A method for preparing a laser diode insulating heat sink

By using the combined technology of copper-clad ceramic substrate and epoxidized polyurethane coating in semiconductor lasers, the problems of thermal expansion coefficient mismatch and surface erosion are solved, the heat dissipation performance and mechanical strength of the laser are improved, the life of the laser is extended and the laser can be used at high temperatures. Maintain stability in the environment.

CN118367433BActive Publication Date: 2024-10-18江苏富乐华功率半导体研究院有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410474960.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-19
Publication Date
2024-10-18
Estimated Expiration
2044-04-19

AI Technical Summary

Technical Problem

During the packaging process of semiconductor lasers, due to the thermal expansion coefficient mismatch between the heat dissipation substrate and the semiconductor chip, thermal stress is generated, which affects the life of the device and the collimation of the laser output. At the same time, the surface is prone to appear in high temperature, high humidity or chemically corrosive environments. erosion, reducing performance.

Method used

A copper-clad ceramic substrate is used as a heat sink, and a through-hole heat sink structure is formed through film pasting, exposure, development, etching, chemical silver plating, electrolytic silver plating, etc., and after vacuum sintering and coating with epoxidized polyurethane paint, a tight Combined heat sink structure to improve heat dissipation performance and mechanical strength.

Benefits of technology

It effectively solves the problem of thermal expansion coefficient mismatch, improves the heat dissipation performance and mechanical strength of the laser, extends the life of the laser, and maintains stability and reliability in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118367433B_ABST
    Figure CN118367433B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor laser technology, and specifically to a method for preparing a laser diode insulating heat sink. The present invention sequentially films, exposes, develops, and etches a copper-clad ceramic substrate, then films the front of the copper-clad ceramic substrate for protection, chemically silver-plates the back, removes the film after completion, performs laser drilling, and cuts to form through holes to obtain a copper-clad ceramic substrate A. Three copper sheets are sequentially films, exposed, developed, and etched to obtain two microchannel layers and a guide layer, respectively, and then the etched surfaces are sequentially subjected to chemical silver plating, electroplating, and electric spark wire cutting. Finally, the copper-clad ceramic substrate A, the microchannel layer, and the guide layer are stacked, vacuum sintered, wire-cut, ground and polished, chemically nickel-gold plated, and coated with an epoxy polyurethane coating to obtain a finished product. The finished product prepared by the present invention has good heat dissipation capacity and corrosion resistance, and therefore has broad application prospects in the field of semiconductor laser technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor lasers, in particular to a method for preparing a laser diode insulating heat sink. Background Art

[0002] Semiconductor lasers are devices that use certain semiconductor materials as working materials to generate lasers. They have the advantages of high photoelectric conversion rate, long life, and small size. They have been widely used in material processing, aerospace, medical cosmetology, optical fiber communication and other fields. During the packaging process of the device, due to the mismatch between the thermal expansion coefficients of the heat dissipation substrate and the semiconductor chip, the chip generates thermal stress during the welding process. These stresses will cause the bandwidth of the active area to change, forming defects, affecting the threshold current, output power, laser wavelength and other characteristics of the laser, and reducing the life of the laser. At the same time, for the laser, the difference in thermal expansion coefficients will cause the chip to produce slight bending deformation, directly causing the laser emitted by the chip to be misaligned, causing the overall light emission of the semiconductor laser array to bend. At present, the microchannel heat sink structure is divided into five layers, two upper and lower closed layers, and the middle is a microchannel layer and a guide layer, and the material uses a high thermal conductivity metal. The present invention introduces a method for preparing a laser diode insulating heat sink, using a copper-clad ceramic substrate as the upper and lower surfaces of the heat sink, and the middle ceramic as an insulating layer to insulate the circuit of the laser diode from the cooling water, while solving the problem of thermal expansion coefficient mismatch between the chip and the heat sink. In addition, semiconductor lasers are prone to surface corrosion in high temperature, high humidity or chemical corrosion environments, which can cause failures in working components and affect the overall performance of the device. Therefore, it is very necessary to improve the surface mechanical strength of semiconductor lasers to improve the overall working performance of semiconductor lasers.

[0003] In order to overcome the defects of the prior art, the present invention provides a method for preparing a laser diode insulating heat sink. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a laser diode insulating heat sink to solve the problems in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a laser diode insulating heat sink comprises the following steps:

[0007] Step 1: sequentially laminating, exposing, developing, and etching the copper-clad ceramic substrate, and then laminating the front side of the copper-clad ceramic substrate for protection, and performing chemical silver plating on the back side. After completion, the laminating film is removed, laser drilling is performed, and through holes are formed by cutting to obtain the copper-clad ceramic substrate A11;

[0008] Step 2: Take three copper sheets and perform film lamination, exposure, development, and etching in sequence to obtain two microchannel layers 12 and one guide layer 13 respectively, and then perform chemical silver plating, electro-silver plating, and electric spark wire cutting on the etched surfaces in sequence;

[0009] Step three: stack and press the copper-clad ceramic substrate A11, microchannel layer 12, guide layer 13, microchannel layer 12, and copper-clad ceramic substrate A11 in order to form a heat sink structure 1, and then perform vacuum sintering, wire cutting, grinding and polishing, and chemical nickel-gold plating in sequence to obtain a finished product.

[0010] More optimally, in step 1, the thickness of the chemically plated silver on the back side of the copper-clad ceramic substrate A is 0.7-0.8 μm.

[0011] More optimally, in step one, the aperture tolerance of the through hole is -10 to 10%, and the offset is -0.02 to 0.02 mm; the through hole includes a coolant inlet, a coolant inlet and a limit hole.

[0012] More optimally, in step 2, the thickness of chemically plated silver on the surface of the copper sheet is 0.3-0.7 μm, and the thickness of electroplated silver on the surface of the copper sheet is 1-2 μm.

[0013] More optimally, in step 3, during vacuum sintering, the vacuum degree is 10 -3 ~10 -2 Pa, temperature is 800-950℃, holding time is 6-12h; wire cutting parameters: wire speed is 2-5m / s, wire diameter is 0.08-0.35mm.

[0014] More optimally, in step three, when the heat sink structure is stacked, the heat sink structure is placed in a graphite fixture, graphite paper is placed on the upper and lower surfaces respectively, and the silver-plated surfaces of each layer are attached to each other and pressure is applied, and the pressure is 30 to 80 MPa.

[0015] More optimally, in step three, the grinding and polishing parameters are: cutting surface roughness <2 μm, surface flatness <1 μm, roughness <0.05 μm; nickel layer thickness 2-5 μm, gold layer thickness 0.05-0.3 μm.

[0016] More optimally, step three includes post-treatment, coating the surface with epoxidized polyurethane coating after chemical nickel-gold plating, curing at 160-170°C for 3-4h, and the thickness of the epoxidized polyurethane coating layer is 2-5μm; wherein the preparation method of the epoxidized polyurethane coating is as follows: S1: in a nitrogen environment, mixing a sodium hydroxide solution with a concentration of 3.3-3.6 mol / L and tetra(4-hydroxyphenyl)ethylene, stirring and reacting at 105-110°C for 1.2-1.6h, then dropping 3-chloro-1,2-propylene glycol, and continuing to react at 105-110°C for 3.5-4.5h, after the reaction is completed, extracting, washing, rotary evaporation concentration, filtering and drying to obtain an ether-containing product; mixing the ether-containing product, diethyl carbonate and anhydrous potassium carbonate, reflux reaction at 115-125°C for 25-30h, and then distilling reaction at 75-80°C for 6.5-7.5h, after the reaction is completed, standing, filtering and washing to obtain cyclic carbonate;

[0017] S2: In a nitrogen environment, cyclic carbonate and hexamethylenediamine are mixed, and the mixture is stirred and reacted at 120-150° C. for 4-5 hours to prepare amino-terminated polyhydroxy polyurethane; amino-terminated polyhydroxy polyurethane, epoxy resin and curing agent ethylenediamine are evenly mixed to obtain an epoxidized polyurethane coating.

[0018] More optimally, in step S1, the reaction molar ratio of tetra(4-hydroxyphenyl)ethylene and 3-chloro-1,2-propylene glycol is (4-5):1; the reaction molar ratio of the ether-containing product and diethyl carbonate is 1:(2-3).

[0019] More optimally, in step S2, the reaction molar ratio of cyclocarbonate and hexamethylenediamine is 1:(1.8-2); the content of each component of the epoxidized polyurethane coating is: by mass fraction, 50-60% amino-terminated polyhydroxy polyurethane, 35-45% epoxy resin, and the balance is ethylenediamine.

[0020] Beneficial effects of the present invention:

[0021] The present invention sequentially performs film lamination, exposure, development, and etching on a copper-clad ceramic substrate, then performs film lamination on the front side of the copper-clad ceramic substrate for protection, performs chemical silver plating on the back side, removes the film after completion, performs laser drilling, and cuts to form through holes to obtain a copper-clad ceramic substrate A. Three copper sheets are sequentially lamination, exposure, development, and etching to obtain two microchannel layers and one guide layer, respectively, and then the etched surfaces are sequentially subjected to chemical silver plating, electro-silver plating, and electric spark wire cutting. Finally, the copper-clad ceramic substrate A, the microchannel layer, and the guide layer are stacked, vacuum sintered, wire-cut, ground and polished, chemically nickel-gold plated, and coated with an epoxidized polyurethane coating to prepare a finished product.

[0022] The feature of the present invention is that in step one and step two, the copper-clad ceramic substrate A is obtained by chemically silver-plating the back of the copper-clad ceramic substrate, and the surface of the copper sheet is chemically silver-plated and electro-silver-plated in sequence. In this step, silver layer bonding can be achieved by silver plating, and by forming a silver layer on the surface of the material, a stable chemical bond or strong adsorption between metals is formed between the two materials, thereby achieving material bonding. In the final heat sink structure formation process, the copper-clad ceramic substrate A, the microchannel layer and the guide layer all need to be bonded by the silver layer. This silver layer bonding can ensure the close bonding between the layers, and improve the stability and durability of the entire structure. At the same time, the thermal conductivity of the silver layer itself also helps to improve the heat dissipation performance of the heat sink structure, making the entire heat dissipation system more efficient and reliable.

[0023] In step three, the copper-clad ceramic substrate A, the microchannel layer, and the guide layer are stacked, vacuum sintered, wire cut, ground and polished, chemically nickel-gold plated, and coated with epoxidized polyurethane coating to prepare a finished product. Among them, the application principle of epoxidized polyurethane coating is as follows: tetra(4-hydroxyphenyl)ethylene and 3-chloro-1,2-propylene glycol are subjected to catalytic dehydrogenation and ester exchange reaction to prepare cyclic carbonate; then the cyclic carbonate and hexamethylenediamine are subjected to condensation reaction to prepare amino-terminated polyhydroxy polyurethane. The amino-terminated polyhydroxy polyurethane and epoxy resin are mixed and cured at high temperature to obtain epoxidized polyurethane. Finally, epoxidized polyurethane, leveling agent, defoamer, thickener and deionized water are used as raw materials to prepare epoxidized polyurethane coating. On the one hand, the epoxidized polyurethane coating prepared by the present invention contains more rigid groups, which can effectively improve the mechanical strength of the surface of the copper-clad ceramic substrate, improve its scratch resistance and wear resistance, and make the substrate more durable and corrosion-resistant; on the other hand, the high degree of cross-linking between the epoxidized polyurethane molecules and the epoxy groups and benzene ring structures contained therein give the molecule excellent thermal stability and high temperature resistance. This means that in a high temperature environment, the epoxy polyurethane coating can maintain its original performance and is not prone to decomposition or failure. Therefore, applying the epoxy polyurethane coating to the surface of the copper-clad ceramic substrate can effectively improve the stability and reliability of the substrate in a high temperature working environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0025] Figure 1 is a schematic diagram of a symmetrical heat sink structure of the present invention;

[0026] Figure 2 It is a schematic diagram of a vacuum sintering jig of the present invention;

[0027] Figure 3is a schematic diagram of a heat sink structure lamination of the present invention;

[0028] Figure 4 is a schematic diagram of the heat sink structure of the present invention;

[0029] In the figure: 1: heat sink structure, 2: graphite fixture, 3: graphite paper, 11: copper-clad ceramic substrate A, 12: microchannel layer, 13: guide layer. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Source of raw materials:

[0032] The copper-clad ceramic substrate is provided by Jiangsu Fulehua Semiconductor Technology Co., Ltd. and meets the AMB substrate standard; the copper sheet is made of oxygen-free copper; the epoxy resin is provided by Langfang Yushi Anti-corrosion Materials Co., Ltd., model 6101.

[0033] Example 1: Step 1: The copper-clad ceramic substrate is sequentially subjected to film lamination, exposure, development, and etching, and then the front side of the copper-clad ceramic substrate is protected by film lamination, and the back side is subjected to chemical silver plating of 0.8 μm. After completion, the film lamination is removed, laser drilling is performed, and through holes are formed by cutting to obtain a copper-clad ceramic substrate A11; the aperture tolerance of the through hole is 10%, and the deviation is 0.02 mm;

[0034] Step 2: Take 3 copper sheets and perform film lamination, exposure, development and etching in sequence to obtain two microchannel layers 12 and one guide layer 13 respectively, and then perform chemical silver plating, electro-silver plating and electric spark wire cutting on the etched surfaces in sequence; wherein the thickness of the chemical silver plating is 0.7 μm, and the thickness of the electro-silver plating is 2 μm;

[0035] Step 3: stack and press the copper-clad ceramic substrate A11, microchannel layer 12, guide layer 13, microchannel layer 12, and copper-clad ceramic substrate A11 in this order to form a heat sink structure 1, and then perform vacuum sintering, wire cutting, grinding and polishing, and chemical nickel-gold plating in sequence; during vacuum sintering, the vacuum degree is 10 -2Pa, the temperature is 950℃, and the holding time is 12h; during wire cutting, the wire speed is 5m / s and the wire diameter is 0.35mm; when the heat sink structure 1 is stacked, the heat sink structure 1 is placed in the graphite fixture 2, and graphite paper 3 is placed on the upper and lower surfaces respectively, and the silver-plated surfaces of each layer are attached to each other and pressure is applied, and the pressure is 80MPa; during grinding and polishing, the cutting surface roughness is 1.5μm, the surface flatness is 0.8μm, and the roughness is 0.04μm; the nickel layer thickness is 5μm, and the gold layer thickness is 0.3μm;

[0036] Step 4: After chemical nickel-gold plating, coat the surface with epoxidized polyurethane coating, and cure at 170°C for 4h to obtain a finished product; the thickness of the epoxidized polyurethane coating layer is 5μm; wherein the preparation method of the epoxidized polyurethane coating is as follows: S1: Under a nitrogen environment, mix a sodium hydroxide solution with a concentration of 3.6mol / L and 4.5mol of tetra(4-hydroxyphenyl)ethylene, stir and react at 110°C for 1.6h, then drop 1mol of 3-chloro-1,2-propylene glycol, and continue to react at 110°C for 4.5h. After the reaction is completed, extract, wash, concentrate by rotary evaporation, filter and dry to obtain an ether-containing product; mix 1mol of the ether-containing product, 2.5mol of diethyl carbonate and anhydrous potassium carbonate, reflux at 125°C for 30h, and then distill and react at 80°C for 7.5h. After the reaction is completed, stand, filter and wash to obtain a cyclic carbonate;

[0037] S2: In a nitrogen environment, 1 mol of cyclic carbonate and 1.8 mol of hexamethylenediamine were mixed, and the mixture was stirred at 150°C for 5 hours to prepare amino-terminated polyhydroxy polyurethane; 55% amino-terminated polyhydroxy polyurethane, 35% epoxy resin and 10% curing agent ethylenediamine were mixed evenly by mass fraction to obtain an epoxidized polyurethane coating.

[0038] Example 2: Step 1: The copper-clad ceramic substrate is sequentially subjected to film lamination, exposure, development, and etching, and then the front side of the copper-clad ceramic substrate is protected by film lamination, and the back side is subjected to chemical silver plating of 0.75 μm. After completion, the film is removed, laser drilling is performed, and through holes are formed by cutting to obtain a copper-clad ceramic substrate A11; the aperture tolerance of the through hole is 5%, and the offset is 10.01 mm;

[0039] Step 2: Take 3 copper sheets and perform film lamination, exposure, development and etching in sequence to obtain two microchannel layers 12 and one guide layer 13 respectively, and then perform chemical silver plating, electro-silver plating and electric spark wire cutting on the etched surfaces in sequence; wherein the thickness of the chemical silver plating is 0.5 μm, and the thickness of the electro-silver plating is 1.5 μm;

[0040] Step 3: The copper-clad ceramic substrate A11, microchannel layer 12, guide layer 13, microchannel layer 12, and copper-clad ceramic substrate A11 are stacked and pressed in order to form a heat sink structure 1, and then vacuum sintering, wire cutting, grinding and polishing, and chemical nickel-gold plating are performed in sequence; during vacuum sintering, the vacuum degree is 0.5×10 -3 Pa, the temperature is 900℃, and the holding time is 8h; during wire cutting, the wire speed is 3m / s and the wire diameter is 0.2mm; when the heat sink structure 1 is stacked, the heat sink structure 1 is placed in the graphite fixture 2, and graphite paper 3 is placed on the upper and lower surfaces respectively, and the silver-plated surfaces of each layer are attached to each other and pressure is applied, and the pressure is 50MPa; during grinding and polishing, the cutting surface roughness is 1μm, the surface flatness is 0.5μm, and the roughness is 0.02μm; the nickel layer thickness is 3μm, and the gold layer thickness is 0.2μm;

[0041] Step 4: After chemical nickel-gold plating, coat the surface with epoxidized polyurethane coating, and cure at 165°C for 3.5h to obtain a finished product; the thickness of the epoxidized polyurethane coating layer is 3μm; wherein the preparation method of the epoxidized polyurethane coating is as follows: S1: Under a nitrogen environment, mix a sodium hydroxide solution with a concentration of 3.4mol / L and 4.5mol of tetra(4-hydroxyphenyl)ethylene, stir and react at 107°C for 1.5h, then drop 1mol of 3-chloro-1,2-propylene glycol, and continue to react at 107°C for 4h. After the reaction is completed, extract, wash, concentrate by rotary evaporation, filter and dry to obtain an ether-containing product; mix 1mol of the ether-containing product, 2.5mol of diethyl carbonate and anhydrous potassium carbonate, reflux at 120°C for 27h, and then distill and react at 77°C for 6.7h. After the reaction is completed, stand, filter and wash to obtain a cyclic carbonate;

[0042] S2: In a nitrogen environment, 1 mol of cyclic carbonate and 1.8 mol of hexamethylenediamine were mixed, and the mixture was stirred and reacted at 130°C for 4.5 hours to prepare amino-terminated polyhydroxy polyurethane; 55% amino-terminated polyhydroxy polyurethane, 35% epoxy resin and 10% curing agent ethylenediamine were mixed evenly by mass fraction to obtain an epoxidized polyurethane coating.

[0043] Example 3: Step 1: The copper-clad ceramic substrate is sequentially subjected to film lamination, exposure, development, and etching, and then the front side of the copper-clad ceramic substrate is protected by film lamination, and the back side is subjected to chemical silver plating of 0.7 μm. After completion, the film lamination is removed, laser drilling is performed, and through holes are formed by cutting to obtain a copper-clad ceramic substrate A11; the aperture tolerance of the through hole is -10%, and the offset is -0.02 mm;

[0044] Step 2: Take 3 copper sheets and perform film lamination, exposure, development and etching in sequence to obtain two microchannel layers 12 and one guide layer 13 respectively, and then perform chemical silver plating, electro-silver plating and electric spark wire cutting on the etched surfaces in sequence; wherein the thickness of the chemical silver plating is 0.3 μm, and the thickness of the electro-silver plating is 1 μm;

[0045] Step 3: stack and press the copper-clad ceramic substrate A11, microchannel layer 12, guide layer 13, microchannel layer 12, and copper-clad ceramic substrate A11 in this order to form a heat sink structure 1, and then perform vacuum sintering, wire cutting, grinding and polishing, and chemical nickel-gold plating in sequence; during vacuum sintering, the vacuum degree is 10 -3 Pa, the temperature is 800℃, and the holding time is 6h; during wire cutting, the wire speed is 2m / s and the wire diameter is 0.08mm; when the heat sink structure 1 is stacked, the heat sink structure 1 is placed in the graphite fixture 2, and graphite paper 3 is placed on the upper and lower surfaces respectively, and the silver-plated surfaces of each layer are attached to each other and pressure is applied, and the pressure is 30MPa; during grinding and polishing, the cutting surface roughness is 0.5μm, the surface flatness is 0.1μm, and the roughness is 0.01μm; the nickel layer thickness is 2μm, and the gold layer thickness is 0.3μm;

[0046] Step 4: After chemical nickel-gold plating, coat the surface with epoxidized polyurethane coating, and cure at 160°C for 3h to obtain a finished product; the thickness of the epoxidized polyurethane coating layer is 2μm; wherein the preparation method of the epoxidized polyurethane coating is as follows: S1: Under a nitrogen environment, mix a sodium hydroxide solution with a concentration of 3.3mol / L and 4.5mol of tetra(4-hydroxyphenyl)ethylene, stir and react at 105°C for 1.2h, then drop 1mol of 3-chloro-1,2-propylene glycol, and continue to react at 105°C for 3.5h. After the reaction is completed, extract, wash, concentrate by rotary evaporation, filter and dry to obtain an ether-containing product; mix 1mol of the ether-containing product, 2.5mol of diethyl carbonate and anhydrous potassium carbonate, reflux at 115°C for 25h, and then distill and react at 75°C for 6.5h. After the reaction is completed, stand, filter and wash to obtain a cyclic carbonate;

[0047] S2: In a nitrogen environment, 1 mol of cyclic carbonate and 1.8 mol of hexamethylenediamine were mixed, and the mixture was stirred and reacted at 120°C for 4 hours to prepare amino-terminated polyhydroxy polyurethane; by mass fraction, 55% amino-terminated polyhydroxy polyurethane, 35% epoxy resin and 10% curing agent ethylenediamine were evenly mixed to obtain an epoxidized polyurethane coating.

[0048] Comparative Example 1: The step of coating the epoxy polyurethane coating in step 4 of the present invention is removed, and the rest is the same as Example 1, and the specific steps are as follows: Step 1: The copper-clad ceramic substrate is sequentially subjected to film lamination, exposure, development, and etching, and then the front side of the copper-clad ceramic substrate is protected by film lamination, and the back side is subjected to chemical silver plating of 0.8 μm. After completion, the film lamination is removed, laser drilling is performed, and through holes are formed by cutting to obtain a copper-clad ceramic substrate A11; the aperture tolerance of the through hole is 10%, and the deviation is 0.02 mm;

[0049] Step 2: Take 3 copper sheets and perform film lamination, exposure, development and etching in sequence to obtain two microchannel layers 12 and one guide layer 13 respectively, and then perform chemical silver plating, electro-silver plating and electric spark wire cutting on the etched surfaces in sequence; wherein the thickness of the chemical silver plating is 0.7 μm, and the thickness of the electro-silver plating is 2 μm;

[0050] Step 3: stack and press the copper-clad ceramic substrate A11, microchannel layer 12, guide layer 13, microchannel layer 12, and copper-clad ceramic substrate A11 in this order to form a heat sink structure 1, and then perform vacuum sintering, wire cutting, grinding and polishing, and chemical nickel-gold plating in sequence; during vacuum sintering, the vacuum degree is 10 -2 Pa, the temperature is 950℃, and the insulation time is 12h; during wire cutting, the wire speed is 5m / s and the wire diameter is 0.35mm; when the heat sink structure 1 is stacked, the heat sink structure 1 is placed in a graphite fixture 2, and graphite paper 3 is placed on the upper and lower surfaces respectively, and the silver-plated surfaces of each layer are attached to each other and pressure is applied, and the pressure is 80MPa; during grinding and polishing, the cutting surface roughness is 1.5μm, the surface flatness is 0.8μm, and the roughness is 0.04μm; the nickel layer thickness is 5μm, and the gold layer thickness is 0.3μm.

[0051] Detection test:

[0052] Wear resistance test: A copper block with a size of 150 mm×70 mm×1 mm is used as a sample block, and the surface is coated with the epoxy polyurethane coating prepared by the present invention to obtain a sample. Referring to GB / T 12444-2006 standard, the test machine is turned on, and the sample and the test ring are rotated at a speed of 500 r / min to contact each other. After the test, the volume wear of the sample is calculated.

[0053] Corrosion resistance test: A copper block with a size of 150 mm×70 mm×1 mm was used as a sample block, and the surface was coated with the epoxy polyurethane coating prepared by the present invention to obtain a sample. Referring to GB / T 10125-2012 standard, an organic solvent was used to clean the surface dirt of the sample, and after cleaning, the sample was placed in a test box for a neutral salt spray test for 50 hours, and the mass loss was calculated after the test.

[0054] Heat dissipation performance test: The laser diode insulating heat sink prepared by the present invention is used as a sample, and a ceramic heating plate is placed on the sample as a heating source to simulate the heat source in actual use; then the temperature of the heating plate is controlled by adjusting the voltage of the heating plate, thereby simulating the heat dissipation requirements under different working conditions. During the heat dissipation test, tap water is used as the coolant, and the water flow rate is set to 1.5ml / s. By recording the temperature difference of the heat source and the inlet and outlet temperature difference, we can obtain important information about the heat handling of the radiator. The results are as follows:

[0055] <![CDATA[Volume wear / (mm 3 )]]> <![CDATA[Mass loss / (g / m 2 )]]> Heat source temperature difference / ℃ Inlet and outlet temperature difference / ℃ Example 1 3.2 42 151 3.9 Example 2 3.3 43 150 3.8 Example 3 3.4 44 149 3.7 Comparative Example 1 4.5 53 150 3.9

[0056] Conclusion: The dosage of Examples 1 to 3 remains unchanged, and only some reaction parameters are modified. From the experimental data, it can be seen that there is no obvious fluctuation in the performance of the samples.

[0057] Comparative Example 1: The step of coating the epoxy polyurethane coating in step 4 of the present invention is removed, and the rest is the same as Example 1. From the experimental data, it can be seen that compared with Example 1, the volume wear is increased by 4.5 mm 3 , the mass loss increased to 53g / m 2 The reason for analysis is: since the epoxidized polyurethane coating has good mechanical properties, the sample obtained by coating the epoxidized polyurethane coating on the surface of the copper block also has good mechanical properties. Therefore, after stopping the coating of the epoxidized polyurethane coating, the volume wear and mass loss of the sample increased, and the corrosion resistance decreased.

[0058] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0059] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a laser diode insulating heat sink, characterized in that: The following steps are involved: Step 1: sequentially laminating, exposing, developing, and etching the copper-clad ceramic substrate, and then laminating the front side of the copper-clad ceramic substrate for protection, and performing chemical silver plating on the back side. After completion, the laminating film is removed, laser drilling is performed, and through holes are formed by cutting to obtain a copper-clad ceramic substrate A (11); Step 2: taking three copper sheets and sequentially subjecting them to film lamination, exposure, development, and etching to obtain two microchannel layers (12) and one guide layer (13), respectively, and then sequentially subjecting the etched surfaces to chemical silver plating, electro-silver plating, and electric spark wire cutting; Step 3: stacking the copper-clad ceramic substrate A (11), the microchannel layer (12), the guide layer (13), the microchannel layer (12), and the copper-clad ceramic substrate A (11) in this order, pressing them to form a heat sink structure (1), and then sequentially performing vacuum sintering, wire cutting, grinding and polishing, and chemical nickel-gold plating to obtain a finished product; After chemical nickel-gold plating, the surface is coated with epoxidized polyurethane coating, and cured at 160-170°C for 3-4h, and the thickness of the epoxidized polyurethane coating layer is 2-5μm; wherein the preparation method of the epoxidized polyurethane coating is as follows: S1: In a nitrogen environment, a sodium hydroxide solution with a concentration of 3.3-3.6 mol / L and tetra(4-hydroxyphenyl)ethylene are mixed, stirred and reacted at 105-110°C for 1.2-1.6h, and then 3-chloro-1,2-propylene glycol is added dropwise, and the reaction is continued at 105-110°C for 3.5-4.5h. After the reaction is completed, the reaction is performed through extraction, washing, rotary evaporation concentration, filtration and drying to obtain an ether-containing product; the ether-containing product, diethyl carbonate and anhydrous potassium carbonate are mixed, refluxed at 115-125° C. for 25-30 hours, and then distilled at 75-80° C. for 6.5-7.5 hours. After the reaction is completed, the reaction is performed through standing, filtration and washing to obtain a cyclic carbonate; wherein the reaction molar ratio of tetra(4-hydroxyphenyl)ethylene to 3-chloro-1,2-propylene glycol is (4-5):1; the reaction molar ratio of the ether-containing product to diethyl carbonate is 1:(2-3); S2: In a nitrogen environment, cyclic carbonate and hexamethylenediamine are mixed, and the mixture is stirred and reacted at 120-150° C. for 4-5 hours to prepare an amino-terminated polyhydroxy polyurethane; the amino-terminated polyhydroxy polyurethane, epoxy resin and curing agent ethylenediamine are evenly mixed to obtain an epoxidized polyurethane coating; wherein the reaction molar ratio of cyclic carbonate and hexamethylenediamine is 1:(1.8-2); the contents of each component of the epoxidized polyurethane coating are: by mass fraction, 50-60% amino-terminated polyhydroxy polyurethane, 35-45% epoxy resin, and the balance ethylenediamine.

2. The method for preparing a laser diode insulating heat sink according to claim 1, characterized in that: In step 1, the thickness of chemically plated silver on the back side of the copper-clad ceramic substrate A (11) is 0.7-0.8 μm.

3. The method for preparing a laser diode insulating heat sink according to claim 1, characterized in that: In step 1, the aperture tolerance of the through hole is -10 to 10%, and the deviation is -0.02 to 0.02 mm.

4. The method for preparing a laser diode insulating heat sink according to claim 1, characterized in that: In step 2, the thickness of chemically plated silver on the surface of the copper sheet is 0.3-0.7 μm, and the thickness of electroplated silver on the surface of the copper sheet is 1-2 μm.

5. The method for preparing a laser diode insulating heat sink according to claim 1, characterized in that: In step 3, during vacuum sintering, the vacuum degree is 10 -3 ~10 -2 Pa, temperature is 800-950℃, holding time is 6-12h; wire cutting parameters: wire speed is 2-5m / s, wire diameter is 0.08-0.35mm.

6. The method for preparing a laser diode insulating heat sink according to claim 1, characterized in that: In step three, when the heat sink structure (1) is stacked, the heat sink structure (1) is placed in a graphite fixture (2), graphite paper (3) is placed on the upper and lower surfaces respectively, and the silver-plated surfaces of each layer are attached to each other and pressure is applied, the pressure is 30 to 80 MPa.

7. The method for preparing a laser diode insulating heat sink according to claim 1, characterized in that: In step three, grinding and polishing parameters: cutting surface roughness <2 μm, surface flatness <1 μm, surface roughness <0.05 μm; nickel layer thickness 2-5 μm, gold layer thickness 0.05-0.3 μm.

Citation Information

Patent Citations

  • Heat sink structure of semiconductor laser and preparation method thereof

    CN115939928A

  • Semiconductor laser microchannel and batch preparation method

    CN116260043A

  • Copper-clad ceramic substrate radiator and preparation method thereof

    CN116435273A

  • Modular microchannel heat exchanger

    US5727618A