Lithium-sulfur secondary battery
By using a specific ratio of nitriles, fluorinated ethers, and disulfides as electrolytes in lithium-sulfur secondary batteries, and by optimizing the porosity and sulfur loading of the cathode, the energy density problem of lithium-sulfur secondary batteries under high load and low porosity conditions was solved, achieving high initial discharge capacity and low overvoltage.
Patent Information
- Application Number
- CN202080028482.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-28
- Filing Date
- 2020-10-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-10-08
AI Technical Summary
Existing lithium-sulfur secondary batteries struggle to achieve high energy density under high load and low porosity conditions. Furthermore, the high viscosity and low ionic conductivity of the electrolyte lead to high overvoltage and deterioration of battery performance.
An electrolyte containing nitrile solvents, fluorinated ether solvents, and disulfide solvents is used, and their volume ratio is adjusted to a specific ratio. The porosity and sulfur loading in the positive electrode are controlled to form a positive electrode structure with high loading and low porosity.
It improves the initial discharge capacity and average discharge voltage of lithium-sulfur secondary batteries, reduces the viscosity of the electrolyte, enhances ionic conductivity, and improves the energy density and voltage performance of the batteries.
Smart Images

Figure CN113692666B_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0134367, filed on October 28, 2019, the entire contents of which are incorporated herein by reference.
[0002] The invention relates to a lithium-sulfur secondary battery. Background Art
[0003] As the application field of secondary batteries expands to electric vehicles (EV) or energy storage systems (ESS), the application of lithium-ion secondary batteries with relatively low energy storage density per unit weight (about 250Wh / kg) in such products is limited. Alternatively, lithium-sulfur secondary batteries have attracted attention as the next generation of secondary battery technology because they can achieve a theoretically high energy storage density per unit weight (about 2600Wh / kg).
[0004] Lithium-sulfur secondary batteries refer to battery systems that use sulfur-based materials with SS bonds (sulfur-sulfur bonds) as positive electrode active materials and lithium metal as negative electrode active materials. Sulfur, the main material of positive electrode active materials, has the advantages of being very abundant in resources, non-toxic, and having a low atomic weight.
[0005] In a lithium-sulfur secondary battery, when the battery is discharged, lithium, which is the negative electrode active material, is oxidized while releasing electrons and thereby ionized, and the sulfur material, which is the positive electrode active material, is reduced while receiving electrons. In this case, the oxidation reaction of lithium is a process in which lithium metal releases electrons and is converted into a lithium cation form. In addition, the reduction reaction of sulfur is a process in which the SS bond receives two electrons and is converted into a sulfur anion form. The lithium cations generated by the oxidation reaction of lithium are transferred to the positive electrode through the electrolyte, and form salts by combining with the sulfur anions generated by the reduction reaction of sulfur. Specifically, the sulfur before discharge has a cyclic S8 structure, which is converted into lithium polysulfide (LiS) by the reduction reaction. x ). When lithium polysulfide is completely reduced, lithium sulfide (Li2S) is generated.
[0006] Sulfur, as the positive electrode active material, is difficult to reactivity with electrons and lithium ions in solid form due to its low conductivity. In existing lithium-sulfur secondary batteries, Li2S is produced to improve the reactivity of sulfur. x The intermediate product lithium polysulfide is formed to cause a liquid phase reaction and improve the reactivity. In this case, an ether solvent (such as dioxolane and ethylene glycol dimethyl ether) having a high solubility for lithium polysulfide is used as a solvent for the electrolyte.
[0007] As described above, lithium polysulfide, which is an intermediate product formed during charge / discharge of a lithium-sulfur secondary battery, plays a role in allowing the battery to operate, but is also a major cause of battery performance degradation.
[0008] In conventional lithium-sulfur secondary batteries, a cathode electrolyte type lithium-sulfur secondary battery system is constructed to improve reactivity. In the case of such a cathode electrolyte type electrolyte, reactivity is improved by using a solvent that can dissolve a large amount of lithium polysulfide. However, due to the characteristics of lithium polysulfide dissolved in the electrolyte, the reactivity and life characteristics of sulfur are affected by the content of the electrolyte. In order to develop lithium-sulfur secondary batteries with a high energy density of more than 500Wh / kg required for aircraft and next-generation electric vehicles, electrodes with high sulfur loading and low porosity are required, and the content of the electrolyte needs to be minimized.
[0009] However, due to the characteristics of the catholyte-type electrolyte, there is a problem that as the electrolyte content decreases, the viscosity increases rapidly during charge / discharge, so that overvoltage may increase and the battery may deteriorate.
[0010] Therefore, a small amount of electrolyte needs to be injected. However, as the content of the electrolyte decreases, the concentration of lithium polysulfide in the electrolyte increases, so that the battery is difficult to operate normally due to reduced fluidity of the active material and increased side reactions.
[0011] Alternatively, research is being conducted on electrolyte systems of sparingly soluble electrolytes (SSEs) that form only trace amounts of lithium polysulfides on the electrode surface.
[0012] Since lithium polysulfide is almost insoluble in the SSE system, the loss of sulfur in the electrode is small, and it can operate even in an electrode with low porosity, but there are problems such as difficulty in construction at room temperature and high overvoltage due to the high viscosity and low ion conductivity of the electrolyte. In addition, the energy density is also close to the limit, so there is a situation where additional measures are required. In order to construct a lithium-sulfur secondary battery with high energy density, a battery system capable of driving an electrode with high load and low porosity is required, and research on such a battery system is being continuously conducted in this technical field.
[0013] Prior art literature
[0014] [Non-patent literature]
[0015] (Non-patent document 1) Abbas Fotouhi et al., Lithium-Sulfur Battery Technology Readiness and Applications―A Review, Energies, 2017, 10, 1937. Summary of the invention
[0016] [Technical issues]
[0017] An object of the present invention is to provide a lithium-sulfur secondary battery comprising a positive electrode satisfying specific conditions of high load and low porosity to construct a lithium-sulfur secondary battery with high energy density, wherein the lithium-sulfur secondary battery has an increased initial discharge capacity and an increased average discharge voltage by containing a nitrile solvent, a fluorinated ether solvent, and a disulfide solvent in an appropriate volume ratio in an electrolyte.
[0018] [Technical solution]
[0019] In order to achieve the above-mentioned object, the present invention provides a lithium-sulfur secondary battery, which comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte contains a lithium salt and a solvent, the solvent contains a nitrile solvent, a fluorinated ether solvent and a disulfide solvent, and based on the total volume of the solvent, the content of the disulfide solvent is 20 volume % to 35 volume %.
[0020] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the lithium salt is at least one selected from the following: LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiB(Ph)4, LiC4BO8, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate and lithium imide.
[0021] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the concentration of the lithium salt is 1.5M (mol / L) to 2.5M (mol / L).
[0022] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the nitrile solvent is at least one selected from the following: acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide.
[0023] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the content of the nitrile solvent is 25 volume % to 35 volume % based on the total volume of the solvent.
[0024] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the fluorinated ether solvent is at least one selected from the following:
[0025] 2,2,2-Trifluoroethyl methyl ether (CF3CH2OCH3);
[0026] 2,2,2-Trifluoroethyldifluoromethyl ether (CF3CH2OCHF2);
[0027] 2,2,3,3,3-pentafluoropropyl methyl ether (CF3CF2CH2OCH3);
[0028] 2,2,3,3,3-pentafluoropropyldifluoromethyl ether (CF3CF2CH2OCHF2);
[0029] 2,2,3,3,3-pentafluoropropyl-1,1,2,2-tetrafluoroethyl ether (CF3CF2CH2OCF2CF2H);
[0030] 1,1,2,2-Tetrafluoroethyl methyl ether (HCF2CF2OCH3);
[0031] 1,1,2,2-Tetrafluoroethyl ethyl ether (HCF2CF2OCH2CH3);
[0032] 1,1,2,2-Tetrafluoroethylpropyl ether (HCF2CF2OC3H7);
[0033] 1,1,2,2-Tetrafluoroethyl butyl ether (HCF2CF2OC4H9);
[0034] 2,2,3,3-Tetrafluoroethyldifluoromethyl ether (H(CF2)2CH2O(CF2)H);
[0035] 1,1,2,2-Tetrafluoroethyl isobutyl ether (HCF2CF2OCH2CH(CH3)2);
[0036] 1,1,2,2-Tetrafluoroethyl isopentyl ether (HCF2CF2OCH2C(CH3)3);
[0037] 1,1,2,2-Tetrafluoroethyl-2,2,2-trifluoroethyl ether (HCF2CF2OCH2CF3);
[0038] 1,1,2,2-Tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HCF2CF2OCH2CF2CF2H);
[0039] Hexafluoroisopropyl methyl ether ((CF3)2CHOCH3);
[0040] 1,1,3,3,3-pentafluoro-2-trifluoromethylpropyl methyl ether ((CF3)2CHCF2OCH3);
[0041] 1,1,2,3,3,3-Hexafluoropropyl methyl ether (CF3CHFCF2OCH3);
[0042] 1,1,2,3,3,3-Hexafluoropropyl ethyl ether (CF3CHFCF2OCH2CH3); and
[0043] 2,2,3,4,4,4-Hexafluorobutyldifluoromethyl ether (CF3CHFCF2CH2OCHF2).
[0044] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the disulfide solvent is dimethyl disulfide.
[0045] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the content of the nitrile solvent is 25 volume % to 35 volume % based on the total volume of the solvent, the content of the fluorinated ether solvent is 30 volume % to 50 volume % based on the total volume of the solvent, and the content of the disulfide solvent is 20 volume % to 35 volume % based on the total volume of the solvent.
[0046] In addition, the present invention provides a lithium-sulfur secondary battery, wherein the content of the nitrile solvent is 25 volume % to 35 volume % based on the total volume of the solvent, and the volume ratio of the fluorinated ether solvent to the disulfide solvent is 1:0.75 to 1:1.
[0047] Furthermore, the present invention provides a lithium-sulfur secondary battery in which a positive electrode has an SC factor value of 0.45 or more represented by the following Formula 1.
[0048] [Formula 1]
[0049]
[0050] Where P is the porosity of the positive electrode active material layer in the positive electrode (%), L is the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode (mg / cm 2 ), and α is 10 (constant)).
[0051] The present invention provides a lithium-sulfur secondary battery, wherein the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode (mg / cm 2 ) is 2.5 mg / cm 2 Up to 5.0mg / cm 2 .
[0052] The present invention provides a lithium-sulfur secondary battery, wherein the porosity (%) of a positive electrode active material layer in a positive electrode is 50% to 70%.
[0053] [Beneficial Effects]
[0054] The lithium-sulfur secondary battery according to the present invention exhibits high initial discharge capacity and average discharge voltage by using an electrolyte containing a nitrile solvent, a fluorinated ether solvent and a disulfide solvent in a specific volume ratio in a solvent for a positive electrode satisfying specific conditions of high loading and low porosity.
[0055] In addition, the electrolyte used in the lithium-sulfur secondary battery according to the present invention contains a solvent containing a nitrile solvent, a fluorinated ether solvent and a disulfide solvent in a specific volume ratio, thereby reducing the viscosity of the electrolyte and improving the ion conductivity of the electrolyte. Therefore, for a positive electrode that meets the specific conditions of high load and low porosity, it shows the effects of increasing the average discharge voltage of the lithium-sulfur secondary battery containing the electrolyte, reducing the overvoltage and increasing the initial discharge capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 is a graph showing the measured viscosities of the electrolyte solutions according to Preparation Example 1 and Comparative Preparation Example 1.
[0057] Figure 2 is a graph showing the measured ion conductivities of the electrolyte solutions according to Preparation Example 1 and Comparative Preparation Example 1.
[0058] Figure 3 is a graph showing initial charge / discharge characteristics (0.1C / 0.1C) of the lithium-sulfur secondary battery according to Example 1.
[0059] Figure 4 is a graph showing initial charge / discharge characteristics (0.1C / 0.1C) of the lithium-sulfur secondary battery according to Comparative Example 1.
[0060] Figure 5 is a graph showing the charge / discharge characteristics (0.1C / 0.3C) of the lithium-sulfur secondary batteries according to Example 1 and Comparative Example 1 in the 10th cycle. DETAILED DESCRIPTION
[0061] All embodiments provided according to the present invention can be realized through the following description. The following description should be understood as describing preferred embodiments of the present invention, and it should be understood that the present invention is not necessarily limited thereto.
[0062] The present invention provides a lithium-sulfur secondary battery, which comprises a positive electrode, a negative electrode, a separator and an electrolyte.
[0063] The lithium-sulfur secondary battery according to the present invention may include a positive electrode having low porosity and high loading of sulfur as a positive electrode active material. In this case, when the porosity in the positive electrode is reduced and the content of the positive electrode active material is increased, the energy density of the battery including the positive electrode is increased. However, in the lithium-sulfur secondary battery, if the porosity of the positive electrode is reduced to a minimum and the sulfur content is increased to a maximum, it is difficult to obtain the target performance when the positive electrode is applied to the lithium-sulfur secondary battery because the ratio of the electrolyte per unit sulfur content is reduced.
[0064] In the present invention, it is intended to provide a lithium-sulfur secondary battery having a high initial discharge capacity and a high average discharge voltage when actually implemented compared with conventional lithium-sulfur secondary batteries by specifying conditions related to sulfur in a positive electrode and limiting conditions of an electrolyte suitable for such a positive electrode.
[0065] In the present invention, the positive electrode is not particularly limited, but may be a positive electrode having a positive electrode active material layer formed on one surface of a current collector. If the positive electrode is a positive electrode having a positive electrode active material layer formed on one surface of a current collector, the positive electrode may be prepared by applying a positive electrode active material slurry containing the positive electrode active material to one surface of the current collector and drying it. In this case, the slurry may further contain additives such as a binder, a conductive material, a filler, and a dispersant in addition to the positive electrode active material.
[0066] The positive electrode active material is not particularly limited, but may be, for example, a sulfur-based active material, a manganese-based spinel active material, a lithium metal oxide, or a mixture thereof.
[0067] Specifically, the sulfur compound can be Li2S n (n≥1), organic sulfur compounds or carbon-sulfur polymers (C2S x ) n : x=2.5 to 50, n≥2). The lithium metal oxide may be a lithium-manganese oxide, a lithium-nickel-manganese oxide, a lithium-manganese-cobalt oxide, and a lithium-nickel-manganese-cobalt oxide.
[0068] Specifically, the positive electrode active material can be LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(Ni a Co b Mnc )O2(where 0 <a<1,0<b<1,0<c<1,a+b+c=1)、LiNi 1-y Co y O2、LiCo 1-y Mn y O2、LiNi 1-y Mn y O2 (where 0≤y<1), Li(Ni d Co e Mn f )O4(where 0 <d<2,0<e<2,0<f<2,d+e+f=2)、LiMn 2-z Ni z O4 or LiMn 2-z Co2O4 (where 0 <z<2)。
[0069] The binder is a component that helps the bonding between the positive active material and the conductive material and the bonding to the current collector, and based on the total amount of the positive active material slurry, the binder can be generally added in an amount of 1% to 30% by weight. The binder is not particularly limited, but can be, for example, any one selected from the following: poly (vinylidene fluoride-to-hexafluoropropylene) (PVDF-to-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene propylene diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber and mixtures thereof.
[0070] The conductive material is not particularly limited, but can be, for example: graphite, such as natural graphite or artificial graphite; carbon black materials, such as carbon black (super-p), acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black and Danka black; conductive fibers, such as carbon fibers or metal fibers; carbon fluoride; metal powders, such as aluminum powder and nickel powder; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; or conductive materials, such as polyphenylene derivatives. The conductive material can be generally present in an amount of 0.05 wt % to 5 wt % based on the total weight of the slurry of the positive active material.
[0071] The filler is a component for suppressing the expansion of the positive electrode. The filler may be used or not used as needed and is not particularly limited as long as it is a fiber material and does not cause chemical changes in the battery, and examples thereof may include: olefin polymers such as polyethylene and polypropylene; and fiber materials such as glass fiber and carbon fiber.
[0072] The dispersant (dispersion body) is not particularly limited but may be, for example, isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or the like.
[0073] The coating can be performed by a method generally known in the art, but for example, the coating can be performed by distributing a slurry of the positive electrode active material on one surface of the positive electrode current collector and then uniformly dispersing the slurry using a scraper, etc. In addition, the coating can be performed by a method such as die casting, comma coating, screen printing, etc.
[0074] Drying is not particularly limited but may be performed in a vacuum oven at 50° C. to 200° C. within 1 day.
[0075] The positive electrode of the present invention manufactured by the above-mentioned material and method is distinguished by the SC factor value represented by Formula 1 as follows.
[0076] [Formula 1]
[0077]
[0078] Where P is the porosity of the positive electrode active material layer in the positive electrode (%), L is the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode (mg / cm 2 ), α is 10 (constant)).
[0079] The mass of sulfur per unit area of the positive electrode active material layer in the positive electrode of the lithium-sulfur secondary battery according to the present invention (mg / cm 2 ) can be 2.5 mg / cm 2 Up to 5.0mg / cm 2 , preferably 3.0 mg / cm 2 Up to 4.5 mg / cm 2 . If the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode is less than the above range, there is a problem that the lithium-sulfur secondary battery containing it is difficult to satisfy an energy density of more than 500Wh / kg. If the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode exceeds the above range, there is a problem that the charge / discharge capacity curve cannot be correctly expressed. Therefore, it is preferred that the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode satisfies the above range.
[0080] In addition, the porosity (%) of the positive electrode active material layer in the positive electrode of the lithium-sulfur secondary battery of the present invention can be 50% to 70%, preferably 55% to 65%. If the porosity (%) of the positive electrode active material layer in the positive electrode exceeds the above range, there is a problem of performance degradation due to increased penetration of the electrolyte and volume change of the active material during the charging / discharging process. If the porosity (%) of the positive electrode active material layer in the positive electrode is less than the above range, there is a problem of reduced energy density per unit volume. Therefore, it is preferred that the porosity of the positive electrode active material layer in the positive electrode satisfies the above range.
[0081] The lithium-sulfur secondary battery according to the present invention may have an SC factor value of 0.45 or more, preferably 0.5 or more, to achieve high energy density through the organic combination of the negative electrode, the separator and the electrolyte and the above-mentioned positive electrode and enable the lithium-sulfur secondary battery to achieve high energy density. If the SC factor value is 0.45 or more, in the case of a conventional lithium-sulfur secondary battery, the performance of the battery such as energy density will deteriorate in actual implementation, but in the case of the lithium-sulfur secondary battery according to the present invention, the performance of the battery is maintained without deterioration even in actual implementation.
[0082] In the present invention, the negative electrode may include a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector.
[0083] The negative electrode active material layer may include a negative electrode active material, a binder, and a conductive material. The negative electrode active material may include: a material capable of reversibly inserting or removing lithium ions (Li + ), materials that can react with lithium ions to reversibly form lithium-containing compounds, lithium metal or lithium alloys. + ) can be, for example, crystalline carbon, amorphous carbon or a mixture thereof. + ) to reversibly form a lithium-containing compound may be, for example, tin oxide, titanium nitrate, or silicon. The lithium alloy may be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), and tin (Sn).
[0084] The adhesive is not limited to the above-mentioned adhesives, and may be any adhesive that can be used as an adhesive in the art.
[0085] The constitution of the current collector and the like, except for the negative electrode active material and the conductive material, can be performed by the materials and methods used in the above-mentioned positive electrode.
[0086] In the present invention, the separator is a physical separator having a function of physically separating the electrodes. Any separator can be used without any particular restriction as long as it is used as a conventional separator. In particular, a separator having excellent moisture retention ability for the electrolyte while showing low resistance to ion migration of the electrolyte is preferred.
[0087] In addition, the separator enables lithium ions to be transferred between the positive electrode and the negative electrode while separating or insulating the positive electrode and the negative electrode from each other. Such a separator may be made of a porous, non-conductive or insulating material having a porosity of 30% to 50%.
[0088] Specifically, a porous polymer film can be used, for example, a porous polymer film made of a polyolefin polymer (such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer), etc., and a non-woven fabric made of a high melting point glass fiber, etc. can be used. Among them, a porous polymer film is preferably used.
[0089] If the polymer film is used as a buffer layer and a separator at the same time, the amount of electrolyte impregnation and ion conductivity decrease, and the effect of reducing overvoltage and improving capacity characteristics becomes less obvious. On the contrary, if a non-woven fabric material is used as a buffer layer and a separator at the same time, the mechanical strength cannot be ensured, and the problem of battery short circuit occurs. However, if a thin film separator and a polymer non-woven fabric buffer layer are used together, the mechanical strength can be ensured while having the effect of improving battery performance obtained by adopting a buffer layer.
[0090] An ethylene homopolymer (polyethylene) polymer film may be used as a separator, and a polyimide nonwoven fabric may be used as a buffer layer. In this case, it is preferred that the polyethylene polymer film has a thickness of 10 to 25 μm and a porosity of 40 to 50%.
[0091] In the present invention, the electrolytic solution is a non-aqueous electrolytic solution containing a lithium salt, and may contain a lithium salt and a solvent.
[0092] The lithium salt is a material that can be easily dissolved in a non-aqueous organic solvent and may be, for example, at least one selected from the group consisting of LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10, LiB(Ph)4, LiC4BO8, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate and lithium imide. In one embodiment of the present invention, the lithium salt may be preferably lithium imide, such as LiTFSI.
[0093] In addition, depending on various factors such as the exact composition of the electrolyte, the solubility of the salt, the conductivity of the dissolved salt, the charging and discharging conditions of the battery, the operating temperature, and other factors known in the field of lithium secondary batteries, the concentration of the lithium salt can be 1.5M (mol / L) to 2.5M (mol / L), preferably 1.7M (mol / L) to 2.3M (mol / L), and more preferably 2.0M (mol / L). If the concentration of the lithium salt is lower than the above range, there is a problem of side reactions between the solvent molecules and the Li metal. If the concentration of the lithium salt is higher than the above range, the ionic conductivity of the electrolyte decreases, which may reduce the battery performance. Therefore, it is preferred to select a suitable lithium salt concentration within the above range.
[0094] The solvent may include nitrile-based solvents, fluorinated ether-based solvents, and disulfide-based solvents.
[0095] The nitrile solvent may be at least one selected from the following: acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorobenzene acetonitrile and 4-fluorobenzene acetonitrile.
[0096] In addition, based on the total volume of the solvent, the content of the nitrile solvent can be 25 volume % to 35 volume %, preferably 30 volume % to 35 volume %, more preferably 30 volume % to 33.3 volume %. If the content of the nitrile solvent is lower than the above-mentioned scope, there is a problem that the concentration of the lithium salt soluble in the electrolyte is restricted. If the content of the nitrile solvent exceeds the above-mentioned scope, there is a problem that the viscosity of the electrolyte increases and the ionic conductivity decreases. Therefore, it is preferred to select the content of the nitrile solvent within the above-mentioned scope.
[0097] The type of the fluorinated ether solvent is not particularly limited as long as it is a fluorinated ether solvent commonly used in the relevant technical field, and for example, may be at least one selected from the following:
[0098] 2,2,2-Trifluoroethyl methyl ether (CF3CH2OCH3), 2,2,2-trifluoroethyl difluoromethyl ether (CF3CH2OCHF2), 2,2,3,3,3-pentafluoropropyl methyl ether (CF3CF2CH2OCH3), 2,2,3,3,3-pentafluoropropyl difluoromethyl ether (CF3CF2CH2OCHF2), 2,2,3,3,3-pentafluoropropyl-1,1,2,2-tetrafluoroethyl ether (CF3CF2CH2OCF2CF 2H), 1,1,2,2-tetrafluoroethyl methyl ether (HCF2CF2OCH3), 1,1,2,2-tetrafluoroethyl ethyl ether (HCF2CF2OCH2CH3), 1,1,2,2-tetrafluoroethyl propyl ether (HCF2CF2OC3H7), 1,1,2,2-tetrafluoroethyl butyl ether (HCF2CF2OC4H9), 2,2,3,3-tetrafluoroethyl difluoromethyl ether (H(CF2)2CH2O(CF2)H), 1,1,2, 2-Tetrafluoroethyl isobutyl ether (HCF2CF2OCH2CH(CH3)2), 1,1,2,2-tetrafluoroethyl isopentyl ether (HCF2CF2OCH2C(CH3)3), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (HCF2CF2OCH2CF3), 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HCF2CF2OCH2CF2CF2H), hexafluoroisopropyl methyl ether ((C F3)2CHOCH3), 1,1,3,3,3-pentafluoro-2-trifluoromethylpropyl methyl ether ((CF3)2CHCF2OCH3), 1,1,2,3,3,3-hexafluoropropyl methyl ether (CF3CHFCF2OCH3), 1,1,2,3,3,3-hexafluoropropyl ethyl ether (CF3CHFCF2OCH2CH3) and 2,2,3,4,4,4-hexafluorobutyl difluoromethyl ether (CF3CHFCF2CH2OCHF2),
[0099] Preferably, it may be 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HCF2CF2OCH2CF2CF2H).
[0100] The disulfide solvent may be at least one selected from the following: dialkyl disulfides, such as dimethyl disulfide, diethyl disulfide, di-n-propyl disulfide, diisopropyl disulfide, di-n-butyl disulfide, diisobutyl disulfide, di-sec-butyl disulfide, di-tert-butyl disulfide, di-n-pentyl disulfide, di-tert-pentyl disulfide, diisopentyl disulfide, di-n-heptyl disulfide, di-tert-octyl disulfide, di-n-decyl disulfide and dicyclohexyl disulfide. disulfide having an aromatic ring group, such as dibenzyl disulfide, diphenyl disulfide, di-p-tolyl disulfide and 5,5'-dithiobis(2-nitrobenzoic acid); disulfide having a heterocyclic group, such as 2,2'-dipyridyl disulfide, 4,4'-dipyridyl disulfide, 2,2'-dithiobis(5-nitropyridine), 6,6'-dithiodicotinoic acid and 2,2'-dipyrimidyl disulfide, and may preferably be dimethyl disulfide.
[0101] In addition, based on the total volume of the solvent, the content of the disulfide solvent can be 10 volume % to 40 volume %, preferably 20 volume % to 35 volume %. If the content of the disulfide solvent is lower than the above range, there is a problem that the effect of reducing the viscosity of the electrolyte and improving the ionic conductivity is insufficient, and the initial discharge capacity of the lithium-sulfur secondary battery containing it decreases due to side reactions with unexpected reaction mechanisms. If the content of the disulfide solvent exceeds the above range, there is a problem that the lithium salt in the electrolyte cannot be fully dissolved and cannot be fully mixed with the nitrile solvent, thereby causing the electrolyte to be stratified. Therefore, it is preferred that the content of the disulfide solvent meets the above range.
[0102] By adjusting the volume ratio of the nitrile solvent, the fluorinated ether solvent and the disulfide solvent in the electrolyte of the present invention, the viscosity of the electrolyte is reduced, the ionic conductivity of the electrolyte is increased, the average discharge voltage of the lithium-sulfur secondary battery containing the electrolyte is increased, and the energy capacity is increased.
[0103] Specifically, in the electrolyte of the present invention, the content of the nitrile solvent can be 25 volume % to 35 volume % based on the total volume of the solvent, the content of the fluorinated ether solvent can be 30 volume % to 50 volume % based on the total volume of the solvent, and the content of the disulfide solvent based on the total volume of the solvent can be 20 volume % to 35 volume %. In addition, in the electrolyte of the present invention, the content of the nitrile solvent can be 25 volume % to 35 volume % based on the total volume of the solvent, and the volume ratio of the fluorinated ether solvent to the disulfide solvent can be 1: 0.75 to 1: 1. If the volume ratio of the fluorinated ether solvent to the disulfide solvent is less than the above range, there is a problem that the effect of reducing the viscosity of the electrolyte and improving the ionic conductivity is insufficient, and the initial discharge capacity of the lithium-sulfur secondary battery containing it is decreased due to a side reaction with an unexpected reaction mechanism. If the volume ratio of the fluorinated ether solvent to the disulfide solvent exceeds the above range, there is a problem that the lithium salt in the electrolyte is not fully dissolved and is not fully mixed with the nitrile solvent, thereby causing the electrolyte to be stratified. Therefore, it is preferred that the volume ratio of the fluorinated ether solvent to the disulfide solvent satisfy the above range.
[0104] The lithium-sulfur secondary battery of the present invention can be manufactured by placing a separator between a positive electrode and a negative electrode to form an electrode assembly, inserting the electrode assembly into a cylindrical battery case or a rectangular battery case, and then injecting an electrolyte. Alternatively, the lithium-sulfur secondary battery of the present invention can also be manufactured by laminating the electrode assembly, impregnating the electrode assembly with an electrolyte, placing the obtained product in a battery case, and then sealing it.
[0105] Preferred Implementation
[0106] Hereinafter, preferred embodiments are listed to help understand the present invention, but the following embodiments are provided only to make it easier to understand the present invention, and the present invention is not limited thereto.
[0107] Example
[0108] Preparation of electrolyte for lithium-sulfur secondary batteries
[0109] Preparation Example 1
[0110] Based on the total volume of the solvent, lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) was added to 30 volume % acetonitrile at a concentration of 2M (mol / L) and dissolved at room temperature for 6 hours, and then 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were added in amounts of 40 volume % and 30 volume % respectively based on the total volume of the solvent, and stirred at room temperature to prepare an electrolyte for a lithium-sulfur secondary battery.
[0111] Preparation Example 2
[0112] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were each added in an amount of 35 volume % based on the total volume of the solvent.
[0113] Preparation Example 3
[0114] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that acetonitrile was added in an amount of 33 volume % based on the total volume of the solvent and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were added in an amount of 33.3 volume % based on the total volume of the solvent.
[0115] Preparation Example 4
[0116] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that acetonitrile was added in an amount of 30 volume % based on the total volume of the solvent, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were added in amounts of 50 volume % and 20 volume % based on the total volume of the solvent, respectively.
[0117] Comparative Preparation Example 1
[0118] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) was added in an amount of 70 volume % based on the total volume of the solvent.
[0119] Comparative Preparation Example 2
[0120] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were respectively added in amounts of 60 vol % and 10 vol % based on the total volume of the solvent.
[0121] Comparative Preparation Example 3
[0122] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were added in amounts of 30 vol % and 40 vol % respectively based on the total volume of the solvent.
[0123] Comparative Preparation Example 4
[0124] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were respectively added in amounts of 20 vol % and 50 vol % based on the total volume of the solvent.
[0125] Comparative Preparation Example 5
[0126] An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Preparation Example 1, except that acetonitrile was added in an amount of 15 volume % based on the total volume of the solvent, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) and dimethyl disulfide (DMDS) were added in amounts of 70 volume % and 15 volume % based on the total volume of the solvent, respectively.
[0127] The compositions of the electrolyte solutions for lithium-sulfur secondary batteries of Preparation Examples 1 to 4 and Comparative Preparation Examples 1 to 5 are shown in Table 1 below.
[0128] Table 1:
[0129]
[0130] Experimental Example 1: Measurement of electrolyte viscosity and ion conductivity
[0131] The electrolytes according to Preparation Examples 1 to 4 and Comparative Preparation Examples 1 to 5 were measured for ion conductivity at 22° C. using an ion conductivity measuring device (Seven compact S230, Mettler Toledo company) and for viscosity at 22° C. using a viscometer (μVISC, Rheo sense company).
[0132] The results are shown in Table 2 and Figure 1 and Figure 2 middle.
[0133] Table 2:
[0134] Ionic conductivity (mS / cm) Viscosity(cP) Preparation Example 1 3.42 4.28 Preparation Example 2 3.43 4.60 Preparation Example 3 4.12 4.00 Preparation Example 4 3.33 4.89 Comparative Preparation Example 1 2.49 7.07 Comparative Preparation Example 2 2.85 5.66 Comparative Preparation Example 3 - - Comparative Preparation Example 4 - - Comparative Preparation Example 5 - -
[0135] As shown in Table 2 above, it was confirmed that when the concentration of the lithium salt (LiTFSI) was as high as 3 to 3.3 M, the electrolytes of Preparation Examples 1 to 4 in which the disulfide-based solvent (DMDS) was added had low viscosity and high ionic conductivity compared to the case where the disulfide-based solvent (DMDS) was not added (Comparative Preparation Example 1) (see the attached Figure 1 and Figure 2). In addition, it was confirmed that when the concentration of the lithium salt (LiTFSI) was 3M, when the content of the disulfide solvent (DMDS) was less than 10% by volume (Comparative Preparation Example 2), the initial capacity of the lithium-sulfur secondary battery decreased. This is because the content of the disulfide solvent (DMDS) is too little, thereby reducing the viscosity and improving the ionic conductivity. The effect is insufficient, and a side reaction with an unexpected reaction mechanism occurs. In addition, it was confirmed that when the content of the disulfide solvent (DMDS) is 40% by volume or more (Comparative Preparation Example 3 and Comparative Preparation Example 4), the lithium salt is not fully dissolved and cannot be fully mixed with the nitrile solvent, resulting in electrolyte stratification. In addition, it was confirmed that when the nitrile solvent is less than 20% by volume (Comparative Preparation Example 5), the viscosity is high and the lithium salt is not fully dissolved.
[0136] Manufacturing of lithium-sulfur secondary batteries
[0137] Example 1
[0138] Water was used as a solvent, and sulfur, Super-P (SP), a conductive material, and a binder were mixed with a ball mill to prepare a composition for forming a positive electrode active material layer. At this time, Danka black was used as a conductive material, and a binder in the form of a mixture of SBR and CMC was used as a binder. The weight mixing ratio was set so that sulfur and SP (ratio of 9:1): conductive material: binder was 90:10:10. The prepared composition for forming a positive electrode active material layer was coated on an aluminum current collector and then dried to prepare a positive electrode (energy density of the positive electrode: 4.2 mAh / cm 2 The porosity of the positive electrode active material layer calculated by measuring the weight and thickness of the electrode in the prepared positive electrode (using TESA-μHITE equipment of TESA) was 58%, and the mass of sulfur per unit area of the positive electrode active material layer was 3.24 mg / cm 2 The SC factor value based on this calculation is 0.59.
[0139] After the positive electrode and the negative electrode prepared by the above method were placed to face each other, a polyethylene separator having a thickness of 20 μm and a porosity of 45% was interposed between the positive electrode and the negative electrode.
[0140] Thereafter, an electrolyte solution was injected into the case to manufacture a lithium-sulfur secondary battery. In this case, the electrolyte solution of the above-mentioned Preparation Example 1 was used as the electrolyte solution.
[0141] Example 2
[0142] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1 except that the electrolyte solution of Preparation Example 2 described above was used as the electrolyte solution.
[0143] Example 3
[0144] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1 except that the electrolyte solution of Preparation Example 3 described above was used as the electrolyte solution.
[0145] Example 4
[0146] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1 except that the electrolyte solution of Preparation Example 4 described above was used as the electrolyte solution.
[0147] Comparative Example 1
[0148] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1, except that the electrolytic solution of Comparative Preparation Example 1 described above was used as the electrolytic solution.
[0149] Comparative Example 2
[0150] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1, except that the electrolytic solution of Comparative Preparation Example 2 described above was used as the electrolytic solution.
[0151] Comparative Example 3
[0152] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1, except that the electrolytic solution of Comparative Preparation Example 3 described above was used as the electrolytic solution.
[0153] Comparative Example 4
[0154] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1, except that the electrolytic solution of Comparative Preparation Example 4 described above was used as the electrolytic solution.
[0155] Comparative Example 5
[0156] A lithium-sulfur secondary battery was manufactured in the same manner as in Example 1, except that the electrolytic solution of Comparative Preparation Example 5 described above was used as the electrolytic solution.
[0157] Experimental Example 2: Measurement of initial discharge capacity and average discharge voltage
[0158] The capacities of the lithium-sulfur secondary batteries according to Examples 1 to 4 and Comparative Examples 1 to 5 were measured at 35° C. from 1.0 V to 3.6 V using a charge / discharge measurement device (LAND CT-2001A, Wuhan).
[0159] Specifically, an initial discharge was first performed at 0.1C, then charge / discharge was performed twice at 0.1C / 0.1C, and then charge / discharge was performed at 0.1C / 0.3C, thereby measuring the first discharge capacity (initial discharge capacity) at 0.1C, and measuring the average discharge voltage at the 10th discharge.
[0160] The results are shown in Table 3 and Figures 3 to 5 middle.
[0161] Table 3:
[0162] Initial discharge capacity (mAh / g) Average discharge voltage(V) Example 1 1709 1.95 Example 2 1654 1.94 Example 3 1655 1.95 Example 4 1510 1.91 Comparative Example 1 1469 1.79 Comparative Example 2 875 1.88 Comparative Example 3 - - Comparative Example 4 - - Comparative Example 5 - -
[0163] As shown in Table 3, it was confirmed that when the concentration of the lithium salt (LiTFSI) was as high as 3 to 3.3 M, the initial discharge capacity of the lithium-sulfur secondary batteries of Examples 1 to 4 to which the disulfide-based solvent (DMDS) was added was significantly improved compared to the case where the disulfide-based solvent (DMDS) was not added (Comparative Example 1), and their average discharge voltage was also significantly improved (see Figures 3 to 5 ). In addition, it was confirmed that the initial discharge capacity of the lithium-sulfur secondary batteries of Examples 1 to 4 in which the disulfide solvent (DMDS) was added in an amount of 20 to 35 volume % was significantly improved compared to the case where the disulfide solvent (DMDS) was added in an amount of 10 volume % or less (Comparative Example 2), and their average discharge voltage was also significantly improved. In contrast, in the above-mentioned Comparative Example 2, although the disulfide solvent was added, the content of the disulfide solvent (DMDS) was insufficient (10 volume %), so the effect of reducing the viscosity of the electrolyte and improving the ionic conductivity was insufficient, and the initial discharge capacity of the lithium-sulfur secondary battery was significantly reduced due to side reactions with unexpected reaction mechanisms. On the other hand, in the case of Comparative Examples 3 to 5, as described in Comparative Preparation Examples 3 to 5, the initial discharge capacity and the average discharge voltage could not be measured due to the stratification of the electrolyte and the insufficient dissolution of the lithium salt.
[0164] All simple variations or modifications of the present invention fall within the protection scope of the present invention, and the specific protection scope of the present invention shall be subject to the appended claims.
Claims
1. A lithium-sulfur secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte contains a lithium salt and a solvent, The solvent includes a nitrile solvent, a fluorinated ether solvent and a disulfide solvent, and Based on the total volume of the solvent, the content of the disulfide solvent is 20 volume % to 35 volume %, The content of the nitrile solvent is 25 volume % to 35 volume % of the total volume of the solvent, and The content of the fluorinated ether solvent is 30 volume % to 50 volume % of the total volume of the solvent. The volume ratio of the fluorinated ether solvent to the disulfide solvent is 1:0.75 to 1:
1. wherein the positive electrode has an SC factor value of 0.45 or more represented by the following formula 1, [Formula 1] Wherein P is the porosity of the positive electrode active material layer in the positive electrode, which is expressed in %, L is the mass of sulfur per unit area of the positive electrode active material layer in the positive electrode, expressed in mg / cm 2 , α is 10 and is a constant.
2. The lithium-sulfur secondary battery according to claim 1, wherein the lithium salt is at least one selected from the group consisting of LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 、LiB(Ph) 4、 LiC4BO8, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, lithium lower aliphatic carboxylates, lithium tetraphenylborate and lithium imide. 3 . The lithium-sulfur secondary battery according to claim 1 , wherein the concentration of the lithium salt is 1.5 mol / L to 2.5 mol / L.
4. The lithium-sulfur secondary battery according to claim 1, wherein the nitrile solvent is at least one selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide.
5. The lithium-sulfur secondary battery according to claim 1, wherein the fluorinated ether solvent is at least one selected from the following: 2,2,2-Trifluoroethyl methyl ether (CF3CH2OCH3); 2,2,2-Trifluoroethyldifluoromethyl ether (CF3CH2OCHF2); 2,2,3,3,3-pentafluoropropyl methyl ether (CF3CF2CH2OCH3); 2,2,3,3,3-pentafluoropropyldifluoromethyl ether (CF3CF2CH2OCHF2); 2,2,3,3,3-pentafluoropropyl-1,1,2,2-tetrafluoroethyl ether (CF3CF2CH2OCF2CF2H); 1,1,2,2-Tetrafluoroethyl methyl ether (HCF2CF2OCH3); 1,1,2,2-Tetrafluoroethyl ethyl ether (HCF2CF2OCH2CH3); 1,1,2,2-Tetrafluoroethylpropyl ether (HCF2CF2OC3H7); 1,1,2,2-Tetrafluoroethyl butyl ether (HCF2CF2OC4H9); 2,2,3,3-Tetrafluoroethyldifluoromethyl ether (H(CF2)2CH2O(CF2)H); 1,1,2,2-Tetrafluoroethyl isobutyl ether (HCF2CF2OCH2CH(CH3)2); 1,1,2,2-Tetrafluoroethyl isopentyl ether (HCF2CF2OCH2C(CH3)3); 1,1,2,2-Tetrafluoroethyl-2,2,2-trifluoroethyl ether (HCF2CF2OCH2CF3); 1,1,2,2-Tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HCF2CF2OCH2CF2CF2H); Hexafluoroisopropyl methyl ether ((CF3)2CHOCH3); 1,1,3,3,3-pentafluoro-2-trifluoromethylpropyl methyl ether ((CF3)2CHCF2OCH3); 1,1,2,3,3,3-Hexafluoropropyl methyl ether (CF3CHFCF2OCH3); 1,1,2,3,3,3-Hexafluoropropyl ethyl ether (CF3CHFCF2OCH2CH3); and 2,2,3,4,4,4-Hexafluorobutyldifluoromethyl ether (CF3CHFCF2CH2OCHF2). The lithium-sulfur secondary battery according to claim 1 , wherein the disulfide-based solvent is dimethyl disulfide.
7. The lithium-sulfur secondary battery according to claim 1, wherein the unit of the positive electrode active material layer in the positive electrode is mg / cm 2 The mass of sulfur per unit area is 2.5 mg / cm 2 Up to 5.0mg / cm 2 . 8 . The lithium-sulfur secondary battery according to claim 1 , wherein the porosity expressed in % of the positive electrode active material layer in the positive electrode is 50% to 70%.