High-rigidity slender tubes and their forming methods

By superimposing an inner stiffness layer and an outer structural layer, and combining specific laying and winding methods, the rigidity and straightness problems of high-rigidity composite slender tubes were solved, achieving efficient molding and high-quality composite slender tubes.

CN118423517BActive Publication Date: 2026-11-17HUBEI SANJIANG AEROSPACE GRP HONGYANG ELECTROMECHANICAL
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410535696.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2026-11-17
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

Existing technologies for molding high-rigidity composite slender tubes suffer from problems such as insufficient structural rigidity, low molding efficiency, and fiber bending deformation, making it difficult to meet the requirements of high rigidity and straightness.

Method used

The design employs a tubular structure with an inner stiffness layer and an outer structural layer. The material of the inner stiffness layer is laid along the length direction, while the material of the outer structural layer is wound around the inner stiffness layer. By combining axial lay-up and spiral winding layer laying methods and controlling fiber tension and curing temperature, the overall stiffness and straightness of the material are improved.

Benefits of technology

The straightness and weight of the high-rigidity slender tube met the requirements, the deflection test met the usage requirements, and the appearance quality and dimensional accuracy met the design standards, thus improving the molding efficiency and structural strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118423517B_ABST
    Figure CN118423517B_ABST
Patent Text Reader

Abstract

This disclosure relates to the field of composite material technology, and more particularly to a high-stiffness slender tube and its forming method. A high-stiffness slender tube is characterized by comprising an inner stiffness layer and an outer structural layer, wherein the inner stiffness layer and the outer structural layer are stacked to form a tubular structure, wherein a pre-set material of the inner stiffness layer is laid along the length direction; and a pre-set material of the outer structural layer is wound around the inner stiffness layer. By implementing the technical solution of this disclosure, the inner stiffness layer provides overall structural stiffness, meeting the product's structural weight and load-bearing deflection requirements, while the outer structural layer meets the product's dimensional accuracy and appearance quality requirements, and also provides structural constraint and load-bearing capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of composite materials technology, and more particularly to a high-rigidity slender tube and a molding method thereof. Background Technology

[0002] Carbon fiber composites possess advantages such as high specific strength and specific stiffness, corrosion resistance, and customizable structural properties, leading to their increasingly widespread application in lightweight structures. As the demands for lightweighting become more stringent, significant challenges are being placed on the structural design and molding processes of composite materials, with high-stiffness composite slender tubes falling into this category.

[0003] The internal shape of this composite tube involves assembly relationships and requires high precision, thus necessitating mold forming. Common forming methods often suffer from limited winding angles, resulting in insufficient structural rigidity in the formed product. Other issues include uneven thickness or challenging localized structures; or low forming efficiency. For annular structures, the lack of winding tension allows fibers to easily bend and deform, leading to poor performance. Ensuring high rigidity and straightness in slender tubes within a given wall thickness or weight presents significant challenges for composite material structure design and molding quality control. Summary of the Invention

[0004] This disclosure aims to address at least one of the technical problems existing in the prior art or related technologies.

[0005] Therefore, in a first aspect of this disclosure, a high-stiffness slender tube is provided, comprising an inner stiffness layer and an outer structural layer, wherein the inner stiffness layer and the outer structural layer are stacked to form a tubular structure, wherein...

[0006] The pre-set material of the inner stiffness layer is laid along the length direction;

[0007] The pre-set material of the outer structural layer is wound and arranged along the inner stiffness layer.

[0008] In one feasible implementation, the inner stiffness layer comprises an axial layup and a helical winding layer, wherein the axial layup is disposed on the helical winding layer, wherein...

[0009] The axial layup includes a first axial layup and multiple second axial layups, wherein the second axial layups are laid along the extension direction of the tubular structure, and the laying direction of the first axial layup is perpendicular to the laying direction of the second axial layup.

[0010] In one feasible implementation, the ratio of the number of the second axial layup to the number of the first axial layup is 39 to 1.

[0011] In one feasible implementation, the outer structural layer includes circumferential fibers and multiple helical fibers, the circumferential fibers being in contact with the inner stiffness layer.

[0012] In one feasible implementation, the thickness of the circumferential fiber is set to 1 mm, and the thickness of the helical fiber is set to 0.5 mm, wherein...

[0013] The winding tension of the circumferential fiber is set to 45N to 50N, and the winding tension of the helical fiber decreases by 2N per layer compared to the winding tension of the circumferential fiber.

[0014] A second aspect of this disclosure provides a method for forming a high-stiffness slender tube, comprising the following steps:

[0015] The inner stiffness layer is formed by first spirally winding the core mold surface for one cycle, then cleaning the surface and performing axial lay-up. During axial lay-up, multiple layers of prepreg are laid on the spirally wound layer along the 0° direction, followed by a layer of prepreg along the 90° direction. The lay-up is then vacuum-heated and pre-pressed, and this process is repeated three times before curing. After the inner stiffness layer has cured, the outer shape of the inner stiffness layer is milled to ensure dimensional accuracy.

[0016] After the inner stiffness layer is processed, the mandrel is transferred to a fiber winding machine to form the outer structural layer. Carbon fiber impregnated with epoxy resin is used to wind the outer structural layer. The curing temperature used for winding the outer structural layer is lower than that used for the resin system of the inner stiffness layer. During winding, circumferential fibers are wound first, followed by spiral fibers. After the outer structural layer is wound, the mandrel is transferred to an oven and cured under vacuum in a vertically suspended state.

[0017] After the outer circumferential layer is cured, the product length is processed with the core mold as a reference, and the molded product is then demolded.

[0018] In one feasible implementation, the inner stiffness layer has a thickness of 12.5 mm, and the outer structural layer has a thickness of 1.5 mm, both molded from M40J carbon fiber and high-temperature resistant epoxy resin.

[0019] The spiral winding is performed on the surface of the mandrel at a winding angle of ±45°, and the thickness of the spiral winding is set to 0.4 mm.

[0020] In one feasible implementation, in the step of forming the inner stiffness layer, the pre-compression pressure is set to 0.6MPa±0.1MPa, and the heating temperature is 80℃±10℃.

[0021] In one feasible implementation, the curing pressure of the inner stiffness layer is set to 0.6MPa±0.1MPa, and the curing temperature is set to less than or equal to 195℃.

[0022] In one feasible implementation, the curing temperature of the outer structural layer is less than or equal to 180°C.

[0023] Compared to existing technologies, this disclosure offers at least the following advantages: This disclosure constructs a tubular structure by stacking an inner stiffness layer 1 and an outer structural layer 2. The inner stiffness layer provides overall structural stiffness, meeting the product's structural weight and load-bearing deflection requirements, while the outer structural layer meets the product's dimensional accuracy and appearance quality requirements. Furthermore, the outer structural layer 2 provides structural constraints and load-bearing capacity. Specifically, the pre-set material of the inner stiffness layer 1 is laid along its length, while the pre-set material of the outer structural layer 2 is wound around the inner stiffness layer 1, ensuring that the straightness and weight of this disclosure meet requirements, and that deflection tests meet usage requirements. Attached Figure Description

[0024] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate embodiments consistent with this disclosure and, together with the description, serve to explain the principles of this disclosure.

[0025] To more clearly illustrate the technical solutions in the embodiments of this disclosure or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of exemplary embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0027] Figure 1 This is a schematic diagram of the cross-sectional structure of the runway-shaped section disclosed herein;

[0028] Figure 2 This is a schematic diagram of the runway-shaped cross-sectional structure disclosed herein;

[0029] Figure 3 This is a schematic diagram of the cross-sectional structure of the circular section disclosed herein;

[0030] Figure 4 This is a schematic diagram of the circular cross-section structure disclosed herein;

[0031] Figure 5 This is a structural schematic diagram of the core mold mounting method disclosed herein;

[0032] Figure 6 This is a schematic diagram of the axial laying direction of this disclosure;

[0033] Figure 7This is a schematic diagram illustrating the circumferential laying direction of this disclosure.

[0034] in, Figures 1 to 7 The correspondence between the reference numerals and component names in the attached drawings is as follows:

[0035] 1-Inner stiffness layer; 2-Outer structural layer; 3-Core mold; 4-Support. Detailed Implementation

[0036] To better understand the above-mentioned objectives, features, and advantages of this disclosure, the solutions disclosed herein will be further described below. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other.

[0037] Numerous specific details are set forth in the following description in order to provide a full understanding of this disclosure, but this disclosure may also be implemented in other ways different from those described herein; obviously, the embodiments in the specification are only some, and not all, of the embodiments of this disclosure.

[0038] Currently, wet winding molding is used. This involves impregnating dry fibers with resin using a fiber winding machine, then winding them onto a mandrel and curing them. This fully automated molding method is highly efficient and produces consistent quality. However, its drawback is the limited winding angle, which results in insufficient structural rigidity in the molded product, failing to meet deflection requirements under load.

[0039] Prepreg winding. This method involves installing a mandrel on a winding machine, rotating the mandrel to continuously wind the prepreg onto the mandrel until the required thickness is achieved, and then removing the mandrel with the prepreg and allowing it to cure. This method is highly efficient, but it is more challenging for products with uneven thickness or localized thickening. Furthermore, for tapered mandrels, the unfolded shape is fan-shaped, while the fibers of the prepreg are parallel. Therefore, it is impossible to guarantee that the fiber direction of the prepreg is consistent with the generatrix direction. The more layers wound, the greater the fiber direction deviation, affecting the structural mechanical properties of the product.

[0040] Prepreg lay-up molding involves impregnating unidirectional fibers with resin to form a prepreg, which is then laid on a mold and cured. This molding method can produce complex structures with irregular shapes or varying thicknesses, but its molding efficiency is relatively low. For ring structures, or when laying prepreg in a circumferential direction, the discontinuous fibers prevent the application of tension, causing the fibers to easily bend and deform under pressure during curing, resulting in poor performance. Furthermore, requiring the molded slender tubes to meet high stiffness and straightness requirements under certain wall thickness or weight conditions presents significant challenges for composite material structural design and molding quality control. Against this technological backdrop, targeted structural design for such high-rigidity composite slender tubes is needed, along with breakthroughs in molding processes.

[0041] Based on this, the present disclosure provides a high-rigidity slender tube, which is formed by stacking an inner stiffness layer 1 and an outer structural layer 2 to form a tubular structure. The inner stiffness layer provides overall structural stiffness, meeting the product's structural weight and load-bearing deflection requirements, while the outer structural layer meets the product's dimensional accuracy and appearance quality requirements, and the outer structural layer 2 can provide structural constraints and load-bearing capacity. The pre-set material of the inner stiffness layer 1 is laid along the length direction, while the pre-set material of the outer structural layer 2 is wound around the inner stiffness layer 1, ensuring that the straightness and weight of the present disclosure meet the requirements, and the deflection test meets the usage requirements.

[0042] The high-rigidity slender tube and its forming method will be described in detail below through specific embodiments:

[0043] Reference Figures 1 to 7 As shown, the first aspect of this disclosure provides a high-rigidity slender tube, including an inner stiffness layer 1 and an outer structural layer 2. The inner stiffness layer 1 and the outer structural layer 2 are stacked to form a tubular structure. A preset material of the inner stiffness layer 1 is laid along the length direction; a preset material of the outer structural layer 2 is wound around the inner stiffness layer 1.

[0044] This disclosure utilizes an inner stiffening layer 1 and an outer structural layer 2 to form a tubular structure. The inner stiffening layer provides overall structural stiffness, meeting the product's structural weight and load-bearing deflection requirements, while the outer structural layer meets the product's dimensional accuracy and appearance quality requirements. Furthermore, the outer structural layer 2 provides structural constraint and load-bearing capacity. The pre-set material of the inner stiffening layer 1 is laid along its length, while the pre-set material of the outer structural layer 2 is wound around the inner stiffening layer 1, ensuring that the straightness and weight of this disclosure meet requirements, and that deflection tests meet usage requirements. The pre-set materials described in this disclosure are determined based on the type and application of the slender tube, such as M40J carbon fiber and high-temperature resistant epoxy resin.

[0045] In some embodiments, the inner stiffness layer 1 of this disclosure includes an axial layup and a helical winding layer. The axial layup is disposed on the helical winding layer. The axial layup includes a first axial layup and multiple second axial layups. The second axial layups are laid along the extension direction of the tubular structure. The laying direction of the first axial layup is perpendicular to the laying direction of the second axial layup.

[0046] In this embodiment, during layup, as follows Figure 6 and 7 As shown, the prepreg of the second axial layup is along the axial direction ( Figure 6 Laying in the 0° direction. Specifically, the ratio of multiple layers of second axial layup to first axial layup can be set to 8 to 40 layers per layer, with an additional first axial layup (in the 0° direction). Figure 7(In the 90° direction), thus increasing structural strength. During the layup process, pre-compression is performed every 3 to 6 mm. Pre-compression can be vacuum pre-compression or vacuum + external pressure, and the pre-compression pressure is generally controlled within 0.8 MPa. After the layup reaches the predetermined thickness, it is heated and pressurized in an autoclave for curing. During curing, it should be placed vertically to reduce the product's deflection caused by the weight of the mandrel. Furthermore, the layup ratio of the second axial layup to the first axial layup is 39:1, that is, after every 39 layers of the second axial layup, one layer of the first axial layup is added, making the structure of the second axial layup more compact, while the first axial layup can change the stress of the second axial layup to further improve the structural strength of the inner stiffness layer.

[0047] In some embodiments, the outer structural layer 2 includes circumferential fibers and multilayer helical fibers, with the circumferential fibers in contact with the inner stiffness layer 1. The circumferential fiber winding enhances the strength and lightness of this disclosure, while the helical fibers wound at ±45° helical angles contribute to the mechanical properties, fatigue resistance, and good impact resistance of this disclosure. The circumferential fibers and multilayer helical fibers significantly improve the structural strength of this disclosure.

[0048] In some embodiments, the thickness of the circumferential fiber is set to 1 mm, and the thickness of the helical fiber is set to 0.5 mm, wherein the winding tension of the circumferential fiber is set to 45 N to 50 N, and the winding tension of the helical fiber decreases by 2 N per layer compared to the winding tension of the circumferential fiber.

[0049] In this embodiment, the thickness of the circumferential fiber is set to 1 mm, and the thickness of the helical fiber is set to 0.5 mm. The winding tension of the circumferential fiber is set to 45 N to 50 N, and the winding tension of the helical fiber decreases by 2 N per layer compared to the winding tension of the circumferential fiber. This 2 N decrease in winding tension per layer compared to the circumferential fiber ensures the strength and bonding strength of the fiber winding and avoids problems such as fiber breakage and excessive deformation. Simultaneously, by controlling the fiber tension, the quality and efficiency of fiber winding can also be guaranteed.

[0050] A second aspect of this disclosure provides a method for forming a high-stiffness slender tube, comprising the following steps:

[0051] The inner stiffness layer 1 is formed by first spirally winding it on the surface of the core mold 3 for one cycle. After winding, the surface is cleaned and axial lay-up is performed. During axial lay-up, multiple layers of prepreg are laid on the spirally wound layer along the 0° direction, and then a layer of prepreg is laid along the 90° direction. The lay-up is then vacuum-heated and pre-pressed. After three lay-up and pre-pressing processes, it is cured. After the inner stiffness layer 1 is cured, the outer shape of the inner stiffness layer 1 is milled to ensure the dimensional accuracy of the inner stiffness layer 1.

[0052] After the inner stiffness layer 1 is processed, the mandrel 3 is transferred to the fiber winding machine. Carbon fiber impregnated epoxy resin is used to wind and form the outer structural layer 2. The curing temperature of the outer structural layer 2 is lower than that of the resin system used to form the inner stiffness layer 1. During winding, the circumferential fibers are wound first, and then the spiral fibers are wound. After the outer structural layer 2 is wound, the mandrel 3 is transferred to the oven and cured under vacuum in a vertically suspended state.

[0053] After the outer circumferential layer is cured, the product length is processed with the core mold 3 as the reference, and the molded product is demolded.

[0054] The slender tube structure disclosed herein consists of an inner stiffening layer and an outer structural layer. The inner stiffening layer 1 primarily provides axial stiffness to the slender tube, meeting its deflection requirements under service loads. The reinforcing material of the inner stiffening layer 1 should be high-modulus fibers. To prevent splitting of the inner fibers during end-face machining, a layer of fibers is spirally wound around the surface of the inner stiffening layer 1. The outer structural layer 2 is formed by circumferential and spiral winding of fibers to circumferentially fix and constrain the inner stiffening layer 1, while also meeting dimensional accuracy requirements and providing a certain structural load-bearing capacity. The reinforcing material of the outer structural layer 2 should be high-strength fibers or high-modulus fibers consistent with those of the inner stiffening layer. The specific materials and thickness of the product are selected after calculation based on factors such as weight, load, support location, material properties, and deflection index.

[0055] During product molding, an inner stiffness layer 1 is formed on a core mold 3. The dimensional accuracy of the core mold 3 meets the internal shape accuracy requirements of the product. The axial cutting position is determined based on the dimensions of the core mold 3 to meet the product size and length requirements.

[0056] To improve the stiffness of the material, the inner stiffness layer mainly uses unidirectional carbon fiber prepreg along its length (e.g., Figure 6 The outer structural layer is primarily constructed using circumferential carbon fiber (e.g., in the 0° direction). To improve the material's strength, the outer structural layer mainly employs circumferential carbon fiber (e.g., in the 0° direction). Figure 7 (90°) Winding molding.

[0057] To improve interfacial bonding performance, the inner spiral winding layer of the inner stiffness layer 1 is co-cured with the prepreg. Pressure is applied during curing to meet the product's internal quality requirements. The curing temperatures of the resins used for the inner spiral winding layer and the prepreg should be consistent. The resin system should meet the product's ambient temperature requirements. After the inner stiffness layer 1 is cured, a machining allowance is left, and the outer structural layer 2 is formed after machining.

[0058] The outer structural layer 2 of this disclosure is formed by circumferential and helical winding of fiber-impregnated resin. The curing temperature of the resin system should not be higher than the curing temperature of the inner stiffness layer, and it should meet the environmental temperature requirements for the product's use. To facilitate product demolding and assembly, a tapered angle is provided within the product's internal shape.

[0059] Winding mandrel design and fabrication:

[0060] The layup mandrel 3 has an outer shape consistent with the inner shape of the slender tube of the composite material and can be equipped with a demolding device to facilitate product demolding. For ease of processing, the mandrel can be equipped with a product fixing device and processing reference. Since the mandrel 3 is a slender rod structure, its deflection under its own weight exceeds the usage requirements. To meet the straightness requirements of the mandrel, the surface of the wound mandrel is formed by side milling.

[0061] Inner stiffness layer 1 forming:

[0062] When laying up the inner stiffness layer 1, allowances can be made for length and shape processing to facilitate adjustments to the product's appearance and improve product quality. Furthermore, to enhance the end-face processing quality, a fiber layer can be wound onto the mandrel 3 first. The resin matrix used for winding is determined primarily based on the product's temperature resistance and must have the same curing and operating temperature as the unidirectional fiber prepreg resin system. After winding, the inner stiffness layer is laid up. The raw material selected for the layup is carbon fiber unidirectional prepreg.

[0063] During layup, the prepreg is mainly laid along the axial direction (e.g., Figure 6 The 0° direction) layup is repeated every 8 to 40 layers, with an additional circumferential layer (e.g., ...). Figure 7 The layup (in the 90° direction) is specifically performed in this disclosure, with an additional circumferential layup layer added after every 39 layups. During the layup process, pre-compression is performed every 3-6 mm of layup, specifically every 4 mm of layup in this disclosure. Pre-compression can be performed using vacuum pre-compression or a combination of vacuum and external pressure, with the pre-compression pressure generally controlled below 0.8 MPa. After the layup reaches the predetermined thickness, it is heated and pressurized in an autoclave for curing. During curing, the product should be placed vertically to reduce product deflection caused by the weight of the mandrel.

[0064] After curing, the allowance of the inner stiffness layer 1 is machined according to the designed dimensions. To reduce or avoid machining deformation, the inner stiffness layer 1 is not demolded and is fixed on the core mold 3, and the shape is machined by side milling.

[0065] Outer structural layer molding:

[0066] After the inner stiffness layer 1 is processed, the outer structural layer 2 is circumferentially and helically wound and cured. The curing temperature should not exceed the curing temperature of the inner stiffness layer. In this disclosure, the outer structural layer 2 is specifically formed by circumferentially and helically wound and cured using fiber impregnated with resin. The shape is not further processed after winding, and the winding thickness is controlled to meet the product dimensional requirements.

[0067] Product processing and demolding:

[0068] After the outer structural layer 1 is wound and cured, the product length allowance is processed using the core mold 3 as a reference. The product is then demolded using a demolding device to obtain the final product.

[0069] In some embodiments, the slender tube of this disclosure has a racetrack-shaped cross section, an inner stiffness layer with a thickness of 12.5 mm, and an outer structural layer with a thickness of 1.5 mm. Both are molded from M40J carbon fiber and high-temperature resistant epoxy resin, thereby meeting the requirements of high strength, high stiffness, and straightness of this disclosure.

[0070] In some embodiments, the inner stiffness layer 1 is composed of a helical winding layer and an axial layup. First, a helical winding is performed on the mandrel surface at a winding angle of ±45° for one cycle, with machining allowances left at both ends of the product length during winding. The helical winding thickness is approximately 0.4 mm. After winding, the surface sludge is cleaned and pre-cured, followed by axial layup to improve interfacial bonding performance.

[0071] In some embodiments, machining allowances are left at both ends of the length during axial layup. 97% of the fibers are laid up in the 0° direction (axial) and 3% of the fibers are laid up in the 90° direction (circumferential). Vacuum heating and pre-compression is performed every 40 layers. During pre-compression, the layup is vacuumed, and the pressure is 0.6MPa±0.1MPa and the temperature is 80℃±10℃.

[0072] In some embodiments, during axial preloading of the ply, in order to improve the surface quality and dimensional accuracy of the ply, a contoured skin can be placed on the ply surface for uniform pressure application.

[0073] In some embodiments, after the inner stiffness layer 1 is laid up, such as Figure 5 As shown, after being vacuum-treated, it was placed vertically in an autoclave and heated and pressurized for curing. The curing pressure was 0.6MPa±0.1MPa, and the maximum curing temperature was 195℃.

[0074] In some embodiments, after the inner stiffness layer 1 has cured, its shape is milled to ensure dimensional accuracy, thus satisfying the requirements of the outer structural layer winding. The dimensional accuracy is controlled within ±0.1 mm, while ensuring straightness is less than or equal to 0.1 mm. During milling of the inner stiffness layer, to reduce the impact of clamping and machining stress on the straightness of the product, side-cutting is used. No length allowance is machined during this process.

[0075] In some embodiments, after the inner stiffness layer 1 is processed, the mandrel 3 is transferred to a fiber winding machine. The outer structural layer 1 is wound using M40J carbon fiber impregnated with epoxy resin. When winding the outer structural layer 1, a resin system with a curing temperature lower than that used for the inner stiffness layer is used. Simultaneously, the heat distortion temperature of the resin system used for the outer structural layer should meet the design operating temperature requirements, thereby improving the material's strength properties.

[0076] In some embodiments, during winding, a 1mm thick circumferential fiber is wound first, followed by a 0.5mm thick ±45° helical fiber. The tension of the first layer is controlled at 45N to 50N, decreasing by 2N with each subsequent layer.

[0077] In some embodiments, after the outer structural layer 1 is wound, the mold is transferred to an oven and vacuum-cured in a vertically suspended state, with a maximum curing temperature of 180°C. After the outer structural layers are cured, the product length allowance is processed based on the core mold. The product is then slowly ejected using a demolding backing block.

[0078] Inspect the product's external dimensions, straightness, internal mass, and weight, and conduct deflection tests under load conditions.

[0079] In this disclosure, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance; the term "multiple" refers to two or more unless otherwise expressly defined. The terms "install," "connect," "link," and "fix" should be interpreted broadly. For example, "connect" can be a fixed connection, a detachable connection, or an integral connection; "link" can be a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this disclosure according to the specific circumstances.

[0080] In the description of this disclosure, it should be understood that the terms "upper," "lower," "left," "right," "front," "rear," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this disclosure and simplifying the description, and do not indicate or imply that the device or unit referred to must have a specific orientation or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this disclosure.

[0081] In the description of this specification, the terms "one embodiment," "some embodiments," "specific embodiment," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of this disclosure. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0082] The above are merely preferred embodiments of this disclosure and are not intended to limit this disclosure. Various modifications and variations can be made to this disclosure by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure.

Claims

1. A method for forming a high-rigidity slender tube, characterized in that, Includes the following steps: The inner stiffness layer is formed by first spirally winding the core mold surface for one cycle, then cleaning the surface and performing axial lay-up. During axial lay-up, multiple layers of prepreg are laid on the spirally wound layer along the 0° direction, followed by a layer of prepreg along the 90° direction. The lay-up is then vacuum-heated and pre-pressed, and this process is repeated three times before curing. After the inner stiffness layer has cured, the outer shape of the inner stiffness layer is milled to ensure dimensional accuracy. After the inner stiffness layer is processed, the mandrel is transferred to a fiber winding machine to form the outer structural layer. Carbon fiber impregnated with epoxy resin is used to wind the outer structural layer. The curing temperature used for winding the outer structural layer is lower than that used for the resin system of the inner stiffness layer. During winding, circumferential fibers are wound first, followed by spiral fibers. After the outer structural layer is wound, the mandrel is transferred to an oven and cured under vacuum in a vertically suspended state. After the outer circumferential layer is cured, the product length is processed with the core mold as a reference, and the molded product is then demolded.

2. The method for forming a high-rigidity slender tube according to claim 1, characterized in that, The inner stiffness layer has a thickness of 12.5 mm, and the outer structural layer has a thickness of 1.5 mm. Both are molded using M40J carbon fiber and high-temperature resistant epoxy resin. The spiral winding is performed on the surface of the mandrel at a winding angle of ±45°, and the thickness of the spiral winding is set to 0.4 mm.

3. The method for forming a high-rigidity slender tube according to claim 1, characterized in that, In the step of forming the inner stiffness layer, the pre-compression pressure is set to 0.6MPa±0.1MPa, and the heating temperature is 80℃±10℃.

4. The method for forming a high-rigidity slender tube according to claim 1, characterized in that, The curing pressure of the inner stiffness layer is set to 0.6MPa±0.1MPa, and the curing temperature is set to less than or equal to 195℃.

5. The method for forming a high-rigidity slender tube according to claim 1, characterized in that, The curing temperature of the outer structural layer is less than or equal to 180°C.

Citation Information

Patent Citations

  • Preparation method of metal lining ring-shaped composite cylinder

    CN104476781A

  • Manufacturing method for glass steel pipeline in zero-degree winding manner

    CN105269828A

  • Forming method of structural part

    CN115709576A