Environmentally friendly composite pigment and its production process

By using a combination of acrylic polymer emulsion and wear-resistant fillers in environmentally friendly composite pigments, combined with polyamic acid cross-linking agent and electrostatic adsorption technology, the problem of insufficient high temperature resistance and wear resistance of pigments is solved, and higher pigments are achieved performance and longevity.

CN118256098BActive Publication Date: 2024-10-11RAINBOW PLASTIC COLOURS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410355748.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-11
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Ordinary environmentally friendly composite pigments have poor high temperature resistance and wear resistance. They are prone to discoloration, fading or decomposition under high temperature conditions, and may suffer from wear, peeling and other problems under friction or external force.

Method used

Using a combination of acrylic polymer emulsion and talc powder, wear-resistant fillers, UV absorbers, film-forming additives, defoaming agents and leveling agents, the cohesion and adhesion of the pigments are improved through polyamic acid cross-linking agents and electrostatic adsorption technology , and through the combination of serpentine powder and aramid fiber, the wear resistance of the pigment is enhanced.

Benefits of technology

It significantly improves the high temperature resistance, adhesion, anti-fouling performance and wear resistance of the composite pigment, extends the service life, and improves the appearance quality and performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256098B_ABST
    Figure CN118256098B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of pigments, and discloses an environmentally friendly composite pigment and a preparation process thereof. The composite pigment comprises the following raw materials: acrylic polymer emulsion, talcum powder, wear-resistant filler, pigment, ultraviolet absorber, film-forming aid, defoamer, and leveling agent; the acrylic polymer emulsion comprises the following raw materials: acrylic acid, hydroxyethyl acrylate, butyl acrylate, diacetone acrylamide, deionized water, emulsifier, polyamic acid crosslinking agent, and ammonium persulfate; wherein the polyamic acid crosslinking agent is a grafted composite of polyamic acid and dichloromethylsilane; the wear-resistant filler is prepared by combining serpentine powder with aramid fiber through electrostatic adsorption, and the composite pigment prepared by the invention has excellent high temperature resistance, adhesion, wear resistance, antifouling performance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pigments, and in particular to an environmentally friendly composite pigment and a production process thereof. Background Art

[0002] In the preparation process of traditional pigments, some chemically polluting substances may be used. These substances may pollute the environment and threaten human health during production, use and exhaust gas. With the improvement of people's environmental awareness, all walks of life pay more and more attention to the environmental performance of products. It is in this context that environmentally friendly composite pigments come into being to meet the market's urgent demand for green, healthy and sustainable products. At the same time, with the development of industrialization, people require products to be beautiful while also putting forward requirements for some special performance of products, and want to give products diversified functions. When used, environmentally friendly composite pigments can not only give the coated objects a colorful appearance, but also protect the coated substrate, reduce the aging rate under ultraviolet radiation and humid and hot environments, and isolate the erosion of moisture, oil and other corrosive substances. They have been widely used in ceramics, painting, printing and other fields.

[0003] However, ordinary environmentally friendly composite pigments do not have good high temperature resistance. They may change color, fade or decompose under high temperature conditions, which will not only seriously affect the appearance and color stability of the product, but may also cause product performance degradation or failure. In addition, pigments with poor wear resistance are prone to wear, peeling or scratches when subjected to friction or external forces, which may cause the paint surface to fade or lighten, affecting the appearance quality of the product.

[0004] Therefore, preparing an environmentally friendly composite pigment with excellent high temperature resistance and wear resistance has become a hot research topic in the current scientific research field. The patent with publication number CN115304934B discloses a method for preparing a high-performance environmentally friendly color composite pigment. The invention forms a composite structure with uniform particle size distribution by grafting organic pigments on the surface of environmentally friendly color inorganic pigments through chemical bonds. The prepared composite pigment has excellent temperature resistance, high hiding power, UV resistance, high coloring performance, and high chromaticity index. However, the wear resistance of the composite pigment needs to be improved because the pigment is easily worn when subjected to friction or external force. Summary of the invention

[0005] The purpose of the present invention is to provide an environmentally friendly composite pigment and a production process thereof, which solves the following technical problems:

[0006] (1) It solves the problem of poor high temperature resistance of common environmentally friendly composite pigments;

[0007] (2) It solves the problem of poor wear resistance of ordinary environmentally friendly composite pigments.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] An environmentally friendly composite pigment comprises the following raw materials in parts by weight: 60-70 parts of acrylic polymer emulsion, 4-8 parts of talc, 4-6 parts of wear-resistant filler, 10-20 parts of pigment, 1-2 parts of ultraviolet absorber, 1-2 parts of film-forming aid, 2-3 parts of defoamer and 1-2 parts of leveling agent.

[0010] Furthermore, the preparation method of the acrylic polymer emulsion comprises the following steps:

[0011] (1) mixing acrylic acid, hydroxyethyl acrylate, butyl acrylate and diacetone acrylamide to obtain a mixed monomer;

[0012] (2) adding an emulsifier and deionized water into a reactor, turning on a mechanical stirrer, setting the system temperature to 70-90° C., then adding 5-10% by weight of a mixed monomer and ammonium persulfate, and keeping the temperature for 10-20 minutes after the addition is completed to obtain a seed emulsion;

[0013] (3) adding the remaining mixed monomers, polyamic acid crosslinking agent and ammonium persulfate dropwise to the reactor for about 3 to 4 hours. After the addition is completed, the temperature is raised to 85 to 95° C. and kept for 40 to 50 minutes, then the temperature is lowered to about 30 to 50° C., and the material is filtered through a 50 to 150 mesh gauze to obtain an acrylic polymer emulsion;

[0014] The acrylic polymer emulsion comprises the following raw materials in parts by weight: 30-40 parts of acrylic acid, 10-20 parts of hydroxyethyl acrylate, 10-15 parts of butyl acrylate, 4-8 parts of diacetone acrylamide, 20-30 parts of deionized water, 1-3 parts of emulsifier, 6-8 parts of polyamic acid crosslinking agent, and 2-5 parts of ammonium persulfate.

[0015] Furthermore, the preparation method of the polyamic acid cross-linking agent comprises the following steps:

[0016] Ⅰ: Add polyamic acid to dimethyl sulfoxide, stir and mix evenly, use nitrogen as protective gas, exhaust the air, then add allyl glycidyl ether, raise the system temperature to 70-80°C, continue to add catalyst, after adding, keep warm and stir for 8-10 hours, cool to room temperature and then discharge to obtain modified polyamic acid;

[0017] Ⅱ: Mix the modified polyamic acid and toluene, stir well, raise the temperature to 60-70°C, pass nitrogen protection, then add dichloromethylsilane and triethylamine. After adding, stir and react for 4-6 hours, wait for the material to cool naturally, discharge the material, and obtain the polyamic acid crosslinking agent.

[0018] Furthermore, in step I, the weight average molecular weight of the polyamic acid is 1000 to 2000.

[0019] Furthermore, in step I, the catalyst is any one of benzyltriethylammonium bromide, tetrabutylammonium bromide or tetrabutylammonium hydrogen sulfate.

[0020] Through the above technical scheme, under the action of a catalyst, the carboxyl group in the polyamic acid structure can undergo a ring-opening reaction with the epoxy group in the allyl glycidyl ether structure, thereby introducing an alkenyl group into the polyamic acid structure to obtain a modified polyamic acid. Since active hydroxyl groups are generated during the ring-opening process, the active hydroxyl groups can react with Si-Cl in the dichloromethylsilane structure under the action of triethylamine, thereby grafting dichloromethylsilane into the polyamic acid structure to obtain a polyamic acid crosslinking agent.

[0021] Furthermore, the preparation method of the wear-resistant filler comprises the following steps:

[0022] S1: adding serpentine powder to N,N-dimethylformamide, ultrasonically dispersing until a uniform dispersion is formed, adding guanidine acetate and a catalyst to the dispersion, raising the system temperature to 100-110° C., stirring for 4-6 hours, and then filtering, washing, vacuum drying, collecting the product, and obtaining modified serpentine powder;

[0023] S2: The aramid fiber is soaked in anhydrous ethanol, ultrasonically cleaned for 45 to 50 hours, then cleaned with deionized water for 5 to 8 times, and then placed in an oven at 50 to 80°C for drying to obtain dried aramid fiber. Then, the aramid fiber, potassium hydroxide and dimethyl sulfoxide are added to the reactor and stirred at room temperature for 6 to 8 days. When the mixed solution turns dark red and forms a uniform transparent liquid, the stirring is stopped to obtain an aramid fiber dispersion.

[0024] S3: Add the modified serpentine powder to the aramid fiber dispersion, disperse it by ultrasonic for 1 to 2 hours, let it stand for 30 to 50 minutes, and then filter and collect the product to obtain the wear-resistant filler.

[0025] Furthermore, in step S1, the catalyst is any one of aminosulfonic acid, p-toluenesulfonic acid or trifluoromethanesulfonic acid.

[0026] Furthermore, in step S2, the diameter of the aramid fiber is 2-5 μm, and the length is 2-6 mm.

[0027] Through the above technical scheme, under the action of a catalyst, the hydroxyl groups on the surface of the serpentine powder can react with the carboxyl groups in the guanidine acetate structure to obtain modified serpentine powder, and then the positive charge of the guanidine groups modified on its surface is used to electrostatically adsorb with the negatively charged aramid fiber dispersion to combine the serpentine powder with the aramid fiber to obtain a wear-resistant filler.

[0028] Furthermore, the pigment is any one of Pigment Violet 29, Phthalocyanine Blue B, Pigment Yellow 110, Magenta 6B or Pigment Black 7; the UV absorber is any one of UV-234, UV-531 or UV-360; the film-forming aid is any one of propylene glycol, propylene glycol methyl ether or ethylene glycol butyl ether; the defoaming agent is any one of dimethyl silicone oil and fatty alcohol polyoxyethylene ether; the leveling agent is any one of polydimethylsiloxane, polybutyl acrylate or polyethyl acrylate.

[0029] A process for producing an environmentally friendly composite pigment comprises the following steps:

[0030] The acrylic polymer emulsion is fully stirred and mixed with talcum powder, wear-resistant filler, pigment, ultraviolet absorber, film-forming aid, defoamer and leveling agent, and after natural defoaming, an environmentally friendly composite pigment is obtained.

[0031] Beneficial effects of the present invention:

[0032] (1) The present invention prepares a polyamic acid crosslinking agent, which contains a polymerizable unsaturated olefin functional group. Under the action of ammonium persulfate, the polyamic acid crosslinking agent can undergo crosslinking polymerization with a polymerizable monomer such as acrylic acid, and has a large crosslinking density, which can make the polyamic acid crosslinking agent have a greater cohesive force and improve the adhesion of the composite pigment. After crosslinking, the rigid benzene ring and the high bond energy silicon oxygen bond can be introduced into the main chain of the acrylic polymer, thereby improving the stability of the acrylic polymer molecular chain and enhancing the high temperature resistance of the composite pigment, effectively avoiding the problems of discoloration, fading or decomposition of the composite pigment under high temperature conditions. At the same time, the low surface energy organic silicon has anti-fouling properties, thereby effectively improving the anti-fouling performance of the composite pigment. In addition, the polyamic acid crosslinking agent contains ether bonds, which can generate a large number of hydrogen bonds with the matrix material, thereby further improving the adhesion of the composite pigment, avoiding the problems of pigment shedding or peeling, and extending the service life of the composite pigment.

[0033] (2) The present invention combines serpentine powder and aramid fiber tightly through the effect of electrostatic adsorption to prepare a wear-resistant filler. After the serpentine powder in the wear-resistant filler is modified with organic matter, good affinity between the serpentine powder and the pigment matrix can be achieved, so that the serpentine powder is evenly dispersed in the pigment matrix. On the one hand, the serpentine powder and the aramid fiber can play a role similar to that of "balls" in rolling bearings, reducing the friction coefficient of the interface, thereby improving the wear resistance of the pigment and avoiding problems such as wear, peeling or scratches when the pigment is subjected to friction or external force. On the other hand, when the pigment is subjected to external force, the aramid fiber can disperse and transfer stress, thereby significantly improving the mechanical properties of the pigment, helping to protect the substrate of the coated object, extending its service life, and improving the overall appearance quality and use effect.

[0034] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0036] Figure 1 This is an infrared spectrum test chart of the polyamic acid and the polyamic acid cross-linking agent prepared in Example 1 of the present invention.

[0037] Figure 2 This is a scanning electron microscope image of the aramid fiber and wear-resistant filler prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] 1. Polyamic acid crosslinking agent

[0041] Ⅰ: Add 5g of polyamic acid with a weight average molecular weight of 1000 to dimethyl sulfoxide, stir and mix evenly, use nitrogen as a protective gas to exhaust the air, then add 1.3g of allyl glycidyl ether, raise the system temperature to 75°C, continue to add 0.2g of benzyltriethylammonium bromide, and after the addition is complete, keep warm and stir for 9h, cool to room temperature and then discharge to obtain modified polyamic acid;

[0042] Ⅱ: Mix 5g of modified polyamic acid with toluene, stir well, raise the temperature to 65°C, pass nitrogen protection, then add 0.8g of dichloromethylsilane and 0.05g of triethylamine. After adding, stir and react for 5h, wait for the material to cool naturally, discharge the material, and obtain a polyamic acid crosslinking agent.

[0043] The polyamide acid and polyamide acid crosslinking agent were tested by infrared spectrometer Vertex 70v of Bruker Company, USA. Figure 1 As shown, analysis shows that in the infrared spectrum of polyamic acid, 3011cm -1 The absorption peak of CH on the benzene ring is 3129cm -1 The absorption peak of -NH in the amide bond is 1657cm -1 The absorption peak of C=O in the amide bond is 1739 cm -1 The absorption peak of the carboxyl group C=O is at 3126cm -1 The absorption peak of -NH in the amide bond is 1660 cm -1 The absorption peak of C=O in the amide bond is 3012 cm -1 The absorption peak of CH on the benzene ring is 1604cm -1 The absorption peak of CC on the benzene ring is 1741cm -1 The absorption peak of the ester group C=O is 3054 cm -1 The absorption peak of the carbon-hydrogen bond in the carbon-carbon double bond is 1025cm -1 The absorption peak of ether bond COC is 1075cm -1 It is the absorption peak of SiO, because the carboxyl group in the polyamic acid structure can undergo a ring-opening reaction with the epoxy group in the allyl glycidyl ether structure, and then the active hydroxyl group produced by the ring-opening reaction can react with the Si-C l in the dichloromethylsilane structure, thereby grafting dichloromethylsilane into the polyamic acid structure to obtain a polyamic acid crosslinker.

[0044] 2. Preparation of wear-resistant filler

[0045] S1: 3 g of serpentine powder was added to N, N-dimethylformamide, and ultrasonically dispersed to form a uniform dispersion, and 1.9 g of guanidine acetate and 0.2 g of p-toluenesulfonic acid were added to the dispersion, and the system temperature was raised to 105 ° C. The mixture was stirred for 5 h, and then filtered, washed, and vacuum dried to collect the product to obtain modified serpentine powder;

[0046] S2: Aramid fibers with a diameter of 4 μm and a length of 2 mm were soaked in anhydrous ethanol, ultrasonically cleaned for 48 h, then washed with deionized water for 7 times, and then dried in an oven at 60°C to obtain dried aramid fibers. Then, 1 g of aramid fibers, 1.5 g of potassium hydroxide and 100 ml of dimethyl sulfoxide were added to the reactor and stirred at room temperature for 7 days. When the mixed solution turned dark red and formed a uniform transparent liquid, stirring was stopped to obtain an aramid fiber dispersion.

[0047] S3: Add 2 g of modified serpentine powder to the aramid fiber dispersion, disperse it by ultrasonic for 1.5 h, let it stand for 40 min, and then filter and collect the product to obtain a wear-resistant filler.

[0048] The morphology of aramid fiber and wear-resistant filler was analyzed using a Quanta 250FEG scanning electron microscope. The test results are shown in Figure 2 , where A is aramid fiber and B is wear-resistant filler. It can be observed from the figure that the surface of aramid fiber is relatively smooth and the edge is regular, while the surface morphology of the wear-resistant filler changes significantly and becomes rough. This is because the aramid fiber and serpentine powder are tightly combined through electrostatic adsorption, so the surface roughness of the wear-resistant filler increases.

[0049] 3. Preparation of environmentally friendly composite pigments

[0050] (1) 30 g of acrylic acid, 10 g of hydroxyethyl acrylate, 10 g of butyl acrylate, and 4 g of diacetone acrylamide were uniformly mixed to obtain a mixed monomer;

[0051] (2) Add 1 g of emulsifier and 20 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 70° C., then add 5% of the mass of the mixed monomer and 0.2 g of ammonium persulfate, and keep warm for 10 min after the addition is completed to obtain a seed emulsion;

[0052] (3) adding the remaining mixed monomers, 6 g of polyamic acid crosslinking agent and 1.8 g of ammonium persulfate to the reactor dropwise for about 3 h. After the addition is complete, the temperature is raised to 85° C. and kept for 40 min, then lowered to about 30° C., and the material is filtered through a 50-mesh gauze to obtain an acrylic polymer emulsion;

[0053] (4) 60 g of acrylic polymer emulsion, 4 g of talc, 4 g of wear-resistant filler, 10 g of pigment, 1 g of UV-234, 1 g of propylene glycol, 2 g of dimethyl silicone oil and 1 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0054] Example 2

[0055] Preparation of environmentally friendly composite pigments

[0056] (1) 35 g of acrylic acid, 15 g of hydroxyethyl acrylate, 12 g of butyl acrylate, and 6 g of diacetone acrylamide were uniformly mixed to obtain a mixed monomer;

[0057] (2) Add 2 g of emulsifier and 25 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 80° C., then add 10% of the mass of the mixed monomer and 0.3 g of ammonium persulfate, and keep warm for 15 min after the addition is completed to obtain a seed emulsion;

[0058] (3) adding the remaining mixed monomers, 7 g of polyamic acid crosslinking agent and 3 g of ammonium persulfate to the reactor dropwise for about 3.5 h. After the addition is complete, the temperature is raised to 90° C. and kept for 45 min, then lowered to about 40° C., and the material is filtered through 100-mesh gauze to obtain an acrylic polymer emulsion;

[0059] (4) 65 g of acrylic polymer emulsion, 6 g of talc, 5 g of wear-resistant filler, 15 g of pigment, 1.5 g of UV-234, 1.5 g of propylene glycol, 2.5 g of dimethyl silicone oil and 1.5 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0060] The preparation method of the polyamic acid crosslinking agent and the wear-resistant filler is the same as that in Example 1.

[0061] Example 3

[0062] Preparation of environmentally friendly composite pigments

[0063] (1) 40 g of acrylic acid, 20 g of hydroxyethyl acrylate, 15 g of butyl acrylate, and 8 g of diacetone acrylamide were mixed to obtain a mixed monomer;

[0064] (2) Add 3 g of emulsifier and 30 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 90° C., then add 15% of the mass of the mixed monomer and 0.5 g of ammonium persulfate, and keep warm for 20 min after the addition is completed to obtain a seed emulsion;

[0065] (3) adding the remaining mixed monomers, 8 g of polyamic acid crosslinking agent and 4.5 g of ammonium persulfate to the reactor dropwise for about 4 h. After the addition is completed, the temperature is raised to 95° C. and kept for 50 min, then the temperature is lowered to about 50° C., and the material is filtered through a 150-mesh gauze to obtain an acrylic polymer emulsion;

[0066] (4) 70 g of acrylic polymer emulsion, 8 g of talc, 6 g of wear-resistant filler, 20 g of pigment, 2 g of UV-234, 2 g of propylene glycol, 3 g of dimethyl silicone oil and 2 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0067] The preparation method of the polyamic acid crosslinking agent and the wear-resistant filler is the same as that in Example 1.

[0068] Comparative Example 1

[0069] Preparation of environmentally friendly composite pigments

[0070] (1) 35 g of acrylic acid, 15 g of hydroxyethyl acrylate, 12 g of butyl acrylate, and 6 g of diacetone acrylamide were uniformly mixed to obtain a mixed monomer;

[0071] (2) Add 2 g of emulsifier and 25 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 80° C., then add 10% of the mass of the mixed monomer and 0.3 g of ammonium persulfate, and keep warm for 15 min after the addition is completed to obtain a seed emulsion;

[0072] (3) adding the remaining mixed monomers, 7 g of polyamic acid crosslinking agent and 3 g of ammonium persulfate to the reactor dropwise for about 3.5 h. After the addition is complete, the temperature is raised to 90° C. and kept for 45 min, then lowered to about 40° C., and the material is filtered through 100-mesh gauze to obtain an acrylic polymer emulsion;

[0073] (4) 65 g of acrylic polymer emulsion, 6 g of talc, 15 g of pigment, 1.5 g of UV-234, 1.5 g of propylene glycol, 2.5 g of dimethyl silicone oil and 1.5 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0074] The preparation method of the polyamic acid crosslinking agent is the same as that in Example 1.

[0075] Comparative Example 2

[0076] Preparation of environmentally friendly composite pigments

[0077] (1) 35 g of acrylic acid, 15 g of hydroxyethyl acrylate, 12 g of butyl acrylate, and 6 g of diacetone acrylamide were uniformly mixed to obtain a mixed monomer;

[0078] (2) Add 2 g of emulsifier and 25 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 80° C., then add 10% of the mass of the mixed monomer and 0.3 g of ammonium persulfate, and keep warm for 15 min after the addition is completed to obtain a seed emulsion;

[0079] (3) adding the remaining mixed monomers and 3 g of ammonium persulfate dropwise into the reactor for about 3.5 h. After the addition is complete, the temperature is raised to 90° C. and kept for 45 min. The temperature is then lowered to about 40° C. and the material is filtered through a 100-mesh gauze to obtain an acrylic polymer emulsion.

[0080] (4) 65 g of acrylic polymer emulsion, 6 g of talc, 5 g of wear-resistant filler, 15 g of pigment, 1.5 g of UV-234, 1.5 g of propylene glycol, 2.5 g of dimethyl silicone oil and 1.5 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0081] The preparation method of the wear-resistant filler is the same as that in Example 1.

[0082] Comparative Example 3

[0083] Preparation of environmentally friendly composite pigments

[0084] (1) 35 g of acrylic acid, 15 g of hydroxyethyl acrylate, 12 g of butyl acrylate, and 6 g of diacetone acrylamide were uniformly mixed to obtain a mixed monomer;

[0085] (2) Add 2 g of emulsifier and 25 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 80° C., then add 10% of the mass of the mixed monomer and 0.3 g of ammonium persulfate, and keep warm for 15 min after the addition is completed to obtain a seed emulsion;

[0086] (3) adding the remaining mixed monomers, 7 g of polyamic acid crosslinking agent and 3 g of ammonium persulfate to the reactor dropwise for about 3.5 h. After the addition is complete, the temperature is raised to 90° C. and kept for 45 min, then lowered to about 40° C., and the material is filtered through 100-mesh gauze to obtain an acrylic polymer emulsion;

[0087] (4) 65 g of acrylic polymer emulsion, 6 g of talc, 3 g of serpentine powder, 2 g of aramid fiber, 15 g of pigment, 1.5 g of UV-234, 1.5 g of propylene glycol, 2.5 g of dimethyl silicone oil and 1.5 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0088] The preparation method of the polyamic acid crosslinking agent is the same as that in Example 1.

[0089] Comparative Example 4

[0090] Preparation of environmentally friendly composite pigments

[0091] (1) 35 g of acrylic acid, 15 g of hydroxyethyl acrylate, 12 g of butyl acrylate, and 6 g of diacetone acrylamide were uniformly mixed to obtain a mixed monomer;

[0092] (2) Add 2 g of emulsifier and 25 g of deionized water into the reactor, turn on the mechanical stirrer, set the system temperature to 80° C., then add 10% of the mass of the mixed monomer and 0.3 g of ammonium persulfate, and keep warm for 15 min after the addition is completed to obtain a seed emulsion;

[0093] (3) adding the remaining mixed monomers and 3 g of ammonium persulfate dropwise into the reactor for about 3.5 h. After the addition is complete, the temperature is raised to 90° C. and kept for 45 min. The temperature is then lowered to about 40° C. and the material is filtered through a 100-mesh gauze to obtain an acrylic polymer emulsion.

[0094] (4) 65 g of acrylic polymer emulsion, 6 g of talc, 15 g of pigment, 1.5 g of UV-234, 1.5 g of propylene glycol, 2.5 g of dimethyl silicone oil and 1.5 g of polyethyl acrylate were fully stirred and mixed, and the mixture was naturally defoamed to obtain an environmentally friendly composite pigment.

[0095] Performance Testing

[0096] The environmentally friendly composite pigments prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were uniformly coated on the clean tinplate surface after sandblasting to prepare samples that met the specifications. After being thoroughly dried, performance tests were performed on the samples. Adhesion tests were performed on the samples according to GB / T 5210-2006 "Adhesion test for paints and varnishes by pull-off method"; the water-based coating samples were placed in an oven at 200°C for 12 hours, and the difference between the samples treated in the oven and the untreated samples was observed to evaluate the high temperature resistance of the samples; the wear resistance of the samples was tested according to GB / T 1768-2006 "Determination of wear resistance of paints and varnishes by rotating rubber grinding wheel method"; deionized water was dripped onto the surface of the film formed by the sample through a pinhole syringe, and the water contact angle of the film was measured using an SDC-100S contact angle tester. The test was performed at 5 different positions of each sample, and each position was measured twice, and the average of 10 values ​​was taken; according to GB / T 1732-2020 "Determination of impact resistance of paint film", the impact resistance of the samples was tested. The specific test results are shown in the table below:

[0097]

[0098] From the test results in the above table, it can be seen that the samples prepared in Examples 1 to 3 all have excellent high temperature resistance, adhesion, wear resistance, antifouling and mechanical properties; in the sample prepared in Comparative Example 1, a polyamic acid cross-linking agent was added, and the high temperature resistance, adhesion and antifouling performance of the sample were good, but no wear-resistant filler was added. Compared with the embodiment, the wear resistance and mechanical properties of the sample were poor; in the sample prepared in Comparative Example 2, a wear-resistant filler was added, and the wear resistance and mechanical properties of the sample were good, but no polyamic acid cross-linking agent was added, and the adhesion and water contact angle values ​​of the sample decreased greatly, and obvious discoloration and blistering occurred, and the high temperature resistance of the sample was poor. The performance, adhesion and antifouling properties are poor; in the sample prepared in Comparative Example 3, polyamic acid cross-linking agent, serpentine powder and aramid fiber were added, and the high temperature resistance, adhesion and antifouling properties of the sample were good. Compared with the examples, the wear resistance and mechanical properties of the sample were average. It is speculated that this may be because the serpentine powder and aramid fiber were not modified, and agglomeration occurred in the matrix, resulting in a decrease in the wear resistance and mechanical properties of the sample; in the sample prepared in Comparative Example 4, neither polyamic acid cross-linking agent nor wear-resistant filler was added. Compared with the examples, the high temperature resistance, adhesion, wear resistance, antifouling and mechanical properties of the sample were very poor.

[0099] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. An environmentally friendly composite pigment, It is characterized in that The invention comprises the following raw materials in parts by weight: 60 to 70 parts of acrylic polymer emulsion, 4 to 8 parts of talc powder, 4 to 6 parts of wear-resistant filler, 10 to 20 parts of pigment, 1 to 2 parts of ultraviolet absorber, 1 to 2 parts of film-forming aid, 2 to 3 parts of defoamer, and 1 to 2 parts of leveling agent; The preparation method of the acrylic acid polymer emulsion comprises the following steps: (1) mixing acrylic acid, hydroxyethyl acrylate, butyl acrylate and diacetone acrylamide to obtain a mixed monomer; (2) adding an emulsifier and deionized water into a reactor, turning on a mechanical stirrer, setting the system temperature to 70-90° C., then adding 5-10% by weight of a mixed monomer and ammonium persulfate, and keeping the temperature for 10-20 minutes after the addition is completed to obtain a seed emulsion; (3) adding the remaining mixed monomers, polyamic acid crosslinking agent and ammonium persulfate dropwise to the reactor for 3 to 4 hours. After the addition is completed, the temperature is raised to 85 to 95° C. and kept for 40 to 50 minutes, then the temperature is lowered to 30 to 50° C., and the material is filtered through a 50 to 150 mesh gauze to obtain an acrylic polymer emulsion; The acrylic polymer emulsion comprises the following raw materials in parts by weight: 30-40 parts of acrylic acid, 10-20 parts of hydroxyethyl acrylate, 10-15 parts of butyl acrylate, 4-8 parts of diacetone acrylamide, 20-30 parts of deionized water, 1-3 parts of emulsifier, 6-8 parts of polyamic acid crosslinking agent, and 2-5 parts of ammonium persulfate; The preparation method of the polyamic acid cross-linking agent comprises the following steps: Ⅰ: Add polyamic acid to dimethyl sulfoxide, stir and mix evenly, use nitrogen as protective gas, exhaust the air, then add allyl glycidyl ether, raise the system temperature to 70-80°C, continue to add catalyst, after adding, keep warm and stir for 8-10 hours, cool to room temperature and then discharge to obtain modified polyamic acid; Ⅱ: Mix the modified polyamic acid and toluene, stir well, raise the temperature to 60-70°C, pass nitrogen protection, then add dichloromethylsilane and triethylamine, stir and react for 4-6 hours after adding, wait for the material to cool naturally, discharge the material, and obtain the polyamic acid crosslinking agent; The preparation method of the wear-resistant filler comprises the following steps: S1: adding serpentine powder to N,N-dimethylformamide, ultrasonically dispersing until a uniform dispersion is formed, adding guanidine acetate and a catalyst to the dispersion, raising the system temperature to 100-110° C., stirring for 4-6 hours, and then filtering, washing, vacuum drying, collecting the product, and obtaining modified serpentine powder; S2: The aramid fiber is soaked in anhydrous ethanol, ultrasonically cleaned for 45 to 50 hours, then cleaned with deionized water for 5 to 8 times, and then placed in an oven at 50 to 80°C for drying to obtain dried aramid fiber. Then, the aramid fiber, potassium hydroxide and dimethyl sulfoxide are added to the reactor and stirred at room temperature for 6 to 8 days. When the mixed solution turns dark red and forms a uniform transparent liquid, the stirring is stopped to obtain an aramid fiber dispersion. S3: Add the modified serpentine powder to the aramid fiber dispersion, disperse it by ultrasonic for 1 to 2 hours, let it stand for 30 to 50 minutes, and then filter and collect the product to obtain the wear-resistant filler.

2. An environmentally friendly composite pigment according to claim 1, It is characterized in that In step I, the weight average molecular weight of the polyamic acid is 1000-2000.

3. An environmentally friendly composite pigment according to claim 1, It is characterized in that In step I, the catalyst is any one of benzyltriethylammonium bromide, tetrabutylammonium bromide or tetrabutylammonium hydrogen sulfate.

4. An environmentally friendly composite pigment according to claim 1, It is characterized in that In step S1, the catalyst is any one of aminosulfonic acid, p-toluenesulfonic acid or trifluoromethanesulfonic acid.

5. An environmentally friendly composite pigment according to claim 1, It is characterized in that In step S2, the aramid fiber has a diameter of 2 to 5 μm and a length of 2 to 6 mm.

6. An environmentally friendly composite pigment according to claim 1, It is characterized in that The pigment is any one of Pigment Violet 29, Phthalocyanine Blue B, Pigment Yellow 110, Magenta 6B or Pigment Black 7; the UV absorber is any one of UV-234, UV-531 or UV-360; the film-forming aid is any one of propylene glycol, propylene glycol methyl ether or ethylene glycol butyl ether; the defoaming agent is any one of dimethyl silicone oil and fatty alcohol polyoxyethylene ether; the leveling agent is any one of polydimethylsiloxane, polybutyl acrylate or polyethyl acrylate.

7. The process for producing an environmentally friendly composite pigment as claimed in claim 1, It is characterized in that The manufacturing process comprises the following steps: The acrylic polymer emulsion is fully stirred and mixed with talcum powder, wear-resistant filler, pigment, ultraviolet absorber, film-forming aid, defoamer and leveling agent, and after natural defoaming, an environmentally friendly composite pigment is obtained.

Citation Information

Patent Citations

  • A method for preparing high-performance environmentally friendly color composite pigments

    CN115304934B

  • Aqueous concoction, aqueous polymer emulsion prepared from same and application thereof

    CN101838370A

  • Oily heat dissipation coating for thin-film capacitor casing and preparation method of heat dissipation coating

    CN106433421A

  • Acrylate emulsion with composite cross-linking function and preparation method of acrylate emulsion

    CN107641175A

  • Preparation process of environment-friendly water-based ink

    CN111423765A