Preparation method and application of high temperature resistant and flame resistant polyetheretherketone
By introducing N,N-(3-phosphate-4-fluoro)phenylpyromellitide as a functional monomer, the copolymerization reaction improves the thermal decomposition temperature and flame retardant properties of polyether ether ketone, solving the problem of polyether ether ketone. The problem of insufficient resistance of ether ether ketone in high temperature and combustion process has achieved better high temperature resistance and flame retardant effect.
Patent Information
- Application Number
- CN202410514343.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-26
AI Technical Summary
Polyetheretherketone materials have poor resistance to high temperatures and combustion processes, and traditional brominated flame retardants can release harmful halogen compounds, causing pollution.
N,N-(3-phosphate-4-fluoro)phenylpyromellitide is used as the functional monomer, and copolymerized with 4,4'-difluorobenzophenone and diphenol monomers. Introducing high-temperature-resistant imide groups and flame-retardant phosphate ester groups to improve the thermal decomposition temperature and flame-retardant properties of polyetheretherketone.
Significantly increases the thermal decomposition temperature of polyetheretherketone, reduces the peak heat release rate, improves flame retardant properties, reduces the amount of residual carbon, and plays a role in isolating heat and hindering oxygen through the generation of phosphoric acid compounds, significantly improving It has high temperature resistance and flame resistance.
Smart Images

Figure BDA0004812920450000031 
Figure BDA0004812920450000041 
Figure BDA0004812920450000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyetheretherketone, in particular to a preparation method and application of high-temperature resistant and flame-resistant polyetheretherketone. Background Art
[0002] Polyetheretherketone is a polymer with a repeating unit of one ketone bond and two ether bonds in the main chain. It has excellent chemical resistance, electrical insulation and mechanical strength. It can be used as a special engineering plastic and is widely used in the fields of electronics, aerospace, etc. By filling and modifying polyetheretherketone with nanomaterials such as graphene, carbon nanotubes, and carbon fibers, a composite material with excellent performance can be obtained. However, nanomaterials such as carbon nanotubes and graphene are expensive and have problems such as poor compatibility with the polyetheretherketone matrix.
[0003] The use of functional monomers to modify polyetheretherketone can improve its high temperature resistance, flame retardancy, viscosity and other properties. Chinese patent CN111943831B discloses a method for preparing a highly flame retardant polyetheretherketone oligomer, using dibromodiphenyl ether as a capping agent, and the end group of the prepared polyetheretherketone contains a bromine group, which has high flame retardancy, low melt viscosity, high temperature thermal stability and other properties. However, bromine-based flame retardants release harmful halides and other substances at high temperatures and during combustion, which is very polluting. The present invention aims to prepare a new type of phosphorus-containing functional monomer to improve the high temperature resistance and flame retardancy of polyetheretherketone. Summary of the invention
[0004] The invention solves the problem that the polyetheretherketone material has poor high temperature resistance and flame resistance.
[0005] The present invention provides the following technical solutions:
[0006] A preparation method of high temperature resistant and flame resistant polyetheretherketone is as follows: a solvent, water-carrying toluene, diphenol monomer, 4,4'-difluorobenzophenone, N,N-(3-phosphate-4-fluoro)phenylpyromellitimide and potassium carbonate are added into a reaction container equipped with a water separator and a condenser, nitrogen is introduced into the reaction container, the temperature is raised to 135-145°C, water is removed for 4-5 hours, the temperature is then raised to 170-180°C, the reaction is carried out for 2-3 hours, the temperature is then raised to 210-220°C, the reaction is carried out for 5-8 hours, methanol is added to the solution after cooling, a precipitate is precipitated, the precipitate is filtered, washed and dried to obtain high temperature resistant and flame resistant polyetheretherketone.
[0007] Preferably, the ratio of the solvent to toluene is 1 L:(0.5-0.6) L; the solvent is dimethyl sulfoxide or sulfolane.
[0008] Preferably, the ratio of the diphenol monomer, 4,4'-difluorobenzophenone, N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and potassium carbonate is 1 mol:(0.85-0.97) mol:(0.03-0.15) mol:(2.4-2.8) mol.
[0009] Preferably, the solvent is dimethyl sulfoxide or sulfolane.
[0010] Preferably, the diphenol monomer is hydroquinone, biphenol or bisphenol A.
[0011] Preferably, the preparation method of N,N-(3-phosphate-4-fluoro)phenyl pyromellitimide is:
[0012] (1) Add N-methylpyrrolidone, water-carrying toluene, pyromellitic anhydride, and 5-amino-2-fluorophenol to a reaction vessel equipped with a water separator and a condenser, first heat to 135-145° C., remove water for 2-3 hours, then heat to 170-185° C., react for 8-12 hours, cool, add methanol to the solution, precipitate, filter, wash the precipitate with water and methanol, and dry to obtain N,N-(3-hydroxy-4-fluoro)phenylpyromellitic anhydride.
[0013] (2) Add toluene solvent, N,N-(3-hydroxy-4-fluoro)phenyl benzyl imide, pyridine, and O,O-dimethylphosphoryl chloride to a reaction container, and react at 15-40° C. for 4-10 hours. After the reaction, distill the solution under reduced pressure, wash the product with water and methanol, and dry it to obtain N,N-(3-phosphate-4-fluoro)phenyl benzyl imide.
[0014] Preferably, the ratio of pyromellitic anhydride to 5-amino-2-fluorophenol in (1) is 1 mol:(2-2.2) mol.
[0015] Preferably, in (2), the ratio of N,N-(3-hydroxy-4-fluoro)phenylpyromellitimide, pyridine and O,O-dimethylphosphoryl chloride is 1 mol:(2.2-2.8) mol:(2.3-2.6) mol.
[0016] The technical effect of the present invention is as follows: the present invention uses pyromellitic anhydride, 5-amino-2-fluorophenol, O,O-dimethylphosphoryl chloride and the like as reactants, and prepares a novel N,N-(3-phosphate-4-fluoro)phenylpyromellitic imide as a difluoro monomer through a simple and efficient preparation method, and then copolymerizes with conventional 4,4'-difluorobenzophenone and diphenol monomers, and introduces a high temperature resistant imide group into the main chain of polyetheretherketone, which significantly increases the thermal decomposition temperature of polyetheretherketone; at the same time, a flame retardant phosphate group is introduced into the side chain of polyetheretherketone, and the phosphoric acid compound generated when the phosphate group burns can promote the dehydration of polyetheretherketone into carbon, which can isolate heat transfer and hinder oxygen from entering the matrix, and has a good flame retardant effect, thereby improving the residual carbon content of polyetheretherketone, reducing the peak value of the heat release rate, and having better flame retardant and flame resistant properties. It is conducive to expanding the practical application of polyetheretherketone in special engineering materials with high temperature resistance and flame retardancy. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1
[0019] (1) Add 10 mL of N-methylpyrrolidone, 4 mL of toluene with water, 5 mmol of pyromellitic anhydride, and 11 mmol of 5-amino-2-fluorophenol to a reaction vessel equipped with a water separator and a condenser, first heat to 135°C, remove water for 3 hours, then heat to 170°C, react for 10 hours, cool and add methanol to the solution to precipitate, filter and wash the precipitate with water and methanol, and dry to obtain N,N-(3-hydroxy-4-fluoro)phenylpyromellitic anhydride. The reaction formula is:
[0020]
[0021] (2) Add 15 mL of toluene solvent, 5 mmol N,N-(3-hydroxy-4-fluoro)phenyl pyromellitimide, 11 mmol pyridine, and 12 mmol O,O-dimethylphosphoryl chloride to a reaction container, and react at 20°C for 6 hours. After the reaction, distill the solution under reduced pressure, wash the product with water and methanol, and dry it to obtain N,N-(3-phosphate-4-fluoro)phenyl pyromellitimide. The reaction formula is:
[0022]
[0023] (3) 300 mL of sulfolane solvent and 150 mL of toluene with water, 100 mmol of hydroquinone, 97 mmol of 4,4'-difluorobenzophenone, 3 mmol of N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and 250 mmol of potassium carbonate are added to a reaction vessel equipped with a water separator and a condenser. Nitrogen is introduced into the reaction vessel, the temperature is raised to 140° C., water is removed for 5 h, the temperature is then raised to 180° C., the reaction is carried out for 2 h, the temperature is then raised to 220° C., the reaction is carried out for 6 h, methanol is added to the solution after cooling, a precipitate is precipitated, the precipitate is filtered, washed with water and methanol, and dried to obtain a high temperature resistant and flame resistant polyetheretherketone.
[0024] Example 2
[0025] (1) Add 8 mL of N-methylpyrrolidone, 4 mL of toluene with water, 5 mmol of pyromellitic anhydride, and 11 mmol of 5-amino-2-fluorophenol to a reaction vessel equipped with a water separator and a condenser, first heat to 145°C, remove water for 3 hours, then heat to 170°C, react for 12 hours, cool and add methanol to the solution to precipitate, filter and wash the precipitate with water and methanol, and dry to obtain N,N-(3-hydroxy-4-fluoro)phenylpyromellitic anhydride.
[0026] (2) Add 20 mL of toluene solvent, 5 mmol N,N-(3-hydroxy-4-fluoro)phenyl benzyl imide, 12 mmol pyridine, and 11.5 mmol O,O-dimethylphosphoryl chloride into a reaction container, and react at 40° C. for 4 hours. After the reaction, distill the solution under reduced pressure, wash the product with water and methanol, and dry it to obtain N,N-(3-phosphate-4-fluoro)phenyl benzyl imide.
[0027] (3) 300 mL of sulfolane solvent and 180 mL of toluene with water, 100 mmol of biphenyldiphenol, 93 mmol of 4,4'-difluorobenzophenone, 7 mmol of N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and 280 mmol of potassium carbonate were added to a reaction vessel equipped with a water separator and a condenser. Nitrogen was introduced into the reaction vessel, the temperature was raised to 135° C., water was removed for 5 h, the temperature was then raised to 175° C., the reaction was continued for 3 h, the temperature was further raised to 210° C., the reaction was continued for 8 h, methanol was added to the solution after cooling, a precipitate was precipitated, the precipitate was filtered, washed with water and methanol, and dried to obtain a high temperature resistant and flame resistant polyetheretherketone.
[0028] Example 3
[0029] (1) Add 10 mL of N-methylpyrrolidone, 5 mL of toluene with water, 5 mmol of pyromellitic anhydride, and 10 mmol of 5-amino-2-fluorophenol to a reaction vessel equipped with a water separator and a condenser, first heat to 145°C, remove water for 2 hours, then heat to 180°C, react for 8 hours, cool, add methanol to the solution, precipitate, filter, wash the precipitate with water and methanol, and dry to obtain N,N-(3-hydroxy-4-fluoro)phenylpyromellitic anhydride.
[0030] (2) Add 20 mL of toluene solvent, 5 mmol N,N-(3-hydroxy-4-fluoro)phenyl benzyl imide, 13 mmol pyridine, and 13 mmol O,O-dimethylphosphoryl chloride to a reaction container, and react at 15° C. for 10 hours. After the reaction, distill the solution under reduced pressure, wash the product with water and methanol, and dry it to obtain N,N-(3-phosphate-4-fluoro)phenyl benzyl imide.
[0031] (3) Add 300 mL of dimethyl sulfoxide solvent and 180 mL of toluene with water, 100 mmol of bisphenol A, 88 mmol of 4,4'-difluorobenzophenone, 12 mmol of N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and 250 mmol of potassium carbonate to a reaction vessel equipped with a water separator and a condenser, introduce nitrogen into the reaction vessel, heat the reaction vessel to 145° C., remove water for 4 h, then heat the reaction vessel to 175° C., react for 3 h, then heat the reaction vessel to 230° C., react for 5 h, cool the reaction vessel, add methanol to the solution, precipitate, filter the solution, wash with water and methanol, and dry the solution to obtain a high temperature resistant and flame resistant polyetheretherketone.
[0032] Example 4
[0033] (1) Add 8 mL of N-methylpyrrolidone, 5 mL of toluene with water, 5 mmol of pyromellitic anhydride, and 10 mmol of 5-amino-2-fluorophenol to a reaction vessel equipped with a water separator and a condenser, first heat to 140°C, remove water for 2 hours, then heat to 185°C, react for 8 hours, cool and add methanol to the solution to precipitate, filter and wash the precipitate with water and methanol, and dry to obtain N,N-(3-hydroxy-4-fluoro)phenylpyromellitic anhydride.
[0034] (2) Add 20 mL of toluene solvent, 5 mmol of N,N-(3-hydroxy-4-fluoro)phenyl benzyl imide, 14 mmol of pyridine, and 13 mmol of O,O-dimethylphosphoryl chloride into a reaction container, and react at 15° C. for 10 hours. After the reaction, distill the solution under reduced pressure, wash the product with water and methanol, and dry it to obtain N,N-(3-phosphate-4-fluoro)phenyl benzyl imide.
[0035] (3) Add 300 mL of dimethyl sulfoxide solvent and 180 mL of toluene with water, 100 mmol of bisphenol A, 85 mmol of 4,4'-difluorobenzophenone, 15 mmol of N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and 240 mmol of potassium carbonate to a reaction vessel equipped with a water separator and a condenser, introduce nitrogen into the reaction vessel, heat the reaction vessel to 145° C., remove water for 4 h, then heat the reaction vessel to 170° C., react for 3 h, then heat the reaction vessel to 220° C., react for 5 h, cool the reaction vessel, add methanol to the solution, precipitate, filter the solution, wash with water and methanol, and dry the solution to obtain a high temperature resistant and flame resistant polyetheretherketone.
[0036] Comparative Example 1
[0037] (1) 300 mL of sulfolane solvent and 150 mL of toluene with water, 100 mmol of hydroquinone, 100 mmol of 4,4'-difluorobenzophenone, and 250 mmol of potassium carbonate are added to a reaction vessel equipped with a water separator and a condenser. Nitrogen is introduced into the reaction vessel, the temperature is raised to 140° C., water is removed for 5 h, the temperature is then raised to 180° C., the reaction is carried out for 2 h, the temperature is then raised to 220° C., the reaction is carried out for 6 h, methanol is added to the solution after cooling, a precipitate is precipitated, the precipitate is filtered, washed with water and methanol, and dried to obtain a high temperature resistant and flame resistant polyetheretherketone.
[0038] The thermal properties of PEEK were tested by thermogravimetric analysis. The thermogravimetric analyzer used air as the test atmosphere and heated from 10°C / min to 800°C.
[0039] The combustion performance of polyetheretherketone was tested using a cone calorimeter. The thermal radiation intensity was 90kW / m 2 The test results are shown in Table 1.
[0040] Table 1 Thermal properties and combustion performance test of polyetheretherketone
[0041]
[0042] Table 1 shows that the temperature at which the mass loss of polyetheretherketone of Examples 1-4 is 5% reaches 494.8-513.7°C, and the high-temperature residual carbon content reaches 17.4-31.3%. The peak heat release rate is only 212.0-402.3 kW / m 2, with better high temperature resistance and flame retardant and flame retardant properties. This is because Example 1-4 uses N,N-(3-phosphate-4-fluoro)phenyl pyromellitic imide as a difluoro monomer, and copolymerizes with conventional 4,4'-difluorobenzophenone and diphenol monomers, introducing high temperature resistant imide groups into the main chain of polyetheretherketone, significantly increasing the thermal decomposition temperature of polyetheretherketone; at the same time, flame retardant phosphate groups are introduced into the side chains of polyetheretherketone. When the phosphate groups burn, the phosphoric acid compounds produced can promote the dehydration of polyetheretherketone into carbon, which can isolate heat transfer and prevent oxygen from entering the matrix, and have a good flame retardant effect, thereby improving the residual carbon content of polyetheretherketone, reducing the peak value of the heat release rate, and having better flame retardant and flame retardant properties.
[0043] In Comparative Example 1, N,N-(3-phosphate-4-fluoro)phenylbenzene tetracarboximide was not added, the high temperature resistant imide group was not introduced into the main chain of polyetheretherketone, and the flame retardant phosphate group was not introduced into the side chain of polyetheretherketone. The thermal decomposition temperature and residual carbon content of polyetheretherketone were lower than those in the embodiment, and the peak value of the heat release rate was large, and the flame retardancy was poor.
[0044] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the concept of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing high temperature resistant and flame resistant polyetheretherketone, characterized in that: The preparation method is as follows: adding a solvent, water-carrying toluene, a diphenol monomer, 4,4'-difluorobenzophenone, N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and potassium carbonate into a reaction container equipped with a water separator and a condenser, introducing nitrogen into the reaction container, heating the reaction container to 135-145° C., removing water for 4-5 hours, then heating the reaction container to 170-180° C., reacting for 2-3 hours, then heating the reaction container to 210-220° C., reacting for 5-8 hours, cooling the reaction solution, adding methanol to the solution, precipitating the precipitate, filtering the precipitate, washing the precipitate, and drying the precipitate to obtain a high temperature resistant and flame resistant polyetheretherketone; The ratio of the diphenol monomer, 4,4'-difluorobenzophenone, N,N-(3-phosphate-4-fluoro)phenylpyromellitimide, and potassium carbonate is 1 mol: (0.85-0.97) mol: (0.03-0.15) mol: (2.4-2.8) mol; The preparation method of the N,N-(3-phosphate-4-fluoro)phenyl pyromellitimide is as follows: (1) Add N-methylpyrrolidone, water-carrying toluene, pyromellitic anhydride, and 5-amino-2-fluorophenol to a reaction vessel equipped with a water separator and a condenser, cool the solution after the reaction, add methanol to the solution to precipitate, filter, wash, and dry the precipitate to obtain N,N-(3-hydroxy-4-fluoro)phenylpyromellitic anhydride; (2) adding toluene solvent, N,N-(3-hydroxy-4-fluoro)phenyl benzyl imide, pyridine, and O,O-dimethylphosphoryl chloride into a reaction container, and after the reaction, distilling the solution under reduced pressure, washing, and drying to obtain N,N-(3-phosphate-4-fluoro)phenyl benzyl imide; The ratio of pyromellitic anhydride to 5-amino-2-fluorophenol in (1) is 1 mol: (2-2.2) mol; In the step (1), the temperature is first raised to 135-145°C, water is removed for 2-3 hours, and then the temperature is raised to 170-185°C, and the reaction is continued for 8-12 hours; The ratio of N,N-(3-hydroxy-4-fluoro)phenylpyromellitimide, pyridine and O,O-dimethylphosphoryl chloride in (2) is 1 mol: (2.2-2.8) mol: (2.3-2.6) mol; The reaction in (2) is carried out at 15-40°C for 4-10 hours.
2. The method for preparing high temperature resistant and flame resistant polyetheretherketone according to claim 1, characterized in that: The ratio of the solvent to toluene is 1 L: (0.5-0.6) L; the solvent is dimethyl sulfoxide or cyclopentane.
3. The method for preparing high temperature resistant and flame resistant polyetheretherketone according to claim 1, characterized in that: The diphenol monomer is hydroquinone, biphenol or bisphenol A.
4. Use of polyetheretherketone obtained by the preparation method according to any one of claims 1 to 3 in high temperature resistant and flame resistant special engineering plastics.
Citation Information
Patent Citations
A method for preparing highly flame-retardant polyether ether ketone oligomers
CN111943831B
Methods of manufacture of salts of hydroxy-substituted aromatic compounds and polyetherimides
CN106232563A
Method for the preparation of polyamide-imides
EP0530703A2
Polyimide resin composition
JP1994179816A
Poly(aryl ether sulfone)-ether imide copolymer and preparation method therefor
WO2019153135A1