Ceramic rock plate with large-area transparent line texture and imitation stone decorative effect and preparation method thereof
Through the combined technology of inkjet printing to remove ink and activated carbon fiber roller adsorption, the problem that existing imitation stone ceramic tiles cannot show transparent lines has been solved, and the three-dimensional effect of ceramic rock slabs has been improved and the decorative effect has been significantly improved.
Patent Information
- Application Number
- CN202410896236.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing imitation stone ceramic tiles cannot show the crystal feel of stone and the transparent lines embedded in it, and lack a three-dimensional effect.
By inkjet printing on the surface of the ceramic rock plate, the ink is removed, and the covered transparent powder surface glaze is removed, exposing the transparent powder layer. Combined with the adsorption effect of the 3D cloth system and the activated carbon fiber roller, a large area of transparent lines is formed. texture.
It realizes the improvement of the three-dimensional sense of ceramic rock slabs, significantly enhances the realism and decorative effect of the stone, and ensures the clarity and integrity of the transparent line texture.
Smart Images

Figure CN118420332B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a ceramic rock plate with a large-area transparent line texture and a stone-like decorative effect and a preparation method thereof, and belongs to the technical field of building ceramic production and manufacturing. Background Art
[0002] In the field of home decoration, imitation stone ceramic tiles are widely used in home decoration such as floors, walls, ceiling lights, and carvings due to their diverse colors and realistic feeling of being close to stone. At the same time, the high durability and weathering resistance of imitation stone ceramic tiles also make them very popular in the landscape design of home gardens. Existing imitation stone ceramic tiles are mainly formed by inkjet printing to form a surface texture close to that of stone, but they cannot present the crystal feeling of stone and the transparent lines embedded in it. Summary of the invention
[0003] In view of the above problems, the present invention provides a ceramic rock plate with a large area of transparent line texture and a method for preparing the same. The surface glaze covering the surface of the transparent powder forming the transparent line texture is peeled off by peeling the ink, so that the transparent powder layer is not covered by the surface glaze layer, and a ceramic rock plate with an inkjet pattern and a transparent line texture decoration corresponding to the inkjet pattern is obtained, which has a more three-dimensional sense of stone. The present invention is realized by the following technical solutions:
[0004] In a first aspect, the present invention provides a method for preparing a ceramic rock plate with a large-area transparent line texture and a stone-like decorative effect. The method for preparing a ceramic rock plate with a large-area transparent line texture and a stone-like decorative effect comprises:
[0005] Step (1) preparing ordinary powder and transparent powder into a blank with transparent line texture according to the layout design;
[0006] Step (2) inkjet printing and spreading ink on the surface of the blank at the position corresponding to the transparent line texture;
[0007] Step (3) applying glaze to the surface of the blank after the ink is removed by inkjet printing;
[0008] Step (4) inkjet printing a pattern on the surface of the green body after the glaze is applied;
[0009] Step (5) applying protective glaze on the surface of the blank after the inkjet printing pattern;
[0010] Step (6) is to fire and polish the green body after applying the protective glaze to obtain the ceramic rock plate with a large area of transparent line texture and imitation stone decorative effect.
[0011] Preferably, the raw material composition of the transparent powder includes, by mass percentage, 10-15% clay, 20-40% quartz, and 45-70% boron frit; wherein, the chemical composition of the boron frit includes, by mass percentage, SiO2: 62-68%, Al2O3: 5-10%, Fe2O3: 0.02-0.05%, TiO2: 0.01-0.05%, CaO: 1-3%, MgO: 1-3%, K2O: 5-10%, Na2O: 1-5%, and B2O3: 15-20%.
[0012] Preferably, the chemical composition of the common powder includes, by mass percentage: loss on ignition: 3~6%, SiO2: 60~70%, Al2O3: 19~25%, Fe2O3: 0.2~0.6%, TiO2: 0.01~0.1%, CaO: 0.2~0.6%, MgO: 0.1~1%, K2O: 2~5%, and Na2O: 2~5%.
[0013] Preferably, the raw material composition of the peeling ink includes, by mass percentage: 65~75% organic solvent, 2~4% hydrophobic coupling agent, 5~10% dispersant, and 20~35% peeling glaze powder; wherein, the chemical composition of the peeling glaze powder includes, by mass percentage: loss on ignition: 3.5~4.5%, SiO2: 43~46%, Al2O3: 24~26%, BaO: 5~6%, CaO: 4~6%, MgO: 2~3%, K2O: 2.5~3.5%, NaO: 3.5~4.5%, B2O3: 3~4%, SrO: 3~4%, and ZnO: 3~4%.
[0014] Preferably, the chemical composition of the glaze includes, by mass percentage: SiO2: 61~65%, Al2O3: 19~23%, Fe2O3: 0.05~0.1%, TiO2: 0.05~0.1%, CaO: 0.1~0.5%, MgO: 0.1~0.5%, K2O: 3~4%, Na2O, 3.1~3.8%, ZrO2: 3.2~9.6%, and loss on ignition: 1.5~2%.
[0015] Preferably, the glaze is applied by spraying; the specific gravity of the glaze is 1.3-1.5 g / cm 3 , glaze application amount is 200~300 g / m 2 .
[0016] Preferably, the chemical composition of the protective glaze includes, by mass percentage, SiO2: 45~50%, Al2O3: 18~22%, Fe2O3: 0.1~1%, TiO2: 0.1~1%, CaO: 0.1~1%, MgO: 4~8%, BaO: 10~15%, ZnO: 2~5%, K2O: 4~8%, Na2O: 1~3%, and loss on ignition: 4~6%.
[0017] Preferably, the protective glaze is applied by spraying; the specific gravity of the protective glaze is 1.3-1.6 g / cm 3 , glaze application amount is 400~500 g / m 2 .
[0018] Preferably, the sintering temperature is 1135-1160° C., and the sintering time is 60-80 minutes.
[0019] Preferably, the preparation method further comprises: before inkjet printing a pattern on the surface of the glazed body, using a roller made of activated carbon fiber and having a pattern carved on the surface that is the same as the transparent line texture to adsorb the glazed body.
[0020] Preferably, a transparent line texture is extracted according to the layout design, vector processing is performed on the extracted transparent line texture to obtain a vector file, the vector file is loaded into a 3D cloth system, transparent powder is distributed at positions corresponding to the transparent line texture and ordinary powder is distributed at positions other than corresponding to the transparent line texture according to the vector file, and then pressed and molded to prepare a blank with a transparent line texture.
[0021] In a second aspect, the present invention provides a ceramic rock plate with a large area of transparent line texture and imitation stone decorative effect. The ceramic rock plate with a large area of transparent line texture and imitation stone decorative effect is obtained according to any of the preparation methods described above.
[0022] Beneficial Effects
[0023] The preparation method of the present invention forms a blank with a transparent line texture corresponding to an inkjet pattern through a 3D cloth system, and then the glaze covering the surface of the transparent powder forming the transparent line texture is peeled off through the peeling action of the ink, so that the transparent powder layer is not covered by the glaze layer, thereby obtaining a ceramic rock slab decorated with an inkjet pattern and a transparent line texture corresponding to the inkjet pattern, which has a more three-dimensional sense of stone. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a transparent line extraction effect diagram of Example 1;
[0025] Figure 2This is the effect diagram of the blank cloth of Example 1; wherein 1-ordinary powder, 2-transparent powder;
[0026] Figure 3 This is a brick surface effect diagram of the ceramic rock slab with imitation stone decorative effect prepared in Example 1;
[0027] Figure 4 The ink-pushing effect diagram of comparative example 1 (left) and the combined effect diagram of ink-pushing and roller adsorption of example 2 under the same design layout conditions (right);
[0028] Figure 5 This is a picture of the brick surface effect of the ceramic rock slab prepared in Example 3. DETAILED DESCRIPTION
[0029] The present invention is further described by the following embodiments, which should be understood to be only used to illustrate the present invention, rather than to limit the present invention. The following is an exemplary description of the preparation method of the ceramic rock plate with large-area transparent line texture and imitation stone decorative effect of the present invention.
[0030] Prepare common powder (also called basic powder). In some embodiments, the chemical composition of the common powder includes, by mass percentage, loss on ignition: 3-6%, SiO2: 60-70%, Al2O3: 19-25%, Fe2O3: 0.2-0.6%, TiO2: 0.01-0.1%, CaO: 0.2-0.6%, MgO: 0.1-1%, K2O: 2-5%, Na2O: 2-5%. Preferably, the chemical composition of the common powder includes, by mass percentage, loss on ignition: 3-5%, SiO2: 60-65%, Al2O3: 19-23%, Fe2O3: 0.2-0.6%, TiO2: 0.01-0.05%, CaO: 0.2-0.6%, MgO: 0.1-0.5%, K2O: 2-3%, Na2O: 2-3%.
[0031] It should be understood that any common powder raw material composition that makes the chemical composition of the common powder fall within the above range can be applied to the present invention. In some embodiments, the raw material composition of the common powder includes, by mass percentage: clay: 30-50%, potassium feldspar: 10-20%, sodium feldspar: 10-20%, medium temperature sand: 10-50%. Weigh each raw material according to the raw material composition of the common powder, add water and ball mill evenly, sieve to remove iron, spray powder and granulate to obtain the common powder. The ball milling speed can be adaptively changed according to demand. The ball milling time can be 10-15h. The slurry fineness after sieving and removing iron can be within 0.3-0.5wt% of the 250 mesh sieve.
[0032] The thermal expansion coefficient of the ordinary powder at 40-600°C is 7.8×10 -6~8.1×10 -6 / K.
[0033] Prepare transparent powder. The raw material composition of the transparent powder includes, by mass percentage, 10-15% clay, 20-40% quartz, and 45-70% boron frit. The refractive index of quartz and glass is close, and light transmission will not be lost and the transparency of the light-transmitting powder will not be affected. Quartz can also adjust the temperature of the transparent powder. The formula of the transparent powder of the present invention contains a large amount of quartz, and the introduction of boron frit can be used as a flux and reduce the temperature of the transparent powder. Moreover, boron will be dissolved in the glass body without producing other crystal phases, so the introduction of boron frit will not affect light transmission, and increase the transparent performance of the transparent powder. In addition, boron frit can also reduce the thermal expansion coefficient of the transparent powder to match it with ordinary powder. The present invention uses a transparent powder of the K-Na-B-Si-Al system, on the one hand, so that the thermal expansion coefficient of the transparent powder is close to that of the ordinary powder, and on the other hand, it is not easy to generate a crystal phase, and exists in the form of a glass phase, has a good sense of transparency, and has good thermal stability.
[0034] If the boron frit content of the transparent powder is too low, the melting temperature of the transparent powder will be too high, the glass phase content will be reduced, and the transparency of the transparent powder will be reduced. If the boron frit content of the transparent powder is too high, the melting temperature of the transparent powder will be too low, and the blank will easily collapse after firing.
[0035] In some embodiments, the chemical composition of the boron frit may include, by mass percentage: SiO2: 62-68%, Al2O3: 5-10%, Fe2O3: 0.02-0.05%, TiO2: 0.01-0.05%, CaO: 1-3%, MgO: 1-3%, K2O: 5-10%, Na2O: 1-5%, B2O3: 15-20%. The boron oxide content of the boron frit is controlled within the above range, which is conducive to the existence of boron in a structural state with a coordination number of four, so that the transparent powder has better thermal stability.
[0036] In some embodiments, the raw material composition of the boron frit includes, by mass percentage, boric acid: 15-20%, borax: 15-30%, potassium feldspar: 20-40%, sodium feldspar: 10-20%, dolomite: 10-20%, and quartz sand: 10-30%. According to the raw material composition of the boron frit, each raw material is weighed, mixed evenly, melted at 1300-1500° C. for 1-3 hours, quenched with water, and crushed to obtain a boron frit.
[0037] Weigh each raw material according to the raw material composition of the transparent powder, add water and ball mill evenly, sieve to remove iron, spray powder and granulate to obtain the transparent powder. The ball milling speed can be adaptively changed according to demand. The ball milling time can be 10~15h. The slurry fineness after sieving and removing iron can be within 0.3~0.5wt% of the 250 mesh sieve residue.
[0038] The thermal expansion coefficient of the transparent powder at 40-600°C is 7.5×10 -6 ~7.8×10 -6 / K. The transparent powder and the common powder have similar thermal expansion coefficients, which can prevent the green body from cracking due to the mismatch of thermal expansion coefficients between the transparent powder and the common powder during the firing process.
[0039] Ordinary powder and transparent powder are prepared into a blank with transparent line texture according to the layout design.
[0040] A 3D distribution system can be used to distribute transparent powder and ordinary powder to prepare a blank with transparent line texture. In the embodiments and comparative examples, a 3D distribution system provided by Sepfit Technology Co., Ltd. can be used to distribute transparent powder and ordinary powder. Specifically, a transparent line texture is extracted according to the layout design, and the extracted transparent line texture is vector processed to obtain a vector file, and the vector file is loaded into the 3D distribution system. According to the vector file, transparent powder is distributed at the position corresponding to the transparent line texture and ordinary powder is distributed at the position other than the transparent line texture, and then pressed and formed to prepare a blank with transparent line texture. In other words, the transparent powder is not randomly distributed, but is distributed according to the layout design corresponding to the inkjet pattern, and finally a blank with a transparent line texture corresponding to the inkjet line texture is formed.
[0041] As an example: first, ordinary powder and transparent powder stored in different hoppers are transported to different micro-cylinder gates. Then the distributor applies the ordinary powder in the micro-cylinder gate to the distribution belt according to the vector file. Then, according to the vector file, the ordinary powder is spread at the position where the transparent line texture is required. Then the transparent powder is spread at the spread position. Finally, the powder after spreading is transported to the press by the feeding belt and pressed into shape to obtain a blank with an ordinary powder layer and a transparent powder layer. The thickness of the transparent powder can be controlled by controlling the spreading depth. The spreading depth can be 2~4mm. The grayscale of the transparent line texture pattern of the vector file can be 20~30%.
[0042] If the thickness of the transparent powder layer is too low, the three-dimensional effect of the blank will be weakened. If the thickness of the transparent powder layer is too high, the gas in the blank cannot be discharged in time, and pinhole phenomenon is likely to occur. In some embodiments, the thickness of the transparent powder layer is 2-4 mm.
[0043] The pressing method is not limited, and any pressing method commonly used in the art can be used. The pressing method can be performed by a press, including but not limited to dry pressing.
[0044] In some embodiments, the chemical composition of the green body includes, by mass percentage, loss on ignition: 1~2%, SiO2: 70~75%, Al2O3: 5~10%, Fe2O3: 0.2~0.6%, TiO2: 0.01~0.05%, CaO: 0.2~0.6%, MgO: 0.1~0.5%, K2O: 5~10%, Na2O: 2~3%, and B2O3: 8~15%.
[0045] Inkjet print the push-off ink at the position corresponding to the transparent line texture on the surface of the blank. The raw material composition of the push-off ink includes, by mass percentage: 65-75% organic solvent, 2-4% hydrophobic coupling agent, 5-10% dispersant, and 20-35% push-off glaze powder. In some embodiments, the chemical composition of the push-off glaze powder includes, by mass percentage: ignition loss: 3.5-4.5%, SiO2: 43-46%, Al2O3: 24-26%, BaO: 5-6%, CaO: 4-6%, MgO: 2-3%, K2O: 2.5-3.5%, NaO: 3.5-4.5%, B2O3: 3-4%, SrO: 3-4%, ZnO: 3-4%.
[0046] The organic solvent includes but is not limited to a mixture of one or more of methyl acetate, ethyl acetate, and isooctyl palmitate. The hydrophobic coupling agent may be a titanate coupling agent and / or a silane coupling agent. The types of titanate coupling agents and silane coupling agents are not limited. The dispersant includes but is not limited to a mixture of one or more of ammonium polyacrylate, polyvinyl pyrrolidone, polyethylene glycol, and sodium alginate. In the embodiments and comparative examples, methyl acetate is specifically used as the organic solvent, a titanate coupling agent is specifically used as the hydrophobic coupling agent, and polyvinyl pyrrolidone is specifically used as the dispersant.
[0047] The grayscale of the inkjet printed ink-pushing pattern affects the amount of ink printed. In some implementations, the grayscale of the inkjet printed ink-pushing pattern is 100%.
[0048] Apply glaze on the surface of the blank after the ink is pushed away during inkjet printing. The glaze can cover the base color and defects of the blank and promote the color development of the inkjet pattern. Under the action of pushing away the ink, the glaze covering the surface of the pushed away ink is pushed away. In some embodiments, the chemical composition of the glaze includes, by mass percentage: SiO2: 61~65%, Al2O3: 19~23%, Fe2O3: 0.05~0.1%, TiO2: 0.05~0.1%, CaO: 0.1~0.5%, MgO: 0.1~0.5%, K2O: 3~4%, Na2O, 3.1~3.8%, ZrO2: 3.2~9.6%, and loss on ignition: 1.5~2%.
[0049] In some implementations, the raw material composition of the glaze includes, by mass percentage, 10-15% kaolin, 30-40% potassium feldspar, 20-30% sodium feldspar, 5-10% zirconium silicate, and 5-35% burnt clay.
[0050] Weigh each raw material according to the mineral composition of the glaze, mix it with sodium tripolyphosphate, sodium carboxymethyl cellulose and water, ball-mill evenly, sieve to remove iron, and obtain a glaze slurry. For example, the glaze slurry includes: in terms of mass percentage, 70% glaze mineral, 0.25% sodium tripolyphosphate, 0.15% sodium carboxymethyl cellulose, and 29.6% water. The glaze slurry has a sieve residue of ≤0.8wt% when passing through a 325-mesh sieve. When applying the glaze, water can be added to the glaze slurry to adjust the final desired glaze specific gravity.
[0051] The glaze can be applied by spraying. Preferably, the specific gravity of the glaze is 1.3-1.5 g / cm 3 , glaze application amount is 200~300 g / m 2 If the amount of glaze applied is too low, the glaze cannot completely cover the body, resulting in the base color and defects of the body not being covered, and the glaze's color-promoting effect will be affected. However, if the amount of glaze applied is too high, the glaze on the transparent line texture surface of the body cannot be effectively removed, and even the use of an adsorption roller cannot completely absorb the glaze on the transparent line texture surface, which will affect the imitation stone decorative effect of the ceramic rock slab.
[0052] The pattern is printed on the surface of the blank after the glaze is applied. That is, the pattern is printed on the surface of the blank after the glaze covering the transparent line texture position of the blank is removed. Ordinary ink can be printed to form the ink pattern. The texture and color of the inkjet printed pattern can be adaptively changed according to the needs. The pattern can be a decorative pattern. Optionally, the blank is dried before the inkjet printing pattern. The drying temperature can be 100~150℃.
[0053] The blank after the inkjet printing pattern is dried again. The drying temperature can be 100~150℃.
[0054] A protective glaze is applied to the surface of the blank after the inkjet printing pattern and drying. The function of the protective glaze is to improve the surface pollution resistance and wear resistance of the ceramic rock plate. The protective glaze commonly used in the art can be used.
[0055] The chemical composition of the protective glaze may include, by mass percentage, SiO2: 45-50%, Al2O3: 18-22%, Fe2O3: 0.1-1%, TiO2: 0.1-1%, CaO: 0.1-1%, MgO: 4-8%, BaO: 10-15%, ZnO: 2-5%, K2O: 4-8%, Na2O: 1-3%, and loss on ignition: 4-6%. Preferably, the chemical composition of the protective glaze includes, by mass percentage, SiO2: 45-50%, Al2O3: 18-22%, Fe2O3: 0.1-0.2%, TiO2: 0.1-0.2%, CaO: 0.1-0.5%, MgO: 4-6%, BaO: 10-13%, ZnO: 2-4%, K2O: 4-5%, Na2O: 1-2%, and loss on ignition: 4-6%.
[0056] In some implementations, the raw material composition of the protective glaze includes, by mass percentage, 50-60% potassium feldspar, 10-15% kaolin, 10-15% barium carbonate, 6-11% talc, 2-5% zinc oxide, and 10-15% quartz powder.
[0057] Weigh each raw material according to the mineral composition of the protective glaze, mix it with sodium tripolyphosphate, sodium carboxymethyl cellulose and water, ball-mill evenly, sieve to remove iron, and obtain a protective glaze slurry. For example, the protective glaze slurry includes: in terms of mass percentage, 70% protective glaze mineral, 0.25% sodium tripolyphosphate, 0.15% sodium carboxymethyl cellulose, and 29.6% water. The sieve residue of the protective glaze slurry passing through a 325-mesh sieve is ≤0.8wt%. When applying the protective glaze, water can be added to the protective glaze slurry to adjust the final required protective glaze specific gravity.
[0058] The protective glaze can be applied by spraying. Preferably, the specific gravity of the protective glaze is 1.3-1.6 g / cm 3 , glaze application amount is 400~500 g / m 2 .
[0059] The green body after applying the protective glaze is dried at a temperature of 100-150°C.
[0060] The dried green body is fired. It can be put into a kiln for firing. The firing temperature can be 1135~1160℃, and the firing time can be 60~80 minutes.
[0061] Polishing and grading into storage.
[0062] In summary, the present invention adopts a 3D digital spreading system to spread ordinary powder and transparent powder according to the layout design pattern, controls the spreading texture and thickness of the transparent powder, and then spreads the glaze through the spreading action of the ink through positioning inkjet printing to expose the transparent powder to form a transparent line texture, thereby obtaining a ceramic rock slab with imitation stone decorative effect.
[0063] During the research and development process, it was found that although the above method can be used to prepare a ceramic rock slab with a stone-like decorative effect, the specifications of the transparent line texture of the stone-like decorative effect are limited. If it is necessary to prepare a ceramic rock slab with a large area of transparent line texture, the above method will result in the glaze covering the transparent line texture position not being completely removed and remaining, which will affect the stone-like decorative effect. Preferably, a roller made of activated carbon fiber and with a surface engraved with the same pattern as the transparent line texture can be used to adsorb the glazed blank. Under the adsorption effect of the roller, the glaze covering the surface of the transparent line texture of the blank is completely adsorbed, thereby exposing the transparent line texture of the blank. The inventor used an ordinary roller in the research and development process. The ordinary roller was made of silicone and could not completely adsorb the glaze covering the surface of the transparent line texture of the blank, resulting in the inability to expose the transparent line texture formed by the transparent powder. That is to say, the present invention uses a roller made of activated carbon fiber material and carves a pattern on the surface of the roller that is the same as the transparent line texture of the blank. Through the combination of the prying effect of the ink and the adsorption effect of the adsorptive roller, the glaze on the surface of the transparent powder is completely pried open and adsorbed, so that the transparent line texture formed by the transparent powder is clearly exposed. In order to make the adsorption effect more excellent, it is preferred to use ultra-fine activated carbon fiber material. For example, the activated carbon fiber material is a nano carbon fiber material. Compared with the use of ink prying or roller adsorption alone, the present invention can combine inkjet printing and roller adsorption to prepare a ceramic rock slab with a smooth surface, a large area of transparent line texture and a stone-like decorative effect.
[0064] As an advantage, a centering device can be provided to further adjust the distance between the blank and the adsorption roller. By adjusting the distance between the blank and the adsorption roller, the position of the glaze adsorbed by the roller and the position of the transparent powder texture are highly consistent.
[0065] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0066] Example 1
[0067] A method for preparing a ceramic rock plate with imitation stone decorative effect comprises the following steps:
[0068] Step 1. Prepare transparent powder. The raw material composition of the transparent powder includes, by mass percentage, 10% clay, 30% quartz, and 60% boron frit. The chemical composition of the boron frit includes, by mass percentage, SiO2: 62%, Al2O3: 6%, Fe2O3: 0.04%, TiO2: 0.03%, CaO: 2%, MgO: 2%, K2O: 7%, Na2O: 3%, and B2O3: 17.93%. The thermal expansion coefficient of the transparent powder at 40-600°C is 7.6×10 -6 / K.
[0069] Step 2. Prepare ordinary powder. The chemical composition of the ordinary powder includes, by mass percentage: ignition loss: 4.87%, SiO2: 65%, Al2O3: 23%, Fe2O3: 0.4%, TiO2: 0.03%, CaO: 0.4%, MgO: 0.3%, K2O: 3%, Na2O: 3%. The thermal expansion coefficient of the ordinary powder at 40-600°C is 8.0×10 -6 / K.
[0070] Step 3. Prepare the common powder and transparent powder into a blank with transparent line texture according to the layout design. Extract the transparent line texture according to the layout design to obtain Figure 1 The transparent line extraction effect diagram shown in the figure is then vectorized to obtain a vector file for the extracted transparent line texture, and the vector file is loaded into the 3D cloth system. According to the vector file, transparent powder is distributed at the position corresponding to the transparent line texture and ordinary powder is distributed at the position other than the transparent line texture, and then pressed and formed to prepare a blank with transparent line texture. Specifically, ordinary powder and transparent powder stored in different hoppers are first transported to different micro-cylinder gates, and then the distributor applies the ordinary powder in the micro-cylinder gate on the cloth belt according to the vector file, and then the ordinary powder is spread at the position where the transparent line texture is required to be presented according to the vector file, and then the transparent powder is spread at the spread position, and finally the powder after the distribution is completed is transported to the press by the feeding belt and pressed and formed to obtain a blank with an ordinary powder layer and a transparent powder layer. The cloth thickness of the transparent powder can be controlled by controlling the spreading depth. The spreading depth is 2~4mm. The grayscale of the transparent line texture pattern of the vector file is 20~30%. The chemical composition of the green body includes, by mass percentage, loss on ignition: 1%, SiO2: 72%, Al2O3: 7%, Fe2O3: 0.4%, TiO2: 0.03%, CaO: 0.4%, MgO: 0.3%, K2O: 7%, Na2O: 2%, and B2O3: 9.87%.
[0071] Step 4. Inkjet print the push-out ink at the position corresponding to the transparent line texture on the surface of the blank. The raw material composition of the push-out ink includes, by mass percentage, organic solvent: 65%, hydrophobic coupling agent: 2%, dispersant: 5%, push-out glaze powder: 28%. The chemical composition of the push-out glaze powder includes, by mass percentage, loss on ignition: 4%, SiO2: 44%, Al2O3: 24%, BaO: 5%, CaO: 5%, MgO: 2%, K2O: 3%, NaO: 4%, B2O3: 3%, SrO: 3%, ZnO: 4%. The pattern grayscale of the inkjet push-out ink pattern is 100%.
[0072] Step 5. Apply glaze to the surface of the blank after the ink is removed by inkjet printing. The chemical composition of the glaze includes, by mass percentage: SiO2: 63%, Al2O3: 21.8%, Fe2O3: 0.05%, TiO2: 0.05%, CaO: 0.3%, MgO: 0.3%, K2O: 3%, Na2O: 3.5%, ZrO2: 6.5%, loss on ignition: 1.5%. The glaze is applied by spraying. The specific gravity of the glaze is 1.4g / cm 3 , glaze application amount is 250 g / m 2 .
[0073] Step 6. Dry the glazed body.
[0074] Step 7. Inkjet print patterns on the surface of the dried blank.
[0075] Step 8. Continue drying the blank after the inkjet printing pattern.
[0076] Step 9. Apply protective glaze on the surface of the body after re-drying. The chemical composition of the protective glaze includes, by mass percentage: SiO2: 48.5%, Al2O3: 21%, Fe2O3: 0.1%, TiO2: 0.1%, CaO: 0.3%, MgO: 5%, BaO: 12%, ZnO: 3%, K2O: 4%, Na2O: 1%, loss on burning: 5%. The protective glaze is applied by spraying. The specific gravity of the protective glaze is 1.5 g / cm 3 , glaze weight is 450 g / m 2 .
[0077] Step 10. Continue to dry the body after applying the protective glaze.
[0078] Step 11. The dried green body is put into the kiln for firing at a temperature of 1145°C and a firing time of 70 minutes.
[0079] Step 12. Polish, wax and pack.
[0080] Figure 2 This is the effect diagram of the blank fabric of Example 1. It can be seen that the blank fabric effect diagram includes a base other than the transparent line texture formed by the applied transparent powder 2 and the transparent line texture formed by the applied ordinary powder 1. Figure 3 This is a brick surface effect diagram of the ceramic rock plate with imitation stone decorative effect prepared in Example 1. It can be seen that the ceramic rock plate with imitation stone decorative effect prepared in Example 1 has a transparent line texture and a flat surface without pinholes.
[0081] Example 2
[0082] A method for preparing a ceramic rock plate with imitation stone decorative effect comprises the following steps:
[0083] Step 1. Prepare transparent powder. The raw material composition of the transparent powder includes, by mass percentage, 10% clay, 30% quartz, and 60% boron frit. The chemical composition of the boron frit includes, by mass percentage, SiO2: 62%, Al2O3: 6%, Fe2O3: 0.04%, TiO2: 0.03%, CaO: 2%, MgO: 2%, K2O: 7%, Na2O: 3%, and B2O3: 17.93%. The thermal expansion coefficient of the transparent powder at 40-600°C is 7.6×10 -6 / K.
[0084] Step 2. Prepare ordinary powder. The chemical composition of the ordinary powder includes, by mass percentage: ignition loss: 4.87%, SiO2: 65%, Al2O3: 23%, Fe2O3: 0.4%, TiO2: 0.03%, CaO: 0.4%, MgO: 0.3%, K2O: 3%, Na2O: 3%. The thermal expansion coefficient of the ordinary powder at 40-600°C is 8.0×10 -6 / K.
[0085] Step 3. Prepare the common powder and transparent powder into a blank with transparent line texture according to the layout design. According to the layout design, the transparent line texture is extracted to obtain the transparent line extraction effect diagram, and then the extracted transparent line texture is vectorized to obtain a vector file, and the vector file is loaded into the 3D distribution system. According to the vector file, transparent powder is distributed at the position corresponding to the transparent line texture and common powder is distributed at the position other than the transparent line texture, and then pressed and formed to prepare a blank with transparent line texture. Specifically, the common powder and transparent powder stored in different hoppers are first transported to different micro-cylinder gates, and then the distributor applies the common powder in the micro-cylinder gate on the distribution belt according to the vector file, and then the common powder is spread at the position where the transparent line texture is required according to the vector file, and then the transparent powder is spread at the spread position, and finally the powder after the distribution is completed is transported to the press by the feeding belt and pressed and formed to obtain a blank with a common powder layer and a transparent powder layer. The distribution thickness of the transparent powder can be controlled by controlling the spreading depth. The spreading depth is 2~4mm. The grayscale of the transparent line texture pattern of the vector file is 20-30%. The chemical composition of the blank includes, by mass percentage: loss on ignition: 1%, SiO2: 72%, Al2O3: 7%, Fe2O3: 0.4%, TiO2: 0.03%, CaO: 0.4%, MgO: 0.3%, K2O: 7%, Na2O: 2%, B2O3: 9.87%.
[0086] Step 4. Inkjet print the push-out ink at the position corresponding to the transparent line texture on the surface of the blank. The raw material composition of the push-out ink includes, by mass percentage, organic solvent: 65%, hydrophobic coupling agent: 2%, dispersant: 5%, push-out glaze powder: 28%. The chemical composition of the push-out glaze powder includes, by mass percentage, loss on ignition: 4%, SiO2: 44%, Al2O3: 24%, BaO: 5%, CaO: 5%, MgO: 2%, K2O: 3%, NaO: 4%, B2O3: 3%, SrO: 3%, ZnO: 4%. The pattern grayscale of the inkjet push-out ink pattern is 100%.
[0087] Step 5. Apply glaze to the surface of the blank after the ink is removed by inkjet printing. The chemical composition of the glaze includes, by mass percentage: SiO2: 63%, Al2O3: 21.8%, Fe2O3: 0.05%, TiO2: 0.05%, CaO: 0.3%, MgO: 0.3%, K2O: 3%, Na2O: 3.5%, ZrO2: 6.5%, loss on ignition: 1.5%. The glaze is applied by spraying. The specific gravity of the glaze is 1.4g / cm 3 , glaze application amount is 250 g / m 2 .
[0088] Step 6. Use a roller made of activated carbon fiber to absorb the glaze on the surface of the transparent powder. Carve a pattern on the surface of the roller with the same texture as the transparent lines, and absorb the glaze, so that the transparent powder is clearly and completely exposed.
[0089] Step 7. Dry the green body after being adsorbed by the roller.
[0090] Step 8. Inkjet print patterns on the surface of the dried blank.
[0091] Step 9. Continue drying the blank after the inkjet printing pattern.
[0092] Step 10. Apply protective glaze on the surface of the body after re-drying. The chemical composition of the protective glaze includes, by mass percentage: SiO2: 48.5%, Al2O3: 21%, Fe2O3: 0.1%, TiO2: 0.1%, CaO: 0.3%, MgO: 5%, BaO: 12%, ZnO: 3%, K2O: 4%, Na2O: 1%, loss on burning: 5%. The protective glaze is applied by spraying. The specific gravity of the protective glaze is 1.5 g / cm 3 , glaze weight is 450 g / m 2 .
[0093] Step 11. Continue to dry the body after applying the protective glaze.
[0094] Step 12. The dried green body is put into the kiln for firing at a temperature of 1145°C and a firing time of 70 minutes.
[0095] Step 13. Polish, wax and pack.
[0096] Comparative Example 1
[0097] The method is basically the same as Example 2, except that step 6 is omitted.
[0098] Figure 4 The figure is a picture of the ink-pushing effect of comparative example 1 (left) and a picture of the combined effect of ink-pushing and roller adsorption of embodiment 2 under the same design layout conditions (right). It can be seen that in comparative example 1, since the area of the ink-pushing is limited, the surface glaze layer on the transparent line texture surface formed by the transparent powder cannot be completely pried away, resulting in the inability to expose the transparent line texture well. On the contrary, through the combination of the prying effect of the ink-pushing and the roller adsorption, the transparent powder is exposed more comprehensively, and the transparent line texture formed has a larger area.
[0099] Comparative Example 2
[0100] It is basically the same as Example 2, except that step 4 is omitted, that is, the glaze is directly applied to the surface of the blank instead of inkjet printing and spreading the ink.
[0101] Similarly, in Comparative Example 2, the roller cannot completely absorb the glaze on the surface of the transparent line texture, resulting in only a small area of the transparent line texture being exposed.
[0102] Comparative Example 3
[0103] It is basically the same as Example 2, except that the raw material composition of the transparent powder includes, by mass percentage, 10% clay, 10% quartz, and 80% boron frit.
[0104] Figure 5 This is a brick surface effect diagram of the ceramic rock board prepared in Example 1. This Example 3 uses a large amount of boron frit. Due to the strong melting effect of the boron frit, the temperature of the transparent powder is low, the gas in the blank is not easy to be discharged, and pinholes appear.
Claims
1. A method for preparing a ceramic rock plate with a large area of transparent line texture and imitation stone decorative effect, characterized in that: The preparation method comprises: Step (1) ordinary powder and transparent powder are prepared into a blank with transparent line texture according to the layout design; the chemical composition of the ordinary powder includes, by mass percentage, loss on ignition: 3-6%, SiO2: 60-70%, Al2O3: 19-25%, Fe2O3: 0.2-0.6%, TiO2: 0.01-0.1%, CaO: 0.2-0.6%, MgO: 0.1-1%, K2O: 2-5%, Na2O: 2-5%; the raw material of the transparent powder is The material composition includes, by mass percentage, 10-15% clay, 20-40% quartz, and 45-70% boron frit; wherein the chemical composition of the boron frit includes, by mass percentage, SiO2: 62-68%, Al2O3: 5-10%, Fe2O3: 0.02-0.05%, TiO2: 0.01-0.05%, CaO: 1-3%, MgO: 1-3%, K2O: 5-10%, Na2O: 1-5%, and B2O3: 15-20%; Step (2) inkjet printing a dispersing ink on the surface of the blank corresponding to the transparent line texture position; the raw material composition of the dispersing ink includes, by mass percentage, 65-75% of an organic solvent, 2-4% of a hydrophobic coupling agent, 5-10% of a dispersant, and 20-35% of a dispersing glaze powder; wherein the chemical composition of the dispersing glaze powder includes, by mass percentage, ignition loss: 3.5-4.5%, SiO2: 43-46%, Al2O3: 24-26%, BaO: 5-6%, CaO: 4-6%, MgO: 2-3%, K2O: 2.5-3.5%, NaO: 3.5-4.5%, B2O3: 3-4%, SrO: 3-4%, and ZnO: 3-4%; Step (3) applying glaze to the surface of the blank after the ink is removed by inkjet printing; Step (4) inkjet printing a pattern on the surface of the glazed body; before inkjet printing the pattern on the surface of the glazed body, using a roller made of activated carbon fiber and having a pattern carved on the surface that is the same as the transparent line texture to adsorb the glazed body; Step (5) applying protective glaze on the surface of the blank after the inkjet printing pattern; Step (6) is to fire and polish the green body after applying the protective glaze to obtain the ceramic rock plate with a large area of transparent line texture and imitation stone decorative effect.
2. The method according to claim 1, characterized in that The chemical composition of the glaze includes, by mass percentage, SiO2: 61~65%, Al2O3: 19~23%, Fe2O3: 0.05~0.1%, TiO2: 0.05~0.1%, CaO: 0.1~0.5%, MgO: 0.1~0.5%, K2O: 3~4%, Na2O, 3.1~3.8%, ZrO2: 3.2~9.6%, and loss on ignition: 1.5~2%.
3. The method according to claim 1, characterized in that The glaze is applied by spraying; the specific gravity of the glaze is 1.3-1.5 g / cm 3 , glaze application amount is 200~300 g / m 2 .
4. The method according to claim 1, characterized in that: The chemical composition of the protective glaze includes, by mass percentage, SiO2: 45~50%, Al2O3: 18~22%, Fe2O3: 0.1~1%, TiO2: 0.1~1%, CaO: 0.1~1%, MgO: 4~8%, BaO: 10~15%, ZnO: 2~5%, K2O: 4~8%, Na2O: 1~3%, and loss on ignition: 4~6%.
5. The method according to claim 1, characterized in that The protective glaze is applied by spraying; the specific gravity of the protective glaze is 1.3-1.6 g / cm 3 , glaze application amount is 400~500 g / m 2 .
6. The method according to claim 1, characterized in that The firing temperature is 1135~1160℃, and the firing time is 60~80 minutes.
7. The method according to claim 1, characterized in that According to the layout design, transparent line texture is extracted, vector processing is performed on the extracted transparent line texture to obtain a vector file, the vector file is loaded into a 3D cloth system, transparent powder is distributed at positions corresponding to the transparent line texture and ordinary powder is distributed at positions other than corresponding to the transparent line texture according to the vector file, and then pressed and formed into a blank with transparent line texture.
8. A ceramic rock plate with a large area of transparent line texture and imitation stone decorative effect, characterized in that: The ceramic rock slab with imitation stone decorative effect and large-area transparent line texture is obtained according to the preparation method described in any one of claims 1 to 7.