Animal and plant-based elastic gas microporous shock-absorbing packaging material and preparation method thereof

Through the low-temperature extrusion closed-cell granulation and high-temperature foam injection molding process of animal and plant-based materials, animal and plant-based elastic gas microporous shock-absorbing packaging materials with gas micropores are prepared, which solves the problem of difficult recycling of existing elastic foam materials. The problems of insufficient utilization and biodegradability have been achieved, and the functional application and environmental performance improvement of materials have been realized.

CN118271684BActive Publication Date: 2024-10-22SHENZHEN GUANGJUTAI PLASTIC INDAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410298093.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2024-10-22
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

Existing elastic foam materials are difficult to recycle, difficult to degrade, and have insufficient biodegradation and environmental protection performance.

Method used

Using animal and plant-based materials and auxiliary materials, through low-temperature extrusion closed-cell granulation and high-temperature foam injection molding processes, animal and plant-based elastic gas microporous shock-absorbing packaging materials with gas micropores are prepared, realizing the functional application of the material. and biodegradability.

Benefits of technology

It replaces non-degradable plastic foam materials, has excellent rebound shock absorption and moisture resistance, and the materials and accessories used are mainly from nature, non-toxic and harmless, has good biodegradability and environmental friendliness, and saves money. Limited petroleum resources and promote waste recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118271684B_ABST
    Figure CN118271684B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of biodegradable materials, and discloses an animal and plant-based elastic gas microporous shock-absorbing packaging material and a preparation method thereof. The animal and plant-based materials and auxiliary materials with good biodegradability and non-toxicity are used, and composite crop waste is added as a filling material, thereby saving limited petroleum resources and realizing the recycling of wastes; gas is introduced into liquid and molten materials to form bubble nuclei, generate expanding and encapsulating micropores, and screened materials are used to fix the microporous structure in the materials, so that the prepared packaging material has light weight and good resilience; water is used as a foaming agent, a low-temperature closed-cell granulation process is adopted, a large number of gas-filled molecules that make the material foam and expand are stored, and a material with good pressure resistance, shock absorption and moisture resistance is prepared through a high-temperature injection foaming molding process, and the process is simple, which lays a good development foundation for the subsequent industrialization and market application of biodegradable materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biodegradable materials, in particular to an animal and plant-based elastic gas microporous shock-absorbing packaging material and a preparation method thereof. Background Art

[0002] At present, in the field of shock-absorbing packaging materials in China, traditional materials mainly based on petroleum-based rubber materials are still widely used. This type of petroleum-based rubber foam plastic is non-degradable after use and disposal.

[0003] At present, there is no unified international standardized definition of fully biodegradable materials in the world. The animal and plant-based elastic gas microporous shock-absorbing packaging material prepared by the present invention has the characteristics of biodegradability and environmental friendliness, and can partially replace traditional petroleum-based rubber foaming materials; the animal and plant-based elastic gas microporous shock-absorbing packaging material is a type of high molecular polymer material formed by a large number of gas micropores dispersed in an animal and plant-based biodegradable composite material, and its definition is: under specific environments, the chemical structure of animal and plant-based materials changes significantly, and microorganisms in the natural environment can biodegrade the molecular chains of materials in the waste treatment system. When microorganisms attack and erode natural high molecular materials, due to the growth of biological cells, the high molecular components are hydrolyzed, ionized or protonated, and then decomposed into oligomer fragments, and the polymer is gradually eroded and degraded by microorganisms in the natural environment; due to the direct action of microorganisms and enzymes, the polymer is decomposed or oxidized into small molecules, and finally decomposed into carbon dioxide and water, and enters the biological combined cycle process, and is completely absorbed by the environment without leaving any polymer.

[0004] The technical invention aims to reduce the harm to the environment and human life caused by petroleum-based plastics such as foam plastics, styrene-butadiene rubber, nitrile rubber, and toxic and harmful additives such as phthalate compounds and Freon foaming agents used in plastics, and to make up for the current situation of insufficient biodegradable and environmentally friendly performance of existing elastic foam materials at home and abroad. Therefore, the present invention also provides an animal and plant-based elastic gas microporous shock-absorbing packaging material and a preparation process method. Summary of the invention

[0005] The technical problem solved by the present invention is: to provide an animal and plant-based elastic gas microporous shock-absorbing packaging material and a preparation method, which solves the problem that the existing elastic foaming materials are difficult to recycle and degrade, and has excellent rebound shock absorption and moisture resistance.

[0006] The technical solution of the present invention is:

[0007] A method for preparing an animal and plant-based elastic gas microporous shock-absorbing packaging material, the preparation method is carried out according to the following steps:

[0008] (1) Add 30-47 parts of plant powder, 3-10 parts of aquatic animal powder and 3-10 parts of plant fiber by weight into a high-speed mixer, stir for 5-10 minutes at a temperature of 30-40° C. and a rotation speed of 4-8 Hz / min, and mix and disperse evenly to obtain an animal and plant-based main ingredient component 1.

[0009] (2) 8-11 parts of glycerol and 0.5-1 part of polyvinyl alcohol by weight are added to a temperature-controlled stirring reactor, stirred at a temperature of 95-110° C. and a rotation speed of 8-12 Hz / min for 10-20 min, and mixed evenly to form an oily colloidal material, thereby obtaining a colloidal material component 2.

[0010] (3) 4-5 parts by weight of siliceous hollow microspheres, 0.3-1.2 parts of surfactants, 0-0.5 parts of animal and plant waxes, 0-6 parts of additives and 27-33 parts of deionized water are added into a food blender, and after being mixed and dispersed uniformly, a material with micropores is formed to obtain an auxiliary material component 3.

[0011] (4) Add the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stir for 5-15 minutes at a temperature of 30-40° C. and a rotation speed of 6-10 Hz / min to obtain a synthetic material, and then add the synthetic material into a twin-screw extruder to perform low-temperature extrusion rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 15-25° C., the temperature of the second zone is 35-45° C., and the temperature of the third zone is 55-70° C. The extrusion and rotary cutting speeds are 15-25 Hz / min. After granulation is completed, add it into an injection molding machine, perform high-temperature injection foaming molding, and package and store to obtain an plant-based elastic gas microporous shock-absorbing packaging material.

[0012] Furthermore, the plant powder in step (1) is one or a combination of corn starch, sweet potato powder, cassava powder, soybean powder, oil residue powder, and potato powder; the oil residue powder is the residue powder remaining after oil is extracted from any one or more oil-containing plants.

[0013] Furthermore, the aquatic animal powder in step (1) is one or a combination of shrimp shell powder, mussel shell powder, clam shell powder, and fish scale powder; the shrimp shell powder is the shell of any one or more shrimps of marine shrimps and freshwater shrimps, which is crushed into 100-mesh shrimp powder after drying; the clam shell powder is the shell of aquatic mussels, which is dried and ground into 100-mesh clam shell powder; the fish scale powder is the outer scale of any one or more fish in seawater or freshwater, which is crushed into 100-mesh scale powder after drying; the clam shell powder is the shell of a shellfish in seawater and freshwater organisms, which is dried and ground into 100-mesh clam shell powder.

[0014] Furthermore, the plant fibers in step (1) are stem fibers of any one or more types of agricultural plants such as rice straw, stalks, and vines.

[0015] Furthermore, the model of the polyvinyl alcohol in step (2) is any one of the commercial models 2488 and 1788.

[0016] Furthermore, in step (3), the hollow silica microspheres have a true density of 0.20-0.60 g / cm 3 Ultra-light inorganic non-metallic material in the form of hollow spherical powder with a particle size of 2-125μm.

[0017] Furthermore, in step (3), the surfactant is coconut oil or fatty acid glyceride; the coconut oil refers to an active vegetable oil prepared by saponifying, acidifying, washing and dehydrating coconut, and the content of unsaturated fatty acids is more than 80%; the fatty acid oil is any one of monoglyceride or diglyceride.

[0018] Furthermore, in step (3), the animal or plant wax is palm wax or beeswax; and the additive is one or a combination of yeast powder, sodium bicarbonate, and talcum powder.

[0019] Furthermore, in step (3), the rotation speed of the food mixer is 140-160 Hz / min, and the mixing time is 7-12 min.

[0020] Furthermore, in step (4), the die opening of the twin-screw extruder equipment is 5-8 holes, and the die aperture is 2-4 mm.

[0021] The beneficial technical effects of the present invention are:

[0022] The present invention replaces non-degradable plastic foam elastic materials through optimized screening and formula combination preparation of natural biopolymer materials; adopts new technical means to optimize the design of the production process route, and adopts low-temperature extrusion closed-cell granulation and high-temperature foaming injection molding processes for animal and plant-based composite materials by physical foaming method to obtain animal and plant-based elastic gas microporous shock-absorbing packaging materials, thereby realizing the functional application of materials.

[0023] The plant-based materials and auxiliary materials used in the present invention are mainly derived from natural substances in nature, are non-toxic and harmless, have good biodegradability and environmental friendliness. At the same time, since the filling materials used in the materials are compositely composed of crop waste, they play a positive role in saving limited petroleum resources and recycling waste.

[0024] The present invention has the following effects and advantages in terms of material screening, formula combination and enhanced functionality: (1) introducing gas into liquid and molten materials to form bubble nuclei and produce encapsulated micropores; (2) causing the bubble micropores to expand during the preparation process; (3) utilizing the physical characteristics of the screened material itself to fix the microporous structure in the material; (4) the prepared material has light weight and good resilience.

[0025] The present invention uses water as a foaming agent and adds it to the material. Through a low-temperature closed-cell granulation process, a large number of gas-filled molecules that cause foaming and expansion are stored in the structural components of the material. When the material is subjected to high-temperature injection foaming molding by an injection molding machine, at room temperature and atmospheric pressure, the material enters a relatively free expansion space, and the gas-filled molecules expand naturally. The preparation process of the degradable material is implemented using general equipment, the process route is concise, and the operation is easy to popularize, which lays a good development foundation for the subsequent industrialization and market application of the degradable material. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the process flow of animal and plant-based elastic gas microporous shock-absorbing packaging materials. DETAILED DESCRIPTION

[0027] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0028] Example 1

[0029] (1) 45 parts of sweet potato flour, 2 parts of oil residue flour, 3 parts of clam shell flour and 3 parts of plant fiber by weight are added to a high-speed mixer, stirred at a temperature of 35° C. and a rotation speed of 6 Hz / min for 8 minutes, and after mixing and dispersing evenly, an animal and plant-based main ingredient component 1 is obtained.

[0030] (2) 8 parts of glycerol and 1 part of polyvinyl alcohol by weight were added into a temperature-controlled stirring reactor, stirred at a temperature of 100° C. and a rotation speed of 10 Hz / min for 15 min, and after being mixed evenly, an oily colloidal material was formed to obtain a colloidal material component 2.

[0031] (3) 4.5 parts by weight of siliceous hollow microspheres, 0.3 parts by weight of fatty acid glyceride, 0.2 parts by weight of palm wax and 33 parts by weight of deionized water were added into a food blender and stirred at a speed of 150 Hz / min for 8 min. After being mixed and dispersed uniformly, a material with micropores was formed to obtain an auxiliary material component 3.

[0032] (4) Add the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stir for 10 minutes at a temperature of 35° C. and a rotation speed of 8 Hz / min to obtain a synthetic material, and then add the synthetic material into a twin-screw extruder for low-temperature extrusion, rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 20° C., the temperature of the second zone is 40° C., and the temperature of the third zone is 60° C. The equipment mold opening is 6 holes, the mold aperture is 3 mm, the extrusion and rotary cutting speed is 20 Hz / min, and after the granulation is completed, it is added to an injection molding machine, subjected to high-temperature injection foaming molding, packaging and storage, to obtain an plant-based elastic gas microporous shock-absorbing packaging material.

[0033] Example 2

[0034] (1) 40 parts by weight of cassava flour, 5 parts by weight of potato flour, 5 parts by weight of fish scale powder and 5 parts by weight of plant fiber were added into a high-speed mixer, stirred at a temperature of 35° C. and a rotation speed of 6 Hz / min for 8 min, and mixed and dispersed uniformly to obtain an animal and plant-based main ingredient component 1.

[0035] (2) 11 parts of glycerol and 1 part of polyvinyl alcohol by weight were added into a temperature-controlled stirring reactor, stirred at a temperature of 110° C. and a rotation speed of 12 Hz / min for 10 min, and after being mixed evenly, an oily colloidal material was formed, thereby obtaining a colloidal material component 2.

[0036] (3) 5 parts by weight of siliceous hollow microspheres, 0.5 parts of fatty acid glyceride, 0.5 parts of palm wax and 27 parts of deionized water were added into a food blender and stirred at a speed of 140 Hz / min for 12 min. After being mixed and dispersed uniformly, a material with micropores was formed to obtain an auxiliary material component 3.

[0037] (4) Add the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stir for 15 minutes at a temperature of 40° C. and a rotation speed of 10 Hz / min to obtain a synthetic material, and then add the synthetic material into a twin-screw extruder for low-temperature extrusion, rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 25° C., the temperature of the second zone is 35° C., and the temperature of the third zone is 55° C. The equipment mold opening is 8 holes, the mold aperture is 4 mm, the extrusion and rotary cutting speed is 15 Hz / min, and after the granulation is completed, it is added to an injection molding machine, subjected to high-temperature injection foaming molding, packaging and storage, to obtain an plant-based elastic gas microporous shock-absorbing packaging material.

[0038] Example 3

[0039] (1) 30 parts by weight of soybean powder, 10 parts of clam shell powder, and 10 parts of plant fiber were added to a high-speed mixer, stirred at a temperature of 30° C. and a speed of 4 Hz / min for 10 min, and mixed and dispersed uniformly to obtain an animal and plant-based main ingredient component 1.

[0040] (2) 8 parts of glycerol and 0.8 parts of polyvinyl alcohol by weight were added to a temperature-controlled stirring reactor, stirred at a temperature of 95° C. and a rotation speed of 8 Hz / min for 20 min, and after being mixed evenly, an oily colloidal material was formed to obtain a colloidal material component 2.

[0041] (3) 4 parts by weight of siliceous hollow microspheres, 1.2 parts of fatty acid glyceride, 1 part of sodium bicarbonate, 5 parts of talc and 30 parts of deionized water were added into a food blender and stirred at a speed of 160 Hz / min for 7 min. After being mixed and dispersed uniformly, a material with micropores was formed to obtain an auxiliary material component 3.

[0042] (4) Add the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stir for 15 minutes at a temperature of 40° C. and a rotation speed of 6 Hz / min to obtain a synthetic material, and then add the synthetic material into a twin-screw extruder for low-temperature extrusion, rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 25° C., the temperature of the second zone is 45° C., and the temperature of the third zone is 70° C. The equipment mold opening is 5 holes, the mold aperture is 4 mm, the extrusion and rotary cutting speed is 25 Hz / min, and after the granulation is completed, it is added to an injection molding machine, subjected to high-temperature injection foaming molding, packaging and storage, to obtain an plant-based elastic gas microporous shock-absorbing packaging material.

[0043] Example 4

[0044] (1) 42 parts of corn starch, 8 parts of shrimp shell powder and 5 parts of plant fiber by weight are added to a high-speed mixer, stirred at a temperature of 35° C. and a rotation speed of 7 Hz / min for 9 minutes, and mixed and dispersed uniformly to obtain an animal and plant-based main ingredient component 1.

[0045] (2) 8 parts of glycerol and 0.6 parts of polyvinyl alcohol by weight were added to a temperature-controlled stirring reactor, stirred at a temperature of 105° C. and a rotation speed of 11 Hz / min for 18 minutes, and after being mixed evenly, an oily colloidal material was formed to obtain a colloidal material component 2.

[0046] (3) 4.4 parts of siliceous hollow microspheres, 1 part of coconut oil, 0.5 parts of beeswax, 1.5 parts of yeast powder, 2 parts of sodium bicarbonate and 27 parts of deionized water were added into a food blender, and stirred at a speed of 155 Hz / min for 9 minutes. After being mixed and dispersed uniformly, a material with micropores was formed to obtain an auxiliary material component 3.

[0047] (4) Add the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stir for 12 minutes at a temperature of 35° C. and a rotation speed of 9 Hz / min to obtain a synthetic material, and then add the synthetic material into a twin-screw extruder for low-temperature extrusion, rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 20° C., the temperature of the second zone is 45° C., and the temperature of the third zone is 65° C. The equipment mold opening is 7 holes, the mold aperture is 3 mm, the extrusion and rotary cutting speed is 25 Hz / min, and after the granulation is completed, it is added to an injection molding machine, subjected to high-temperature injection foaming molding, packaging and storage, to obtain an plant-based elastic gas microporous shock-absorbing packaging material.

[0048] Example 5

[0049] (1) 30 parts by weight of cassava flour, 5 parts by weight of potato flour, 10 parts by weight of fish scale powder and 5 parts by weight of plant fiber are added into a high-speed mixer, stirred at a temperature of 40° C. and a rotation speed of 5 Hz / min for 8 min, and mixed and dispersed uniformly to obtain an animal and plant-based main ingredient component 1.

[0050] (2) 10 parts by weight of glycerol and 1 part of polyvinyl alcohol were added to a temperature-controlled stirring reactor, stirred at a temperature of 110° C. and a rotation speed of 10 Hz / min for 15 min, and mixed evenly to form an oily colloidal material, thereby obtaining a colloidal material component 2.

[0051] (3) 5 parts by weight of siliceous hollow microspheres, 1 part of coconut oil, 0.2 parts of beeswax, 1.8 parts of sodium bicarbonate and 31 parts of deionized water were added into a food blender and stirred at a speed of 145 Hz / min for 9 minutes. After being mixed and dispersed uniformly, a material with micropores was formed to obtain an auxiliary material component 3.

[0052] (4) Add the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stir for 15 minutes at a temperature of 35° C. and a rotation speed of 9 Hz / min to obtain a synthetic material, and then add the synthetic material into a twin-screw extruder for low-temperature extrusion, rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 25° C., the temperature of the second zone is 40° C., and the temperature of the third zone is 70° C. The equipment mold opening is 6 holes, the mold aperture is 3 mm, the extrusion and rotary cutting speed is 20 Hz / min, and after the granulation is completed, it is added to an injection molding machine, subjected to high-temperature injection foaming molding, packaging and storage, to obtain an plant-based elastic gas microporous shock-absorbing packaging material.

[0053] Comparative Example 1

[0054] The apparent density is 2e -5 g / mm3 Expanded polystyrene (EPS) packaging material.

[0055] Comparative Example 2

[0056] Class III expanded polyethylene (EPE) packaging material specified in QB / T1649-92, with an apparent density of 2.58e -5 g / mm 3 .

[0057] Compression performance test: Prepare standard samples according to GB / T8168-2008, use compression testing machine to gradually increase the load on the sample along the thickness direction at a speed of 10mm / min, the compression load is 5N, and the compression stress calculation formula is Q=P / A×10 3 , where Q is the compressive stress (MPa), P is the compressive load (N), and A is the bearing area of ​​the specimen (mm 2 ).

[0058] Rebound performance test: Use a compression tester to load along the thickness direction of the test sample at a speed of 15mm / min. When the deformation is 50%, maintain the pressure for 3 minutes. After leaving it for 30 seconds, measure its thickness with a vernier caliper. Repeat the compression three times, and the time interval between repeated compressions is 1 minute. The calculation formula of the rebound rate is: t j =(T j -T i / 2) / (T i / 2)×100%, where t j is the rebound rate after j tests (%), j = 1, 2, 3; T i is the thickness before the i-th compression (mm), i = 1, 2, 3; T j is the thickness after j times of compression (mm), j=1,2,3.

[0059] Compression performance (MPa) Rebound rate (%) Example 1 4.12 89.1 Example 2 3.96 88.7 Example 3 4.08 90.0 Example 4 4.25 89.3 Example 5 4.17 88.6 Comparative Example 1 2.18 76.5 Comparative Example 2 2.53 85.2

[0060] The compression resistance and resilience are the most important mechanical performance indicators of packaging materials, which reflect the pressure bearing capacity of the material when subjected to external load impact and the recovery capacity of the material under multiple load impact conditions. It can be seen from the test results in the above table that the rebound rate of the animal and plant-based elastic gas microporous shock-absorbing packaging material prepared in the embodiment is higher than that of the expanded polystyrene packaging material of Comparative Example 1 and the expanded polyethylene material of Comparative Example 2. Therefore, the resilience performance of the packaging material of the present invention can meet the general packaging use requirements, avoid the gap between the packaged product and the outer packaging container, protect the packaged product from secondary impact, and have a shock-absorbing and buffering effect; this is because the filling material used in the present invention is a composite composition of crop waste, through the bonding effect of animal and plant powder and the mutual overlap of plant fibers, a uniform spatial network structure is formed inside the product, gas is introduced into the liquid and molten materials, bubble nuclei are formed, and encapsulated micropores are generated, so that the bubble micropores expand during the preparation process, which is conducive to the molded foaming, thereby improving the buffering performance of the product on the basis of ensuring the mechanical properties, so that the prepared material has light weight and good resilience.

[0061] The animal and plant-based elastic gas microporous shock-absorbing packaging material prepared by the present invention can completely replace non-degradable foamed polystyrene, foamed polyethylene materials and other cushioning packaging materials. The cushioning performance of the packaging material can fully meet the requirements for protecting products, and plays a positive role in saving limited petroleum resources and recycling waste.

[0062] Drop resistance test: Make the material to be tested into a packaging box shape, drop it from a height of 1m, and observe the damage of the material.

[0063] Moisture resistance test: In an environment with a relative humidity of 90%, place a 10kg weight on the packaging box made of the material to be tested for 48 hours, observe its deformation, then remove the weight, and then place it for 30 days, record whether the material is moldy or has any odor.

[0064]

[0065] It can be seen from the test results in the above table that the animal and plant-based elastic gas microporous shock-absorbing packaging material prepared by the present invention has good anti-fall performance, mainly because the material is a foamed product, and the air in the pores has good elasticity and cushioning performance, so that the prepared material has a good shock-absorbing effect; the excellent moisture resistance of the material is mainly due to the use of a low-temperature closed-cell manufacturing process, which stores a large amount of inflatable molecules that cause foaming and expansion in the material structure components. When the material is subjected to high-temperature injection foaming molding by an injection molding machine, at room temperature and atmospheric pressure, the material enters a relatively free expansion space, and the inflated molecules expand naturally, which has a good water resistance and excellent moisture resistance.

[0066] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an animal and plant-based elastic gas microporous shock-absorbing packaging material, It is characterized in that The preparation method is carried out according to the following steps: (1) Add 30-47 parts by weight of plant powder, 3-10 parts of aquatic animal powder and 3-10 parts of plant fiber into a high-speed mixer, stir for 5-10 minutes at a temperature of 30-40° C. and a speed of 4-8 Hz / min, and mix and disperse evenly to obtain an animal and plant-based main ingredient component 1; (2) adding 8-11 parts of glycerol and 0.5-1 parts of polyvinyl alcohol by weight into a temperature-controlled stirring reactor, stirring for 10-20 minutes at a temperature of 95-110° C. and a rotation speed of 8-12 Hz / min, and mixing evenly to form an oily colloidal material to obtain a colloidal material component 2; (3) adding 4-5 parts by weight of hollow silica microspheres, 0.3-1.2 parts of surfactants, 0-0.5 parts of animal and plant waxes, 0-6 parts of additives and 27-33 parts of deionized water into a food mixer, and mixing and dispersing the mixture uniformly to form a material having micropores, thereby obtaining an auxiliary material component 3; (4) Adding the plant-based main ingredient component 1, the colloid component 2 and the auxiliary agent component 3 into a high-speed mixer, stirring for 5-15 minutes at a temperature of 30-40°C and a rotation speed of 6-10 Hz / min to obtain a synthetic material, and then adding the synthetic material into a twin-screw extruder for low-temperature extrusion, rotary cutting and granulation to obtain a finished granular material. The temperature of the first zone of the twin-screw extruder is 15-25°C, the temperature of the second zone is 35-45°C, and the temperature of the third zone is 55-70°C. The extrusion and rotary cutting speeds are 15-25 Hz / min. After the granulation is completed, adding the material into an injection molding machine, high-temperature injection foaming molding, packaging and storage, to obtain an plant-based elastic gas microporous shock-absorbing packaging material; The plant powder in step (1) is one or a combination of corn starch, sweet potato powder, cassava powder, soybean powder, oil residue powder, and potato powder; the oil residue powder is the residue powder remaining after oil is pressed from any one or more oil-containing plants; In step (1), the aquatic animal powder is one or a combination of shrimp shell powder, mussel shell powder, clam shell powder, and fish scale powder; the shrimp shell powder is the shell of any one or more shrimps of marine shrimps and freshwater shrimps, which is dried and ground into shrimp powder of 100 mesh; the clam shell powder is the shell of aquatic mussels, which is dried and ground into clam shell powder of 100 mesh; the fish scale powder is the outer scale of any one or more fishes in seawater or freshwater, which is dried and ground into scale powder of 100 mesh; the clam shell powder is the shell of a shellfish in seawater and freshwater, which is dried and ground into clam shell powder of 100 mesh; The plant fibers in step (1) are stem fibers of any one or more plant types such as straws and vines.

2. The method for preparing the animal and plant-based elastic gas microporous shock-absorbing packaging material according to claim 1, It is characterized in that The model of the polyvinyl alcohol in the step (2) is any one of the commercial models 2488 and 1788.

3. The method for preparing the animal and plant-based elastic gas microporous shock-absorbing packaging material according to claim 1, It is characterized in that The siliceous hollow microspheres in step (3) are ultra-light inorganic non-metallic materials in the form of hollow round bead powders with a true density of 0.20-0.60 g / cm3 and a particle size of 2-125 μm.

4. The method for preparing the animal and plant-based elastic gas microporous shock-absorbing packaging material according to claim 1, It is characterized in that The surfactant in step (3) is coconut oil or fatty acid glyceride; the coconut oil refers to an active vegetable oil prepared by saponifying, acidifying, washing and dehydrating coconut, and the content of unsaturated fatty acids in the oil is more than 80%; the fatty acid oil is any one of monoglyceride or diglyceride.

5. The method for preparing the animal and plant-based elastic gas microporous shock-absorbing packaging material according to claim 1, It is characterized in that In step (3), the animal or plant wax is palm wax or beeswax; and the additive is one or a combination of yeast powder, sodium bicarbonate, and talcum powder.

6. The method for preparing the animal and plant-based elastic gas microporous shock-absorbing packaging material according to claim 1, It is characterized in that In step (3), the rotation speed of the food mixer is 140-160 Hz / min, and the mixing time is 7-12 min.

7. The method for preparing the animal and plant-based elastic gas microporous shock-absorbing packaging material according to claim 1, It is characterized in that In the step (4), the twin-screw extruder equipment mold opening has 5-8 holes, and the mold aperture is 2-4 mm.