A lithium-containing phosphate material, a lithium-ion battery positive electrode, and a preparation method and application thereof

By embedding nano-sized particles on the surface of micron-sized particles of lithium phosphate, an embedded material is formed, which solves the problems of slow electron/ion conductivity and high water absorption of lithium manganese iron phosphate materials, and improves the reversible capacity and rate of lithium-ion batteries. performance.

CN118380570BActive Publication Date: 2024-10-11BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410793743.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Lithium iron manganese phosphate materials have problems such as slow electron/ion conduction rate, high water absorption and high risk of gelation in battery applications, resulting in limited reversible capacity and rate performance of the battery.

Method used

Lithium-containing phosphate micron-sized particles with pores on the surface are used to embed nano-sized particles to form embedded materials, which improves porosity and lithium ion transmission channels, and reduces water absorption and gel risks.

Benefits of technology

The material has many reactive active sites, suitable water absorption, and sufficient lithium ion transmission channels, which improves the reversible capacity and rate performance of lithium-ion batteries while avoiding the risk of gelation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present disclosure relates to a lithium-containing phosphate material, a lithium-ion battery positive electrode, and a preparation method and application. The lithium-containing phosphate material comprises lithium-containing phosphate micron-sized particles having pores on the surface, and the pores of the lithium-containing phosphate micron-sized particles are embedded with lithium-containing phosphate nanoparticles. When the lithium-containing phosphate material of the present disclosure is applied to the positive electrode material layer of a lithium-ion battery, it has more reactive sites, and can improve the compaction density and porosity of the positive electrode material layer, provide a lithium ion transmission channel for the electrolyte, so that the reversible capacity of the lithium-ion battery is high and the battery has better rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of lithium-ion batteries, and in particular to a lithium-containing phosphate material, a lithium-ion battery positive electrode, and a preparation method and application thereof. Background Art

[0002] Lithium iron phosphate (LiFePO 4 ) As a positive electrode material for lithium batteries, it has the advantages of good structural stability, high safety, and good cycle performance. It has been widely used in lithium-ion batteries for power units of new energy vehicles. Lithium iron manganese phosphate positive electrode material (LiMn x Fe 1-x PO 4 , 0<x<1) is to use manganese to partially replace LiFePO 4 The iron in the positive electrode material forms a new type of material. This doping improves the LiFePO 4 voltage platform, further improving its energy density, and therefore has received much research attention.

[0003] Lithium manganese iron phosphate materials have the problem of slow electron / ion conduction rate. Nano-modification is an important technology to improve the electron / ion conduction rate of lithium manganese iron phosphate materials. The use of nano-sized lithium manganese iron phosphate particles can increase the specific surface area of ​​the positive electrode material, make the electrolyte and the positive electrode material fully contact, increase the reaction active sites, and greatly shorten the Li + transmission distance, improving the reversible capacity and rate performance of the battery. However, the surface energy of nano-sized lithium iron manganese phosphate particles is high, and they are prone to agglomeration, making it difficult to disperse evenly in the slurry during the preparation of the electrode. In addition, the increase in the specific surface area of ​​the nano-sized positive electrode material will make the positive electrode material extremely easy to absorb water. After water contacts the hydrophilic Li phase on the surface of the positive electrode material, a lithium reaction occurs, which affects the storage capacity retention rate of the battery. In addition, the alkaline substance generated by the lithium reaction will undergo an elimination reaction with the binder polyvinylidene fluoride. The double bonds generated cause a cross-linking reaction between the molecular chains of the binder polyvinylidene fluoride to form a gel, resulting in poor coating of the positive electrode material on the aluminum foil or the formation of gel pits, which hinders the migration of lithium ions and causes risks such as uneven current distribution and lithium precipitation. In short, the existing LiMn x Fe 1-x PO 4 It is difficult for the material to achieve a balance in terms of the number of active sites, water absorption and ion conduction rate, which affects the further improvement of the battery's reversible capacity and rate performance. Summary of the invention

[0004] The purpose of the present disclosure is to provide a lithium-containing phosphate material, a lithium-ion battery positive electrode, and a preparation method and application. The lithium-containing phosphate material can provide more reactive sites, and the material has a suitable specific surface area and water absorption. When used in lithium-ion batteries, it can provide sufficient lithium-ion transmission channels, thereby improving the reversible capacity and rate performance of the battery while reducing the risk of gelation.

[0005] In order to achieve the above objectives, the first aspect of the present disclosure provides a lithium-containing phosphate material, which includes lithium-containing phosphate micron-sized particles having pores on the surface, and lithium-containing phosphate nanoparticles are embedded in the pores of the lithium-containing phosphate micron-sized particles.

[0006] Optionally, the lithium phosphate-containing micron-sized particles have a D 50 Particle size and D of the lithium phosphate nanoparticles 50 The particle size ratio is 5~10.

[0007] Optionally, the pores of the lithium phosphate micron-sized particles have a D 50 Pore ​​size and D of the lithium phosphate nanoparticles 50 The particle size ratio is 0.8~1.

[0008] Optionally, the lithium phosphate nanoparticles D 50 The particle size is 0.5~0.9μm.

[0009] Optionally, the lithium phosphate-containing micron-sized particles have a D 50 The particle size is 2.5~10μm, and the D 50 The pore diameter is 0.4~0.9μm.

[0010] Optionally, the porosity of the lithium phosphate material is 10-15%.

[0011] Optionally, the lithium phosphate micron-sized particles have LiA x B 1-x PO 4 A is one or more of Ti, V, Mn, Fe, Co and Ni, B is one or more of Ti, V, Mn, Fe, Co and Ni, and x is any value between 0 and 1;

[0012] The lithium phosphate nanoparticles have LiA' y B´ 1-y PO 4 A' is one or more of Ti, V, Mn, Fe, Co and Ni, B' is one or more of Ti, V, Mn, Fe, Co and Ni, and y is any value between 0 and 1.

[0013] A second aspect of the present disclosure provides a method for preparing a lithium-containing phosphate material, the preparation method comprising the following steps:

[0014] (1) mixing a first lithium source, a first metal source and a first phosphorus source, and performing a first pre-sintering on the obtained mixture to obtain a first pre-sintered product; performing a first secondary sintering on the first pre-sintered product, a first carbon source and a pore-forming agent, and performing a first crushing treatment or a first granulation treatment on the first secondary sintered product to obtain lithium-containing phosphate micron-sized particles;

[0015] Mixing a second lithium source, a second metal source, and a second phosphorus source, and performing a second pre-sintering on the obtained mixture to obtain a second pre-sintering product; performing a second secondary sintering on the second pre-sintering product and a carbon source, and performing a second crushing treatment or a second granulation treatment on the second secondary sintering product to obtain lithium-containing phosphate nanoparticles;

[0016] (2) Mixing the lithium-containing phosphate nanoparticles and the lithium-containing phosphate micron-sized particles.

[0017] Optionally, the first metal source and the second metal source are each a compound containing one or more elements of Ti, V, Mn, Fe, Co and Ni; the first carbon source and the second carbon source are each selected from one or more of sucrose, glucose, citric acid, phenolic resin, starch and carbon black.

[0018] Optionally, in step (1), the mass of the pore-forming agent accounts for 1-5% of the total mass of the first pre-sintered product and the pore-forming agent; the pore-forming agent is selected from one or more of ethanol, oxalic acid, ammonium bicarbonate, ammonium carbonate, urea and ammonium chloride.

[0019] Optionally, in step (1), the first pre-sintering conditions include: being carried out in an inert atmosphere, the pre-sintering temperature is 500-650° C., and the pre-sintering time is 2-6 hours;

[0020] The conditions of the first and second sintering include: being carried out in an inert atmosphere, the sintering temperature is 710-900°C, and the sintering time is 6-12h;

[0021] The conditions of the first crushing treatment include: crushing the first secondary sintering product using a ball mill, the ball milling speed is 400-500 r / min, and the ball milling time is 8-10 h;

[0022] The conditions of the first granulation treatment include: feed gas pressure of 0.8-1.2 MPa, inert protective gas flow rate of 30-50 L / min, gas preheating temperature of 100-150° C., and feed solid content of 45-55%.

[0023] Optionally, in step (1), the second pre-sintering conditions include: being carried out in an inert atmosphere, the pre-sintering temperature is 500-650° C., and the pre-sintering time is 2-6 hours;

[0024] The second secondary sintering conditions include: being carried out in an inert atmosphere, the sintering temperature is 600-700° C., and the sintering time is 4-8 hours;

[0025] The conditions of the second crushing treatment include: crushing the second secondary sintering product using a ball mill, the ball milling speed is 450-600 r / min, and the ball milling time is 10-15 h;

[0026] The conditions of the second granulation treatment include: feed gas pressure of 1-1.5 MPa, inert protective gas flow rate of 40-60 L / min, gas preheating temperature of 100-150° C., and feed solid content of 45-55%.

[0027] Optionally, in step (2), the mixing is solid phase mixing and is carried out under stirring conditions, the stirring rate is 500-1200 rpm, the mixing temperature is 25-35° C., and the mixing time is 30-60 min.

[0028] Optionally, in step (2), the lithium phosphate nanoparticles D 50 The particle size is 0.5-0.9 μm; the D 50 The particle size is 2.5-10 μm; the D of the lithium phosphate micron-sized particles 50 The particle size of lithium phosphate nanoparticles is D 50 5~10 times the particle size.

[0029] A third aspect of the present disclosure provides a lithium-containing phosphate material prepared by the preparation method described in the second aspect of the present disclosure.

[0030] In a fourth aspect, the present disclosure provides a method for preparing a positive electrode of a lithium-ion battery, the method comprising: mixing a lithium-containing phosphate material, a conductive agent, a binder and a solvent to form a positive electrode slurry; forming a positive electrode slurry layer on a positive electrode current collector with the positive electrode slurry, and removing the solvent in the positive electrode slurry layer to form a positive electrode sheet containing a positive electrode material layer;

[0031] Wherein, the lithium-containing phosphate material is the lithium-containing phosphate material described in the first aspect of the present disclosure and the third aspect of the present disclosure.

[0032] Optionally, the method further comprises: before forming the positive electrode slurry layer, performing a shearing treatment on the positive electrode slurry, wherein the conditions of the shearing treatment include: a shearing rate of 4000-8000 rpm, and a shearing treatment temperature of 20-35°C.

[0033] Optionally, the mass ratio of the lithium-containing phosphate micron-sized particles to the lithium-containing phosphate nanometer-sized particles is 1:(50-200).

[0034] A fifth aspect of the present disclosure provides a lithium-ion battery positive electrode prepared by the method described in the fourth aspect of the present disclosure.

[0035] A sixth aspect of the present disclosure provides a lithium-ion battery positive electrode, the positive electrode comprising a current collector and a positive electrode material layer; a lithium-containing phosphate material is distributed in the positive electrode material layer; wherein the lithium-containing phosphate material is the lithium-containing phosphate material described in the first aspect of the present disclosure and / or the third aspect of the present disclosure.

[0036] Optionally, the porosity of the positive electrode material layer is 15-25%.

[0037] Optionally, the positive electrode material layer further contains positive electrode material nanoparticles;

[0038] The cathode material nanoparticles have LiA´´ z B´´ 1-z PO 4 A chemical formula, wherein A´´ is one or more of Ti, V, Mn, Fe, Co and Ni, B´´ is one or more of Ti, V, Mn, Fe, Co and Ni, and z is any value between 0 and 1;

[0039] The mass ratio of the positive electrode material nanoparticles to the lithium-containing phosphate material is (50-200):1.

[0040] A seventh aspect of the present disclosure provides a lithium-ion battery, comprising the lithium-ion battery positive electrode described in the sixth aspect of the present disclosure.

[0041] Through the above technical scheme, the lithium-containing phosphate material disclosed in the present invention includes lithium-containing phosphate nanoparticles and lithium-containing phosphate micron-sized particles with pores on the surface, the nanoparticles are embedded in the pores of the micron-sized particles with porous surfaces to form embedded lithium-containing phosphate materials; the lithium-containing phosphate material has pores on the surface, which improves the porosity of the material, forms more reactive sites, and can provide more lithium ion transmission channels. In addition, the pores of the micron-sized particles are embedded with nanoparticles. Compared with the positive electrode material using nanoparticles, the lithium-containing phosphate material disclosed in the present invention has lower water absorption and surface energy, which can avoid particle agglomeration in the preparation of positive electrode slurry and avoid the phenomenon of lithium reaction with water, and is conducive to the dispersion of binders and conductive agents, which can inhibit crosslinking and gelation in the slurrying process, and improve the distribution uniformity of each component in the positive electrode material layer. The positive electrode of the lithium-ion battery disclosed in the present invention contains the above-mentioned lithium-containing phosphate material, which has a balanced number of active sites, specific surface area and water absorption, and the pores of the micron-sized particles can increase the porosity of the positive electrode material, provide lithium ion transmission channels for the electrolyte, and improve the rate performance of the lithium-ion battery without gelation; the mutual grading of the micron-sized particles and the nano-sized particles can increase the compaction density of the positive electrode material layer, thereby increasing the reversible capacity of the lithium-ion battery.

[0042] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0043] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.

[0044] A first aspect of the present disclosure provides a lithium-containing phosphate material, wherein the lithium-containing phosphate material comprises lithium-containing phosphate micron-sized particles having pores on the surface, wherein lithium-containing phosphate nanon-sized particles are embedded in the pores of the lithium-containing phosphate micron-sized particles.

[0045] The lithium-containing phosphate material disclosed in the present invention includes lithium-containing phosphate nanoparticles and lithium-containing phosphate micron-sized particles with pores on the surface. The nanoparticles are embedded in the pores of the micron-sized particles with porous surfaces to form embedded lithium-containing phosphate materials. The surface of the lithium-containing phosphate material has pores, which improves the porosity of the material, forms more reactive sites, and can provide more lithium ion transmission channels. In addition, the pores of the micron-sized particles are embedded with nanoparticles. Compared with the positive electrode material using nano-sized particles, the lithium-containing phosphate material disclosed in the present invention has lower water absorption and surface energy, can avoid particle agglomeration in the preparation of positive electrode slurry, avoid the phenomenon of lithium reaction with water, and is conducive to the dispersion of binders, can inhibit cross-linking and gelation in the slurrying process, and improve the distribution uniformity of each component in the positive electrode material layer.

[0046] According to one embodiment of the present disclosure, the D of the lithium phosphate nanoparticles 50 The particle size is 0.5-0.9 μm, preferably 0.6-0.8 μm. The above embodiment is beneficial to the two particle gradations, providing more reactive sites for the positive electrode material.

[0047] According to one embodiment of the present disclosure, the D of the lithium phosphate micron-sized particles 50 The particle size is 2.5-10 μm, preferably 4-8 μm; the D 50 The pore size is 0.4-0.9 μm, preferably 0.6-0.8 μm. The surface of the lithium-containing phosphate micronized particles includes one or more pores, preferably a porous structure. In the present disclosure, D 50 The pore size refers to the D of the surface opening. 50 The above implementation is conducive to providing a lithium ion transmission channel for the electrolyte, increasing the porosity of the lithium phosphate material, and improving the rate performance of the battery.

[0048] According to one embodiment of the present disclosure, the D of the lithium phosphate micron-sized particles 50 Particle size and D of the lithium-containing phosphate nanoparticles 50 The ratio of the particle size is 5 to 10. The above implementation is conducive to the reasonable accumulation of micron-sized particles and nano-sized particles, is conducive to the two particle gradings, balances the pressure compaction and wettability of the pole piece, and can meet the requirements of the reversible capacity and rate performance of the battery when used in the battery.

[0049] According to one embodiment of the present disclosure, the D of the pores of the lithium phosphate micron-sized particles is 50 Pore ​​size and D of the lithium phosphate nanoparticles 50 The ratio of the particle size is 0.8 to 1. The above implementation is conducive to improving the porosity of the lithium-containing phosphate material and the positive electrode sheet, providing a lithium ion transmission channel for the electrolyte, and further improving the reversible capacity and rate performance of the battery.

[0050] According to the present disclosure, in the lithium-containing phosphate material, the proportion of the lithium-containing phosphate nanoparticles embedded in the pores of the lithium-containing phosphate micron-sized particles is not particularly limited.

[0051] According to one embodiment of the present disclosure, the porosity of the lithium phosphate material is 10-15%, preferably 12-14%. The above embodiment is conducive to improving the porosity of the positive electrode plate, providing a lithium ion transmission channel for the electrolyte, and further improving the reversible capacity and rate performance of the battery. In the present disclosure, the porosity of the lithium phosphate material refers to the porosity of a single lithium phosphate particle. In practical applications, there may be a certain error in the porosity of the lithium phosphate material. For example, in a specific embodiment, based on the total weight of the lithium phosphate material, the mass proportion of a single lithium phosphate particle with a porosity of 10-15% can be more than 95%; in further embodiments, the mass proportion can be more than 96%, more than 97%, or more than 98%.

[0052] Furthermore, in the lithium-containing phosphate material provided by the present disclosure, the mass ratio of the lithium-containing phosphate micron-sized particles to the lithium-containing phosphate nano-sized particles can vary within a wide range, and the present disclosure does not particularly limit the mass ratio of the two. For example, the mass ratio of the lithium-containing phosphate micron-sized particles to the lithium-containing phosphate nano-sized particles can be 1:(50-200), preferably 1:(50-150). The specific surface area of ​​the lithium-containing phosphate material is 14-20 m 2 / g, preferably 14~16m 2 / g. The above implementation is conducive to obtaining lithium-containing phosphate materials with a small specific surface area, thereby reducing the water absorption of the positive electrode raw materials; in the process of mixing and slurrying, since most of the nano-scale particles are embedded in the pores of the micron-scale particles and are not directly present in the slurry, the probability of particle agglomeration can be reduced, which is conducive to the uniform dispersion of the binder and the conductive agent, so that each component is evenly distributed and their cross-linking leading to gelation is inhibited. The above implementation not only provides more reactive sites but also increases the compaction density and porosity of the positive electrode material layer, so that the reversible capacity of the lithium-ion battery is high and the battery's rate performance is better.

[0053] According to one embodiment of the present disclosure, the lithium phosphate micron-sized particles have LiA x B 1-x PO 4 A is one or more of Ti, V, Mn, Fe, Co and Ni, B is one or more of Ti, V, Mn, Fe, Co and Ni, and x is any value between 0 and 1; the lithium-containing phosphate nanoparticles have LiA´ y B´ 1-y PO 4A' is one or more of Ti, V, Mn, Fe, Co and Ni, B' is one or more of Ti, V, Mn, Fe, Co and Ni, and y is any value between 0 and 1. In one embodiment, A is Mn, B is Fe, and the lithium phosphate micron-sized particles have LiMn x Fe 1- x PO 4 The chemical formula of x is any value from 0 to 1; A' is Mn, B' is Fe, and the lithium phosphate nanoparticles have LiMn y Fe 1- y PO 4 The chemical formula is: y is any value between 0 and 1. The above implementation is beneficial to improving the rate performance of the battery.

[0054] A second aspect of the present disclosure provides a method for preparing a lithium-containing phosphate material, the preparation method comprising the following steps:

[0055] (1) mixing a first lithium source, a first metal source and a first phosphorus source, and performing a first pre-sintering on the obtained mixture to obtain a first pre-sintered product; performing a first secondary sintering on the first pre-sintered product, a first carbon source and a pore-forming agent, and performing a first crushing treatment or a first granulation treatment on the first secondary sintered product to obtain lithium-containing phosphate micron-sized particles;

[0056] Mixing a second lithium source, a second metal source, and a second phosphorus source, and performing a second pre-sintering on the obtained mixture to obtain a second pre-sintering product; performing a second secondary sintering on the second pre-sintering product and a second carbon source, and performing a second crushing treatment or a second granulation treatment on the second secondary sintering product to obtain lithium-containing phosphate nanoparticles;

[0057] (2) Mixing the lithium-containing phosphate nanoparticles and the lithium-containing phosphate micron-sized particles.

[0058] The preparation method disclosed in the present invention can provide more reactive sites, increase the porosity of the positive electrode material, and provide a lithium ion transmission channel for the electrolyte; at the same time, the compaction density of the positive electrode material layer is increased by appropriately grading nano-scale particles and micron-scale particles, thereby further increasing the reversible capacity of the lithium-ion battery and improving the rate performance of the battery.

[0059] According to the present disclosure, the composition of the lithium phosphate micron-sized particles and the lithium phosphate nano-sized particles can be the same or different. Those skilled in the art can understand that in the embodiment where the nano-sized particles and the micron-sized particles have the same composition, the steps of preparing the first pre-sintered product and preparing the second pre-sintered product can also be combined, for example, a part of the obtained first pre-sintered product is used for the first secondary sintering to prepare the micron-sized particles, and another part of the first pre-sintered product is used for the second secondary sintering to prepare the nano-sized particles.

[0060] According to one embodiment of the present disclosure, the first lithium source and the second lithium source are each a compound containing a lithium element, and the compound containing a lithium element may be selected from one or more of lithium carbonate, lithium bicarbonate, lithium dihydrogen phosphate, lithium hydroxide and lithium oxalate.

[0061] According to one embodiment of the present disclosure, the first metal source and the second metal source are each a compound containing one or more elements of Ti, V, Mn, Fe, Co and Ni; the compound containing the Ti element can be selected from one or more of titanium dioxide, titanium tetrachloride, titanium nitrate, tetraalkoxy titanium and acyl titanium; the compound containing the V element can be selected from one or more of vanadium pentoxide, ammonium metavanadate and vanadium oxalate; the compound containing the Mn element can be selected from one or more of manganese carbonate, manganous sulfate, manganese phosphate, manganese nitrate and manganese oxide; the compound containing the Fe element can be selected from one or more of ferrous oxide, ferric oxide, ferrous oxalate, ferrous acetate; the compound containing the Co element can be selected from one or more of cobalt oxide, cobalt carbonate, cobalt chloride and cobalt acetate; the compound containing the Ni element can be selected from one or more of nickel oxide, nickel carbonate, nickel chloride and nickel acetate.

[0062] According to one embodiment of the present disclosure, the first phosphorus source and the second phosphorus source may each be selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, ammonium monohydrogen phosphate, and lithium dihydrogen phosphate.

[0063] According to one embodiment of the present disclosure, the first carbon source and the second carbon source can each be selected from an organic carbon source or an inorganic carbon source, and can further be selected from one or more of sucrose, glucose, citric acid, phenolic resin, starch and carbon black.

[0064] According to an embodiment of the present disclosure, the pore-forming agent is a substance that is easily decomposed into gas, so that a pore structure is generated in the material, and the pore-forming agent can be selected from one or more of ethanol, oxalic acid, ammonium bicarbonate, ammonium carbonate, urea and ammonium chloride. The above embodiment is conducive to making the micron-sized particles have a pore structure, which is conducive to providing a lithium ion transmission channel, so that the reversible capacity of the lithium-ion battery is high and the battery's rate performance is better.

[0065] In a further embodiment, in step (1), the mass of the pore former accounts for 1% to 5% of the total mass of the first pre-sintered product and the pore former, preferably 3% to 5%. The above embodiment is conducive to the formation of lithium-containing phosphate micron-sized particles with more suitable size and number of pores, providing a lithium ion transmission channel for the electrolyte, so that the reversible capacity of the lithium-ion battery is high and the battery has better rate performance; on the other hand, it is conducive to the embedding of nano-sized particles, reducing the specific surface area of ​​the material, thereby reducing the water absorption of the raw material, and reducing the agglomeration of nano-particles in the mixing and slurrying process, which is conducive to the uniform distribution of the binder and the conductive agent, and inhibiting their cross-linking to cause gel.

[0066] In the present disclosure, the amount of the first / second lithium source, the first / second metal source and the first / second phosphorus source is not particularly limited, and those skilled in the art can feed the materials according to the stoichiometric ratio of each element in the chemical formula of the prepared lithium-containing phosphate material. The order of step (1) and step (2) of the present disclosure is not particularly limited, for example, those skilled in the art can first prepare lithium-containing phosphate micron-sized particles, or first prepare lithium-containing phosphate nano-sized particles.

[0067] According to an embodiment of the present disclosure, in step (1), the first pre-sintering conditions include: being carried out under an inert atmosphere, wherein the inert atmosphere includes one or more of nitrogen, argon, helium and hydrogen; the pre-sintering temperature is 500-650°C, preferably 550-600°C, and the pre-sintering time is 2-6 hours, preferably 2-4 hours. The above embodiment is conducive to forming micron-sized particles with suitable size and suitable pores, providing lithium ion transmission channels, and further improving the rate performance of the battery.

[0068] According to an embodiment of the present disclosure, in step (1), the conditions of the first and second sintering include: being carried out under an inert atmosphere, wherein the inert atmosphere includes one or more of nitrogen, argon, helium and hydrogen; the sintering temperature is 710-900°C, preferably 750-850°C, and the sintering time is 6-12h, preferably 8-10h. The above embodiment is conducive to forming micron-sized particles with suitable size and suitable pores, providing lithium ion transmission channels, and further improving the rate performance of the battery.

[0069] According to an embodiment of the present disclosure, the first secondary sintering product is formed into lithium phosphate micron-sized particles through a first crushing treatment, and the conditions of the first crushing treatment can be conventional conditions in the art that can make the sintering product into micron-sized particles. In a further embodiment, the conditions of the first crushing treatment include: using a ball mill to crush the first secondary sintering product, the ball milling speed is 400~500r / min, preferably 420~480r / min, and the ball milling time is 8~10h, preferably 8.5~9.5h. The above embodiment is conducive to forming micron-sized particles with suitable size and suitable pores, providing lithium ion transmission channels, and further improving the rate performance of the battery.

[0070] According to another embodiment of the present disclosure, the first secondary sintering product is formed into micron-sized particles by a first granulation treatment. The conditions of the first granulation treatment may be conventional conditions in the art that can make the sintered product into micron-sized particles. In a further embodiment, the conditions of the first granulation treatment include: the feed gas pressure is 0.8~1.2MPa, preferably 0.9~1.1MPa, the inert protective gas flow rate is 30~50L / min, preferably 40~45 L / min, the gas preheating temperature is 100~150℃, preferably 120~140℃, and the feed solid content is 45~55%, preferably 48~52%. In a further embodiment, the first granulation treatment includes mixing the first secondary sintering product with a solvent to obtain a slurry with a solid content of 45~55%, and performing a first granulation treatment on the slurry; the solvent used may be water or anhydrous ethanol. The above embodiment is conducive to the formation of micron-sized particles with suitable sizes and suitable pores, providing lithium ion transmission channels, and further improving the rate performance of the battery.

[0071] According to an embodiment of the present disclosure, in step (1), the second pre-sintering conditions include: being carried out under an inert atmosphere, wherein the inert atmosphere includes one or more of nitrogen, argon, helium and hydrogen; the pre-sintering temperature is 500-650°C, preferably 550-600°C, and the pre-sintering time is 2-6 hours, preferably 2-4 hours. The above embodiment is conducive to forming lithium-containing phosphate nanoparticles of suitable size, providing reactive sites, and further improving the rate performance of the battery.

[0072] According to an embodiment of the present disclosure, in step (1), the conditions of the second secondary sintering include: being carried out under an inert atmosphere, wherein the inert atmosphere includes one or more of nitrogen, argon, helium and hydrogen; the sintering temperature is 600-700°C, preferably 620-680°C, and the sintering time is 4-8h, preferably 6-7h. The above embodiment is conducive to forming lithium-containing phosphate nanoparticles of suitable size, providing reactive sites, and further improving the rate performance of the battery.

[0073] According to an embodiment of the present disclosure, in step (1), the second secondary sintering product is formed into lithium phosphate nanoparticles by a second crushing treatment. The conditions of the first crushing treatment can be conventional conditions in the art that can make the sintering product into nanoparticles. In a further embodiment, the conditions of the second crushing treatment include: crushing the second secondary sintering product using a ball mill, the ball milling speed is 450-600r / min, and the ball milling time is 10-15h. The above embodiment is conducive to forming lithium phosphate nanoparticles of suitable size, providing reactive sites, and further improving the rate performance of the battery.

[0074] According to another embodiment of the present disclosure, the second secondary sintering product is formed into nano-scale particles by a second granulation treatment. The conditions of the second granulation treatment can be conventional conditions in the art that can make the sintering product into nano-scale particles. In a further embodiment, the conditions of the second granulation treatment include: the feed gas pressure is 1~1.5MPa, preferably 1.2~1.4MPa, the inert protective gas flow rate is 40~60L / min, preferably 45~55 L / min, the gas preheating temperature is 100~150℃, preferably 120~140℃, and the feed solid content is 45~55%, preferably 48~52%. In a further embodiment, the second granulation treatment includes mixing the second secondary sintering product with a solvent to obtain a slurry with a solid content of 45~55%, and performing a second granulation treatment on the slurry; the solvent used can be water or anhydrous ethanol. The above embodiment is conducive to the formation of lithium phosphate nanoparticles of suitable size, providing reactive sites, and further improving the rate performance of the battery.

[0075] According to an embodiment of the present disclosure, in step (2), the mixing is solid phase mixing and is carried out under stirring, the stirring rate is 500-1200 rpm, the mixing temperature is 25-35°C, and the mixing time is 30-60 min. The present disclosure does not impose any specific restrictions on the mixing equipment, which can be a conventional commercially available product. The above embodiment is conducive to providing more reactive sites while increasing the compaction density of the positive electrode material layer, while providing an appropriate number of pores to provide a transmission channel for lithium ions, further improving the rate performance of the battery.

[0076] According to one embodiment of the present disclosure, in step (2), the D containing lithium phosphate nanoparticles 50 The particle size is 0.5-0.9 μm, preferably 0.6-0.8 μm; the D 50 The particle size is 2.5-10 μm, preferably 4-8 μm; the D 50 The particle size of lithium phosphate nanoparticles is D50 The particle size is 5 to 10 times, preferably 6 to 8 times. The above embodiment is conducive to providing more reactive sites and providing an appropriate number of pores to provide transmission channels for lithium ions, thereby further improving the rate performance of the battery.

[0077] A third aspect of the present disclosure provides a lithium-containing phosphate material prepared by the method described in the second aspect of the present disclosure.

[0078] A fourth aspect of the present disclosure provides a method for preparing a positive electrode for a lithium-ion battery, the method comprising: mixing a lithium-containing phosphate material, a conductive agent, a binder and a solvent to form a positive electrode slurry; forming a positive electrode slurry layer on a positive electrode current collector with the positive electrode slurry, and removing the solvent in the positive electrode slurry layer to form a positive electrode sheet containing a positive electrode material layer; wherein the lithium-containing phosphate material is the lithium-containing phosphate material described in the first aspect of the present disclosure and / or the third aspect of the present disclosure.

[0079] The present invention uses lithium-containing phosphate materials to prepare positive electrodes, wherein the nano-scale particles and micron-scale particles can provide more reactive sites, and the micron-scale particles have pores, which can increase the porosity of the positive electrode material and provide a lithium ion transmission channel for the electrolyte. The appropriate grading of the two can increase the compaction density of the positive electrode material layer, thereby increasing the reversible capacity of the lithium-ion battery and improving the rate performance of the battery.

[0080] According to one embodiment of the present disclosure, the mass ratio of the lithium-containing phosphate material, the conductive agent, the binder, the dispersant and the solvent can be 1: 0.02-0.05: 0.03-0.06: 0.6-0.8, preferably 1: 0.02-0.03: 0.04-0.05: 0.65-0.75. The conductive agent can be one or more of carbon black, carbon nanotubes, acetylene black and graphene; the binder can be one or more of polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA) and polytetrafluoroethylene (PTFE); the solvent can be one or more of N-methylpyrrolidone, N-methylformamide, ethanol and acetone.

[0081] According to one embodiment of the present disclosure, the positive electrode slurry also includes a dispersant, and the dispersant may be one or more of polyvinyl pyrrolidone (PVP), polyacrylic acid (PAA), polyethyleneimine (PEI) and acrylic acid-maleic acid copolymer (PAMA); the mass ratio of the lithium-containing phosphate material to the dispersant may be 1:0.01~0.03, preferably 1:0.015~0.025.

[0082] According to an embodiment of the present disclosure, the method further comprises: before forming the positive electrode slurry layer, shearing the positive electrode slurry, the shearing treatment conditions comprising: a shear rate of 4000-8000rpm, preferably 5000-7000rpm; the solid content of the positive electrode slurry can be 45-60% by weight, preferably 50-55% by weight; in an optional embodiment, the shearing temperature is 20-35°C, preferably 25-30°C. The shear rate of the present disclosure is 1.2-2 times the conventional shear rate. The above embodiment is conducive to the weak part of the lithium phosphate material particles, that is, the embedded boundary, being split by stress, so that the positive electrode material wrapped with quantitative auxiliary materials is separated into nano-scale particles and micron-scale particles, ensuring the stable dispersion of the slurry, and also ensuring that there are more reactive sites in the positive electrode sheet, and the compaction density of the positive electrode sheet is increased by nano-scale particles with porous micron-scale large particles, exposing the pore structure to provide lithium ion transmission channels for the electrolyte, further improving the reversible capacity of the battery, and improving the rate performance of the battery.

[0083] According to an embodiment of the present disclosure, the mass ratio of the lithium-containing phosphate micron-sized particles to the lithium-containing phosphate nano-sized particles is 1: (50-200), preferably 1: (100-150). The above embodiment is conducive to obtaining a positive electrode material layer with suitable gradation, providing a lithium ion transmission channel while providing more reactive sites, improving the porosity of the positive electrode material, improving the compaction density of the positive electrode material layer, and further improving the reversible capacity and rate performance of the battery.

[0084] According to an embodiment of the present disclosure, the positive electrode slurry further comprises positive electrode material nanoparticles, and further, the mass ratio of the positive electrode material nanoparticles to the lithium-containing phosphate material is (50-200):1, preferably (100-150):1. The above embodiment is conducive to obtaining a positive electrode material layer with suitable gradation, and is conducive to providing lithium ion transmission channels while providing more reactive active sites, improving the porosity of the positive electrode material, improving the compaction density of the positive electrode material layer, and further improving the reversible capacity and rate performance of the battery.

[0085] In a further specific embodiment, the cathode material nanoparticles may be added during the slurry preparation step.

[0086] In another further specific embodiment, the positive electrode material nanoparticles can be added together when preparing the lithium-containing phosphate material, for example, the positive electrode material nanoparticles are added in the step of mixing the nano-sized particles and the micro-sized particles. In the embodiment where the composition of the positive electrode material nanoparticles is the same as that of the nano-sized particles, the nano-sized particles and the micro-sized particles can be directly prepared according to the mass ratio of the positive electrode material nanoparticles to the lithium-containing phosphate material of (50-200):1. The above embodiment is conducive to reducing the probability of nanoparticle agglomeration during the mixing and slurrying process, facilitating the uniform dispersion of the binder and the conductive agent, making the components uniformly distributed, and inhibiting their cross-linking to cause gel; it is conducive to the appropriate grading of the positive electrode material nanoparticles and the lithium-containing phosphate material, while providing more reactive sites, increasing the compaction density of the positive electrode material layer, and further improving the reversible capacity and rate performance of the battery.

[0087] The fifth aspect of the present disclosure provides a lithium-ion battery positive electrode prepared by the method described in the fourth aspect of the present disclosure.

[0088] The sixth aspect of the present disclosure provides a positive electrode for a lithium-ion battery, the positive electrode comprising a positive electrode current collector and a positive electrode material layer, wherein a lithium-containing phosphate material is distributed in the positive electrode material layer; wherein the lithium-containing phosphate material is the lithium-containing phosphate material described in the first aspect of the present disclosure and the third aspect of the present disclosure. The positive electrode material layer of the positive electrode of the present disclosure is distributed with micron-sized particles and nano-sized particles with porous surfaces, which ensures a large number of reactive active sites, and at the same time, improves the compaction density and porosity of the positive electrode sheet by combining nano-sized particles with porous micron-sized large particles, further improving the reversible capacity of the battery and the rate performance of the battery.

[0089] According to one embodiment of the present disclosure, the positive electrode material layer further contains positive electrode material nanoparticles; the mass ratio of the positive electrode material nanoparticles to the lithium-containing phosphate material is (50-200):1, preferably (100-150):1. In this embodiment, the composition of the positive electrode material nanoparticles can be the same as or different from the lithium-containing phosphate material nanoparticles. Further, the positive electrode material nanoparticles have LiA´´ z B´´ 1-z PO 4 The chemical formula is as follows, wherein A'' is one or more of Ti, V, Mn, Fe, Co and Ni, B'' is one or more of Ti, V, Mn, Fe, Co and Ni, and z is any value between 0 and 1. The above implementation is conducive to the appropriate grading of the positive electrode material nanoparticles and the lithium-containing phosphate material, while providing more reactive sites and increasing the compaction density of the positive electrode material layer, further improving the reversible capacity and rate performance of the battery.

[0090] In a further embodiment, the porosity of the positive electrode material layer is 15-25%, preferably 17-20%. The above embodiment is conducive to improving the porosity of the positive electrode material layer, providing a lithium ion transmission channel for the electrolyte, and improving the rate performance of the lithium ion battery of the battery.

[0091] A seventh aspect of the present disclosure provides a lithium-ion battery, comprising the lithium-ion battery positive electrode described in the fifth aspect of the present disclosure and / or the sixth aspect of the present disclosure.

[0092] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.

[0093] The following examples and comparative examples are used to prepare lithium iron manganese phosphate containing lithium phosphate materials as an example, wherein LiMn x Fe 1- x PO 4 Where x=0.8. The raw materials and reagents used in the examples and comparative examples are all battery grade; unless otherwise specified, the chemical reagents used in the following examples and comparative examples are commercially available products.

[0094] In the present disclosure, the specific surface area of ​​the composite particles is tested using the BET method on a gas adsorption instrument of model TriStarⅡ3020; the porosity of the composite particles, the porosity of the lithium phosphate material, the porosity of the positive electrode material layer, and the D 50 The pore size was measured on a ZEISS Crossbeam 550 focused ion beam scanning electron microscope; the D 50 Particle size and D of nanoparticles 50 The particle size was measured on a laser particle size analyzer model PSA200702. The viscosity of the positive electrode slurry was measured on a rotational rheometer model ViscoQC 300 (L).

[0095] Example 1

[0096] (1) According to the stoichiometric ratio, lithium carbonate, iron oxide, manganese carbonate and ammonium dihydrogen phosphate in a molar ratio of 0.5:0.8:0.1:1 are ball-milled and stirred until they are uniformly mixed, and the mixed raw materials are added into a high-temperature sintering furnace, argon gas is introduced, and the pre-sintering temperature is maintained at 600°C. The sintering is continued for 2 hours to obtain a first pre-sintered product; the first pre-sintered product after standing and cooling is poured into a ball mill, and glucose is added and ball-milled until it is uniformly dispersed, and then 3 weight % of ammonium bicarbonate based on the total weight of the first pre-sintered product and ammonium bicarbonate is added and mixed, and the powder of the mixed pore-forming agent is put into the sintering furnace again for secondary sintering at a temperature of 750°C for 8 hours, and then the product after the secondary sintering is mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%, and the slurry is spray granulated at a feed pressure of 1 MPa, an argon gas flow rate of 40 L / min, and an argon gas preheating temperature of 120°C to obtain porous micron-sized LMFP particles, D 50 The particle size is 4 μm, D 50 The pore size is 0.6 μm;

[0097] According to the stoichiometric ratio, lithium carbonate, iron oxide, manganese carbonate, and ammonium dihydrogen phosphate with a molar ratio of 0.5:0.8:0.1:1 are ball-milled and stirred until they are uniformly mixed, and the mixed raw materials are added to a high-temperature sintering furnace, argon gas is introduced, and the pre-sintering temperature is maintained at 600°C, and the sintering is continued for 2 hours to obtain a second pre-sintered product; the second pre-sintered product after standing and cooling is poured into a ball mill, and glucose is added and ball-milled until it is uniformly dispersed, and the mixed glucose powder is put into the sintering furnace again for secondary sintering at a temperature of 650°C for 6 hours, and then the product after the secondary sintering is mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%, and the slurry is spray granulated at a feed pressure of 1.2MPa and an argon flow rate of 50L / min to obtain nano-sized LMFP particles, and the argon preheating temperature is 120°C. The D of the nano-sized LMFP particles 50 Particle size: 0.65 μm;

[0098] (2) The porous micron-sized particles and nano-sized particles obtained above were stirred and mixed at a mass ratio of 1:100, and most of the nano-sized particles were allowed to enter the pores of the micron-sized particles to form composite particles. The mixing temperature was 25° C., the mixing time was 40 min, and the stirring rate was 800 rpm.

[0099] (3) The above-mentioned composite particles are mixed with a conductive agent CNT, a binder PVDF, a dispersant PVP and a solvent NMP in a mass ratio of 1:0.02:0.04:0.02:0.7 to form a positive electrode slurry, and the solid content of the positive electrode slurry is 50% by weight; then the positive electrode slurry is sheared at a shear rate of 6000 rpm at 25°C. After stirring for 20 minutes, the sheared slurry is coated on the current collector to form a positive electrode slurry layer on the current collector. During shearing, some nano-scale particles are separated from the pores of the micron-scale particles. The sheared positive electrode slurry contains a lithium phosphate material with an embedded structure and dispersed positive electrode material nanoparticles; the solvent in the positive electrode slurry layer is removed to form a positive electrode sheet containing a positive electrode material layer, and the positive electrode sheet is assembled with a separator, a graphite negative electrode, etc. into a full battery for testing.

[0100] Example 2

[0101] The same as Example 1, except that the mass proportion of the pore-forming agent ammonium bicarbonate in step (1) is 1%.

[0102] Example 3

[0103] The same as Example 1, except that the conditions for preparing porous micron-sized particles in step (1) are different, specifically as follows:

[0104] The first pre-sintered product, which was cooled, was poured into a ball mill, and glucose was added for ball milling until it was evenly dispersed, and then 3% by mass of ammonium bicarbonate was added for mixing. The powder of the mixed pore-forming agent was put into the sintering furnace again for secondary sintering at a temperature of 850°C for 6 hours. The product after the secondary sintering was mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%. The slurry was spray granulated at a feed pressure of 1 MPa, an argon flow rate of 40 L / min, and an argon preheating temperature of 120°C to obtain porous micron-sized LMFP particles. The D of the micron-sized particles was 50 The pore size is 0.5μm.

[0105] Example 4

[0106] The same as Example 1, except that the conditions for preparing porous micron-sized particles in step (1) are different, specifically as follows:

[0107] The first pre-sintered product, which was cooled, was poured into a ball mill, and glucose was added for ball milling until it was evenly dispersed, and then 3% by mass of ammonium bicarbonate was added for mixing. The powder of the mixed pore-forming agent was put into the sintering furnace again for secondary sintering at a temperature of 750°C for 8 hours, and then the product after the secondary sintering was mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%. The slurry was spray granulated at a feed pressure of 1.3 MPa, an argon flow rate of 52 L / min, and an argon preheating temperature of 120°C to obtain porous micron-sized LMFP particles. Micron-sized particles D 50 The particle size is 3μm.

[0108] Example 5

[0109] The same as Example 1, except that in step (2), the mass ratio of the porous micron-sized particles to the nano-sized particles is 1:50.

[0110] Example 6

[0111] The same as Example 1, except that in step (3), the shear rate is 4800 rpm.

[0112] Example 7

[0113] The same as Example 1, except that in step (1), when preparing nano-sized particles, the feed gas pressure is 1 MPa, the argon flow rate is 40 L / min, the argon preheating temperature is 120°C, and the D 50 The particle size is 0.9μm.

[0114] Example 8

[0115] The same as Example 1, except that in step (1), when preparing micron-sized particles: the secondary sintering temperature is 900°C, the sintering time is 12 hours; the feed gas pressure is 0.8 MPa, the argon flow rate is 30 L / min, and the argon preheating temperature is 120°C, and the D of the obtained micron-sized LMFP particles is 50 The particle size is 10μm.

[0116] Example 9

[0117] The same as Example 1, except that in step (1), when preparing nano-scale particles: the secondary sintering temperature is 600°C, the sintering time is 4h; the feed gas pressure is 1.5MPa, the argon flow rate is 60L / min, and the argon preheating temperature is 120°C. The D of the obtained nano-scale LMFP particles is 50 The particle size is 0.5μm.

[0118] Comparative Example 1

[0119] According to the stoichiometric ratio, lithium carbonate, iron oxide, manganese carbonate, and ammonium dihydrogen phosphate with a molar ratio of 0.5:0.8:0.1:1 are ball-milled and stirred until they are uniformly mixed, and the mixed raw materials are added into a high-temperature sintering furnace, argon is introduced, and the pre-sintering temperature is maintained at 600°C, and the sintering is continued for 2 hours to obtain a pre-sintered product; the pre-sintered product that has been cooled is poured into a ball mill, and glucose is added and ball-milled until it is uniformly dispersed, and the powder is put into the sintering furnace again for secondary sintering at a temperature of 650°C for 6 hours, and then the product after the secondary sintering is mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%, and the slurry is spray granulated, the feed pressure is 1.2MPa, the argon flow rate is 50L / min, and the argon preheating temperature is 120°C to obtain nano-sized LMFP particles, D 50 The particle size is 0.65μm; the nano-scale LMFP particles are mixed with the conductive agent CNT, the binder PVDF, the dispersant PVP and the solvent NMP in a mass ratio of 1:0.02:0.04:0.02:0.7 to form a slurry, coated on the current collector, and assembled with the separator, graphite negative electrode, etc. into a full battery for testing.

[0120] Comparative Example 2

[0121] The method of this comparative example is the same as that of Example 1, except that the pore-forming agent ammonium bicarbonate is not added in step (1), and the specific method is as follows:

[0122] (1) According to the stoichiometric ratio, lithium carbonate, iron oxide, manganese carbonate and ammonium dihydrogen phosphate in a molar ratio of 0.5:0.8:0.1:1 are ball-milled and stirred until they are uniformly mixed. The mixed raw materials are added into a high-temperature sintering furnace, argon is introduced, and the pre-sintering temperature is maintained at 600°C. The sintering is continued for 2 hours to obtain a first pre-sintered product. The first pre-sintered product that has been cooled is poured into a ball mill, and glucose is added and ball-milled until it is uniformly dispersed. The powder is put into the sintering furnace again for secondary sintering at a temperature of 750°C for 8 hours. The product after the secondary sintering is then mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%. The slurry is subjected to spray granulation treatment. The feed pressure is 1 MPa, the argon flow rate is 40 L / min, and the argon preheating temperature is 120°C to obtain non-porous micron-sized LMFP particles. 50 Particle size: 4 μm;

[0123] According to the stoichiometric ratio, lithium carbonate, iron oxide, manganese carbonate, and ammonium dihydrogen phosphate with a molar ratio of 0.5:0.8:0.1:1 are ball-milled and stirred until they are uniformly mixed, and the mixed raw materials are added into a high-temperature sintering furnace, argon gas is introduced, and the pre-sintering temperature is maintained at 600°C, and the sintering is continued for 2 hours to obtain a second pre-sintered product; the second pre-sintered product that has been allowed to stand and cool is poured into a ball mill, and glucose is added and ball-milled until it is uniformly dispersed, and the mixed glucose powder is put into the sintering furnace again for secondary sintering at a temperature of 650°C for 6 hours, and then the product after the secondary sintering is mixed with anhydrous ethanol to obtain a slurry with a solid content of 50%, and the slurry is spray granulated under the conditions of a feed pressure of 1.2MPa, an argon flow rate of 50L / min, and an argon preheating temperature of 120°C to obtain nano-sized LMFP particles, and the D of the nano-sized LMFP particles is 50 Particle size: 0.65 μm;

[0124] (2) stirring and mixing the non-porous micron-sized particles and the nano-sized particles obtained above at a mass ratio of 1:100 to obtain mixed particles containing non-porous micron-sized particles and nano-sized particles, the mixing temperature being 25° C. and the stirring rate being 800 rpm;

[0125] (3) The above-mentioned composite particles are mixed with the conductive agent CNT, the binder PVDF, the dispersant PVP and the solvent NMP in a mass ratio of 1:0.02:0.04:0.02:0.7 to form a positive electrode slurry; then the positive electrode slurry is sheared at a shear rate of 6000 rpm, the solid content of the positive electrode slurry is 50% by weight, and the shearing is carried out at 25°C. After stirring for 20 minutes, the sheared slurry is coated on the current collector, and the slurry forms a positive electrode slurry layer on the current collector. The solvent in the positive electrode slurry layer is removed to form a positive electrode sheet containing a positive electrode material layer, and the positive electrode sheet is assembled with a separator, a graphite negative electrode, etc. into a full battery for testing.

[0126] Test Example 1

[0127] The D of the micron-sized particles obtained in Examples 1 to 9 and Comparative Examples 1 to 2 50 Particle size, D 50 Pore ​​size, nano-particle D 50 The particle size, specific surface area and porosity of the composite particles, the specific surface area of ​​the lithium phosphate material, and the porosity of the positive electrode material layer were tested; the test results are shown in Table 1.

[0128] The characterization of the lithium phosphate material in the present disclosure is performed by testing the particles after filtering, drying and sieving the sheared slurry.

[0129] The specific surface areas of the composite particles of Examples 1 to 9 in Table 1 refer to the specific surface areas of the composite particles obtained by mixing in step (2).

[0130] The porosity of the composite particles in the present disclosure refers to the percentage of the volume of the pores inside a single composite particle to the total volume. The porosity of the composite particles of Examples 1 to 9 in Table 1 is the porosity of the composite particles obtained by mixing in step (2).

[0131] The porosity of lithium phosphate materials refers to the percentage of the volume of pores inside a single particle to the total volume.

[0132] The porosity of the positive electrode material layer refers to the percentage of the pore volume in the unit block material to the total volume of the material in its natural state.

[0133] Table 1

[0134]

[0135] The specific surface area of ​​the mixed particles containing non-porous micron-sized particles and nano-sized particles obtained in step (2) in Comparative Example 2 is 18.6 m 2 / g. According to the data in Table 1, compared with Comparative Example 2, the specific surface area of ​​the composite particles obtained by mixing in step (2) in Example 1 is smaller, indicating that during the mixing process, the nano-sized particles are embedded in the pores of the micron-sized particles. According to the comparison between the porosity of the composite particles in Example 1 and the porosity of the lithium phosphate-containing material, after the shearing treatment in step (3), the porosity of the lithium phosphate-containing material after shearing is higher than the porosity of the composite particles, indicating that part of the nano-sized particles fall off from the pores of the micron-sized particles by shearing.

[0136] Test Example 2

[0137] The state of the positive electrode slurry after shearing of Examples 1 to 9 and Comparative Examples 1 to 2 was observed, and the viscosity of the slurry was tested at 0 h, 2 h, 8 h and 12 h after discharge. If the slurry viscosity exceeded 3500 mPa·s, the slurry was defined as gelling. If the viscosity did not exceed 3500 mPa·s within 12 h, the slurry was judged to be in good condition. The results are shown in Table 2.

[0138] Table 2

[0139]

[0140] Test Example 3

[0141] The rate performance of the full batteries assembled in Examples 1 to 9 and Comparative Examples 1 to 2 was tested by 1 / 3C constant current and constant voltage charge / discharge at room temperature. The test results are shown in Table 3.

[0142] Table 3

[0143]

[0144] Comparative Example 1 The specific surface area of ​​the nanoparticles is 21 m 2 / g. According to the data in Table 1, Table 2 and Table 3, compared with Comparative Example 1, the specific surface area of ​​the lithium-containing phosphate material prepared by the method of the present invention is small. When used to prepare the positive electrode sheet of a lithium-ion battery, the water absorption degree of the positive electrode raw material can be reduced; in the process of mixing and slurrying, the probability of particle agglomeration can be reduced, which is beneficial to the uniform dispersion of the binder and the conductive agent, and the cross-linking thereof is inhibited to cause gelation, thereby ensuring the stable dispersion of the slurry. The compaction density of the positive electrode material is increased by combining nano-scale particles with porous micron-scale large particles, and the pore structure of the micron-scale particles is exposed to provide a lithium ion transmission channel for the electrolyte, thereby further increasing the reversible capacity of the battery and improving the rate performance of the battery.

[0145] Compared with Comparative Example 1, Examples 1 to 7 show that the positive electrode slurry particles of the present disclosure have less agglomeration phenomenon, and the positive electrode slurry will not form gel within 4 hours; Comparative Example 1 has severe gelation in 1 hour, forming continuous particle agglomeration, which significantly affects the ion transmission rate of the battery. Comparative Example 2 does not add a pore-forming agent. Compared with Example 1, its overall particle specific surface area increases, further increasing the water absorption rate and the cross-linking reaction area with the binder. The prepared slurry forms a gel within 2 hours, and the micron-sized particles have no pore structure, resulting in an extended solid-phase lithium ion transmission distance and poor rate performance.

[0146] Compared with Example 1, Example 2 shows that the content of the pore-forming agent in Example 1 is within the preferred range of the present disclosure, so that the micron-sized particles can better form a porous structure, which is more conducive to embedding nano-sized particles, reducing the probability of water absorption and avoiding the appearance of gel in the slurry. Similarly, compared with Example 1, it can be seen that the D 50 Pore ​​size and D of nanoparticles 50 The particle size ratio is within the preferred range of the present disclosure, which is more conducive to the embedding of nano-sized particles into the pores of micro-sized particles, avoiding agglomeration, and is more conducive to improving the rate performance of the battery. 50 Particle size and D of nanoparticles 50 The ratio of the particle sizes is within the preferred range of the present disclosure, which avoids the slurry from gelling within 4 hours, and is more conducive to improving the rate performance of the battery. Example 5 Compared with Example 1, the grading of the porous micron-sized particles and nano-sized particles in Example 1 is better than that in Example 5, which is more conducive to improving the active sites and further improving the rate performance of the battery. Example 6 Compared with Example 1, the shear rate of Example 1 is within the preferred range of the present disclosure, which is conducive to better separation of nano-sized particles from micron-sized particles, and is conducive to improving the rate performance of the battery. Example 7 Compared with Example 1, the D of the micron-sized particles in Example 1 is 50 Particle size and D of nanoparticles 50 The ratio of particle size, D of micron-sized particles50 Pore ​​size and D of nanoparticles 50 The particle size ratio is within the preferred range of the present disclosure, which is more conducive to the embedding of nano-sized particles into the pores of micro-sized particles, avoiding agglomeration, and is conducive to improving the rate performance of the battery. 50 Particle size and D of nanoparticles 50 The ratio of the particle size is within the preferred range of the present disclosure, which is beneficial to improving the porosity of the positive electrode material layer, facilitating lithium ion transmission, and improving the rate performance of the battery. 50 Pore ​​size and D of nanoparticles 50 The ratio of the particle sizes is within the preferred range disclosed in the present invention, which avoids agglomeration and prevents the slurry from gelling within 4 hours, and is more conducive to improving the rate performance of the battery.

[0147] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0148] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

Claims

1. A lithium phosphate material, characterized in that: The lithium-containing phosphate material comprises lithium-containing phosphate micron-sized particles having pores on the surface, lithium-containing phosphate nanoparticles are embedded in the pores of the lithium-containing phosphate micron-sized particles, and the porosity of the lithium-containing phosphate material is 10-15%.

2. The lithium phosphate material according to claim 1, wherein: The lithium phosphate micron-sized particles D 50 Particle size and D of the lithium phosphate nanoparticles 50 The particle size ratio is 5~10.

3. The lithium phosphate material according to claim 1, wherein: The pores of the lithium phosphate micron-sized particles have a D 50 Pore ​​size and D of the lithium phosphate nanoparticles 50 The particle size ratio is 0.8~1.

4. The lithium phosphate material according to any one of claims 1 to 3, wherein The lithium phosphate nanoparticles D 50 The particle size is 0.5~0.9μm.

5. The lithium phosphate material according to any one of claims 1 to 3, wherein: The lithium phosphate micron-sized particles D 50 The particle size is 2.5~10μm, and the D 50 The pore diameter is 0.4~0.9μm.

6. The lithium phosphate material according to claim 1, wherein: The porosity of the lithium phosphate material is 12-14%.

7. The lithium phosphate material according to claim 1, wherein: The lithium phosphate micron-sized particles have LiA x B 1-x The chemical formula of PO4, wherein A is one or more of Ti, V, Mn, Fe, Co and Ni, B is one or more of Ti, V, Mn, Fe, Co and Ni, and x is any value between 0 and 1; The lithium phosphate nanoparticles have LiA' y B´ 1-y The chemical formula of PO4, wherein A´ is one or more of Ti, V, Mn, Fe, Co and Ni, B´ is one or more of Ti, V, Mn, Fe, Co and Ni, and y is any value between 0 and 1.

8. A method for preparing a lithium-containing phosphate material, characterized in that: The preparation method comprises the following steps: (1) mixing a first lithium source, a first metal source and a first phosphorus source, and performing a first pre-sintering on the obtained mixture to obtain a first pre-sintered product; performing a first secondary sintering on the first pre-sintered product, a first carbon source and a pore-forming agent, and performing a first crushing treatment or a first granulation treatment on the first secondary sintered product to obtain lithium-containing phosphate micron-sized particles; mixing a second lithium source, a second metal source and a second phosphorus source, and performing a second pre-sintering on the obtained mixture to obtain a second pre-sintered product; The second pre-sintered product and the second carbon source are subjected to a second secondary sintering, and the second secondary sintered product is subjected to a second crushing treatment or a second granulation treatment to obtain lithium-containing phosphate nanoparticles; (2) mixing the lithium-containing phosphate nanoparticles and the lithium-containing phosphate micron-sized particles; Wherein, in step (1), the mass of the pore-forming agent accounts for 1-5% of the total mass of the first pre-sintered product and the pore-forming agent.

9. The preparation method according to claim 8, wherein: The first metal source and the second metal source are each a compound containing one or more elements of Ti, V, Mn, Fe, Co and Ni; the first carbon source and the second carbon source are each selected from one or more of sucrose, glucose, citric acid, phenolic resin, starch and carbon black.

10. The preparation method according to claim 8, wherein: In step (1), the mass of the pore-forming agent accounts for 3-5% of the total mass of the first pre-sintered product and the pore-forming agent; the pore-forming agent is selected from one or more of ethanol, oxalic acid, ammonium bicarbonate, ammonium carbonate, urea and ammonium chloride.

11. The preparation method according to claim 8, wherein: In step (1), the first pre-sintering conditions include: being carried out in an inert atmosphere, the pre-sintering temperature is 500-650° C., and the pre-sintering time is 2-6 hours; The conditions of the first and second sintering include: being carried out in an inert atmosphere, the sintering temperature is 710-900°C, and the sintering time is 6-12h; The conditions of the first crushing treatment include: crushing the first secondary sintering product using a ball mill, the ball milling speed is 400-500 r / min, and the ball milling time is 8-10 h; The conditions of the first granulation treatment include: feed gas pressure of 0.8-1.2 MPa, inert protective gas flow rate of 30-50 L / min, gas preheating temperature of 100-150° C., and feed solid content of 45-55%.

12. The preparation method according to claim 8, wherein: In step (1), the second pre-sintering conditions include: being carried out in an inert atmosphere, the pre-sintering temperature is 500-650° C., and the pre-sintering time is 2-6 hours; The second secondary sintering conditions include: being carried out in an inert atmosphere, the sintering temperature is 600-700° C., and the sintering time is 4-8 hours; The conditions of the second crushing treatment include: crushing the second secondary sintering product using a ball mill, the ball milling speed is 450-600r / min, and the ball milling time is 10-15h; The conditions of the second granulation treatment include: feed gas pressure of 1-1.5 MPa, inert protective gas flow rate of 40-60 L / min, gas preheating temperature of 100-150° C., and feed solid content of 45-55%.

13. The preparation method according to claim 8, wherein: In step (2), the mixing is solid phase mixing and is carried out under stirring conditions. The stirring rate is 500-1200 rpm, the mixing temperature is 25-35° C., and the mixing time is 30-60 min.

14. The preparation method according to claim 8, wherein: In step (2), the lithium phosphate nanoparticles D 50 Particle size is 0.5~0.9μm; The lithium phosphate micron-sized particles D 50 Particle size is 2.5~10μm; The lithium phosphate micron-sized particles D 50 The particle size of lithium phosphate nanoparticles is D 50 5~10 times the particle size.

15. A lithium-containing phosphate material prepared by the preparation method according to any one of claims 8 to 14.

16. A method for preparing a positive electrode of a lithium ion battery, characterized in that: The method comprises: mixing a lithium phosphate material, a conductive agent, a binder and a solvent to form a positive electrode slurry; forming a positive electrode slurry layer on a positive electrode current collector with the positive electrode slurry, and removing the solvent in the positive electrode slurry layer to form a positive electrode sheet containing a positive electrode material layer; Wherein, the lithium-containing phosphate material is the lithium-containing phosphate material according to any one of claims 1 to 7 and claim 15.

17. The method according to claim 16, wherein: The method further comprises: before forming the positive electrode slurry layer, performing a shearing treatment on the positive electrode slurry, wherein the conditions of the shearing treatment include: a shearing rate of 4000-8000 rpm, and a shearing treatment temperature of 20-35°C.

18. The method according to claim 16, wherein: The mass ratio of the lithium-containing phosphate micron-sized particles to the lithium-containing phosphate nanometer-sized particles is 1:(50-200).

19. A lithium ion battery positive electrode prepared by the method according to any one of claims 16 to 18.

20. A positive electrode for a lithium ion battery, characterized in that: It comprises a positive electrode current collector and a positive electrode material layer; the positive electrode material layer contains a lithium phosphate material; Wherein, the lithium-containing phosphate material is the lithium-containing phosphate material according to any one of claims 1 to 7 and claim 15.

21. The lithium ion battery positive electrode according to claim 20, wherein: The porosity of the positive electrode material layer is 15-25%.

22. The lithium ion battery positive electrode according to claim 20, wherein: The positive electrode material layer also contains positive electrode material nanoparticles; The cathode material nanoparticles have LiA´´ z B´´ 1-z The chemical formula of PO4, wherein A´´ is one or more of Ti, V, Mn, Fe, Co and Ni, B´´ is one or more of Ti, V, Mn, Fe, Co and Ni, and z is any value between 0 and 1; The mass ratio of the positive electrode material nanoparticles to the lithium-containing phosphate material is (50-200):

1.

23. A lithium ion battery, characterized in that: A lithium-ion battery positive electrode comprising any one of claims 19 to 22.