A sodium ion battery electrolyte
By using additive A containing enbutylpiperidine cation and bisfluorosulfonimide anion, and additive B with biphenyl and vinyl sulfate structure in the sodium ion battery electrolyte, a stable SEI film is formed and the problem of sodium ions is solved. The battery electrolyte has poor SEI film stability and flammability problems at high temperatures, which improves cycle performance and flame retardant properties, extends battery life and prevents overcharging.
Patent Information
- Application Number
- CN202410636709.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-05-22
AI Technical Summary
The existing sodium-ion battery electrolyte has poor stability of the SEI membrane at high temperatures and is easily damaged by hydrofluoric acid, resulting in reduced cycle performance. The organic solvent is flammable, which can easily lead to poor battery performance.
Additive A containing enbutyl piperidine cation, bisfluorosulfonyl imide anion and organic phosphate structure is used, combined with additive B having biphenyl and vinyl sulfate structure, to form a stable SEI film and improve the film-forming performance of the electrolyte and electrical conductivity, and protects against hydrofluoric acid damage at high temperatures.
Significantly improves the cycle performance of sodium-ion batteries and the flame retardant properties of the electrolyte, prolongs battery life, prevents voltage and current from exceeding the normal range under overcharge conditions, and maintains stable battery performance.
Smart Images

Figure BDA0004851968360000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery electrolyte. Background Art
[0002] Sodium is rich in content, widely distributed, low in cost, and has similar physical and chemical properties to lithium. Sodium-ion batteries are considered to be an ideal substitute for lithium-ion batteries and have received extensive attention from researchers. Sodium-ion batteries are composed of positive electrodes, negative electrodes, electrolytes, and separators. When charging, under the action of the electric field, sodium ions are released from the positive electrode material, and through ion transport in the electrolyte, they reach the negative electrode material for embedding; the corresponding electrons flow from the external circuit through the positive electrode to the negative electrode; the discharge process is the opposite of the above-mentioned charging process.
[0003] The electrolyte in the battery will form a solid electrolyte interface (SEI) film on the surface of the negative electrode, which can selectively transmit sodium ions, hinder the solvent molecules from embedding into the negative electrode, and is not easy to fall off or dissolve. It can also be stable on the electrode surface at high temperatures. Therefore, improving the SEI film-forming performance of the electrolyte is crucial to the battery performance of sodium-ion batteries. Organic electrolytes are mainly composed of organic solvents, sodium salts and additives. Compared with aqueous electrolytes, non-aqueous organic electrolytes are easier to form a stable SEI film on the electrode surface, but most organic solvents are flammable and have an adverse effect on battery performance. In addition, since the electrolyte of the sodium-ion battery uses fluorine-containing sodium salts such as sodium hexafluorophosphate as electrolytes and uses fluorine-containing additives, hydrofluoric acid will inevitably be introduced into the battery. Hydrofluoric acid will react with the alkaline components in the SEI film to produce harmful gases to weaken the rigid SEI film, resulting in a decrease in the cycle performance of the sodium-ion battery. Ionic liquids are room temperature molten salts composed entirely of ions. They have negligible vapor pressure, are non-flammable, have high thermal and chemical stability, a wide electrochemical window, and high ionic conductivity. They are widely used as electrolyte additives, but piperidine-based ionic liquids have disadvantages such as high viscosity. In daily use, batteries are overcharged, which can cause voltage and current to exceed the normal applicable range, making them unsuitable for recycling.
[0004] In view of this, it is necessary to develop new additives to improve the comprehensive performance of the electrolyte to meet the use requirements of sodium-ion batteries. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a sodium ion battery electrolyte.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A sodium ion battery electrolyte comprises the following raw materials in parts by weight: 80-90 parts of an organic solvent, 10-20 parts of a sodium salt, 1-2 parts of an additive A and 1-2 parts of an additive B.
[0008] The organic solvent is vinylene carbonate;
[0009] The sodium salt is sodium hexafluorophosphate, and the concentration of the sodium hexafluorophosphate in the sodium ion battery electrolyte is 0.90-1.10 mol / L.
[0010] The preparation of the additive A comprises the following steps:
[0011] Step A1: Sodium formate, formic acid and formaldehyde solution are added into a flask and stirred. After 15-20 minutes, 4-piperidineethanol is slowly added dropwise into the flask within 1 hour. The reaction temperature is controlled at 70-80° C. After the addition is completed, the reaction is continued for 2-2.5 hours. The reaction product 1 is obtained by extraction with cyclohexane and drying.
[0012] Furthermore, the dosage ratio of sodium formate, formic acid, formaldehyde solution and 4-piperidineethanol is 1.85 mol: 0.93 mol: 2.80 mol: 2.34 mol, and the mass fraction of the formaldehyde solution is 37%;
[0013] During the reaction of step A1, under the reduction of sodium formate / formic acid, 4-piperidineethanol and formaldehyde react to generate reaction product 1, wherein the reaction product 1 contains an N-methylpiperidine structure and an alcoholic hydroxyl group;
[0014] Step A2: Add the reaction product 1 and bis(4-nitrobenzyl)chlorophosphate to chloroform, start reflux stirring, raise the temperature to 60° C., reflux stirring for 6-7 hours, and distill under reduced pressure to obtain the reaction product 2;
[0015] Further, the amount ratio of the reaction product 1, bis(4-nitrobenzyl) chlorophosphate and chloroform is 0.1 mol:0.1 mol:130-150 mL;
[0016] During the reaction of step A2, phosphoryl chloride of bis(4-nitrobenzyl) chlorophosphate reacts with the alcoholic hydroxyl group of reaction product 1 to generate reaction product 2 containing a phosphate ester structure;
[0017] Step A3: Add the reaction product 2, iron powder, ammonium chloride and mixed solvent into a flask, start reflux stirring, raise the temperature to 80-90°C, reflux stirring at constant temperature for 3-4h, filter while hot, rotary evaporate and extract to obtain the reaction product 3;
[0018] Furthermore, the amount ratio of the reaction product 2, iron powder, ammonium chloride, and mixed solvent is 1 mol:4 mol:2 mol:150-170 mL, and the mixed solvent is prepared by mixing water and methanol in a volume ratio of 1:3;
[0019] During the reaction of step A3, the nitro group of the reaction product 2 is reduced to an amino group to obtain the reaction product 3;
[0020] Step A4: Add the reaction product 3, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add 2-methoxypropionyl chloride to the dimethyl sulfoxide solution to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in a 0°C ice water bath, after the dropwise addition is completed, heat to 40°C, react at a constant temperature for 8-10 hours, and distill under reduced pressure to obtain a reaction product 4;
[0021] Further, the usage ratio of 2-methoxypropionyl chloride, reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.2 mol: 0.1 mol: 0.01-0.015 mol: 130-150 mL;
[0022] During the reaction of step A4, the reaction product 3 reacts with 2-methoxypropionyl chloride to generate an amide product, namely, the reaction product 4;
[0023] Step A5: Add 4-bromo-1-butene, reaction product 4 and ethyl acetate to a reaction flask, start stirring, heat to 60-70°C, react with constant temperature stirring for 32-36h, filter and vacuum dry for 24h to obtain reaction product 5; then add reaction product 5, sodium bis(fluorosulfonyl)imide (NaFS I) and deionized water to a flask, stir and react at room temperature for 12h, extract with dichloromethane until no light yellow turbidity appears in the dichloromethane phase by silver nitrate solution detection, and obtain ionic liquid, i.e. additive A, after rotary evaporation and drying;
[0024] Further, the dosage ratio of 4-bromo-1-butene, reaction product 4 and ethyl acetate is 1 mol: 1 mol: 100-120 mL; the dosage ratio of reaction product 5, sodium bis(fluorosulfonyl)imide and deionized water is 1 mol: 1 mol: 120-140 mL, and the concentration of the silver nitrate solution is 1 mol / L;
[0025] During the reaction of step A5, 4-bromo-1-butene reacts with the N-methylpiperidine structure of the reaction product 4 to generate a piperidine-type quaternary ammonium salt, namely, the reaction product 5. The reaction product 5 then undergoes anion exchange with NaFS I to generate additive A.
[0026] The preparation of the additive B comprises the following steps:
[0027] Step B1: Add 4-pentyloxy-4'-cyanobiphenyl to toluene, start stirring, then add a tetrahydrofuran solution of lithium aluminum hydride, and stir at room temperature for 1.5-2h to obtain a reaction product a;
[0028] Further, the dosage ratio of 4-pentyloxy-4'-cyanobiphenyl, toluene and tetrahydrofuran solution of lithium aluminum hydride is 0.1 mol:85-95 mL:100-110 mL, and the concentration of tetrahydrofuran solution of lithium aluminum hydride is 1 mol / L;
[0029] During the reaction of step B1, the cyano group of 4-pentyloxy-4'-cyanobiphenyl is reduced to a primary amine to obtain a reaction product a;
[0030] Step B2: Add 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride and acetonitrile into a flask, place the flask in an ice-water bath and start stirring, slowly dropwise add potassium persulfate aqueous solution under stirring, and continue stirring for 45-60 minutes after the dropwise addition is completed to obtain reaction product b;
[0031] Further, the dosage ratio of 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride, acetonitrile and potassium persulfate aqueous solution is 0.12-0.13 mol:0.1 g:105-115 mL:100 mL, and the concentration of potassium persulfate aqueous solution is 1 mol / L;
[0032] During the reaction of step B2, under the catalysis of ruthenium trichloride, 4-(chloromethyl)-1,3,2-dioxolane 2-oxide is oxidized by potassium persulfate to form reaction product b;
[0033] Step B3: Add the reaction product b and the reaction product a into methanol, then add sodium bisulfate, start stirring, stir and react at 50-60° C. for 8-10 hours, filter, extract and dry to obtain additive B;
[0034] Further, the dosage ratio of reaction product b, reaction product a, methanol and sodium bisulfate is 0.2 mol: 0.1 mol: 120-150 mL: 0.0010-0.0015 g;
[0035] During the reaction of step B3, sodium bisulfate catalyzes the dehydrochlorination of the reaction product b and the reaction product a to generate additive B.
[0036] Beneficial effects of the invention: The invention discloses a sodium ion battery electrolyte, comprising an organic solvent, a sodium salt, an additive A and an additive B. The additive A is an ionic liquid, which contains an butylpiperidinium cation, a bis(fluorosulfonyl)imide anion (FSI -), organic phosphate structure, amide bond, ether bond. After the introduction of butylene, the effect of the double bond makes it easier for the piperidinium cation to obtain electrons, so that the additive A is more preferentially reduced on the negative electrode surface. Affected by the double bond and carbon chain length in the butylene, the vibration of the covalent bond between atoms is intensified, which reduces the chemical hardness of the ionic liquid and makes it easier to form a solid electrolyte interphase (SE I) film, making the electrolyte have excellent film-forming properties; bis(fluorosulfonyl)imide anion (FS I - ) has a smaller molecular volume and weaker contact with the cations in additive A, which reduces the viscosity of additive A, facilitates ion migration, and improves the conductivity of the electrolyte; the ether bond introduced on the side chain of additive A increases the Na + The solubility of the additive in the ionic liquid is improved, and the high viscosity of the additive A caused by the large molecular volume is reduced, and the conductivity of the electrolyte is further improved; the organic phosphate structure has the advantages of phosphorus-based flame retardants, and has excellent flame retardant properties for electrolyte systems containing flammable organic solvents; the amide bond is a basic group, which can combine with hydrofluoric acid and trace water in the electrolyte, thereby removing hydrofluoric acid and trace water, avoiding damage to the solid electrolyte interphase (SE I) membrane, shortening the battery life, and helping to solve the problems of increased battery impedance and decreased cycle performance.
[0037] The synthesized additive B contains biphenyl structure, vinyl sulfate structure and ether bond in its molecular structure. When the voltage is too high, the biphenyl structure undergoes electropolymerization, consumes the current generated during overcharging, prevents the voltage from continuing to rise, and maintains the voltage and current of the battery within the normal range, so that the electrolyte has anti-overcharge performance; the vinyl sulfate structure is used to inhibit the decrease in the initial capacity of the battery, increase the initial discharge capacity, reduce the volume expansion of the battery after high-temperature storage, and improve the battery's charge and discharge performance and cycle times, thereby improving the battery's cycle performance. The vinyl sulfate structure can also decompose to form sulfate and sulfite to stabilize the SE I film, thereby improving the performance of the sodium ion battery and extending its life; the ether bond structure makes additive B and additive A have good compatibility, which helps the two coexist in the electrolyte without affecting the normal performance of the battery. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] An additive A, the preparation of which comprises the following steps:
[0041] Step A1: sodium formate, formic acid and formaldehyde solution are added into a flask, stirring is started, and after 15 minutes, 4-piperidineethanol is slowly added dropwise into the flask within 1 hour, and the reaction temperature is controlled at 70° C. After the addition is completed, the reaction is continued for 2 hours, and the reaction product 1 is obtained by extraction with cyclohexane and drying; the dosage ratio of sodium formate, formic acid, formaldehyde solution and 4-piperidineethanol is 1.85 mol: 0.93 mol: 2.80 mol: 2.34 mol, and the mass fraction of the formaldehyde solution is 37%;
[0042] Step A2: adding the reaction product 1 and bis(4-nitrobenzyl) chlorophosphate to chloroform, starting stirring, heating to 60°C, stirring for reaction for 6 hours, and distilling under reduced pressure to obtain the reaction product 2; the amount ratio of the reaction product 1, bis(4-nitrobenzyl) chlorophosphate and chloroform is 0.1 mol:0.1 mol:130 mL;
[0043] Step A3: Add the reaction product 2, iron powder, ammonium chloride and a mixed solvent into a flask, start reflux stirring, raise the temperature to 80°C, reflux and stir to react for 3 hours at a constant temperature, filter while hot, rotary evaporate and extract to obtain the reaction product 3; the amount ratio of the reaction product 2, iron powder, ammonium chloride and the mixed solvent is 1 mol:4 mol:2 mol:150 mL, and the mixed solvent is prepared by mixing water and methanol in a volume ratio of 1:3;
[0044] Step A4: adding the reaction product 3, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding 2-methoxypropionyl chloride into the dimethyl sulfoxide solution to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice water bath at 0°C, after the dropping is completed, heating to 40°C, reacting at a constant temperature for 8h, and distilling under reduced pressure to obtain a reaction product 4; the amount ratio of 2-methoxypropionyl chloride, reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.2 mol: 0.1 mol: 0.01 mol: 130 mL;
[0045] Step A5: Add 4-bromo-1-butene, reaction product 4 and ethyl acetate to a reaction flask, start stirring, heat to 60°C, react at constant temperature with stirring for 32 hours, filter and vacuum dry for 24 hours to obtain reaction product 5; then add reaction product 5, sodium bis(fluorosulfonyl)imide (NaFS I) and deionized water to a flask, stir and react at room temperature for 12 hours, extract with dichloromethane until no light yellow turbidity appears in the dichloromethane phase when detected by silver nitrate solution, and obtain ionic liquid, i.e. additive A, after rotary evaporation and drying; the amount ratio of 4-bromo-1-butene, reaction product 4 and ethyl acetate is 1 mol:1 mol:100 mL; the amount ratio of reaction product 5, sodium bis(fluorosulfonyl)imide and deionized water is 1 mol:1 mol:120 mL, and the concentration of silver nitrate solution is 1 mol / L.
[0046] Example 2
[0047] An additive A, the preparation of which comprises the following steps:
[0048] Step A1: sodium formate, formic acid and formaldehyde solution are added into a flask, stirring is started, and after 17 minutes, 4-piperidineethanol is slowly added dropwise into the flask within 1 hour, and the reaction temperature is controlled at 75° C. After the addition is completed, the reaction is continued for 2.2 hours, and the reaction product 1 is obtained by extraction with cyclohexane and drying; the dosage ratio of sodium formate, formic acid, formaldehyde solution and 4-piperidineethanol is 1.85 mol: 0.93 mol: 2.80 mol: 2.34 mol, and the mass fraction of the formaldehyde solution is 37%;
[0049] Step A2: adding the reaction product 1 and bis(4-nitrobenzyl) chlorophosphate to chloroform, starting reflux stirring, heating to 60°C, reacting with reflux stirring for 6.5h, and distilling under reduced pressure to obtain the reaction product 2; the amount ratio of the reaction product 1, bis(4-nitrobenzyl) chlorophosphate and chloroform is 0.1 mol:0.1 mol:140 mL;
[0050] Step A3: Add the reaction product 2, iron powder, ammonium chloride and a mixed solvent into a flask, start reflux stirring, raise the temperature to 85°C, reflux and stir to react for 3.5 hours at a constant temperature, filter while hot, rotary evaporate and extract to obtain the reaction product 3; the amount ratio of the reaction product 2, iron powder, ammonium chloride and the mixed solvent is 1 mol:4 mol:2 mol:160 mL, and the mixed solvent is prepared by mixing water and methanol in a volume ratio of 1:3;
[0051] Step A4: adding the reaction product 3, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding 2-methoxypropionyl chloride into the dimethyl sulfoxide solution to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice water bath at 0°C, after the dropping is complete, heating to 40°C, reacting at constant temperature for 9 hours, and distilling under reduced pressure to obtain a reaction product 4; the amount ratio of 2-methoxypropionyl chloride, reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.2 mol: 0.1 mol: 0.012 mol: 140 mL;
[0052] Step A5: Add 4-bromo-1-butene, reaction product 4 and ethyl acetate to a reaction flask, start stirring, heat to 65°C, react at constant temperature with stirring for 34 hours, filter and vacuum dry for 24 hours to obtain reaction product 5; then add reaction product 5, sodium bis(fluorosulfonyl)imide (NaFS I) and deionized water to a flask, stir and react at room temperature for 12 hours, extract with dichloromethane until no light yellow turbidity appears in the dichloromethane phase when detected by silver nitrate solution, rotary evaporate and dry to obtain ionic liquid, i.e. additive A; the amount ratio of 4-bromo-1-butene, reaction product 4 and ethyl acetate is 1 mol:1 mol:110 mL; the amount ratio of reaction product 5, sodium bis(fluorosulfonyl)imide and deionized water is 1 mol:1 mol:130 mL, and the concentration of silver nitrate solution is 1 mol / L.
[0053] Example 3
[0054] An additive A, the preparation of which comprises the following steps:
[0055] Step A1: sodium formate, formic acid and formaldehyde solution are added into a flask, stirring is started, after 20 minutes, 4-piperidineethanol is slowly added dropwise into the flask within 1 hour, the reaction temperature is controlled at 80° C. After the addition is completed, the reaction is continued for 2.5 hours, and the reaction product 1 is obtained by extraction with cyclohexane and drying; the dosage ratio of sodium formate, formic acid, formaldehyde solution and 4-piperidineethanol is 1.85 mol: 0.93 mol: 2.80 mol: 2.34 mol, and the mass fraction of the formaldehyde solution is 37%;
[0056] Step A2: adding the reaction product 1 and bis(4-nitrobenzyl) chlorophosphate to chloroform, starting reflux stirring, heating to 60°C, reflux stirring for 7 hours, and distilling under reduced pressure to obtain the reaction product 2; the amount ratio of the reaction product 1, bis(4-nitrobenzyl) chlorophosphate and chloroform is 0.1 mol:0.1 mol:150 mL;
[0057] Step A3: Add the reaction product 2, iron powder, ammonium chloride and a mixed solvent into a flask, start reflux stirring, raise the temperature to 90°C, reflux and stir at a constant temperature for 4 hours, filter while hot, rotary evaporate and extract to obtain the reaction product 3; the amount ratio of the reaction product 2, iron powder, ammonium chloride and the mixed solvent is 1 mol:4 mol:2 mol:170 mL, and the mixed solvent is prepared by mixing water and methanol in a volume ratio of 1:3;
[0058] Step A4: adding the reaction product 3, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding 2-methoxypropionyl chloride into the dimethyl sulfoxide solution to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropping is completed, heating to 40°C, reacting at a constant temperature for 10 hours, and distilling under reduced pressure to obtain a reaction product 4; the amount ratio of 2-methoxypropionyl chloride, reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.2 mol: 0.1 mol: 0.015 mol: 150 mL;
[0059] Step A5: Add 4-bromo-1-butene, reaction product 4 and ethyl acetate to a reaction flask, start stirring, heat to 70°C, react at constant temperature with stirring for 36 hours, filter and vacuum dry for 24 hours to obtain reaction product 5; then add reaction product 5, sodium bis(fluorosulfonyl)imide (NaFS I) and deionized water to a flask, stir and react at room temperature for 12 hours, extract with dichloromethane until no light yellow turbidity appears in the dichloromethane phase when detected by silver nitrate solution, rotary evaporate and dry to obtain ionic liquid, i.e. additive A; the amount ratio of 4-bromo-1-butene, reaction product 4 and ethyl acetate is 1 mol:1 mol:120 mL; the amount ratio of reaction product 5, sodium bis(fluorosulfonyl)imide and deionized water is 1 mol:1 mol:140 mL, and the concentration of silver nitrate solution is 1 mol / L.
[0060] Example 4
[0061] An additive B, the preparation of which comprises the following steps:
[0062] Step B1: Add 4-pentyloxy-4'-cyanobiphenyl to toluene, start stirring, then add a tetrahydrofuran solution of lithium aluminum hydride, and stir the reaction at room temperature for 1.5 hours to obtain a reaction product a; the dosage ratio of 4-pentyloxy-4'-cyanobiphenyl, toluene and the tetrahydrofuran solution of lithium aluminum hydride is 0.1 mol:85 mL:100 mL, and the concentration of the tetrahydrofuran solution of lithium aluminum hydride is 1 mol / L;
[0063] Step B2: Add 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride and acetonitrile to a flask, place the flask in an ice-water bath and start stirring, slowly dropwise add potassium persulfate aqueous solution under stirring, and continue stirring for 45 minutes after the dropwise addition is completed to obtain reaction product b; the amount ratio of 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride, acetonitrile and potassium persulfate aqueous solution is 0.12 mol: 0.1 g: 105 mL: 100 mL, and the concentration of potassium persulfate aqueous solution is 1 mol / L;
[0064] Step B3: Add reaction product b and reaction product a to methanol, then add sodium bisulfate, start stirring, stir and react at 50°C for 8 hours, filter, extract and dry to obtain additive B; the dosage ratio of reaction product b, reaction product a, methanol and sodium bisulfate is 0.2 mol:0.1 mol:120 mL:0.0010 g.
[0065] Example 5
[0066] An additive B, the preparation of which comprises the following steps:
[0067] Step B1: Add 4-pentyloxy-4'-cyanobiphenyl to toluene, start stirring, then add a tetrahydrofuran solution of lithium aluminum hydride, and stir the reaction at room temperature for 1.7 hours to obtain a reaction product a; the dosage ratio of 4-pentyloxy-4'-cyanobiphenyl, toluene and the tetrahydrofuran solution of lithium aluminum hydride is 0.1 mol:90 mL:105 mL, and the concentration of the tetrahydrofuran solution of lithium aluminum hydride is 1 mol / L;
[0068] Step B2: Add 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride and acetonitrile to a flask, place the flask in an ice-water bath and start stirring, slowly dropwise add potassium persulfate aqueous solution under stirring, and continue stirring for 50 minutes after the dropwise addition is completed to obtain reaction product b; the amount ratio of 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride, acetonitrile and potassium persulfate aqueous solution is 0.125 mol: 0.1 g: 110 mL: 100 mL, and the concentration of potassium persulfate aqueous solution is 1 mol / L;
[0069] Step B3: Add reaction product b and reaction product a to methanol, then add sodium bisulfate, start stirring, stir and react at 55°C for 9 hours, filter, extract and dry to obtain additive B; the dosage ratio of reaction product b, reaction product a, methanol and sodium bisulfate is 0.2 mol:0.1 mol:135 mL:0.0012 g.
[0070] Example 6
[0071] An additive B, the preparation of which comprises the following steps:
[0072] Step B1: Add 4-pentyloxy-4'-cyanobiphenyl to toluene, start stirring, then add a tetrahydrofuran solution of lithium aluminum hydride, and stir the reaction at room temperature for 2 hours to obtain a reaction product a; the dosage ratio of 4-pentyloxy-4'-cyanobiphenyl, toluene and the tetrahydrofuran solution of lithium aluminum hydride is 0.1 mol:95 mL:110 mL, and the concentration of the tetrahydrofuran solution of lithium aluminum hydride is 1 mol / L;
[0073] Step B2: Add 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride and acetonitrile to a flask, place the flask in an ice-water bath and start stirring, slowly dropwise add potassium persulfate aqueous solution under stirring, and continue stirring for 60 minutes after the dropwise addition is completed to obtain reaction product b; the amount ratio of 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride, acetonitrile and potassium persulfate aqueous solution is 0.13 mol: 0.1 g: 115 mL: 100 mL, and the concentration of potassium persulfate aqueous solution is 1 mol / L;
[0074] Step B3: Add reaction product b and reaction product a to methanol, then add sodium bisulfate, start stirring, stir and react at 60°C for 10 hours, filter, extract and dry to obtain additive B; the dosage ratio of reaction product b, reaction product a, methanol and sodium bisulfate is 0.2 mol:0.1 mol:150 mL:0.0015 g.
[0075] Example 7
[0076] A sodium ion battery electrolyte comprises the following raw materials in parts by weight: 80 parts of an organic solvent, 10 parts of a sodium salt, 1 part of an additive A and 1 part of an additive B; the organic solvent is vinylene carbonate; the sodium salt is sodium hexafluorophosphate, and the concentration of the sodium hexafluorophosphate in the sodium ion battery electrolyte is 0.90 mol / L.
[0077] The sodium ion battery electrolyte is prepared by the following steps:
[0078] In a glove box filled with argon, sodium hexafluorophosphate was slowly added to vinylene carbonate and stirred for 30 minutes. Then, additive A obtained in Example 1 and additive B obtained in Example 4 were added and stirred for 15 minutes to obtain a sodium ion battery electrolyte.
[0079] Example 8
[0080] A sodium ion battery electrolyte comprises the following raw materials in parts by weight: 85 parts of an organic solvent, 15 parts of a sodium salt, 1.5 parts of an additive A and 1.5 parts of an additive B; the organic solvent is vinylene carbonate; the sodium salt is sodium hexafluorophosphate, and the concentration of the sodium hexafluorophosphate in the sodium ion battery electrolyte is 1.00 mol / L.
[0081] The sodium ion battery electrolyte is prepared by the following steps:
[0082] In a glove box filled with argon, sodium hexafluorophosphate was slowly added to vinylene carbonate and stirred for 35 minutes. Then, additive A obtained in Example 2 and additive B obtained in Example 5 were added and stirred for 20 minutes to obtain a sodium ion battery electrolyte.
[0083] Example 9
[0084] A sodium ion battery electrolyte comprises the following raw materials in parts by weight: 90 parts of an organic solvent, 20 parts of a sodium salt, 2 parts of an additive A and 2 parts of an additive B; the organic solvent is vinylene carbonate; the sodium salt is sodium hexafluorophosphate, and the concentration of the sodium hexafluorophosphate in the sodium ion battery electrolyte is 1.10 mol / L.
[0085] The sodium ion battery electrolyte is prepared by the following steps:
[0086] In a glove box filled with argon, sodium hexafluorophosphate was slowly added to vinylene carbonate and stirred for 45 minutes. Then, additive A obtained in Example 3 and additive B obtained in Example 6 were added and stirred for 25 minutes to obtain a sodium ion battery electrolyte.
[0087] Comparative Example 1
[0088] This comparative example is a commercially available sodium ion battery electrolyte.
[0089] Comparative Example 2
[0090] Compared with Example 9, the additive A was replaced with the piperidinium ionic liquid (pp14) containing butylene in the paper "Study on High Temperature Performance of Piperidinyl Ionic Liquids in Sodium Ion Batteries", and the rest was exactly the same as Example 9 to prepare a sodium ion battery electrolyte.
[0091] Comparative Example 3
[0092] Compared with Example 9, the additive B was replaced with biphenyl, and the rest was exactly the same as Example 9 to prepare a sodium ion battery electrolyte.
[0093] Comparative Example 4
[0094] Compared with Example 9, the additive B was replaced with vinyl sulfate, and the rest was exactly the same as Example 9 to prepare a sodium ion battery electrolyte.
[0095] The sodium ion battery electrolyte prepared by the present invention is further tested for its effect, and the test results are as follows.
[0096] In order to test the sodium ion battery electrolyte prepared by the present invention, the flame retardant performance of the electrolyte was measured according to the following method; the sodium ion battery electrolyte of each embodiment and comparative example was applied to a sodium ion battery, and the cycle performance of the battery was measured according to the following method; an overcharge test was performed under the conditions of SOC100%, 1C / 10V, and the test results were recorded in Table 1;
[0097] Test method for flame retardancy of electrolyte: soak glass fiber paper in electrolyte, then pick it up with tweezers and ignite it, and record its natural extinguishing time in Table 1;
[0098] Battery cycle performance test method: Place the sodium ion battery in a constant temperature box at 25°C, charge to 4.3V (cut-off current is 0.05C) at a constant current and constant voltage of 1C, let the battery stand for 5 minutes after being fully charged, and then discharge to 2.0V at a constant current of 1C, record the discharge capacity after the first cycle, and after 400 charge / discharge cycles, determine the capacity retention rate of the sodium ion battery, the 400th cycle capacity retention rate (%) = (400th cycle discharge capacity / first cycle discharge capacity) × 100%, and record the capacity retention rate in Table 1;
[0099] Table 1:
[0100]
[0101] According to the data in Table 1, compared with Comparative Example 1, it can be seen that, compared with commercially available sodium ion battery electrolytes, the sodium ion battery electrolyte prepared by the present invention is applied to sodium ion batteries, and the electrolyte has excellent flame retardant properties, and the sodium ion battery has excellent cycle performance and capacity retention rate; compared with the piperidinium ionic liquid (pp14) of butylene, the introduction of organic phosphate structure, amide bond and ether bond helps to form a more stable SE I film, improve the cycle performance of the battery and the flame retardant properties of the electrolyte; compared with Comparative Example 3, it can be seen that ether bonds and vinyl sulfate are introduced on the basis of biphenyl to further form a stable SE I film, which is beneficial to the improvement of battery cycle performance; compared with Comparative Example 4, it can be seen that the absence of a biphenyl structure with anti-overcharge performance will cause the battery temperature to rise abnormally.
[0102] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A sodium ion battery electrolyte, characterized in that: The invention comprises the following raw materials in parts by weight: 80-90 parts of an organic solvent, 10-20 parts of a sodium salt, 1-2 parts of an additive A and 1-2 parts of an additive B; the organic solvent is vinylene carbonate; the sodium salt is sodium hexafluorophosphate, and the concentration of the sodium hexafluorophosphate in the sodium ion battery electrolyte is 0.90-1.10 mol / L; The preparation of the additive A comprises the following steps: Step A1: Sodium formate, formic acid and formaldehyde solution are added into a flask and stirred. After 15-20 minutes, 4-piperidineethanol is slowly added dropwise into the flask within 1 hour. The reaction temperature is controlled at 70-80° C. After the addition is completed, the reaction is continued for 2-2.5 hours. The reaction product 1 is obtained by extraction with cyclohexane and drying. Step A2: Add the reaction product 1 and bis(4-nitrobenzyl)chlorophosphate to chloroform, start reflux stirring, raise the temperature to 60° C., reflux stirring for 6-7 hours, and distill under reduced pressure to obtain the reaction product 2; Step A3: Add the reaction product 2, iron powder, ammonium chloride and mixed solvent into a flask, start reflux stirring, raise the temperature to 80-90°C, reflux stirring at constant temperature for 3-4h, filter while hot, rotary evaporate and extract to obtain the reaction product 3; Step A4: adding the reaction product 3, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding 2-methoxypropionyl chloride into the dimethyl sulfoxide solution to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice water bath at 0°C, after the dropping is complete, heating to 40°C, reacting at a constant temperature for 8-10 hours, and distilling under reduced pressure to obtain a reaction product 4; Step A5: Add 4-bromo-1-butene, reaction product 4 and ethyl acetate to a reaction flask, start stirring, heat to 60-70°C, react with constant temperature stirring for 32-36h, filter and vacuum dry for 24h to obtain reaction product 5; then add reaction product 5, sodium bis(fluorosulfonyl)imide and deionized water to a flask, stir and react at room temperature for 12h, extract with dichloromethane until no light yellow turbidity appears in the dichloromethane phase by silver nitrate solution detection, rotary evaporate and dry to obtain ionic liquid, i.e., additive A; The preparation of the additive B comprises the following steps: Step B1: Add 4-pentyloxy-4'-cyanobiphenyl to toluene, start stirring, then add a tetrahydrofuran solution of lithium aluminum hydride, and stir at room temperature for 1.5-2h to obtain a reaction product a; Step B2: Add 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride and acetonitrile into a flask, place the flask in an ice-water bath and start stirring, slowly dropwise add potassium persulfate aqueous solution under stirring, and continue stirring for 45-60 minutes after the dropwise addition is completed to obtain reaction product b; Step B3: Add the reaction product b and the reaction product a into methanol, then add sodium bisulfate, start stirring, stir and react at 50-60° C. for 8-10 hours, filter, extract and dry to obtain additive B.
2. A sodium ion battery electrolyte according to claim 1, characterized in that: In step A1, the usage ratio of sodium formate, formic acid, formaldehyde solution and 4-piperidineethanol is 1.85 mol: 0.93mol:2.80mol:2.34mol, the mass fraction of formaldehyde solution is 37%.
3. A sodium ion battery electrolyte according to claim 1, characterized in that: In step A2, the usage ratio of reaction product 1, bis(4-nitrobenzyl)chlorophosphate and chloroform is 0.1 mol:0.1 mol:130-150 mL.
4. A sodium ion battery electrolyte according to claim 1, characterized in that: In step A3, the dosage ratio of reaction product 2, iron powder, ammonium chloride and mixed solvent is 1 mol: 4 mol: 2 mol: 150-170 mL, and the mixed solvent is prepared by mixing water and methanol in a volume ratio of 1:
3.
5. A sodium ion battery electrolyte according to claim 1, characterized in that: In step A4, the usage ratio of 2-methoxypropionyl chloride, reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.2 mol: 0.1 mol: 0.01-0.015 mol: 130-150 mL.
6. A sodium ion battery electrolyte according to claim 1, characterized in that: In step A5, the usage ratio of 4-bromo-1-butene, reaction product 4 and ethyl acetate is 1 mol: 1 mol: 100-120 mL; the usage ratio of reaction product 5, sodium bis(fluorosulfonyl)imide and deionized water is 1 mol: 1 mol: 120-140 mL, and the concentration of the silver nitrate solution is 1 mol / L.
7. A sodium ion battery electrolyte according to claim 1, characterized in that: In step B1, the usage ratio of 4-pentyloxy-4'-cyanobiphenyl, toluene and tetrahydrofuran solution of lithium aluminum hydride is 0.1 mol:85-95 mL:100-110 mL, and the concentration of the tetrahydrofuran solution of lithium aluminum hydride is 1 mol / L.
8. A sodium ion battery electrolyte according to claim 1, characterized in that: In step B2, the usage ratio of 4-(chloromethyl)-1,3,2-dioxolane 2-oxide, ruthenium trichloride, acetonitrile and potassium persulfate aqueous solution is 0.12-0.13 mol:0.1 g:105-115 mL:100 mL, and the concentration of potassium persulfate aqueous solution is 1 mol / L.
9. A sodium ion battery electrolyte according to claim 1, characterized in that: In step B3, the usage ratio of reaction product b, reaction product a, methanol and sodium bisulfate is 0.2 mol: 0.1 mol: 120-150 mL: 0.0010-0.0015 g.
Citation Information
Patent Citations
Preparation method and application of novel piperidine ionic liquid electrolyte
CN115621548A
Synthesis method and application of cucurbit [7] uril-truxene derivative
CN115626930A