A kind of stone imitation ceramic tile and preparation method thereof
Through the combination of phase-separated opacification glaze and phase-separation suppression glaze, the multi-layer glaze technology is used to solve the problem that existing imitation stone ceramic tiles cannot achieve the real stone effect, achieve the echo of opacification and transparent substances, and improve the Three-dimensional feeling.
Patent Information
- Application Number
- CN202410734661.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Existing stone-like ceramic tiles cannot achieve a real stone effect through a transparent glaze layer, and phase-separated opacifying glaze is not used to achieve a three-dimensional effect in which the opacification and transparent substances in the stone echo.
Using the method of phase-separated opacifying glaze combined with phase-separated suppressed glaze, through inkjet printing and multi-layer glaze technology, top glaze, isolation glaze, phase-separated opacifying glaze and phase-separated suppressed glaze are applied to control the chemistry and mineralogy of the glaze layer. The composition and application method achieve the echo of opacities and transparent substances.
Successfully achieved the three-dimensional effect of echoing the opacification and transparent substances in the stone, improving the authenticity and three-dimensionality of the imitation stone ceramic tiles.
Smart Images

Figure CN118307346B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a stone-like ceramic tile and a preparation method thereof, belonging to the technical field of building ceramic production and manufacturing. Background Art
[0002] Natural stone usually contains opaque substances and transparent substances that echo each other, especially colored substances can show a strong three-dimensional effect at different transparency positions. In recent years, architectural ceramic companies have begun to develop tiles with imitation stone effects, mainly through inkjet printing to achieve stone texture, and then apply a thicker layer of transparent glaze, and achieve a three-dimensional effect through a thicker transparent glaze layer and pattern design. However, although the imitation stone ceramic tiles prepared in this way have a certain three-dimensional effect, the pattern presented in the transparent glaze cannot really achieve a more realistic stone effect.
[0003] The hazy transparency of phase-separated opalescent glaze is similar to the effect of semi-emulsified substances in stone, but currently no building ceramics company has used phase-separated opalescent glaze to prepare stone-like ceramic tiles. Summary of the invention
[0004] In view of the problems raised by the background technology, the present invention provides a stone-like ceramic tile and a preparation method thereof, which realizes a three-dimensional effect in which the opacity in the stone material corresponds to the transparent substance by adopting a phase-separation opacifying glaze combined with a phase-separation inhibiting glaze.
[0005] In a first aspect, the present invention provides a method for preparing stone-like ceramic tiles, comprising the following steps: applying a glaze on the surface of a green body; inkjet printing an ink pattern on the surface of the green body after the glaze is applied; applying an isolation glaze on the surface of the green body after the ink pattern is inkjet printed; applying a phase-separation opacifying glaze on the surface of the green body after the isolation glaze is applied; positioningly applying a phase-separation inhibiting glaze on the surface of the green body after the phase-separation opacifying glaze is applied; and firing and polishing the green body after the phase-separation inhibiting glaze is applied to obtain the stone-like ceramic tiles.
[0006] Preferably, the chemical composition of the phase separation inhibition glaze includes, by mass percentage: SiO2: 45-55%; Al2O3: 18-25%; MgO: 1.5-3%; CaO: 5-12%; BaO: 0.5-1.8%; ZnO: 3-5%; K2O: 0.5-1.5%; Na2O: 3-5%; loss on ignition: 5-10%.
[0007] Preferably, the mineral composition of the phase separation inhibition glaze includes, by mass percentage, 35-45% albite, 10-20% kaolin, 3-5% zinc oxide, 10-20% calcite, 3-6% talc, 3-6% quartz, 1-2% barium carbonate, 3-6% alumina, and 10-15% calcined kaolin.
[0008] Preferably, the phase-separation suppression glaze is applied in a fixed manner by inkjet printing; the amount of the phase-separation suppression glaze applied is 120-160 g / m 2 .
[0009] Preferably, the chemical composition of the phase-separated opalescent glaze includes, by mass percentage, the following: SiO2: 48-60%; Al2O3: 8-12%; Fe2O3: 0.1-0.2%; TiO2: 5.5-11.8%; MgO: 3-5%; CaO: 7-15%; ZnO: 1.8-4%; P2O5: 1.5-4%; K2O: 0.2-0.5%; Na2O: 4-5%; loss on ignition: 4-8%.
[0010] Preferably, the mineral composition of the phase-separated opalescent glaze includes, by mass percentage, 45-55% albite, 4-8% kaolin, 2-4% zinc oxide, 10-20% calcite, 8-15% talc, 10-20% quartz, 3-9% calcium phosphate, and 6-12% titanium dioxide.
[0011] Preferably, the phase-separated opacified glaze is applied by spraying or pouring; the specific gravity of the phase-separated opacified glaze is 1.55-1.65 g / cm 3 , glaze application amount is 550~750 g / m 2 .
[0012] Preferably, the chemical composition of the isolation glaze includes, by mass percentage: SiO2: 55-65%; Al2O3: 10-15%; Fe2O3: 0.1-0.3%; TiO2: 0.1-0.2%; MgO: 1.5-3%; CaO: 1-2.5%; BaO: 7-12%; ZnO: 1.5-5%; K2O: 5-7%; Na2O: 1-3%; loss on ignition: 4-7%.
[0013] Preferably, the mineral composition of the isolation glaze includes, by mass percentage, 50-60% potassium feldspar, 10-15% kaolin, 10-15% barium carbonate, 3-5% talc, 3-6% dolomite, 2-5% zinc oxide, and 10-15% quartz.
[0014] Preferably, the insulating glaze is applied by screen printing.
[0015] Preferably, the chemical composition of the glaze includes, by mass percentage, SiO2: 60-68%; Al2O3: 17-22%; Fe2O3: 0.1-0.3%; TiO2: 0.05-0.2%; CaO: 0.1-0.4%; MgO: 0.5-1.8%; K2O: 3.0-4.0%; Na2O: 2.5-3.5%; ZrO2: 5.0-8.5%; and loss on ignition: 1-2%.
[0016] Preferably, the mineral composition of the glaze includes, by mass percentage, 28-35% potassium feldspar, 15-21% sodium feldspar, 12-18% kaolin, 12-18% quartz sand, 8-12% zirconium silicate, 2-5% alumina, 2-4% calcined talc, and 3-8% calcined kaolin.
[0017] Preferably, the glaze is applied by spraying or pouring; the specific gravity of the glaze is 1.40-1.50 g / cm 3 , glaze application amount is 450~650 g / m 2 .
[0018] Preferably, the sintering temperature is 1180-1220° C., and the sintering period is 70-90 min.
[0019] In a second aspect, the present invention provides a stone-like ceramic tile, wherein the stone-like ceramic tile is obtained according to any one of the preparation methods described above.
[0020] Beneficial Effects
[0021] The preparation method of the present invention adopts a phase-separation opacifying glaze combined with a phase-separation inhibiting glaze to prepare stone-like ceramic tiles, thereby achieving a three-dimensional effect in which the opacity in the stone material corresponds to the transparent substance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a brick surface effect diagram of Example 1;
[0023] Figure 2 This is the brick surface effect diagram of Example 1;
[0024] Figure 3 This is the brick surface effect diagram of Example 2;
[0025] Figure 4 This is the brick surface effect diagram of Example 3. DETAILED DESCRIPTION
[0026] The present invention is further described by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention. Unless otherwise specified, each percentage refers to the percentage by mass. The following is an exemplary description of the preparation method of the stone-like ceramic tile of the present invention.
[0027] The green body powder is pressed into a green body. The chemical composition of the green body is not limited, and the green body powder commonly used in the art can be used. For example, the chemical composition of the green body may include, by mass percentage: SiO2: 65.21-68.63%, Al2O3: 18.63-22.05%, Fe2O3: 0.08-0.25%, TiO2: 0.05-0.09%, CaO: 0.3-0.6%, MgO: 1.93-2.35%, K2O: 3.23-3.88%, Na2O: 2.65-3.17%, and loss on ignition: 4.5-5.0%. Preferably, the chemical composition of the blank includes, by mass percentage, SiO2: 65.67%, Al2O3: 20.33%, Fe2O3: 0.17%, TiO2: 0.07%, CaO: 0.48%, MgO: 2.06%, K2O: 3.46%, Na2O: 2.96%, and loss on ignition: 4.8%.
[0028] The green body is dried. A drying kiln can be used for drying. The moisture content of the green body after drying can be 0.5~0.8wt%.
[0029] Apply glaze on the surface of the body. The function of the glaze is to cover the base color and defects of the body and promote the coloring of the inkjet pattern. In some embodiments, the chemical composition of the glaze includes, by mass percentage: SiO2: 60-68%; Al2O3: 17-22%; Fe2O3: 0.1-0.3%; TiO2: 0.05-0.2%; CaO: 0.1-0.4%; MgO: 0.5-1.8%; K2O: 3.0-4.0%; Na2O: 2.5-3.5%; ZrO2: 5.0-8.5%; loss on ignition: 1-2%.
[0030] As an example, the mineral composition of the glaze includes, by mass percentage: 28-35% potassium feldspar, 15-21% sodium feldspar, 12-18% kaolin, 12-18% quartz sand, 8-12% zirconium silicate, 2-5% aluminum oxide, 2-4% calcined talc, and 3-8% calcined kaolin.
[0031] Weigh each raw material according to the mineral composition of the glaze, mix it with sodium tripolyphosphate, sodium carboxymethyl cellulose and water, ball-mill evenly, sieve to remove iron, and obtain a glaze slurry. For example, the glaze slurry includes: in terms of mass percentage, 70% glaze mineral, 0.25% sodium tripolyphosphate, 0.15% sodium carboxymethyl cellulose, and 29.6% water. The glaze slurry has a sieve residue of ≤0.8wt% when passing through a 325-mesh sieve. When applying the glaze, water can be added to the glaze slurry to adjust the final desired glaze specific gravity.
[0032] The glaze is applied by spraying or pouring. Preferably, the glaze is applied by spraying. In some technical solutions, the specific gravity of the glaze is 1.40-1.50 g / cm 3 , glaze application amount is 450~650 g / m 2 .
[0033] The ink pattern is printed on the surface of the body after the glaze is applied. Conventional inkjet ink can be used. The texture and color of the inkjet printed ink pattern can be adaptively changed according to the needs.
[0034] Apply an isolation glaze on the surface of the blank after the ink pattern is inkjet printed. The function of the isolation glaze is to prevent the subsequent application of the phase-separated opacifying glaze from affecting the color of the ink pattern. In some embodiments, the chemical composition of the isolation glaze includes, by mass percentage: SiO2: 55-65%; Al2O3: 10-15%; Fe2O3: 0.1-0.3%; TiO2: 0.1-0.2%; MgO: 1.5-3%; CaO: 1-2.5%; BaO: 7-12%; ZnO: 1.5-5%; K2O: 5-7%; Na2O: 1-3%; loss on ignition: 4-7%.
[0035] As an example, the mineral composition of the isolation glaze includes, by mass percentage, 50-60% potassium feldspar, 10-15% kaolin, 10-15% barium carbonate, 3-5% talc, 3-6% dolomite, 2-5% zinc oxide, and 10-15% quartz.
[0036] Weigh each raw material according to the mineral composition of the isolation glaze, mix it with sodium tripolyphosphate, sodium carboxymethyl cellulose and water, ball-mill evenly, sieve to remove iron, and obtain an aqueous slurry of the isolation glaze. For example, the aqueous slurry of the isolation glaze includes: in terms of mass percentage, 70% isolation glaze mineral, 0.25% sodium tripolyphosphate, 0.15% sodium carboxymethyl cellulose, and 29.6% water. The residue of the aqueous slurry of the isolation glaze passing through a 325-mesh sieve is ≤0.5wt%. The specific gravity of the aqueous slurry of the isolation glaze can be 1.8~1.9 g / cm 3 When applying the isolation glaze, water may be added to the isolation glaze aqueous slurry to adjust the final desired specific gravity of the isolation glaze aqueous slurry.
[0037] The isolation glaze is applied by screen printing. Because the color of the phase-separated opacified glaze is poor, the glaze layer of the isolation glaze must reach a certain thickness to reduce the effect of the phase-separated opacified glaze on the inkjet printing ink, but if the isolation glaze is too thick, its transparency will be reduced, thereby affecting the color. By screen printing the isolation glaze, compared with the roller printing isolation glaze, the thickness of the screen printing isolation glaze is moderate and the glaze surface is smoother. If the isolation glaze is applied by spraying glaze, the glaze surface has poor uniformity and is prone to yin and yang color defects. At the same time, the spraying glaze requires a very low specific gravity of the isolation glaze, which leads to an increase in the moisture content of the brick blank, reduces the strength of the brick blank, and causes glaze line rotten bricks. When screen printing the isolation glaze, 60~70wt% of the isolation glaze aqueous slurry and 30~40wt% of the printing paste can be evenly mixed to prepare an isolation glaze slurry for screen printing. A 100~120 mesh screen can be used.
[0038] Phase-separated opaque glaze is applied on the surface of the body after the isolation glaze is applied. In the prior art, phase-separated opaque glaze is usually used as white glaze, mainly to cover the color of the body, or various coloring oxides are added to the phase-separated opaque glaze for coloring to form different colors in different liquid phases, which is mainly used in artistic porcelain and kiln-changed glaze. The present invention can achieve an opaque effect similar to that in stone by applying phase-separated opaque glaze.
[0039] In some embodiments, the chemical composition of the phase-separated opalescent glaze includes, by mass percentage: SiO2: 48-60%; Al2O3: 8-12%; Fe2O3: 0.1-0.2%; TiO2: 5.5-11.8%; MgO: 3-5%; CaO: 7-15%; ZnO: 1.8-4%; P2O5: 1.5-4%; K2O: 0.2-0.5%; Na2O: 4-5%; loss on ignition: 4-8%.
[0040] As an example, the mineral composition of the phase-separated opalescent glaze includes, by mass percentage, 45-55% albite, 4-8% kaolin, 2-4% zinc oxide, 10-20% calcite, 8-15% talc, 10-20% quartz, 3-9% calcium phosphate, and 6-12% titanium dioxide.
[0041] Weigh each raw material according to the mineral composition of the phase-separated opalescent glaze, mix it with sodium tripolyphosphate, sodium carboxymethyl cellulose and water, ball-mill evenly, sieve to remove iron, and obtain a phase-separated opalescent glaze slurry. For example, the phase-separated opalescent glaze slurry includes: in terms of mass percentage, 70% of phase-separated opalescent glaze minerals, 0.25% of sodium tripolyphosphate, 0.15% of sodium carboxymethyl cellulose, and 29.6% of water. The residue of the phase-separated opalescent glaze slurry passing through a 325-mesh sieve is ≤0.5wt%. When applying the phase-separated opalescent glaze, water can be added to the phase-separated opalescent glaze slurry to adjust the final required specific gravity of the phase-separated opalescent glaze.
[0042] The phase-separated opacified glaze is applied by spraying or pouring. Preferably, the phase-separated opacified glaze is applied by spraying. In some technical solutions, the specific gravity of the phase-separated opacified glaze is 1.55-1.65 g / cm 3 , glaze application amount is 550~750 g / m 2 Controlling the glazing amount of the phase-separation opacified glaze within the above range can avoid the phase-separation opacified glaze being too low and unable to achieve phase-separation opacification, and can also avoid the phase-separation opacified glaze being too high and causing the gas generated by the body during the firing process to be difficult to discharge and form glaze defects.
[0043] Apply phase separation inhibiting glaze on the surface of the body after applying phase separation opacifying glaze. The main function of phase separation inhibiting glaze is to prevent phase separation of phase separation opacifying glaze. In some embodiments, the chemical composition of the phase separation inhibiting glaze includes by mass percentage: SiO2: 45-55%; Al2O3: 18-25%; MgO: 1.5-3%; CaO: 5-12%; BaO: 0.5-1.8%; ZnO: 3-5%; K2O: 0.5-1.5%; Na2O: 3-5%; loss on ignition: 5-10%.
[0044] As an example, the mineral composition of the phase-separation inhibition glaze includes, by mass percentage, 35-45% albite, 10-20% kaolin, 3-5% zinc oxide, 10-20% calcite, 3-6% talc, 3-6% quartz, 1-2% barium carbonate, 3-6% alumina, and 10-15% calcined kaolin. Weigh the materials according to the mineral composition of the phase-separation inhibition glaze, then mix the raw materials with the solvent, (super) dispersant, surfactant and defoamer, and grind them to a fineness of D 50<400nm, and obtain a slurry; the slurry is filtered to obtain a phase-separation inhibition glaze ink. The dispersant can be a dispersant commonly used in digital inks. Including but not limited to styrene-maleic anhydride copolymer, polyethylene glycol, EO-PO block copolymer and EO-PO-EO triblock copolymer. Commercial dispersants such as HLD-18 / AJ (Silcona, Germany) can also be used. In the embodiments and comparative examples, the dispersant specifically uses PEG4000. The mass percentage of the dispersant in the phase-separation inhibition glaze ink can be 1% to 5%. The solvent can be a solvent commonly used in digital glaze inks. Including but not limited to one or more of diethylene glycol, ethylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, glycerol, D-sorbitol, 1,2,6-hexanetriol, trimethylolpropane, 1,2-propylene glycol, polyols, polyol ethers, and polysaccharides. In the embodiments and comparative examples, the solvent specifically uses a mixture of ethylene glycol and 1,3-propylene glycol in a volume ratio of 1:1. The mass percentage of the solvent in the phase-splitting glaze ink can be 50% to 70%. The surfactant can be an ionic surfactant, a non-ionic surfactant, or a mixture of the two. Surfactants include but are not limited to sodium stearate, alkyl sulfates, sodium alkylbenzene trimethylene sulfonate, sodium alkylbenzene sulfonate, polyoxyethylene propylene glycol stearate, polyoxyethylene sorbitan laurate, etc. In the embodiments and comparative examples, the surfactant specifically uses sodium alkylbenzene trimethylene sulfonate. The mass percentage of the surfactant in the phase-splitting glaze ink is 0.01% to 3.0%. The defoamer includes but is not limited to one or more of a polyether-modified silicone defoamer, an emulsion-type polysiloxane, and a polyether block defoamer. In the embodiments and comparative examples, the defoamer specifically uses a polyether-modified silicone defoamer. The mass percentage of the defoamer in the phase-splitting glaze ink can be 1% to 3%. The mass percentage of the defoamer in the phase-separation inhibition glaze ink may be 1% to 3%. In some embodiments, the ink specific gravity of the phase-separation inhibition glaze ink may be 1.30 to 1.40 g / cm 3 .
[0045] The high temperature viscosity of the phase separation inhibiting glaze is significantly greater than that of the phase separation opacifying glaze. During the firing process, the phase separation inhibiting glaze will react with the phase separation opacifying glaze to prevent the generation of phase separation, so that the position where the phase separation inhibiting glaze is applied will appear transparent.
[0046] The phase-separation suppression glaze is applied by inkjet printing. For example, the phase-separation suppression glaze is inkjet printed to form a phase-separation suppression glaze pattern. Positioning the phase-separation suppression glaze means that the phase-separation suppression glaze pattern is matched with the inkjet printing ink pattern according to the design requirements. That is, the phase-separation suppression glaze is printed at the position where a transparent effect is required, and the other positions are not printed with the phase-separation opacified glaze but are opacified.
[0047] The glaze amount of the phase separation inhibition glaze is 120-160 g / m 2If the amount of phase-separation inhibition glaze applied is too high, the high-temperature viscosity of the upper glaze layer will be greater than that of the lower glaze layer, causing glaze defects such as bubbles on the glaze surface. If the amount of phase-separation inhibition glaze applied is too low, the area where the phase-separation inhibition glaze is applied will only show a spotty transparent effect.
[0048] Please note that the order of applying the phase-separation opacifying glaze and the phase-separation suppressing glaze of the present invention cannot be reversed, otherwise the phase-separation suppressing glaze will lose its effect and cannot prevent the phase-separation opacifying glaze from separating. The phase-separation suppressing glaze must be placed above the phase-separation opacifying glaze to achieve an opacifying effect at the location where the phase-separation opacifying glaze is applied and a transparent effect at the location where the phase-separation suppressing glaze is applied, otherwise the entire brick surface will appear opaque.
[0049] Firing: The firing temperature is 1180-1220°C, and the firing cycle is 70-90 minutes.
[0050] Polishing. Grading.
[0051] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0052] Example 1
[0053] The preparation method of the imitation stone ceramic tile comprises the following steps:
[0054] Step 1: Prepare the green body and dry it.
[0055] Step 2. Apply glaze on the surface of the body. The mineral composition of the glaze includes, by mass percentage: 31% potassium feldspar, 20% sodium feldspar, 15% kaolin, 15% quartz sand, 10% zirconium silicate, 2% alumina, 3% calcined talc, and 4% calcined kaolin. The chemical composition of the glaze includes, by mass percentage: SiO2: 65.63%, Al2O3: 18.00%, Fe2O3: 0.15%, TiO2: 0.14%, CaO: 0.27%, MgO: 1.09%, K2O: 3.51%, Na2O: 3.04%, ZrO2: 6.37%, and loss on ignition: 1.80%. The glaze is applied by spraying. The specific gravity of the glaze is 1.45 g / cm 3 , glaze application amount is 500 g / m 2 .
[0056] Step 3: Inkjet printing an ink pattern on the surface of the body after the glaze is applied.
[0057] Step 4. Apply an isolation glaze on the surface of the body after the inkjet printing ink pattern. The mineral composition of the isolation glaze includes, by mass percentage: 55% potassium feldspar, 10% kaolin, 10% barium carbonate, 4% talc, 4% dolomite, 3% zinc oxide, and 14% quartz. The chemical composition of the isolation glaze includes, by mass percentage: SiO2: 59.36%; Al2O3: 12.96%; Fe2O3: 0.15%; TiO2: 0.13%; MgO: 2.2%; CaO: 1.55%; BaO: 7.80%; ZnO: 2.98%; K2O: 5.64%; Na2O: 1.91%; loss on ignition: 5.32%. Weigh the raw materials according to the mineral composition of the isolation glaze, mix them with sodium tripolyphosphate, sodium carboxymethyl cellulose and water, ball mill evenly, sieve to remove iron, and obtain an isolation glaze aqueous slurry. The aqueous slurry of the isolation glaze includes: by mass percentage, 70% of the isolation glaze mineral, 0.25% of sodium tripolyphosphate, 0.15% of sodium carboxymethyl cellulose, and 29.6% of water. The residue of the aqueous slurry of the isolation glaze passing through a 325-mesh screen is ≤0.5wt%. The application method of the isolation glaze is screen printing. 65wt% of the aqueous slurry of the isolation glaze and 35wt% of the printing paste are evenly mixed to prepare the isolation glaze slurry for screen printing. A 100-mesh screen is used.
[0058] Step 5. Apply phase-separated opalescent glaze on the surface of the body after the isolation glaze is applied. The mineral composition of the phase-separated opalescent glaze includes, by mass percentage: albite 46%, kaolin 5%, zinc oxide 2.5%, calcite 12%, talc 8.5%, quartz 13%, calcium phosphate 5%, titanium dioxide 8%. The chemical composition of the phase-separated opalescent glaze includes, by mass percentage: SiO2: 53.87%; Al2O3: 9.94%; Fe2O3: 0.12%; TiO2: 7.77%; MgO: 3.16%; CaO: 9.03%; ZnO: 2.48%; P2O5: 2.34%; K2O: 0.38%; Na2O: 4.58%; loss on ignition: 6.33%. The phase-separated opalescent glaze is applied by spraying. The specific gravity of the phase-separated opalescent glaze is 1.60 g / cm 3 , glaze weight is 630 g / m 2 .
[0059] Step 6. Apply phase-separation inhibiting glaze on the surface of the body after applying the phase-separation opacifying glaze. The chemical composition of the phase-separation inhibiting glaze includes, by mass percentage, SiO2: 52.77%; Al2O3: 22.97%; MgO: 1.97%; CaO: 5.59%; BaO: 1.56%; ZnO: 3.95%; K2O: 0.53%; Na2O: 3.88%; loss on ignition: 6.78%. The mineral composition of the phase-separation inhibiting glaze includes, by mass percentage, 40% albite, 15% kaolin, 4% zinc oxide, 10% calcite, 5% talc, 5% quartz, 2% barium carbonate, 4% aluminum oxide, and 15% calcined kaolin. The phase-separation inhibiting glaze is applied by inkjet printing. The amount of the phase-separation inhibiting glaze applied is 140 g / m 2 Positioning the application of phase-separation suppression glaze means that the inkjet printing phase-separation suppression glaze pattern matches the inkjet printing ink pattern according to the design requirements. That is, the phase-separation suppression glaze is printed at the position where a transparent effect is required, and the other positions are not printed with phase-separation opacity glaze but are opacity.
[0060] Step 7. Firing. The firing temperature is 1220°C and the firing cycle is 80 minutes.
[0061] Step 8. Polishing.
[0062] Step 9. Classification.
[0063] Figure 1 This is a brick surface effect diagram of Example 1. Figure 1 It can be seen that the location where the phase-separation opacifying glaze is applied has a clear opacifying effect, while the location where the phase-separation suppressing glaze is applied has no phase separation but presents a transparent effect according to the design pattern.
[0064] Comparative Example 1
[0065] The invention is basically the same as Example 1, except that the mineral composition of the phase-separation inhibiting glaze includes, by mass percentage, 52% albite, 10% kaolin, 6% zinc oxide, 20% calcite, 5% calcined talc, 2% quartz, 1% barium carbonate, 2% aluminum oxide, and 2% calcined kaolin. The chemical composition of the phase-separation inhibiting glaze includes, by mass percentage, 48.99% SiO2, 15.37% Al2O3, 2.14% MgO, 10.99% CaO, 0.79% BaO, 5.97% ZnO, 0.45% K2O, 4.96% Na2O, and 10.34% loss on ignition.
[0066] Figure 2 This is the brick surface effect diagram of Example 1. Figure 2It can be seen that the position where the phase-separation opacifying glaze is applied has an obvious opacifying effect, and the position where the phase-separation inhibiting glaze is applied also has an opacifying effect. This is because the high-temperature viscosity of the phase-separation inhibiting glaze is relatively low, resulting in the phase-separation inhibiting glaze having little effect on the high-temperature viscosity and high-temperature fluidity of the phase-separation opacifying glaze, and failing to prevent the occurrence of phase separation.
[0067] Comparative Example 2
[0068] The same as Example 1, except that the amount of the phase separation inhibition glaze applied is 80 g / m 2 .
[0069] Figure 3 This is the brick surface effect diagram of Example 2. Figure 3 It can be seen that although the position where the phase-separation opacifying glaze is applied has an obvious opacifying effect, the position where the phase-separation suppressing glaze is applied does not show the expected transparent effect, but shows a spotty opacifying effect. This is because the amount of the phase-separation suppressing glaze applied is low, resulting in the phase-separation suppressing glaze only affecting the phase separation of the phase-separation opacifying glaze at some positions, that is, the undesirable phase-separation effect is still produced in some positions.
[0070] Comparative Example 3
[0071] The same as Example 1, except that the amount of the phase separation inhibition glaze applied is 240 g / m 2 .
[0072] Figure 4 This is the brick surface effect diagram of Example 3. Figure 4 It can be seen that although the location where the phase-separation opacifying glaze is applied has an obvious opacifying effect, and the location where the phase-separation inhibiting glaze is applied has a transparent effect, there are obvious glaze bubble defects on the glaze surface. This is because the glaze amount of the phase-separation inhibiting glaze is high, resulting in a high viscosity at high temperature in the location where the phase-separation inhibiting glaze is applied, and bubbles cannot be completely eliminated, resulting in the formation of glaze bubbles.
[0073] Comparative Example 4
[0074] It is basically the same as Example 1, except that the order of applying the phase separation opacifying glaze and the phase separation inhibiting glaze in step 5 and step 6 is exchanged.
[0075] In this comparative example, the phase separation inhibiting glaze loses its effect and cannot prevent the phase separation of the phase separation opacifying glaze, and the entire brick surface appears opaque.
Claims
1. A method for preparing a stone-like ceramic tile, It is characterized in that The following steps are involved: Applying glaze on the surface of the body; inkjet printing an ink pattern on the surface of the green body after the glaze is applied; Applying an isolation glaze on the surface of the blank after the ink pattern is inkjet printed; Apply phase separation opacifying glaze on the surface of the body after the isolation glaze is applied; The chemical composition of the phase-separated opacified glaze includes, by mass percentage: SiO 2 :48~60%;Al 2 O 3 :8~12%;Fe 2 O 3 :0.1~0.2%;TiO 2 :5.5~11.8%; MgO: 3~5%; CaO: 7~15%; ZnO: 1.8~4%; P 2 O 5 :1.5~4%; K 2 O: 0.2~0.5%; Na 2 O: 4-5%; Loss on burning: 4-8%; After the phase-separation opacifying glaze is applied, a phase-separation inhibiting glaze is applied on the surface of the body; the chemical composition of the phase-separation inhibiting glaze includes, by mass percentage: SiO 2 :45~55%;Al 2 O 3 : 18~25%; MgO: 1.5~3%; CaO: 5~12%; BaO: 0.5~1.8%; ZnO: 3~5%; K 2 O: 0.5-1.5%; Na 2 O: 3-5%; loss on burning: 5-10%; applying phase-separation suppression glaze by inkjet printing; the amount of phase-separation suppression glaze applied is 120-160g / m 2 ; The green body after applying the phase-separation inhibition glaze is fired and polished to obtain the stone-like ceramic tile.
2. The preparation method according to claim 1, It is characterized in that The mineral composition of the phase separation inhibition glaze includes, by mass percentage, 35-45% albite, 10-20% kaolin, 3-5% zinc oxide, 10-20% calcite, 3-6% talc, 3-6% quartz, 1-2% barium carbonate, 3-6% aluminum oxide, and 10-15% calcined kaolin.
3. The preparation method according to claim 1, It is characterized in that The mineral composition of the phase-separated opalescent glaze includes, by mass percentage, 45-55% albite, 4-8% kaolin, 2-4% zinc oxide, 10-20% calcite, 8-15% talc, 10-20% quartz, 3-9% calcium phosphate, and 6-12% titanium dioxide.
4. The preparation method according to claim 1, It is characterized in that The phase-separated opacified glaze is applied by spraying or pouring; the specific gravity of the phase-separated opacified glaze is 1.55-1.65 g / cm 3 , glaze application amount is 550~750 g / m 2 .
5. The preparation method according to claim 1, It is characterized in that The chemical composition of the isolation glaze includes, by mass percentage: SiO 2 :55~65%;Al 2 O 3 :10~15%;Fe 2 O 3 :0.1~0.3%;TiO 2 : 0.1~0.2%; MgO: 1.5~3%; CaO: 1~2.5%; BaO: 7~12%; ZnO: 1.5~5%; K 2 O: 5-7%; Na 2 O: 1~3%; loss on burning: 4~7%.
6. The preparation method according to claim 5, It is characterized in that The mineral composition of the isolation glaze includes, by mass percentage, 50-60% potassium feldspar, 10-15% kaolin, 10-15% barium carbonate, 3-5% talc, 3-6% dolomite, 2-5% zinc oxide, and 10-15% quartz.
7. The preparation method according to claim 1, It is characterized in that The isolation glaze is applied by screen printing.
8. The preparation method according to claim 1, It is characterized in that The chemical composition of the glaze includes, by mass percentage: SiO 2 :60~68%;Al 2 O 3 :17~22%;Fe 2 O 3 :0.1~0.3%;TiO 2 :0.05~0.2%; CaO: 0.1~0.4%; MgO: 0.5~1.8%; K 2 O: 3.0-4.0%; Na 2 O: 2.5-3.5%; ZrO 2 : 5.0~8.5%; loss on burning: 1~2%.
9. The preparation method according to claim 8, It is characterized in that The mineral composition of the glaze includes, by mass percentage, 28-35% potassium feldspar, 15-21% sodium feldspar, 12-18% kaolin, 12-18% quartz sand, 8-12% zirconium silicate, 2-5% aluminum oxide, 2-4% calcined talc, and 3-8% calcined kaolin.
10. The preparation method according to claim 1, It is characterized in that The glaze is applied by spraying or pouring; the specific gravity of the glaze is 1.40-1.50 g / cm 3 , glaze application amount is 450~650 g / m 2 .
11. The preparation method according to claim 1, It is characterized in that The firing temperature is 1180-1220°C, and the firing period is 70-90 minutes.
12. A stone-like ceramic tile, It is characterized in that The stone-like ceramic tile is obtained according to the preparation method described in any one of claims 1 to 11.
Citation Information
Patent Citations
Three-dimensional hierarchical glazed ceramic brick and method for preparing same
CN102653476A
Whole-body rock brick with characteristics of wear resistance, skid resistance, easy cleaning and natural stone particle texture, and preparation method thereof
CN111072406A
Rock plate with meteorite crater surface and preparation method thereof
CN114507085A