2 eV, possesses advantages such as high breakdown field strength and high saturated carrier mobility. Therefore, AlGaN is widely used in optoelectronic fields such as sterilization and secure communication, as well as in power electronics fields such as radio frequency devices and high-power devices. However, related devices still face many problems such as low luminous efficiency and short device lifetime. One of the main methods to improve device performance is to improve the quality of AlGaN material.
[0003] Due to the lack of low-cost, high-quality homogeneous substrates, annealed AlN templates are currently the primary choice for heteroepitaxial growth. However, during AlN template fabrication, a significant lattice mismatch between the AlN layer and the sapphire substrate leads to an extremely high dislocation density within the AlN template. High-temperature thermal annealing can reduce the dislocation density of the AlN template to 10-1. 8 cm -2 The oxygen concentration is on the order of magnitude, but this operation causes a significant amount of oxygen from the sapphire substrate to diffuse into the AlN layer. When other AlGaN structures are epitaxially grown using annealed AlN templates, the oxygen concentration can increase to 10⁻⁶. 18 cm -3 This can lead to serious consequences for AlGaN materials, such as reduced material doping efficiency, reduced carrier mobility, and the formation of abnormal spectra in light-emitting devices, resulting in reduced efficiency of the light-emitting devices.
[0004] Given the current drawback of high oxygen concentration during annealing in AlN templates, it is necessary to improve this. Summary of the Invention
[0005] This invention provides an AlN template and its preparation method to overcome the deficiencies in the prior art.
[0006] In a first aspect, the present invention provides a method for preparing an AlN template, comprising the following steps:
[0007] Provide substrate;
[0008] The first AlN layer was prepared on the substrate by magnetron sputtering.
[0009] The second AlN layer was prepared on the first AlN layer using the MOCVD method;
[0010] A third AlN layer was prepared on the second AlN layer by magnetron sputtering.
[0011] The carbon impurity concentration in the second AlN layer is higher than that in the first and third AlN layers.
[0012] Preferably, the method for preparing the AlN template, specifically using MOCVD to prepare the second AlN layer on the first AlN layer, includes:
[0013] Using trimethylaluminum as the aluminum source and ammonia as the nitrogen source, with a V / III ratio of aluminum to nitrogen source of 50 to 5000, a second AlN layer containing carbon impurities was prepared at a temperature of 1000 to 1500 °C.
[0014] Preferably, the method for preparing the AlN template, specifically using magnetron sputtering to prepare the first AlN layer on the substrate, includes:
[0015] The first AlN layer was prepared using AlN as the target material under a pressure of 4–10 mtorr, a temperature of 600–800 °C, and a sputtering power of 3–5 kW.
[0016] Preferably, the method for preparing the AlN template, specifically employing magnetron sputtering to prepare the third AlN layer on the second AlN layer, includes:
[0017] A third AlN layer was prepared using AlN as the target material at a pressure of 4–10 mtorr, a temperature of 600–800 °C, and a sputtering power of 3–5 kW.
[0018] Preferably, in the method for preparing the AlN template, the thickness of the first AlN layer is greater than or equal to 10 nm.
[0019] Preferably, in the method for preparing the AlN template, the second AlN layer has a thickness of 10–200 nm, and the thickness of the third AlN layer has a thickness of 50–1000 nm.
[0020] Preferably, the method for preparing the AlN template further includes, after obtaining the third AlN layer, annealing the substrate with the third AlN layer in an inert atmosphere.
[0021] Preferably, the AlN template preparation method involves an annealing temperature of 1100–1800°C and an annealing time of 0.5–10 h.
[0022] Inert atmospheres include at least one of nitrogen, helium, neon, and argon.
[0023] Preferably, in the method for preparing the AlN template, the carbon impurity concentration in the second AlN layer is 4 × 10⁻⁶. 16 ~8×10 16 cm -3;
[0024] The carbon impurity concentration in the first AlN layer is 3 × 10⁻⁶. 16 ~3.5×10 16 cm -3 ;
[0025] The carbon impurity concentration in the third AlN layer is 3 × 10⁻⁶. 16 ~3.9×10 16 cm -3 .
[0026] Secondly, the present invention also provides an AlN template, which is prepared using the preparation method described above.
[0027] The method for preparing the AlN template of the present invention has the following advantages over the prior art:
[0028] The method for preparing the AlN template of the present invention involves preparing a second AlN layer on a first AlN layer using MOCVD. The carbon impurity concentration in the second AlN layer is higher than that in the first and third AlN layers. The higher carbon impurity concentration in the second AlN layer means that the carbon impurities will occupy more aluminum vacancies (V0). Al ), and form carbon accounting for V Al (C Al Point defect; due to V Al Point defects are C Al Substitution will prevent oxygen impurities from forming lower-energy and more stable Va in the AlN layer prepared by MOCVD during the thermal annealing process. Al Oxygen occupies nitrogen vacancies (O N Point defect complexes (V) Al -O N This invention suppresses the diffusion of oxygen impurity point defects from the substrate to the upper AlN layer during thermal annealing, thereby significantly reducing the concentration of oxygen impurity point defects in the AlN template. The AlN template prepared by this invention can effectively reduce the concentration of oxygen impurity point defects in the thermally annealed AlN template, thus reducing the diffusion of oxygen impurities into subsequent epitaxial structures. This is crucial for improving the quality of subsequent epitaxial AlGaN materials and the performance of AlGaN-based devices, and has significant implications for improving the performance of optoelectronic and electronic devices. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0030] Figure 1 This is a schematic flowchart of the AlN template preparation method of the present invention;
[0031] Figure 2 This is a schematic diagram of the structure of the AlN template prepared in this invention;
[0032] Figure 3 V in the AlN template prepared in Example 1 Al -O N V Al and C Al Plot showing the variation of point defect formation energy with Fermi level.
[0033] Figure 4 This is a schematic diagram of the secondary ion mass spectrometry (SIMS) test results of different C impurity concentrations in the AlN layer of the AlN template prepared in Example 1. Detailed Implementation
[0034] The technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0035] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0036] In the description of this invention, it should be understood that the orientation or positional relationship indicated by terms such as "above" is based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship in which the product of this invention is usually placed when in use, or the orientation or positional relationship in which those skilled in the art are usually understood. It is only for the convenience of describing this invention and simplifying the description, and is not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, it should not be construed as a limitation of this invention.
[0037] The following provides a detailed description of each example. It should be noted that the order of description of the embodiments below is not intended to limit the preferred order of the embodiments. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single digits within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.
[0038] This invention provides a method for preparing an AlN template, such as... Figure 1 As shown, it includes the following steps:
[0039] S1, Provide a substrate;
[0040] S2. The first AlN layer was prepared on the substrate by magnetron sputtering.
[0041] S3. A second AlN layer is prepared on the first AlN layer using the MOCVD method;
[0042] S4. A third AlN layer is prepared on the second AlN layer by magnetron sputtering.
[0043] The carbon impurity concentration in the second AlN layer is higher than that in the first and third AlN layers.
[0044] In order to reduce the oxygen concentration introduced into the AlN template by the thermal annealing operation, the method for preparing the AlN template of the present invention proposes an oxygen point defect blocking structure that can prevent oxygen impurities from diffusing from the sapphire substrate to the AlN layer during the thermal annealing process. This point defect diffusion structure is mainly inserted into a second AlN layer prepared by MOCVD. The carbon impurity concentration in the second AlN layer is higher than that in the first and third AlN layers. The second AlN layer with a higher carbon impurity concentration will have more carbon impurities occupying more aluminum vacancies (V). Al This prevents oxygen impurities diffusing from the substrate during thermal annealing from forming a more stable V in the second AlN layer prepared by the MOCVD method. Al -O N The complex reduces the oxygen impurity point defect concentration in the annealed AlN template, which can fundamentally reduce the oxygen impurity concentration in subsequent AlGaN epitaxial layers.
[0045] Specifically, the principle of this method is as follows: by having carbon impurities occupy V Al The formation energy is lower than that of C-V. Al (C Al Point defects (C) Al (i.e., point defects formed by C atoms occupying Al vacancies), to prevent oxygen impurities from forming stable V in the second AlN layer prepared by MOCVD. Al Oxygen occupies nitrogen vacancies (O N Point defect complexes (V) Al -O N Based on fundamental principles, the annealed AlN template structure described in this invention mainly consists of an AlN layer grown by magnetron sputtering and an AlN layer grown by MOCVD. When preparing the second AlN layer using MOCVD, a high concentration of carbon impurities can be introduced into this layer by adjusting the proportion of metal-organic compounds, thereby replacing V. Al And form C Al Point defects, which lead to the formation of the lowest and most stable V in oxygen impurity point defects. Al -O N The complex cannot form in the second AlN layer prepared by the MOCVD method, thereby inhibiting the formation of oxygen impurity point defects in the second AlN layer prepared by the MOCVD method, and thus reducing the concentration of oxygen impurity point defects in the AlN template from the root.
[0046] This invention provides a method for preparing an AlN template. The reason for not directly using an AlN epitaxial layer grown by MOCVD as the annealing template is that the stability and uniformity of AlN layers grown by MOCVD are inferior to those grown by magnetron sputtering, and MOCVD easily introduces more impurities during epitaxial growth, affecting the annealing effect. However, by using only AlN grown by MOCVD as the insertion layer, while the main body of the annealing AlN template remains magnetron sputtered AlN, a good annealing effect can be achieved while simultaneously using the introduction of C impurities by MOCVD to block the diffusion of O defects.
[0047] In some embodiments, the epitaxial method for the second AlN layer includes, but is not limited to, epitaxial growth methods that can increase the metal source flow rate and result in high carbon content, such as ammonia pulse method and metal-organic chemical vapor deposition.
[0048] In some embodiments, the preparation of a second AlN layer on a first AlN layer using MOCVD specifically includes:
[0049] A second AlN layer was prepared by using trimethylaluminum as the aluminum source and ammonia as the nitrogen source, with a V / III (molar ratio) of aluminum source to nitrogen source of 50 to 5000, at a temperature of 1000 to 1500 °C.
[0050] In some embodiments, the preparation of the first AlN layer on the substrate by magnetron sputtering specifically includes:
[0051] The first AlN layer was prepared using AlN as the target material under a pressure of 4–10 mtorr, a temperature of 600–800 °C, and a sputtering power of 3–5 kW.
[0052] In some embodiments, the method for creating the third AlN layer includes, but is not limited to, low-carbon epitaxial growth techniques such as magnetron sputtering, hydride vapor phase epitaxy, and molecular beam epitaxy.
[0053] In some embodiments, the preparation of a third AlN layer on a second AlN layer using magnetron sputtering specifically includes:
[0054] The first AlN layer was prepared using AlN as the target material under a pressure of 4–10 mtorr, a temperature of 600–800 °C, and a sputtering power of 3–5 kW.
[0055] In some embodiments, the thickness of the first AlN layer is greater than or equal to 10 nm. Specifically, the thickness of the first AlN layer is 10 nm, 20 nm, 30 nm, 40 nm, 50 nm...100 nm, etc.
[0056] In some embodiments, the second AlN layer is 10–200 nm thick. Specifically, if the second AlN layer is too thin, it cannot effectively block the diffusion of O defects; if it is too thick, it will affect the annealing effect and the uniformity of the sample.
[0057] In some embodiments, the thickness of the third AlN layer is 50–1000 nm. Specifically, if the third AlN layer is too thin, a good annealing effect cannot be obtained; if it is too thick, it is prone to cracking during the annealing process.
[0058] In some embodiments, after the third AlN layer is prepared, the method further includes annealing the substrate with the third AlN layer prepared in an inert atmosphere.
[0059] In some embodiments, the annealing temperature is 1100–1800°C and the annealing time is 0.5–10 h.
[0060] In some embodiments, the inert atmosphere includes at least one of nitrogen, helium, neon, and argon.
[0061] In some embodiments, the substrate includes any one of a sapphire substrate, a Si substrate, a SiC substrate, and an Al2O3 substrate. Preferably, the substrate is a sapphire substrate, and its bevel angle includes, but is not limited to, 0°. The sapphire substrate includes, but is not limited to, the c-plane and the a-plane.
[0062] In some embodiments, the carbon impurity concentration in the second AlN layer is 4 × 10⁻⁶. 16~8×10 16 cm -3 .
[0063] In some embodiments, the carbon impurity concentration in the first AlN layer is 3 × 10⁻⁶. 16 ~3.5×10 16 cm -3 .
[0064] In some embodiments, the carbon impurity concentration in the third AlN layer is 3 × 10⁻⁶. 16 ~3.9×10 16 cm -3 .
[0065] Secondly, the present invention also provides an AlN template, which is prepared by the above-described preparation method.
[0066] For details, please refer to Figure 2 As shown, the prepared AlN template includes a substrate 1, a first AlN layer 2, a second AlN layer 3, and a third AlN layer 4. Based on the conventional AlN template preparation, this invention inserts a MOCVD AlN layer (i.e., the second AlN layer 3) of a certain thickness between the AlN layers epitaxially grown by a magnetron sputtering system. This prevents oxygen impurity point defects from diffusing from the sapphire substrate to the AlN layer during thermal annealing. The principle is as follows: When epitaxially growing AlN layers using an MOCVD system, the introduction of the organic gas source trimethylaluminum (TMAl) results in a large amount of carbon impurities. These carbon impurities significantly occupy the V in the AlN material. Al And form C Al Point defect; due to V Al Point defects are C Al Substitution will prevent oxygen impurities from forming lower-energy and more stable Va in the AlN layer prepared by MOCVD during the thermal annealing process. Al -O N The complex inhibits the diffusion of oxygen impurity point defects from the substrate to the upper AlN layer during thermal annealing, thereby significantly reducing the concentration of oxygen impurity point defects in the AlN template.
[0067] The AlN template of the present invention can effectively reduce the concentration of oxygen impurity point defects in the thermally annealed AlN template, thereby reducing the diffusion of oxygen impurities into the subsequent epitaxial structure. This is crucial for improving the quality of subsequent epitaxial AlGaN materials and enhancing the performance of AlGaN-based devices.
[0068] The preparation method of the AlN template of this application is further illustrated below with specific embodiments. This section further illustrates the content of the present invention with reference to specific embodiments, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0069] Example 1
[0070] This application provides a method for preparing an AlN template, comprising the following steps:
[0071] S1. Provide a c-plane sapphire substrate;
[0072] S2. A first AlN layer with a thickness of 31 nm was prepared on the substrate using magnetron sputtering; the specific sputtering process is as follows:
[0073] The first AlN layer was prepared using AlN as the target material under a pressure of 8 mtorr, a temperature of 700 °C, and a sputtering power of 4 kW.
[0074] S3. A second AlN layer containing carbon impurities with a thickness of 73 nm was prepared on the first AlN layer using the MOCVD method; the specific process is as follows:
[0075] Using trimethylaluminum as the aluminum source and ammonia as the nitrogen source, with a V / III ratio of aluminum source to nitrogen source of 80, a second AlN layer was prepared at a temperature of 1200℃.
[0076] S4. A third AlN layer with a thickness of 60 nm was prepared on the second AlN layer using magnetron sputtering; the specific sputtering process is as follows:
[0077] A third AlN layer was prepared using AlN as the target material at a pressure of 8 mtorr, a temperature of 700 °C, and a sputtering power of 4 kW.
[0078] S5. Anneal the substrate with the third AlN layer at 1700°C for 1 hour under a nitrogen atmosphere.
[0079] Figure 3 V in the AlN template prepared in Example 1 Al -O N V Al and C Al Plot showing the variation of point defect formation energy with Fermi level.
[0080] from Figure 3 As can be seen from this, the intrinsic AlN (i.e., the Fermi level located at 3.1 eV between the conduction band minimum (CBM) and the valence band maximum (VBM)) contains V Al -ON The formation energy of point defects in complexes is significantly less than V. Al and C Al The point defect formation energy indicates that O impurity point defects readily combine with V. Al Stable complexes are formed, leading to enrichment in the AlN template. However, because V Al The formation energy is greater, so V Al The concentration of V is significantly lower than that of O and C impurity point defects. Al -O N The concentration of point defects in the complex depends primarily on V. Al Meanwhile, due to the presence of C in intrinsic AlN materials... Al The formation energy of point defects is less than V. Al The formation energy of V is such that C impurity point defects preferentially occupy V. Al Formation C Al This leads to V Al The concentration further decreased. When the AlN template underwent high-temperature thermal annealing, V... Al -O N The formation of complex point defects in the MOCVD-grown AlN layer is suppressed, which prevents O impurity point defects from diffusing into the third AlN layer, and thus suppresses the diffusion of O impurity point defects into the subsequent AlGaN epitaxial layer.
[0081] Figure 4 This is a schematic diagram of the SIMS results for the C impurity concentration in different AlN layers of the AlN template prepared in Example 1.
[0082] from Figure 4 As can be seen, the average concentration of carbon impurities in the second AlN layer is approximately 5.8 × 10⁻⁶. 16 cm -3 The average concentration of carbon impurities in the first AlN layer is approximately 3.3 × 10⁻⁶. 16 cm -3 The average concentration of carbon impurities in the third AlN layer is 3.5 × 10⁻⁶. 16 cm -3 Therefore, it can be seen that the C impurity concentration in the second AlN layer grown by MOCVD is significantly higher than that in the AlN layer grown by magnetron sputtering. Thus, this AlN template preparation scheme can suppress the enrichment of O impurity concentration in the high-temperature thermally annealed AlN template.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing an AlN template, characterized in that, Includes the following steps: Provide substrate; The first AlN layer was prepared on the substrate by magnetron sputtering. The second AlN layer was prepared on the first AlN layer using the MOCVD method; A third AlN layer was prepared on the second AlN layer by magnetron sputtering. The carbon impurity concentration in the second AlN layer is higher than that in the first AlN layer and the third AlN layer. The second AlN layer prepared on the first AlN layer using the MOCVD method specifically includes: Using trimethylaluminum as the aluminum source and ammonia as the nitrogen source, with a V / III ratio of aluminum to nitrogen of 50–5000, a second AlN layer was prepared at a temperature of 1000–1500 °C; carbon impurities in this layer occupied more aluminum vacancies (V... Al ), and form carbon accounting for V Al (C Al Point defect; due to V Al Point defects are C Al Substitution will prevent oxygen impurities from forming lower-energy and more stable Vo in the second AlN layer prepared by MOCVD during the thermal annealing process. Al With oxygen occupying nitrogen vacancies (O N Point defect complexes (V) Al -O N This suppresses the diffusion of oxygen impurity point defects from the substrate to the upper AlN layer during the thermal annealing process.
2. The method for preparing the AlN template as described in claim 1, characterized in that, The preparation of the first AlN layer on the substrate by magnetron sputtering specifically includes: The first AlN layer was prepared using AlN as the target material under a pressure of 4-10 mtorr, a temperature of 600-800℃, and a sputtering power of 3-5 kW.
3. The method for preparing the AlN template as described in claim 1, characterized in that, The third AlN layer was prepared on the second AlN layer by magnetron sputtering, specifically including: A third AlN layer was prepared using AlN as the target material at a pressure of 4-10 mtorr, a temperature of 600-800℃, and a sputtering power of 3-5 kW.
4. The method for preparing the AlN template as described in claim 1, characterized in that, The thickness of the first AlN layer is greater than or equal to 10 nm.
5. The method for preparing the AlN template as described in claim 1, characterized in that, The thickness of the second AlN layer is 10~200nm; the thickness of the third AlN layer is 50~1000nm.
6. The method for preparing the AlN template according to any one of claims 1 to 5, characterized in that, After obtaining the third AlN layer, the process also includes annealing the substrate with the third AlN layer in an inert atmosphere.
7. The method for preparing the AlN template as described in claim 6, characterized in that, The annealing temperature is 1100~1800℃, and the annealing time is 0.5~10h; Inert atmospheres include at least one of nitrogen, helium, neon, and argon.
8. The method for preparing the AlN template according to any one of claims 1 to 5, characterized in that, The carbon impurity concentration in the second AlN layer is 4 × 10⁻⁶. 16 ~8×10 16 cm -3 ; The carbon impurity concentration in the first AlN layer is 3 × 10⁻⁶. 16 ~3.5×10 16 cm -3 ; The carbon impurity concentration in the third AlN layer is 3 × 10⁻⁶. 16 ~3.9×10 16 cm -3 .
9. An AlN template, characterized in that, It is prepared by any one of the preparation methods described in claims 1 to 8.
Citation Information
Patent Citations
Method for obtaining high-quality AlN template
CN107768234A