Method for preparing titanium-based pt-tio2 / ief-11 composite photocatalyst

By preparing a titanium-based Pt-TiO2/IEF-11 composite photocatalyst, the problem of low CO2 reduction efficiency was solved, achieving the effect of efficient CO2 reduction into valuable chemicals, which is suitable for large-scale production.

CN118268039BActive Publication Date: 2026-11-10HANGZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410359778.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2026-11-10
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively convert CO2 into valuable chemicals and energy, and traditional photocatalysts are inefficient in the CO2 reduction process.

Method used

A titanium-based Pt-TiO2/IEF-11 composite photocatalyst was prepared by introducing a portion of TiO2 through calcination and a trace amount of Pt promoter through photodeposition technology, resulting in a catalyst with a large specific surface area and dispersed active sites.

Benefits of technology

It achieves efficient CO2 reduction with a CO yield of over 4.4 μmol/(g·h), making it suitable for large-scale production applications. Furthermore, the preparation method is mild and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118268039B_ABST
    Figure CN118268039B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst. According to the method, square acid is added into isopropyl alcohol, magnetic stirring and ultrasonic treatment are carried out, glacial acetic acid is added, and ultrasonic treatment is carried out again; a Ti precursor is added, an orange suspension is obtained after heating, and the orange suspension is sealed and heated; filtration, washing and drying are carried out to obtain a precursor; the precursor is calcined and dispersed in a mixed solution of H2O and MeOH, an aqueous solution of chloroplatinic acid hexahydrate is added, the system is purged with Ar, and irradiation is carried out under a UV-Vis lamp; after filtration, washing and drying, the target product is obtained. The titanium-based Pt-TiO2 / IEF-11 composite photocatalyst prepared by the method has the advantages of a large specific surface area, active site dispersion and the like, the synthesis method has the characteristics of mild conditions, high yield and the like, and is suitable for large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalyst technology, especially the field of photocatalytic carbon dioxide (CO2) reduction, and specifically relates to a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst and its preparation method. Background Technology

[0002] With increasing use of resources such as oil, timber, and coal, more CO2 is generated, leading to the greenhouse effect and global warming. The greenhouse effect has many adverse effects on people's lives and production, including: increased land drought and desertification; increased pests and diseases; abnormal climate and more frequent ocean storms; and rising sea levels. Excessive CO2 emissions are a major contributing factor to global warming and extreme weather events. Therefore, the targeted conversion of CO2 into valuable chemicals, energy, and materials has become a hot topic with enormous application potential, which can alleviate environmental problems and reduce human dependence on fossil fuels. Scientists have explored a large number of CO2 reduction photocatalysts. Metal-organic frameworks (MOFs) are a class of organic-inorganic hybrid materials composed of organic ligands and inorganic metal ions or clusters through coordination bonds. By selecting different organic ligands and metal ions or changing the synthesis strategy, their function and activity can be effectively tuned and enhanced. Therefore, MOFs have a wide range of applications and promising prospects in CO2RR photocatalysis. Summary of the Invention

[0003] The purpose of this invention is to provide a method for preparing a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0004] The method of this invention is as follows:

[0005] Step (1) Add isopropanol to the container, then add squaric acid with an average particle size of 10-100 mesh after grinding, stir magnetically at 20-25°C for 5-10 minutes, and then sonicate for 10-30 minutes; 1g of squaric acid corresponds to 300-400mL of isopropanol.

[0006] Step (2) Add glacial acetic acid and sonicate again for 10-30 minutes; add 200-300 mL of glacial acetic acid for every 1 g of squaric acid.

[0007] Step (3) Add Ti precursor under stirring, and then heat at 50-70°C for 30-60 minutes; the molar ratio of added squaric acid to Ti precursor is 1:1; the Ti precursor is tetrabutyl titanate Ti(OBu)4 or tetraisopropoxide titanium Ti(iPrO)4.

[0008] Step (4) Seal the obtained orange suspension and heat it at 110–130°C for 24–48 hours, with a heating and cooling rate of 1–2°C·min during the process. -1 ;

[0009] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0010] Step (6) Calcine the dried precursor at 300-400℃ for 5-30 minutes, with a heating and cooling rate of 4-6℃·min during the process. -1 ;

[0011] Step (7) Disperse the calcined product in a quartz tube containing a mixed solution. The mixed solution is a mixture of H2O and MeOH with a volume ratio of 1:1 to 2. 1g of the calcined product is dispersed in 320 to 480mL of the mixed solution.

[0012] Step (8) Add 1-2 g·L to the quartz tube -1 Add 1g of the calcined product to 10-30mL of chloroplatinic acid hexahydrate aqueous solution; then purge the system with Ar for 30-60 minutes, and then irradiate the mixture with a UV-Vis lamp for 3-5 hours;

[0013] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 60-100℃ for 12-24 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0014] This invention utilizes a calcination method to introduce a portion of TiO2 and employs photodeposition technology to introduce trace amounts of Pt catalyst, successfully achieving the application of Ti-MOF photocatalysis in CO2 reduction, providing another option for CO2 reduction. The titanium-based Pt-TiO2 / IEF-11 composite photocatalyst prepared by this invention possesses advantages such as large specific surface area and dispersed active sites, exhibiting excellent performance and a CO yield exceeding 4.4 μmol / (g·h). The synthesis method provided by this invention features relatively mild conditions and high yield, making it suitable for large-scale production applications. Attached Figure Description

[0015] Figure 1 The XRD pattern of a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst prepared according to an embodiment of the present invention is shown.

[0016] Figure 2 This is a TEM image of a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst prepared according to an embodiment of the present invention;

[0017] Figure 3This is a SEM image of a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst prepared according to an embodiment of the present invention;

[0018] Figure 4 This is a graph showing the change in CO content over time as detected by gas chromatograph for a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst prepared according to an embodiment of the present invention. Detailed Implementation

[0019] Example 1.

[0020] Step (1) Add 300mL of isopropanol to the container, then add 1g of squaric acid with an average particle size of 20 mesh after grinding, stir magnetically for 8 minutes at 22℃, and then sonicate for 20 minutes.

[0021] Step (2) Add 200 mL of glacial acetic acid and sonicate again for 10 minutes;

[0022] Step (3) Add 2984 mg of Ti(OBu)4 with stirring, and then heat at 50°C for 60 minutes;

[0023] Step (4) Seal the obtained orange suspension and heat it at 120°C for 36 hours, with a heating and cooling rate of 1.5°C·min. -1 ;

[0024] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0025] Step (6) Calcine the precursor at 350°C for 25 minutes, with a heating and cooling rate of 5°C·min. -1 ;

[0026] Step (7) Weigh the calcined product and prepare a mixed solution according to the ratio of 350 mL per gram; the mixed solution is a 1:1 volume ratio of H2O and MeOH; disperse the calcined product in a quartz tube containing the mixed solution;

[0027] Step (8) According to the ratio of 15 mL for every gram of calcined product, add 1.5 g·L -1 An aqueous solution of chloroplatinic acid hexahydrate was added to a quartz tube; then the system was purged with Ar for 40 minutes, and the mixture was irradiated with a UV-Vis lamp for 4 hours.

[0028] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 100°C for 12 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0029] Example 2.

[0030] Step (1) Add 350 mL of isopropanol to the container, then add 1 g of squaric acid with an average particle size of 10 mesh after grinding, stir magnetically for 8 minutes at 23°C, and then sonicate for 10 minutes.

[0031] Step (2) Add 220 mL of glacial acetic acid and sonicate again for 20 minutes;

[0032] Step (3) Add 2492 mg of Ti(iPrO)4 with stirring, and then heat at 55°C for 50 minutes;

[0033] Step (4) Seal the obtained orange suspension and heat it at 110°C for 48 hours, with a heating and cooling rate of 1°C·min. -1 ;

[0034] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0035] Step (6) Calcine the precursor at 300°C for 30 minutes, with a heating and cooling rate of 4°C·min. -1 ;

[0036] Step (7) Weigh the calcined product and prepare a mixed solution according to the ratio of 320 mL per gram; the mixed solution is a mixture of H2O and MeOH with a volume ratio of 1:2; disperse the calcined product in a quartz tube containing the mixed solution;

[0037] Step (8) According to the ratio of 10 mL for every gram of calcined product, add 2 g·L -1 An aqueous solution of chloroplatinic acid hexahydrate was added to a quartz tube; then the system was purged with Ar for 35 minutes, and the mixture was irradiated with a UV-Vis lamp for 4.5 hours.

[0038] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 85°C for 15 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0039] Example 3.

[0040] Step (1) Add 400mL of isopropanol to the container, then add 1g of squaric acid with an average particle size of 30 mesh after grinding, stir magnetically for 7 minutes at 22℃, and then sonicate for 30 minutes.

[0041] Step (2) Add 280 mL of glacial acetic acid and sonicate again for 25 minutes;

[0042] Step (3) Add 2984 mg of Ti(OBu)4 with stirring, and then heat at 60°C for 45 minutes;

[0043] Step (4) Seal the obtained orange suspension and heat it at 130°C for 24 hours, with a heating and cooling rate of 2°C·min. -1 ;

[0044] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0045] Step (6) Calcine the precursor at 400℃ for 5 minutes, with a heating and cooling rate of 4.5℃·min. -1 ;

[0046] Step (7) Weigh the calcined product and prepare a mixed solution according to the ratio of 360 mL per gram; the mixed solution is a mixture of H2O and MeOH in a volume ratio of 2:3; disperse the calcined product in a quartz tube containing the mixed solution;

[0047] Step (8) According to the ratio of 30 mL for every gram of calcined product, add 1 g·L -1 An aqueous solution of chloroplatinic acid hexahydrate was added to a quartz tube; then the system was purged with Ar for 50 minutes, and the mixture was irradiated with a UV-Vis lamp for 3.5 hours.

[0048] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 65°C for 24 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0049] Example 4.

[0050] Step (1) Add 380mL of isopropanol to the container, then add 1g of squaric acid with an average particle size of 50 mesh after grinding, stir magnetically for 6 minutes at 24℃, and then sonicate for 15 minutes.

[0051] Step (2) Add 240 mL of glacial acetic acid and sonicate again for 20 minutes;

[0052] Step (3) Add 2492 mg of Ti(iPrO)4 with stirring, and then heat at 65°C for 40 minutes;

[0053] Step (4) Seal the obtained orange suspension and heat it at 115°C for 45 hours, with a heating and cooling rate of 2°C·min during the process. -1 ;

[0054] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0055] Step (6) involves calcining the precursor at 320°C for 25 minutes, with a heating and cooling rate of 5.5°C·min. -1 ;

[0056] Step (7) Weigh the calcined product and prepare a mixed solution according to the ratio of 400 mL per gram; the mixed solution is a 1:1 volume ratio of H2O and MeOH; disperse the calcined product in a quartz tube containing the mixed solution;

[0057] Step (8) According to the ratio of 15 mL for every gram of calcined product, the product with a concentration of 1.8 g·L⁻¹ is added. -1 An aqueous solution of chloroplatinic acid hexahydrate was added to a quartz tube; then the system was purged with Ar for 60 minutes, and the mixture was irradiated with a UV-Vis lamp for 3 hours.

[0058] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 70°C for 20 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0059] Example 5.

[0060] Step (1) Add 330mL of isopropanol to the container, then add 1g of squaric acid with an average particle size of 100 mesh after grinding, stir magnetically for 10 minutes at 20℃, and then sonicate for 25 minutes.

[0061] Step (2) Add 300 mL of glacial acetic acid and sonicate again for 15 minutes;

[0062] Step (3) Add 2984 mg of Ti(OBu)4 with stirring, and then heat at 70°C for 30 minutes;

[0063] Step (4) Seal the obtained orange suspension and heat it at 125°C for 30 hours, with a heating and cooling rate of 1.5°C·min. -1 ;

[0064] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0065] Step (6) Calcine the precursor at 360°C for 15 minutes, with a heating and cooling rate of 6°C·min. -1 ;

[0066] Step (7) Weigh the calcined product and prepare a mixed solution according to the ratio of 480 mL per gram; the mixed solution is a mixture of H2O and MeOH with a volume ratio of 1:2; disperse the calcined product in a quartz tube containing the mixed solution;

[0067] Step (8) According to the ratio of 25 mL for every gram of calcined product, the product with a concentration of 1.2 g·L⁻¹ is added. -1An aqueous solution of chloroplatinic acid hexahydrate was added to a quartz tube; then the system was purged with Ar for 30 minutes, and the mixture was irradiated with a UV-Vis lamp for 5 hours.

[0068] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 60°C for 24 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0069] Example 6.

[0070] Step (1) Add 320mL of isopropanol to the container, then add 1g of squaric acid with an average particle size of 60 mesh after grinding, stir magnetically for 5 minutes at 25℃, and then sonicate for 20 minutes.

[0071] Step (2) Add 250 mL of glacial acetic acid and sonicate again for 30 minutes;

[0072] Step (3) Add 2492 mg of Ti(iPrO)4 with stirring, and then heat at 60°C for 40 minutes;

[0073] Step (4) Seal the obtained orange suspension and heat it at 120°C for 40 hours, with a heating and cooling rate of 1°C·min. -1 ;

[0074] Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor;

[0075] Step (6) Calcine the precursor at 350°C for 20 minutes, with a heating and cooling rate of 5°C·min during the process. -1 ;

[0076] Step (7) Weigh the calcined product and prepare a mixed solution according to the ratio of 450 mL per gram; the mixed solution is a mixture of H2O and MeOH in a volume ratio of 2:3; disperse the calcined product in a quartz tube containing the mixed solution;

[0077] Step (8) According to the ratio of 20 mL for every gram of calcined product, add 1.5 g·L -1 An aqueous solution of chloroplatinic acid hexahydrate was added to a quartz tube; then the system was purged with Ar for 45 minutes, and the mixture was irradiated with a UV-Vis lamp for 4 hours.

[0078] Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 80°C for 18 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.

[0079] The XRD pattern of the prepared titanium-based Pt-TiO2 / IEF-11 composite photocatalyst is shown below. Figure 1As shown, the strongest diffraction peak in the product's diffraction data corresponds to the standard diffraction peak of IEF-1, and characteristic diffraction peaks of TiO2 can be observed in the sample. This indicates that IEF-1 was successfully synthesized, and that IEF-1 and TiO2 coexist in the sample.

[0080] TEM image of the prepared titanium-based Pt-TiO2 / IEF-11 composite photocatalyst is shown below. Figure 2 As shown, the SEM image is as follows: Figure 3 As shown, by Figure 2 and Figure 3 The projection and scanning electron microscope images show that the product has a uniformly sized cylindrical three-dimensional structure.

[0081] The graph shows the change in CO concentration over time as detected by gas chromatography for this composite photocatalyst. Figure 4 As shown, the product CO changes over time. Data was collected every hour for product testing. The slope, after unit conversion, represents the CO yield, which is 4.46 μmol / (g·h).

[0082] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. The application of titanium-based Pt-TiO2 / IEF-11 composite material in photocatalytic reduction of CO2, characterized in that, The preparation method of the titanium-based Pt-TiO2 / IEF-11 composite material is as follows: Step (1) Add isopropanol to the container, then add squaric acid with an average particle size of 10-100 mesh after grinding, stir magnetically at 20-25°C for 5-10 minutes, and then sonicate for 10-30 minutes; 1g of squaric acid corresponds to 300-400mL of isopropanol. Step (2) Add glacial acetic acid and sonicate again for 10-30 minutes; add 200-300 mL of glacial acetic acid for every 1 g of squaric acid. Step (3) Add Ti precursor under stirring, and then heat at 50-70°C for 30-60 minutes; the molar ratio of added squaric acid to Ti precursor is 1:1; the Ti precursor is Ti(OBu)4 or Ti(iPrO)4; Step (4) Seal the obtained orange suspension and heat it at 110–130°C for 24–48 hours, with a heating and cooling rate of 1–2°C·min during the process. -1 ; Step (5) Centrifuge and filter, wash the orange-brown solid obtained with i-PrOH, and dry it in the air at room temperature to obtain the precursor; Step (6) Calcine the dried precursor at 300-400℃ for 5-30 minutes, with a heating and cooling rate of 4-6℃·min during the process. -1 ; Step (7) Disperse the calcined product in a quartz tube containing a mixed solution. The mixed solution is a mixture of H2O and MeOH with a volume ratio of 1:1 to 2. 1g of the calcined product is dispersed in 320 to 480mL of the mixed solution. Step (8) Add 1-2 g·L to the quartz tube -1 Add an aqueous solution of chloroplatinic acid hexahydrate, then purge the system with Ar for 30-60 minutes, and then irradiate the mixture with a UV-Vis lamp for 3-5 hours. Add 1g of the calcined product to 10-30mL of the aqueous solution of chloroplatinic acid hexahydrate. Step (9) Centrifuge and filter, wash the obtained solid with water, and dry it in an oven at 60-100℃ for 12-24 hours to obtain a titanium-based Pt-TiO2 / IEF-11 composite photocatalyst.