A method for increasing the output power of a battery assembly
By adding light processing and detection processes during the manufacturing process of battery components, hydrogen and metal impurities in the battery sheets are activated, and defects and impurities are passivated. This solves the problem of substandard power of battery components, improves output power and service life, and simplifies Troubleshooting process.
Patent Information
- Application Number
- CN202410393369.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-04-02
AI Technical Summary
The power of battery cells stored for a long time does not meet the standard after being made into battery components, resulting in frequent downshifting of battery components, and traditional troubleshooting of downshifting problems is cumbersome.
Add a light treatment process in the manufacturing process of battery components, perform light treatment on the cell sheets to increase the concentration of electrons and holes, activate hydrogen and metal impurities through heating and multiple light injections, passivate defects and impurities, and improve the battery conversion efficiency. And add testing in each process to ensure compliance.
It effectively increases the output power of battery components, reduces the power loss of incoming battery cells, ensures the overall output power and service life of battery components, and simplifies the process of troubleshooting downshifting problems.
Smart Images

Figure CN118299462B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a method for improving the output power of a battery assembly. Background Art
[0002] At present, the conventional process at the battery assembly end is that the finished battery cells made in the battery workshop are directly welded in series for production. However, the battery cells themselves have a certain degree of dark decay. Most of the battery cells need a period of time from the battery end to the assembly end, and long-term storage and complex transportation conditions will aggravate the dark decay of the battery cells. The actual power of most of the incoming battery cells at the assembly end is lower than the labeled power. Finally, the power does not meet the standard after the battery assembly is made, and the EL is uneven, resulting in frequent downshifts in the battery assembly. The traditional way to troubleshoot the downshift problem is to take the battery cells to the battery workshop to test the efficiency and compare it with the labeled efficiency. Troubleshooting the downshift problem is also cumbersome. The long-term dark decay of the battery cells will cause the efficiency to be downgraded after the IV test after being welded into the assembly, which seriously affects the CTM index of the assembly. It is urgent to find a solution to the problem of the battery assembly power not meeting the standard. Summary of the invention
[0003] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a method for improving the output power of a battery assembly, so as to solve the problem in the prior art that the power of battery cells stored for a long time does not meet the standard after being made into a battery assembly.
[0004] To achieve the above purposes and other related purposes,
[0005] The present invention provides a method for improving the output power of a battery assembly, wherein the attenuated battery sheet is subjected to the following steps to obtain a battery assembly:
[0006] S1 phototreatment: phototreatment of the cell to increase the concentration of electrons and holes, thereby improving the conversion efficiency of the cell;
[0007] Pre-S2 test: Check the performance and appearance of the solar cells after light treatment to ensure they meet the standards;
[0008] S3 series welding, connecting multiple battery cells in series to form a battery string group;
[0009] S4 stacking, using the swing template to lay the glass, front EVA, battery string, back EVA, and back panel in order from bottom to top;
[0010] S5 lamination: put the laid battery string into the laminator, vacuumize and heat to melt the EVA, so that the glass, battery cell and backplane are glued together to form a battery assembly;
[0011] S6 IV test, to test the output power of the battery module, test the output characteristics, and determine its output level;
[0012] S7 framing, adding a frame to the battery assembly and adding filler between the battery assembly and the frame;
[0013] S8 is equipped with a junction box, and a junction box for connecting with other equipment or batteries is welded at the electrode lead of the battery assembly;
[0014] The S9 EL test applies a positive or negative bias to the battery module through a regulated power supply to form an infrared thermal image to determine whether the battery module has hidden cracks or cold soldering defects.
[0015] In one embodiment of the present invention, the S1 light treatment comprises the following steps:
[0016] 1) Heat the battery cell and control the temperature to 200-300°C and keep it warm for 10-30S;
[0017] 2) injecting light once into the front and back sides of the cell and controlling the temperature within a first temperature range for a first time;
[0018] 3) performing secondary light injection on the front and back sides of the cell and controlling the temperature within a second temperature range for a second time;
[0019] 4) Light is injected three times on the front and back sides of the cell, and annealing is performed in a third temperature range for a third time.
[0020] In one embodiment of the present invention, the primary light injection intensity is greater than the secondary light injection intensity, the secondary light injection intensity is greater than the tertiary light injection intensity, the first temperature range is greater than the second temperature range, and the first time is greater than the second time.
[0021] In one embodiment of the present invention, the primary light injection intensity is 50-70 suns, the first temperature range is 190-220° C., and the first time is 30-60 seconds;
[0022] The secondary light injection intensity is 30-50 suns, the second temperature range is 180-210°C, and the second time is 20-40S;
[0023] The three light injection intensities are 2-20 suns, the third temperature range is 60-120° C., and the third time is 5-20 min.
[0024] In one embodiment of the present invention, the primary light injection intensity is 55-65 suns, the first temperature range is 200-210° C., and the first time is 30-40 seconds;
[0025] The secondary light injection intensity is 30-40 suns, the second temperature range is 190-200° C., and the second time is 20-30 seconds.
[0026] The intensity of the three light injections is 2-10 suns, the third temperature range is 60-90° C., and the third time is 10-15 minutes.
[0027] In one embodiment of the present invention, the light source in the light treatment is an infrared light source, a laser light source or an LED light source.
[0028] In one embodiment of the present invention, the wavelength of the light source is less than 1000 nm.
[0029] In one embodiment of the present invention, nitrogen is introduced into the three light injections.
[0030] In one embodiment of the present invention, the pre-test includes an EL test, a quantum efficiency test, and a PL test.
[0031] In one embodiment of the present invention, the lamination temperature in S5 is 100-150° C., the lamination time is 15-30 min, and the pressure is 1000-2500N.
[0032] As described above, a method for improving the output power of a battery assembly of the present invention has the following beneficial effects:
[0033] 1. The present invention adds a light treatment process before the manufacture of photovoltaic cell modules, and the cells that have been stored for a long time are subjected to light treatment again to stimulate the recombination of electrons and holes in the cells to increase the concentration of electrons and holes, thereby improving the efficiency of the cells. The efficiency of the cells improved by light treatment offsets the efficiency of dark decay, so that the efficiency is improved to the original level, so as to achieve the purpose of controlling the dark decay of the power of the incoming cells of the battery module, reducing the power loss of the incoming cells, and thus improving the output power of the module.
[0034] 2. This application also adds a pre-test after the light treatment process, because the electrical performance parameters of the battery cells will change after the light treatment, and the power of some battery cells will be inconsistent with the label power. Direct string welding production will cause problems such as poor EL, power exceeding the standard or power failing to meet the standard. Therefore, it is necessary to re-test and pass the standard before processing and producing the battery components.
[0035] 3. By adding multiple testing steps in the battery assembly production process to detect the performance parameters of the battery, and ensuring that it will flow into the next process only after passing the test, the overall output power of the battery assembly is effectively guaranteed.
[0036] 4. The heating process can quickly activate the hydrogen and metal impurities in the battery cell, prompting the conversion of H+ to HO. HO can passivate BO defects and metal impurities, facilitating subsequent precipitation treatment.
[0037] 5. The hydrogen dielectric film on both sides of the cell is stimulated by the injection of high-intensity light, thereby passivating the defects and impurities in the cell body and improving the conversion efficiency of the battery; the stronger the light intensity, the higher the concentration of the photons emitted, which can increase the concentration of electrons and holes in a short time; the temperature of the cell affects the effectiveness of light injection, so the cell is heated before light injection to accelerate the transformation of BO pairs into BO defect states, promote the activation and aggregation of metal impurities in the silicon wafer, and through primary light injection, secondary light injection, and tertiary light injection, high-intensity light accelerates the transformation of BO defect states into BO passivated states and forms non-recombination centers, ultimately achieving a good passivation effect and achieving the purpose of increasing the output power of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Shown is a process flow chart of the present invention. DETAILED DESCRIPTION
[0039] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0040] The present invention provides a method for improving the output power of a battery assembly, wherein the attenuated battery cells are subjected to the following steps to obtain a battery assembly, S1: light treatment, in which the battery cells are subjected to light treatment to increase the concentration of electrons and holes, thereby improving the conversion efficiency of the battery cells; S2: pre-test, in which the performance and appearance of the battery cells after the light treatment are tested to ensure that they meet the standards; S3: series welding, in which a plurality of battery cells are connected in series to form a battery string group; S4: stacking, in which glass, front EVA, battery string group, back EVA, and back plate are laid in order from bottom to top through a swinging template; S5: lamination, in which the laid battery string group is placed in a laminating machine, and the EVA is melted by vacuuming and heating, so that the glass, battery cells, and back plate are pasted together to form a battery assembly; S6: IV test, in which the output power of the battery assembly is tested, the output characteristics are tested, and the output level thereof is determined; S7: framing, in which a frame is added to the battery assembly, and a filler is added between the battery assembly and the frame; S8: junction box installation, in which a junction box for connecting with other devices or batteries is welded at the electrode lead of the battery assembly; S9: EL testing applies positive or negative bias to the battery module through a regulated power supply to form an infrared thermal image to determine whether the battery module has hidden cracks or cold soldering defects.
[0041] Dark decay is actually light decay caused by carriers. High-intensity illumination can accelerate the regeneration process, and the "BO light decay" caused by the attenuated cells is basically eliminated. The present invention adds a light treatment process before the manufacture of photovoltaic cell modules. The cells that have been stored for a long time are subjected to light treatment again to stimulate the recombination of electrons and holes in the cells to increase the concentration of electrons and holes, thereby improving the efficiency of the cells. The efficiency of the cells is improved after light treatment to offset the efficiency of dark decay, so that the efficiency is improved to the original level, so as to achieve the purpose of controlling the dark decay of the power of the incoming cells of the battery module, reducing the power loss of the incoming cells, and thus improving the output power of the module.
[0042] This application also adds a pre-test after the light treatment process, because the electrical performance parameters of the battery cells will change after the light treatment, and the power of some battery cells will be inconsistent with the label power. Direct string welding production will cause problems such as poor EL, power exceeding the standard or power failing to meet the standard. Therefore, re-testing is required to meet the standards before the battery components can be processed and produced.
[0043] The frame is used to increase the strength of the battery assembly, further seal the battery assembly, and extend the service life of the battery. Silicone is used to fill the space between the frame and the battery assembly. The frames are connected with angle keys to increase stability. After the S8 junction box installation process, we also need to add a cleaning process to remove surface stains and increase light transmittance. After the EL test, appearance inspection and packaging are carried out.
[0044] By adding multiple testing steps to the battery assembly production process to detect the performance parameters of the battery, and ensuring that the battery will flow into the next step only after passing the test, the overall output power of the battery assembly is effectively guaranteed.
[0045] The S1 light treatment includes the following steps: 1) heating the battery cell and controlling the temperature to 200-300°C and keeping the temperature for 10-30S; 2) injecting light once into the front and back sides of the battery cell and controlling the temperature within a first temperature range for a first time; 3) injecting light twice into the front and back sides of the battery cell and controlling the temperature within a second temperature range for a second time; 4) injecting light three times into the front and back sides of the battery cell and controlling the temperature within a third temperature range for annealing for a third time.
[0046] The heating process can quickly activate hydrogen and metal impurities in the cell, prompting H+ to be converted into HO. HO can passivate BO defects and metal impurities, making it easier for subsequent precipitation treatment.
[0047] The hydrogen dielectric film on both sides of the cell is stimulated by the injection of high-intensity light, thereby passivating the defects and impurities in the cell body and improving the conversion efficiency of the battery; the stronger the light intensity, the higher the concentration of the photons emitted, which can increase the concentration of electrons and holes in a short time; the temperature of the cell affects the effectiveness of light injection, so the cell is heated before light injection to accelerate the transformation of BO pairs into BO defect states, promote the activation and aggregation of metal impurities in the silicon wafer, and through primary light injection, secondary light injection, and tertiary light injection, high-intensity light accelerates the transformation of BO defect states into BO passivated states, reduces the recombination rate, and effectively prevents minority carriers from being captured by defects.
[0048] The primary light injection intensity is greater than the secondary light injection intensity, the secondary light injection intensity is greater than the tertiary light injection intensity, the first temperature range is greater than the second temperature range, and the first time is greater than the second time.
[0049] The hydrogen atoms in the battery cell are activated by heating the cell, and the temperature, time, and light intensity are controlled. The valence state of the hydrogen atoms is controlled by three light injections to form non-recombination centers, ultimately achieving a good passivation effect and improving the conversion efficiency of the battery.
[0050] The first light injection intensity is 50-70 suns, the first temperature range is 190-220°C, and the first time is 30-60S; the second light injection intensity is 30-50 suns, the second temperature range is 180-210°C, and the second time is 20-40S; the tertiary light injection intensity is 2-20 suns, the third temperature range is 60-120°C, and the third time is 5-20min.
[0051] Preferably, the primary light injection intensity is 55-65 suns, the first temperature range is 200-210°C, and the first time is 30-40 seconds; the secondary light injection intensity is 30-40 suns, the second temperature range is 190-200°C, and the second time is 20-30 seconds. The tertiary light injection intensity is 2-10 suns, the third temperature range is 60-90°C, and the third time is 10-15 minutes.
[0052] The surface recombination on both sides of the cell has a very important impact on the efficiency of the cell. Improving the passivation quality of the cell can effectively reduce its surface recombination, thereby improving the efficiency of the cell. This application uses light injection and auxiliary heating to provide a high light injection amount in a very short time, thereby greatly improving the passivation effect. The metal impurities in the cell can be effectively precipitated through the annealing process, effectively reducing the attenuation of hydrogen-induced attenuation and the attenuation of cell performance caused by metal impurities.
[0053] The light source in the light treatment is an infrared light source, a laser light source or an LED light source. The wavelength of the light source is less than 1000nm. The wavelength of light injection is closely related to the device structure and material selection. For some heterojunction cells, it is necessary to select light with energy higher than the band gap energy for injection to achieve effective separation of photogenerated electron-hole pairs; for other heterojunction cells, it is necessary to select light with energy lower than the band gap energy for injection to reduce thermal failure caused by light irradiation. Therefore, it is necessary to comprehensively consider the matching of light injection wavelength with device structure and material. Nitrogen is introduced in all three light injections. The light treatment is carried out in a nitrogen atmosphere to prevent oxidation of the cell and the formation of more BO defects.
[0054] The pre-test includes EL test, quantum efficiency test and PL test. The spectral response of the cell is detected by the quantum efficiency test, and the problem of low spectral response area of the cell is diagnosed by its quantum efficiency. The excitation source of the PL test is light, which is illuminated to the cell to be tested through a uniform light spot, and the image is captured to determine whether the cell has defects.
[0055] In the S5, the lamination temperature is 100-150°C, the lamination time is 15-30 minutes, and the pressure is 1000-2500 N. By applying a certain pressure on the surface of the battery assembly, the EVA is melted under heating and the battery sheet, glass and back plate are tightly pressed together. After the lamination is completed, the battery assembly is cooled to room temperature.
[0056] The present invention will be further described below with reference to specific embodiments.
[0057] Example 1
[0058] The attenuated battery cells are subjected to the following steps to obtain a battery assembly;
[0059] S1 phototreatment: phototreatment of the cell to increase the concentration of electrons and holes, thereby improving the conversion efficiency of the cell;
[0060] Pre-S2 test: Check the performance and appearance of the solar cells after light treatment to ensure they meet the standards;
[0061] S3 series welding, connecting multiple battery cells in series to form a battery string group;
[0062] S4 stacking, using the swing template to lay the glass, front EVA, battery string, back EVA, and back panel in order from bottom to top;
[0063] S5 lamination: put the laid battery string into the laminator, vacuumize and heat to melt the EVA, so that the glass, battery cell and backplane are glued together to form a battery assembly;
[0064] S6 IV test, to test the output power of the battery module, test the output characteristics, and determine its output level;
[0065] S7 framing, adding a frame to the battery assembly and adding filler between the battery assembly and the frame;
[0066] S8 is equipped with a junction box, and a junction box for connecting with other equipment or batteries is welded at the electrode lead of the battery assembly;
[0067] The S9 EL test applies a positive or negative bias to the battery module through a regulated power supply to form an infrared thermal image to determine whether the battery module has hidden cracks or cold soldering defects.
[0068] The S1 light treatment comprises the following steps:
[0069] 1) Heat the battery cell and control the temperature to 200-300°C and keep it warm for 30 seconds;
[0070] 2) Inject light once on both sides of the cell, and control the intensity to 55-65 suns, the temperature to 200-210°C, and the time to 30 seconds;
[0071] 3) Perform secondary light injection on both sides of the cell, and control the intensity to 30-40 suns, the temperature range to 190-200°C, and the time to 20 seconds.
[0072] 4) Carry out three light injections on the front and back sides of the cell, and control the intensity to 2-10 suns, the temperature range to 60-90°C, and the time to 10-15 minutes.
[0073] Example 2
[0074] The difference from the embodiment 1 is that the S1 light treatment includes the following steps:
[0075] 1) Heat the battery cell and control the temperature to 200-300°C and keep it warm for 30 seconds;
[0076] 2) Inject light once on both sides of the cell, and control the intensity to 55-65 suns, the temperature to 200-210°C, and the time to 60 seconds;
[0077] 3) Perform secondary light injection on both sides of the cell, and control the intensity to 30-40 suns, the temperature range to 190-200°C, and the time to 20 seconds.
[0078] 4) Carry out three light injections on the front and back sides of the cell, and control the intensity to 2-10 suns, the temperature range to 60-90°C, and the time to 10-15 minutes.
[0079] Example 3
[0080] The difference from the embodiment 1 is that the S1 light treatment includes the following steps:
[0081] 1) Heat the battery cell and control the temperature to 200-300°C and keep it warm for 30 seconds;
[0082] 2) Inject light once on both sides of the cell, and control the intensity to 55-65 suns, the temperature to 200-210°C, and the time to 40 seconds;
[0083] 3) Perform secondary light injection on both sides of the cell, and control the intensity to 30-40 suns, the temperature range to 190-200°C, and the time to 20 seconds.
[0084] 4) Carry out three light injections on the front and back sides of the cell, and control the intensity to 2-10 suns, the temperature range to 60-90°C, and the time to 10-15 minutes.
[0085] Example 4
[0086] The difference from the embodiment 3 is that the S1 light treatment includes the following steps:
[0087] 1) Heat the battery cell and control the temperature to 200-300°C and keep it warm for 30 seconds;
[0088] 2) Inject light once on both sides of the cell, and control the intensity to 55-65 suns, the temperature to 200-210°C, and the time to 40 seconds;
[0089] 3) Perform secondary light injection on both sides of the cell, and control the intensity to 30-40 suns, the temperature range to 190-200°C, and the time to 30 seconds.
[0090] 4) Carry out three light injections on the front and back sides of the cell, and control the intensity to 2-10 suns, the temperature range to 60-90°C, and the time to 10-15 minutes.
[0091] Comparative Example 1
[0092] The difference from the embodiment 1 is that the steps of preparing the battery assembly do not use light treatment and pre-testing, which specifically include:
[0093] S1 series welding, connecting multiple battery cells in series to form a battery string group;
[0094] S2 stacking, laying the glass, front EVA, battery string, back EVA, and back sheet in order from bottom to top by swinging the template;
[0095] S3 lamination: put the laid battery string into the laminator, vacuumize and heat to melt the EVA, so that the glass, battery cells and backplane are glued together to form a battery assembly;
[0096] S4 IV test, to test the output power of the battery module, test the output characteristics, and determine its output level;
[0097] S5 framing, adding a frame to the battery assembly and adding filler between the battery assembly and the frame;
[0098] S6 is equipped with a junction box, where a junction box for connecting with other equipment or between batteries is welded at the electrode lead of the battery assembly;
[0099] The S7EL test applies a positive or negative bias to the battery module through a regulated power supply to form an infrared thermal image to determine whether the battery module has hidden cracks or cold soldering defects.
[0100] The performance tests were performed using 100 battery assemblies in each of Examples 1-4 and Comparative Example 1. The test results are as follows:
[0101] Group Eta(%) Pmax(W) Example 1 23.22 6.14 Example 2 23.33 6.21 Example 3 23.28 6.16 Example 4 23.32 6.18 Comparative Example 1 22.35 5.95
[0102] It can be seen that the power and conversion efficiency of the battery components can be greatly improved after light treatment.
[0103] The present invention adds a light treatment process before the manufacture and production of photovoltaic cell modules, and the cells that have been stored for a long time are subjected to light treatment again to stimulate the recombination of electrons and holes in the cells to increase the concentration of electrons and holes, thereby improving the efficiency of the cells. The efficiency of the cells is improved after light treatment to offset the efficiency of dark decay, so that the efficiency is improved to the original level, so as to achieve the purpose of controlling the dark decay of the power of the incoming cells of the battery module, reducing the power loss of the incoming cells, and thus improving the output power of the module. After the light treatment process, a pre-test is also added, because the electrical performance parameters of the cells after light treatment will change, and the power of some cells will be inconsistent with the label power. Direct series welding production will cause problems such as poor EL, power exceeding the standard or power not meeting the standard, so it is necessary to re-test and meet the standard before processing and producing the battery module.
[0104] The hydrogen dielectric film on both sides of the cell is stimulated by the injection of high-intensity light, thereby passivating the defects and impurities in the cell body and improving the conversion efficiency of the battery; the stronger the light intensity, the higher the concentration of the photons emitted, which can increase the concentration of electrons and holes in a short time; the temperature of the cell affects the effectiveness of light injection, so the cell is heated before light injection to accelerate the transformation of BO pairs into BO defect states, promote the activation and aggregation of metal impurities in the silicon wafer, and through primary light injection, secondary light injection, and tertiary light injection, high-intensity light accelerates the transformation of BO defect states into BO passivated states and forms non-recombination centers, ultimately achieving a good passivation effect and achieving the purpose of increasing the output power of the battery.
[0105] By adding multiple testing steps to the battery assembly production process to detect the battery's performance parameters and ensuring that it will flow into the next step only after passing the test, the overall output power of the battery assembly is effectively guaranteed. The heating process can quickly activate the hydrogen and metal impurities in the battery cell, prompting H+ to be converted into HO, which can passivate BO defects and metal impurities, making it easier to carry out precipitation treatment later.
[0106] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. All equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for increasing the output power of a battery assembly, characterized in that: The attenuated battery cells are used to obtain battery components using the following steps: S1 phototreatment: phototreatment of the cell to increase the concentration of electrons and holes, thereby improving the conversion efficiency of the cell; S2 pre-test: to test the performance and appearance of the light-treated cells to ensure they meet the standards. The pre-test includes EL test, quantum efficiency test and PL test; S3 series welding, connecting multiple battery cells in series to form a battery string group; S4 stacking, using the swing template to lay the glass, front EVA, battery string, back EVA, and back panel in order from bottom to top; S5 lamination, putting the laid battery string group into the laminator, vacuuming and heating to melt the EVA, so that the glass, battery cells and backplane are pasted together to form a battery assembly; S6 IV test, testing the output power of the battery assembly, testing the output characteristics, and determining its output level; S7 framing, adding a frame to the battery assembly and adding filler between the battery assembly and the frame; S8 is equipped with a junction box, and a junction box for connecting with other equipment or batteries is welded at the electrode lead of the battery assembly; S9 EL test, through the voltage-stabilized power supply, applies positive bias or negative bias to the battery module to form an infrared thermal image to determine whether the battery module has hidden cracks or cold soldering defects; The S1 light treatment comprises the following steps, 1) Heat the battery cell and control the temperature to 200-300°C and keep it warm for 10-30S; 2) injecting light once into the front and back sides of the cell and controlling the temperature within a first temperature range for a first time; 3) performing secondary light injection on the front and back sides of the cell and controlling the temperature within a second temperature range for a second time; 4) Light is injected three times on the front and back sides of the cell, and annealing is performed in a third temperature range for a third time.
2. A method for increasing the output power of a battery assembly according to claim 1, characterized in that: The primary light injection intensity is greater than the secondary light injection intensity, the secondary light injection intensity is greater than the tertiary light injection intensity, the first temperature range is greater than the second temperature range, and the first time is greater than the second time.
3. A method for increasing the output power of a battery assembly according to claim 2, characterized in that: The primary light injection intensity is 50-70 suns, the first temperature range is 190-220° C., and the first time is 30-60 seconds; The secondary light injection intensity is 30-50 suns, the second temperature range is 180-210°C, and the second time is 20-40S; The three light injection intensities are 2-20 suns, the third temperature range is 60-120° C., and the third time is 5-20 min.
4. A method for increasing the output power of a battery assembly according to claim 2, characterized in that: The primary light injection intensity is 55-65 suns, the first temperature range is 200-210° C., and the first time is 30-40 seconds; The secondary light injection intensity is 30-40 suns, the second temperature range is 190-200°C, and the second time is 20-30S; The intensity of the three light injections is 2-10 suns, the third temperature range is 60-90° C., and the third time is 10-15 minutes.
5. A method for increasing the output power of a battery assembly according to claim 1, characterized in that: The light source in the light treatment is an infrared light source, a laser light source or an LED light source.
6. A method for increasing the output power of a battery assembly according to claim 5, characterized in that: The wavelength of the light source is less than 1000 nm.
7. A method for increasing the output power of a battery assembly according to claim 1, characterized in that: Nitrogen was introduced during the three light injections.
8. A method for increasing the output power of a battery assembly according to claim 1, characterized in that: In the S5, the lamination temperature is 100-150° C., the lamination time is 15-30 min, and the pressure is 1000-2500 N.