A method for testing fiber dispersion in ECC material mixtures

By using a penetration resistance meter to detect the fiber dispersion in the ECC material mixture, the problem of inaccurate fiber dispersion detection in the existing technology is solved, ensuring the performance of the ECC material and ensuring the safety of the construction site.

CN118443914BActive Publication Date: 2024-10-08HUADIAN JINSHAJIANG UPSTREAM HYDROPOWER DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410645422.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-08
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

The existing technology lacks an effective method to accurately detect the dispersion of fibers in the ECC material mixture, resulting in unsafe construction site operations and the inability to ensure the uniformity and high toughness of the material.

Method used

A penetration resistance meter is used to detect fiber dispersion. By recording the water addition time and the penetration pressure test after vibration of the vibration table, the fiber dispersion deviation rate is calculated to ensure the uniformity of the fiber in the mixture.

Benefits of technology

It achieves accurate detection of fiber dispersion in the ECC material mixture, ensures the mechanical properties and durability of the material, and provides real-time feedback and operational safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118443914B_ABST
    Figure CN118443914B_ABST
Patent Text Reader

Abstract

The present invention provides a method for detecting fiber dispersion in ECC material mixtures. The method uses a penetration resistance instrument to perform at least three penetration resistance tests on a prepared ECC mixture specimen with reference to the concrete mixture setting time test in the existing specification, and the test is completed before the mixture of the test specimen begins to set; and the fiber dispersion deviation rate σ in each test is calculated. i , and then calculate the fiber dispersion deviation rate σ in at least three tests i The average value is used to determine the uniformity of fiber dispersion in the mixture. The lower the average value of the deviation rate, the more uniform the fiber dispersion in the mixture. The present invention detects the uniformity of fiber dispersion in the freshly mixed stage of ECC materials. Compared with other testing methods, the present invention is scientific, convenient, timely and effective, and provides a technical basis for optimizing the ECC mixing process and improving material performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cement concrete materials, and in particular to a method for detecting fiber dispersion in ECC material mixtures. Background Art

[0002] ECC (Engineered Cementitious Composite) is an engineering cement-based composite material (also known as fiber-reinforced cement-based composite material or high-ductility cement-based composite material, etc.), which was successfully developed by Professor Victor C. Li of the University of Michigan in the United States in the 1990s. It even has tensile strengthening properties similar to those of metal materials, and its ultimate tensile strain can reach 5% to 6%, which is almost equivalent to the plastic deformation capacity of steel. It is a cement-based composite material that is deformable like metal. The compressive strength of ECC is similar to that of ordinary concrete, and its compressive elastic modulus is low, but its compressive deformation capacity is much greater than that of ordinary concrete. In addition, its fire resistance and durability have also been proven to exceed those of ordinary concrete. In view of the excellent performance of ECC materials, many domestic teams have also carried out related research and applications.

[0003] As a cement-based composite material with high toughness, ECC mainly uses PVA (high-strength and high-modulus polyvinyl alcohol) or PE (ultra-high molecular weight polyethylene) artificial synthetic fibers. Based on the fiber reinforcement mechanism at the microscopic level, it bends instead of breaking when subjected to huge pressure. ECC has a large ability to absorb energy, so it can significantly improve the seismic performance of concrete structures and can be used for earthquake-resistant structures, impact-resistant structures, structural crack control and damage-resistant engineering structures.

[0004] From the material composition, the raw materials of ECC include cement, mineral admixtures, fine sand, artificial synthetic fibers, functional additives and water. The commonly used PVA fiber volume content is usually 2% (by mass, the fiber dosage is 26kg / m 3 ), the dosage is significantly higher than that of ordinary fiber concrete (PVA fiber is about 1.0kg / m 3 ). In order to achieve the expected performance effect, ECC materials must be prevented during mixing to ensure that a large amount of fibers are evenly dispersed in the cement mortar without aggregation or agglomeration. Otherwise, the homogenization effect of the material will be reduced, resulting in concentrated damage under load after hardening and loss of high toughness (ductility) application function. Therefore, the ability to evenly disperse fibers is the key to ensuring good performance of ECC; evenly dispersed fibers in ECC mixtures such as Figure 1 As shown in a, the fiber clusters are Figure 1 As shown in b.

[0005] At present, there is no mature method for detecting the fiber dispersion inside the ECC mixture. Generally, by observing with the naked eye or touching and pressing the mixture with hands, one can roughly feel whether there are "hard" clumped fibers inside. However, this method is only sensory and too rough. It is also unsafe to operate at the construction site, and it is impossible to accurately judge whether the fiber dispersion in the ECC mixture is uniform.

[0006] GB / T21120 "Synthetic Fibers for Cement Concrete and Mortar" recommends the "water washing method" to detect the dispersion performance of fibers in concrete or mortar mixtures. Use a square hole sieve with a pore size of 75 microns to wash and separate the synthetic fibers from the tested concrete or mortar. After washing, dry them in an oven at a temperature of (105±5)℃ to constant weight. After cooling to room temperature, weigh them respectively, accurate to 0.01g. The calculation formula for fiber dispersion performance is: β=(G1-G0) / G0×100, where β is the relative error of specimen dispersion (%), G0 is the theoretical calculated value of specimen content (g), and G1 is the arithmetic mean of the synthetic fiber content of three batches of tests. The “water washing method” can quantify the relative error of fiber dispersion. However, the actual process of separating the synthetic fibers from the ECC mixture by water washing using the above method is very troublesome. First, PVA fiber is a hydrophilic material and has been adhered to the cement mortar during the mortar mixing process, making it difficult to wash it clean with clean water. Second, during multiple flushing processes, some fibers will pass through the screen and be lost, resulting in large discrete results and making the method difficult to implement and promote. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the above-mentioned background technology and provide a detection method suitable for the fiber dispersion in the ECC material mixture, which can accurately test the dispersion of PVA fibers in the mixture, evaluate the mixing quality of the ECC material, and provide real-time feedback on the raw materials, mix ratio and mixing process to ensure the later mechanical, deformation and durability properties of the ECC material and ensure the long-term durability of the project.

[0008] In order to solve the problems existing in the prior art, the present invention provides a method for detecting fiber dispersion in an ECC material mixture, and the specific steps are as follows:

[0009] (1) Prepare the penetration resistance instrument for the test, referring to the setting time test of concrete mixture in the existing specifications;

[0010] (2) Prepare the ECC mixture according to the specified mixing process, record the water adding time, take the prepared ECC mixture and put it into the test mold. The surface of the ECC mixture in the test mold is 9 to 11 mm lower than the test mold mouth. Vibrate it on a vibration table to make it flat and dense; place it in an environment with a temperature of 20 ± 2 ° C, add a cover to prevent water loss, and form a test specimen;

[0011] (3) performing a penetration pressure test on the test specimen in the test mold in step (2), wherein the pressure measurement value during the penetration pressure test satisfies 25N to 175N, i.e., the penetration resistance value is 0.5MPa to 3.5MPa; the process of the penetration pressure test is as follows: placing the test mold on the base plate of the penetration resistance meter, peeling and zeroing, pressing down the handle to make the end of the probe of the penetration resistance meter contact the surface of the ECC mixture in the test mold, and then uniformly applying force to make the probe penetrate the ECC mixture, and after 9 to 11 seconds, the 25mm depth mark of the probe returns to the surface of the ECC mixture, reading the instrument indication value or the maximum indication value of the pressure gauge, and obtaining the penetration pressure value P of a single measuring point; the test specimen Start timing from the time when the mixture is prepared and water is added. Start penetration pressure test after 3 to 4 hours, and measure once every 1 to 3 hours. You can also extend or shorten the interval time appropriately according to the actual situation to ensure that at least i times of measurement are performed before the initial setting of the mixture of the test specimen, and i≧3. At least n points are measured continuously for each test, and n≧20. The test is completed within 5 minutes, and the penetration pressure value of each measuring point in each test is recorded. During each test, the measuring points are arranged in the order of periphery first and then center. Each test avoids the measuring points of the previous test, and the distance between the measuring points of two tests is not less than 15mm. The distance between all measuring points and the inner wall of the test mold should not be less than 20mm.

[0012] (4) Statistically calculate the penetration pressure values ​​of the i groups of measuring points recorded in the i tests in step (3), and calculate the average penetration pressure values ​​of the n measuring points in each test. And calculate the fiber dispersion deviation rate σ in each test i , a total of i fiber dispersion deviation rates σ are calculated i ;

[0013] Fiber dispersion deviation rate σ in each test i The calculation process is as follows: Calculate the penetration pressure value P of each measuring point in the n measuring points in the same test in turn. n With the average The penetration pressure value P of each measuring point is calculated. n With the average The difference accounts for the average When the calculated result exceeds 15%, the measuring point is judged as a suspicious point. The calculation formula is: Count the number of suspicious points x in the penetration pressure values ​​of each group of n test points i , and calculate the number of suspicious points x according to the following formula ① i The percentage of the total measurement points n, that is, the fiber dispersion deviation rate σ i ;

[0014] σ i =x i / n×100①

[0015] Where: i —Fiber dispersion deviation rate, %;

[0016] x i —The average pressure of the measuring point The number of suspicious points with deviations exceeding 15%;

[0017] n—the total number of measurement points in each test, n≧20;

[0018] (5) Calculate the fiber dispersion deviation rate σ of group i obtained in step (4) according to formula ② i The average value σ is used to determine the uniformity of fiber dispersion in the mixture. The lower the average value σ of the deviation rate is and the closer it is to zero, the more uniform the fiber dispersion in the mixture is.

[0019] σ=(σ1+σ2+……+σ i ) / i ②

[0020] In the formula, σ1, σ2, ... i are the fiber dispersion deviation rates in each set of tests, respectively;

[0021] i is the number of penetration pressure tests.

[0022] The preferred technical solution of the present invention is as follows: in the step (1), the setting time test of concrete mixture in DL / T 5150-2017 "Test Procedure for Hydraulic Concrete" or SL / T 352-2020 "Test Procedure for Hydraulic Concrete" is referred to; and the following supporting test tools are prepared according to the test requirements: a penetration resistance meter, a dynamometer range of not less than 1kN, a graduation value of not more than 1N, and a probe cross-sectional area of ​​50mm 2 , measuring needle length 100mm, with a mark 25mm away from the penetration end; vibration table, frequency (50±3)Hz, amplitude of the center of the table when unloaded (0.5±0.1)mm; timing clock and pipette.

[0023] A preferred technical solution of the present invention is as follows: in the step (2), the test mold adopts a matching mortar cylinder with an upper diameter of 160 mm, a lower diameter of 150 mm, and a net height of 150 mm, or other containers with similar sizes and no leakage; the prepared ECC mixture is sampled and loaded into at least five test molds, and when the penetration pressure test is performed in step (3), one or several test molds are taken at each time point for the penetration pressure test, at least 20 measuring points are taken in the same or several test molds to obtain the penetration pressure values ​​of at least 20 groups of measuring points, and the average pressure of the ECC mixture at that time point is calculated.

[0024] A preferred technical solution of the present invention is as follows: in the step (3), after the test specimen is prepared and the surface of the mixture placed in the test mold is slightly dry, the penetration pressure test is started; before each test, the test mold is taken out, and if there is water seepage or water accumulation on the surface of the specimen, one side of the bottom of the cylinder is raised to tilt the test mold, and the surface water layer is sucked away with a pipette before the penetration pressure test is performed; the pressure value of the initial setting point of the ECC mixture is 175N or the resistance value is 3.5MPa.

[0025] A preferred technical solution of the present invention: the initial setting time of the ECC mixture in the step (3) is determined according to the following method: after each test is completed, the effective penetration resistance R of the test is calculated, and then a relationship curve between the test time and the corresponding effective penetration resistance R is plotted with the test time as the horizontal coordinate and the corresponding effective penetration resistance R as the vertical coordinate, and the test time corresponding to the effective penetration resistance R of 3.5 MPa is taken as the initial setting time of the ECC mixture; the effective penetration resistance R is directly calculated by dividing the effective penetration pressure by the probe area; the above steps can be used to scientifically and accurately obtain the initial setting time of ECC, and it is helpful to verify that at least 3 dispersion tests are within the initial setting critical point time.

[0026] A preferred technical solution of the present invention: in the step (3), after each test, the mortar adhering to the measuring needle should be wiped clean, the test mold should be removed, covered and put back into the constant temperature chamber until the next test.

[0027] The preferred technical solution of the present invention is: the effective penetration pressure is the average measured value of the penetration pressure values ​​of other measuring points after eliminating the suspicious point pressure values ​​in the penetration pressure values ​​of n measuring points tested each time. The effective penetration resistance R is calculated according to formula ③, and the result is accurate to 0.1MPa;

[0028]

[0029] Where: R——effective penetration resistance value, MPa;

[0030] ——The average value of the penetration pressure values ​​of other measuring points after removing the suspicious points in the i-th test, N;

[0031] A——The cross-sectional area of ​​the corresponding measuring needle, i.e. 50mm 2 .

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention uses a penetration resistance meter to test the dispersion of fibers in a high-dosage fiber mortar ECC mixture. The main basis is that once the fibers are clumped or partially missing, they will affect the microstructure of the cement mortar, thereby causing an abnormality in the static pressure required for penetration. Therefore, the fiber dispersion deviation rate can be calculated based on the measurement results of multiple measuring points. The lower the deviation rate (tending to zero), the more uniform the fiber dispersion in the mixture, thereby determining the quality level of the fiber dispersion.

[0034] (2) This method can detect the mixture on site and provide real-time feedback on the results. The test is convenient and accurate, simple, scientific, reasonable, efficient and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 a is a schematic diagram of uniform fiber dispersion in ECC mixture;

[0036] Figure 1 Figure b is a schematic diagram of fiber agglomeration in ECC mixture;

[0037] Figure 2 It is the relationship curve between penetration resistance and corresponding time in the present invention. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with the accompanying drawings and embodiments. The technical solutions shown in the accompanying drawings are specific solutions of the embodiments of the present invention and are not intended to limit the scope of the invention claimed for protection. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] In the following examples, the fiber dispersion deviation rate σ is tested each time. i The calculation process is as follows: Calculate the penetration pressure value P of each measuring point in the n measuring points in the same test in turn. n With the average The penetration pressure value P of each measuring point is calculated. n With the average The difference accounts for the average When the calculated result exceeds 15%, the measuring point is judged as a suspicious point. The calculation formula is: Count the number of suspicious points x in the penetration pressure values ​​of each group of n test points i , and calculate the number of suspicious points x according to the following formula ① i The percentage of the total measurement points n, that is, the fiber dispersion deviation rate σ i ;

[0040] σ i =x i / n×100 ①

[0041] Where: i —Fiber dispersion deviation rate, %;

[0042] x i —The average pressure of the measuring point The number of suspicious points with deviations exceeding 15%;

[0043] n—the total number of measurement points in each test, n≧20;

[0044] Then, the dispersion deviation rate σ of the i-th fiber is calculated according to formula ② i The average value σ is used to determine the uniformity of fiber dispersion in the mixture. The lower the deviation rate is, the closer it is to zero, indicating that the fiber dispersion in the mixture is more uniform.

[0045] σ=(σ1+σ2+……+σ i ) / i ②

[0046] In the formula, σ1, σ2, ... i are the fiber dispersion deviation rates in each set of tests, respectively;

[0047] i is the number of penetration pressure tests.

[0048] In the embodiment, the setting time test of the ECC mixture refers to the setting time test of the concrete mixture in DL / T 5150-2017 "Test Procedure for Hydraulic Concrete" or SL / T 352-2020 "Test Procedure for Hydraulic Concrete"; and the following supporting test tools are prepared according to the test requirements: a penetration resistance meter, a dynamometer range of not less than 1kN, a graduation value of not more than 1N, and a probe cross-sectional area of ​​50mm 2 , the probe is 100mm long and has a mark 25mm away from the penetration end; the vibration table has a frequency of (50±3)Hz and an amplitude of (0.5±0.1)mm at the center of the table when unloaded; a clock and a pipette for timing. Lower Mouth A matching mortar cylinder with a net height of 150 mm, or other containers of similar size that do not leak, such as a cubic test mold with a side length of 150 mm.

[0049] The initial setting time of the ECC mixture in the following embodiments is determined by the following method: after each test is completed, the effective penetration resistance R of the test is calculated, and then a relationship curve between the test time and the corresponding effective penetration resistance R is plotted with the test time as the horizontal coordinate and the corresponding effective penetration resistance R as the vertical coordinate. The test time corresponding to the effective penetration resistance R of 3.5 MPa is the initial setting time of the ECC mixture; the effective penetration resistance R is calculated according to formula ③, and the result is accurate to 0.1 MPa.

[0050]

[0051] Where: R——effective penetration resistance value, MPa;

[0052] ——The average value of the penetration pressure values ​​of other measuring points after removing the suspicious points in the i-th test, N;

[0053] A——The cross-sectional area of ​​the corresponding measuring needle, i.e. 50mm 2 .

[0054] The embodiment provides a method for detecting fiber dispersion in an ECC material mixture, and the specific steps are as follows:

[0055] (1) Prepare an ECC material mixture, add 2% PVA fiber by volume, and record the water addition time as 8:00 am; take samples and put them into 5 mortar tubes, with the surface of the specimens about 10 mm below the tube mouth, and vibrate them on a vibration table to make them flat and dense; place them in an environment with a temperature of (20±2)℃, cover them with a thin plastic film to prevent water loss, and prepare five test specimens;

[0056] (2) At 14:00 in the afternoon, two of the test specimens were taken out for testing. The testing process of 20 points was completed from the two test specimens within five minutes. Before the test, the covering film of each test specimen was lifted, and the accumulated water on the surface of the specimen was sucked away with a pipette. The specimen was placed on the base plate of the penetration resistance meter and peeled and reset to zero. The handle was pressed down to make the end of the probe contact the surface of the mixture, and then the probe was penetrated into the mixture with uniform force. After about 10 seconds, the 25mm depth mark of the probe returned to the surface of the mixture, and the maximum indication of the pressure gauge, i.e., the penetration pressure value P of a single measuring point, was read. The measuring points were measured in accordance with the principle of "first the periphery and then the center, each measuring point avoiding the previous measuring hole, the spacing was not less than 15mm, and the distance between the measuring point and the mortar tube wall was not less than 20mm". The test results of the 20 measuring points are shown in Table 1. The effective penetration resistance and uniform pressure value at the first time were calculated.

[0057] Table 1 First test results (test time 14:00)

[0058]

[0059] (3) At 16:10 and 17:10, the second and third tests were conducted respectively. The test process was in accordance with step (2). One or more test specimens could be taken for each test to ensure that the test points met the test requirements. The results of the two tests are shown in Tables 2 and 3, and the effective penetration resistance and uniform pressure values ​​in the second and third tests were calculated respectively. It can be seen from the calculation that in the third test, the penetration resistance of the mixture was 3.43 MPa, indicating that the initial setting time was approaching.

[0060] Table 2 Second test results (test time 16:10)

[0061]

[0062] Table 3 The third test results (test time 17:10)

[0063]

[0064]

[0065] At 17:30 on the same day, the fourth test was conducted. The test results are shown in Table 4. The calculated penetration resistance value was 4.45 MPa, which exceeded 3.5 MPa. At this time, the mixture had exceeded the initial setting stage and was not suitable for fiber dispersion evaluation. Therefore, the test points were reduced and the test was stopped.

[0066] Table 4 Results of the fourth test (test time 17:30)

[0067]

[0068] (4) According to the test results, it is found that the fourth test no longer meets the requirements, so according to the formula σ i =x i / n×100 to calculate the fiber dispersion deviation rate of the first three tests: σ1=0.15, σ2=0.10, σ3=0.10, and then according to the formula σ=(σ1+σ2+……+σ i ) / i=(0.15+0.10+0.10) / 3=0.12, calculate the third dispersion deviation rate σ i The average value is 0.12, and the deviation rate is low, indicating that the fiber dispersion in the ECC mixture prepared in the embodiment is good.

[0069] According to the test results, the penetration resistance at different time points was statistically analyzed, see Table 5, and the relationship curve between the penetration resistance and the corresponding test time was drawn, see Figure 2 ; It can be seen from the curve that the initial setting time of the mixture is 555min. The above steps can be used to scientifically and accurately obtain the initial setting time of ECC, and it is helpful to verify that at least 3 dispersion tests are within the initial setting critical point time.

[0070] Table 5 Analysis results of penetration resistance at different test times

[0071]

[0072]

[0073] The above is only one embodiment of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for detecting fiber dispersion in ECC material mixtures, characterized in that: The specific steps are as follows: (1) Prepare the penetration resistance meter for the test. The setting time test of ECC mixture shall refer to the setting time test of concrete mixture in DL / T 5150-2017 "Testing Procedure for Hydraulic Concrete" or SL / T 352-2020 "Testing Procedure for Hydraulic Concrete"; (2) Prepare the ECC mixture according to the specified mixing process, take the prepared ECC mixture sample and put it into the test mold. The surface of the ECC mixture in the test mold is 9 to 11 mm lower than the test mold opening. Vibrate it on a vibration table to make it flat and dense; place it in an environment with a temperature of 20 ± 2 ° C, add a cover to prevent water loss, and form a test specimen; (3) A penetration pressure test is performed on the test specimen in the test mold in step (2), wherein the pressure measurement value during the penetration pressure test satisfies 25N~175N, that is, the penetration resistance value is 0.5MPa~3.5MPa; the process of the penetration pressure test is: placing the test mold on the base plate of the penetration resistance meter, peeling and zeroing, pressing down the handle to make the end of the probe of the penetration resistance meter contact with the surface of the ECC mixture in the test mold, and then uniformly applying force to make the probe penetrate the ECC mixture, and after 9~11s, the 25mm depth mark of the probe returns to the surface of the ECC mixture, reading the instrument indication value or the maximum indication value of the pressure gauge, that is, obtaining the single measuring point pressure. Penetration pressure value P; the test specimen starts timing from the time when the mixture is prepared and water is added. The penetration pressure test is started after 3 to 4 hours, and is measured every 1 to 3 hours. At least i times are measured before the mixture of the test specimen is initially set, and i≧3. At least n points are measured continuously for each test, and n≧20. The test is completed within 5 minutes, and the penetration pressure value of each measuring point in each test is recorded. During each test, the measuring points are arranged in the order of periphery first and then center. Each test avoids the measuring points of the previous test, and the distance between the measuring points of two tests is not less than 15mm. The distance between all measuring points and the inner wall of the test mold should not be less than 20mm; (4) For the penetration pressure values ​​of each measuring point recorded in the i tests in step (3), statistics are performed to calculate the average penetration pressure values ​​of the n measuring points in each test. , and calculate the fiber dispersion deviation rate σ in each test i , a total of i fiber dispersion deviation rates σ are calculated i ; Fiber dispersion deviation rate σ in each test i The calculation process is as follows: Calculate the penetration pressure value P of each measuring point in the n measuring points in the same test in turn. n With the average The penetration pressure value P of each measuring point is calculated. n With the average The difference accounts for the average When the calculated result exceeds 15%, the measuring point is judged as a suspicious point. The calculation formula is |P n - | / ×100; count the number of suspicious points x in the penetration pressure values ​​of n measuring points in each test group i , and calculate the number of suspicious points x according to the following formula ① i The percentage of the total measurement points n, that is, the fiber dispersion deviation rate σ i ; s i =x i / n×100 ① Where: i —Fiber dispersion deviation rate, %; x i —The average pressure of the measuring point The number of suspicious points with deviations exceeding 15%; n—the total number of measurement points in each test, n≧20; (5) Calculate the total i-th fiber dispersion deviation rate σ obtained in step (4) according to formula ②: i The average value σ is used to determine the uniformity of fiber dispersion in the mixture. The lower the average value σ of the deviation rate is and the closer it is to zero, the more uniform the fiber dispersion in the mixture is. σ=(σ1+σ2+……+σ i ) / i ② In the formula, σ1, σ2, ... i are the fiber dispersion deviation rates in each set of tests, respectively; i is the number of penetration pressure tests.

2. A method for detecting fiber dispersion in ECC material mixture according to claim 1, characterized in that: In step (1), the following supporting test tools are prepared according to the test requirements: a penetration resistance meter, a dynamometer with a range of not less than 1 kN, a graduation value of not more than 1 N, and a probe cross-sectional area of ​​50 mm 2 , the measuring needle is 100mm long and there is a mark 25mm away from the penetration end; the vibration table has a frequency of 50±3Hz and an amplitude of 0.5±0.1mm at the center of the table when unloaded; a clock and a pipette for timing.

3. A method for detecting fiber dispersion in an ECC material mixture according to claim 1, characterized in that: The test mold in step (2) adopts a matching mortar tube with an upper diameter of 160 mm, a lower diameter of 150 mm, and a net height of 150 mm, or a cubic test mold with a side length of 150 mm; the prepared ECC mixture is sampled and loaded into at least five test molds, and when the penetration pressure test is performed in step (3), one or several test molds are taken at each time point for penetration pressure test, and at least 20 measuring points are taken in the same or several test molds to obtain the penetration pressure values ​​of at least 20 measuring points, and the average pressure of the ECC mixture at that time point is calculated. .

4. A method for detecting fiber dispersion in an ECC material mixture according to claim 1, characterized in that: In step (3), when the test specimen is prepared and the surface of the mixture placed in the test mold is slightly dry, the penetration pressure test is started; Before each test, take out the test mold. If there is water seepage or accumulation on the surface of the test piece, raise one side of the bottom of the cylinder to tilt the test mold, and use a pipette to suck away the surface water layer before conducting a penetration pressure test. The initial setting point of the ECC mixture is a pressure value of 175N or a resistance value of 3.5MPa.

5. A method for detecting fiber dispersion in ECC material mixture according to claim 1, characterized in that: The initial setting time of the ECC mixture in step (3) is determined by the following method: after each test is completed, the effective penetration resistance R of the test is calculated, and then a relationship curve between the test time and the corresponding effective penetration resistance R is plotted with the test time as the horizontal coordinate and the corresponding effective penetration resistance R as the vertical coordinate. The test time corresponding to the effective penetration resistance R of 3.5 MPa is taken as the initial setting time of the ECC mixture; the effective penetration resistance R is directly calculated by dividing the effective penetration pressure by the probe area.

6. A method for detecting fiber dispersion in ECC material mixture according to claim 1, characterized in that: In step (3), after each test, the mortar adhering to the probe should be wiped clean, the test mold should be removed, covered and placed back in the constant temperature chamber until the next test.

7. A method for detecting fiber dispersion in ECC material mixture according to claim 5, characterized in that: The effective penetration pressure is the average penetration pressure value of other measuring points calculated after removing the suspicious point pressure value from the penetration pressure values ​​of n measuring points in each test. ´, the effective penetration resistance R is calculated according to formula ③, and the result is accurate to 0.1MPa; R= ´ / A ③ Where: R——effective penetration resistance value, MPa; ´——the average value of the penetration pressure values ​​of other measuring points after removing the suspicious points in the i-th test, N; A——The cross-sectional area of ​​the corresponding measuring needle, i.e. 50mm 2 .