Positive electrode slurry and preparation method thereof, positive electrode sheet, and lithium ion battery

By using binders generated from polymers with amino groups in lithium-ion batteries, the problems of solvent contamination and insufficient bonding ability of PVDF binders are solved, and the structural stability and electrochemical performance of lithium-ion batteries are improved to meet the needs of meet green environmental protection requirements.

CN118460169BActive Publication Date: 2024-10-18SHANGHAI JIAOTONG UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410924570.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-18
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The polyvinylidene fluoride (PVDF) binder used in existing lithium-ion batteries has problems with solvent contamination and insufficient bonding ability, which affects the electrochemical performance and environmental protection requirements of lithium-ion batteries.

Method used

A polymer with an amino group is used as the first reactant to react with dicarboxylic acid to form a binder that has cations and anions in the molecular chain, thereby improving the water solubility of the binder and its binding force with active substances. Water serves as a dispersion medium and improves the transmission efficiency of lithium ions through intermolecular forces and molecular chain entanglement.

Benefits of technology

It achieves high structural stability and improved electrochemical performance of lithium-ion batteries, meets the needs of green environmental protection, and improves the charge-discharge rate and specific capacity of lithium-ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118460169B_ABST
    Figure CN118460169B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of lithium-ion batteries, and discloses a positive electrode slurry and a preparation method thereof, a positive electrode sheet, and a lithium-ion battery. The binder of the positive electrode slurry is obtained by reacting a first reactant with a second reactant, and the molecular chain of the binder includes cations and anions at the same time, and can be well dissolved in an aqueous dispersion medium to meet the application requirements of green environmental protection. At the same time, the anions on the molecular chain of the binder can play a role in transmitting lithium ions, which can effectively reduce the resistance of lithium ion transmission on the positive electrode sheet, so that lithium ions can be more easily released from the positive electrode sheet, thereby improving the electrochemical performance of the lithium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a positive electrode slurry and a preparation method thereof, a positive electrode sheet, and a lithium-ion battery. Background Art

[0002] As a storage medium for clean and renewable energy, lithium-ion batteries have the advantages of high specific energy, high voltage, and environmental friendliness, and have been widely used in many fields. Among them, the positive electrode slurry, as an important material for the preparation of lithium-ion batteries, affects the electrochemical performance of lithium-ion batteries. Therefore, the electrochemical performance of lithium-ion batteries can be improved by improving the positive electrode slurry. The current common method is to modify and optimize the active substances in the positive electrode slurry, such as element doping, carbon coating, and particle size control. As an important inactive component in the positive electrode slurry, the performance of the binder also directly affects the electrochemical performance of lithium-ion batteries.

[0003] In the industrial production of lithium-ion batteries, polyvinylidene fluoride (PVDF) is mainly used as the binder of the positive electrode slurry. However, PVDF still has the following disadvantages: (1) The solvent used to dissolve PVDF is usually highly polarized, such as volatile and highly toxic N-methylpyrrolidone (NMP), which will cause environmental pollution and is not conducive to recycling; (2) It mainly relies on weak interaction van der Waals forces to form a bonding network, so the bonding ability between the active material is insufficient, which is not conducive to the structural stability of the lithium-ion battery during the charge and discharge process, and affects the electrochemical performance of the lithium-ion battery.

[0004] Therefore, it is necessary to improve the binder in the positive electrode slurry so that it meets the requirements of green environmental protection and can improve the electrochemical performance of lithium-ion batteries. Summary of the invention

[0005] The purpose of this application is to improve the binder to meet the demand for green and environmentally friendly positive electrode slurry and effectively improve the electrochemical performance of lithium-ion batteries.

[0006] To achieve the above-mentioned purpose, the first aspect of the present application provides a positive electrode slurry, wherein the binder of the positive electrode slurry is obtained by reacting a first reactant with a second reactant, wherein: the first reactant is selected from at least one of polyethyleneimine, ethylenediamine core dendritic polyamideamine, 1,4-butanediamine core dendritic polyamideamine, cystamine core dendritic polyamideamine, hyperbranched polyamide, and hyperbranched polyamideamine; the second reactant is selected from at least one of dicarboxylic acid, anhydride, 1,4-butane sultone, 1,3-propane sultone, 1,8-naphthalene sultone, propylene carbonate, 4-hydroxyacetoacetic acid lactone, and isocitrate lactone.

[0007] In some embodiments of the first aspect, the first reactant is polyethyleneimine and / or ethylenediamine core dendritic polyamidoamine; and the second reactant is selected from at least one of succinic anhydride, 1,8-naphthalenesulfonate and propylene carbonate.

[0008] In some embodiments of the first aspect, the number average molecular weight of the first reactant is 1000-5000.

[0009] In some embodiments of the first aspect, the reaction conditions of the first reactant and the second reactant satisfy at least one of the following: (1) the molar ratio of the first reactant to the second reactant is 1:1 to 1:50; (2) the reaction temperature of the first reactant and the second reactant is 30° C. to 100° C., and the reaction time is 1 hour to 40 hours.

[0010] In some embodiments of the first aspect, the binder is obtained by ionizing the first reactant and the second reactant in a solvent, and the solvent is selected from at least one of water, methanol, ethanol, toluene, xylene, acetonitrile, pyridine, cyclohexane, petroleum ether, n-hexane, ether, acetone, butanone, ethyl acetate, butyl acetate, dichloromethane, tetrahydrofuran, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0011] In some embodiments of the first aspect, the positive electrode slurry also includes an active material, a conductive agent and a dispersion medium, and the mass ratio of the binder, the active material, the conductive agent and the dispersion medium is (0.05~0.15):(0.6~1.0):(0.05~0.15):(3~5).

[0012] In some embodiments of the first aspect, the active material includes at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, and lithium manganese oxide; the conductive agent includes at least one of conductive carbon black, conductive graphite, and carbon nanotubes; and the dispersion medium includes water and / or an organic solvent.

[0013] The second aspect of the present application provides a method for preparing the positive electrode slurry, comprising: adding a dispersion medium to a mixture of a binder, an active material and a conductive agent and stirring the mixture to obtain the positive electrode slurry.

[0014] The third aspect of the present application provides a positive electrode sheet, comprising: a current collector and a positive electrode material layer located on the surface of the current collector, and the positive electrode material layer is formed by coating and drying the positive electrode slurry prepared by any of the positive electrode slurries described above or the positive electrode slurry preparation method described above.

[0015] A fourth aspect of the present application provides a lithium-ion battery, comprising the above-mentioned positive electrode sheet.

[0016] Compared with the prior art, the technical solution of the present application has the following beneficial effects:

[0017] The present application uses a polymer with an amino group as the first reactant, a substance that can react with the first reactant to form anions as the second reactant, and the product obtained after the two react as the binder of the positive electrode slurry, and the molecular chain of the binder has cations and anions, so that it can be well dissolved in water, so that the positive electrode slurry can use water as a dispersion medium to meet the needs of green environmental protection. At the same time, the anions on the molecular chain of the binder can play the role of transmitting lithium ions, which can effectively reduce the transmission resistance of lithium ions on the positive electrode sheet, so that lithium ions can be more easily removed from the positive electrode sheet, thereby improving the charge and discharge rate, specific capacity and cycle performance of the lithium ion battery. In addition, the molecular chain of the binder is relatively long, and it can be combined with the active material through intermolecular forces and / or molecular chain entanglement, so that the active material can be tightly bonded to the collector of the positive electrode sheet, so that the lithium ion battery has a higher structural stability during the charge and discharge process, thereby improving the performance of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only used for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale. Among them:

[0019] Figure 1 This is a schematic diagram of the structure of the binder in the positive electrode slurry of the present application;

[0020] Figure 2 The charge and discharge cycle test curves of the lithium ion batteries prepared in Examples 1 to 2 of the present application and Comparative Example 1 at currents of 0.1C, 0.5C, 1C, 2C, and 3C;

[0021] Figure 3 The charge and discharge cycle test curves of the lithium-ion batteries prepared in Example 3 and Comparative Examples 1-2 of the present application at a current of 6C;

[0022] Figure 4 The charge and discharge test curves of the lithium-ion batteries prepared in Example 1, Example 3 and Comparative Example 1 of the present application at a current of 1C;

[0023] Figure 5 This is an impedance test curve diagram of the lithium-ion battery prepared in Comparative Example 1 of the present application;

[0024] Figure 6 This is an impedance test curve diagram of the lithium-ion battery prepared in Examples 1-2 of the present application. DETAILED DESCRIPTION

[0025] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.

[0026] The present application provides a positive electrode slurry, wherein the binder of the positive electrode slurry is obtained by reacting a first reactant with a second reactant, wherein the first reactant is a polymer having an amino group, wherein the amino group is a reactive functional group of the first reactant, and after reacting with the reactive functional group of the second reactant, a quaternary ammonium cation can be formed to improve the water solubility of the binder. The present application selects a polymer as the first reactant, so that the prepared binder has a longer molecular chain, so that it can be combined with the positive electrode active material through intermolecular forces and molecular chain entanglement, thereby improving the bonding force with the positive electrode active material, and further improving the structural stability of the lithium-ion battery during the charge and discharge process.

[0027] In some specific embodiments, the first reactant is selected from polyethyleneimine (Mn can be 300, 600, 1200, 1800, 10000, 25000, 60000, 70000, etc.), ethylenediamine core dendritic polyamidoamine (generation number G can be 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, etc.), 1,4-butanediamine core dendritic polyamidoamine with similar performance to the ethylenediamine core dendritic polyamidoamine At least one of a cystamine core dendritic polyamide amine (the generation number G can be 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, etc.), a cystamine core dendritic polyamide amine (the generation number G can be 1.0, 2.0, 3.0, 4.0, 5.0, etc.) having similar properties to the ethylenediamine core dendritic polyamide amine, a hyperbranched polyamide having similar properties to the ethylenediamine core dendritic polyamide amine, and a hyperbranched polyamide amine having similar properties to the ethylenediamine core dendritic polyamide amine.

[0028] In order to further balance the water solubility and bonding performance of the binder, the number average molecular weight of the first reactant is preferably 300-10000, more preferably 1000-5000, and even more preferably 1000-4000.

[0029] The second reactant is selected from substances that can react with the first reactant to form anions, and the anions are preferably carboxylate (-COO - ), sulfonate (-SO3 - ) or carbonate (-CO3 - ).

[0030] In some specific embodiments, the second reactant is at least one of dicarboxylic acid, anhydride, 1,4-butane sultone, 1,3-propane sultone, 1,8-naphthalene sultone, propylene carbonate, 4-hydroxyacetoacetic acid lactone, and isocitrate lactone. The dicarboxylic acid is preferably at least one of malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, hexadecanedioic acid, methylmalonic acid, maleic acid, phenylmalonic acid, phenylsuccinic acid, malic acid, citric acid, and itaconic acid. The anhydride is preferably at least one of phthalic anhydride, itaconic anhydride, trimellitic anhydride, maleic anhydride, succinic anhydride, glutaric anhydride, citraconic anhydride, biphenyl anhydride, methylsuccinic anhydride, pyromellitic anhydride, 3-methylglutaric anhydride, 1,2-cyclohexanedicarboxylic anhydride, and 2,2-dimethylsuccinic anhydride.

[0031] refer to Figure 1 The binder prepared by the reaction of the first reactant and the second reactant contains both quaternary ammonium cations and anions, wherein the quaternary ammonium cations are provided by the first reactant, and the anions are provided by the second reactant, and the anions can be carboxylate anions (-COO ¯ ), sulfonate anion (-SO3 - ) or carbonate (-CO3 - ). Since the binder molecular chain of the present application includes both cations and anions, it has good water solubility. Therefore, the positive electrode slurry using the binder can use water instead of volatile, highly toxic organic solvents as a dispersion medium, thereby meeting the application requirements of green environmental protection. At the same time, the anions on the side chains of the binder can play a role in transmitting lithium ions, which can effectively reduce the resistance of lithium ions to the transmission of the positive electrode sheet, so that lithium ions can be more easily escaped from the positive electrode sheet, forming a molecular chain transmission path, thereby improving the charge and discharge rate, specific capacity and cycle performance of the lithium ion battery. The binder can also be combined with the positive electrode active material through non-covalent interaction (intermolecular forces and / or molecular chain entanglement), so that the positive electrode active material can be tightly bonded to the current collector of the positive electrode sheet.

[0032] In some preferred embodiments, the first reactant is polyethyleneimine and / or ethylenediamine core dendritic polyamidoamine, and the second reactant is at least one of succinic anhydride, 1,8-naphthalenesulfonate and propylene carbonate.

[0033] In some more preferred embodiments, the first reactant is polyethyleneimine, the second reactant is succinic anhydride, and the two react to obtain a binder as shown in Formula 1; or, the first reactant is polyethyleneimine, the second reactant is 1,8-naphthalenesulfone, and the two react to obtain a binder as shown in Formula 2; or, the first reactant is ethylenediamine core dendritic polyamidoamine, the second reactant is propylene carbonate, and the two react to obtain a binder as shown in Formula 3:

[0034] ;

[0035] ;

[0036]

[0037] In some preferred embodiments, the molar ratio of the first reactant to the second reactant is 1:1 to 1:50, for example, the molar ratio of the two can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, etc., or a specific ratio between all ratio ranges composed of the above-mentioned ratios. Limiting the molar ratio of the two within the above range can effectively promote the reaction to produce the binder of the present application.

[0038] In some preferred embodiments, the reaction temperature of the first reactant and the second reactant is 30°C to 100°C, and the reaction time is 1 hour to 40 hours. Preferably, the reaction time is 1 hour to 24 hours. The reaction temperature and reaction time may be conducive to the formation of the product, wherein the reaction temperature may also be 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, etc. and any other point value within the above temperature range, and the reaction time may also be 2, 3, 4, 5, 6, 8, 10, 12, 13, 14, 15, 16, 18, 20 hours, etc. and any other point value within the above time range, and those skilled in the art may adjust according to the actual reaction situation.

[0039] In some preferred embodiments, the binder is obtained by an ionization reaction of the first reactant and the second reactant in a solvent, and the solvent is selected from at least one of water (or deionized water), methanol, ethanol, toluene, xylene, acetonitrile, pyridine, cyclohexane, petroleum ether, n-hexane, ether, acetone, butanone, ethyl acetate, butyl acetate, dichloromethane, tetrahydrofuran, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0040] In the above embodiment, the ionization reaction of the commercial first reactant and the second reactant is mainly used to directly obtain the binder for the positive electrode slurry. The preparation method is simple and mature, and can be widely used in the industrial production of lithium-ion batteries.

[0041] In some embodiments, in addition to the binder, the positive electrode slurry also includes an active material, a conductive agent and a dispersion medium, and the mass ratio of the binder, the active material, the conductive agent and the dispersion medium is (0.05~0.15):(0.6~1.0):(0.05~0.15):(3~5).

[0042] In some embodiments, the active material includes at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, and lithium manganate, and the conductive agent includes at least one of conductive carbon black (such as acetylene black), conductive graphite, and carbon nanotubes. The dispersion medium includes water and / or an organic solvent, preferably water, and the organic solvent can be a commonly used solvent for positive electrode slurry such as N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0043] The present application also provides a method for preparing the positive electrode slurry, comprising: adding a dispersion medium to a mixture of a binder, an active material and a conductive agent and stirring the mixture to obtain the positive electrode slurry.

[0044] The present application also provides a positive electrode sheet, comprising: a current collector and a positive electrode material layer located on the surface of the current collector, and the positive electrode material layer is formed by coating and drying the above-mentioned positive electrode slurry or the positive electrode slurry prepared by the above-mentioned positive electrode slurry preparation method.

[0045] The present application also provides a lithium-ion battery, comprising the above-mentioned positive electrode sheet. In some embodiments, the lithium-ion battery further comprises a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet and the separator can adopt any existing structure.

[0046] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Unless otherwise specified, the reagents and raw materials used can be purchased through commercial channels. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0047] In the following examples, polyethyleneimine (Mn=1200, 3500), ethylenediamine core dendritic polyamidoamine (G=2.0), succinic anhydride, 1,8-naphthalenesulfonate, and propylene carbonate were all purchased from Adamas; lithium iron phosphate, acetylene black, aluminum foil current collector, and PVDF (HSV900) were all purchased from Shenzhen Kejing; metal lithium sheets were purchased from Benoit Battery Materials Co., Ltd.; PP diaphragm (Celgard 2500) was purchased from Zhengzhou Jinghong New Energy Technology Co., Ltd.; and LiPF6 electrolyte was purchased from Suzhou Fosai.

[0048] The prepared adhesive product was confirmed by gel permeation chromatography and nuclear magnetic resonance hydrogen spectrum. The gel permeation chromatography test used a Japanese Shimadzu LC-20ADXR liquid chromatograph, equipped with a Shodex KD-804 chromatographic column and a chromatographically pure DMF containing 0.03 mol / L H3PO4 as the mobile phase. The nuclear magnetic resonance test used a Bruker AVANCE III HD 400, and the solvent was DMSO- d 6. The test frequency was 400 MHz, and the chemical shift relative to tetramethylsilane (TMS) was obtained.

[0049] Example 1

[0050] (1) Preparation of binder

[0051] 5 g of polyethyleneimine PEI (Mn=1200) was dissolved in 50 mL of anhydrous ethanol, and 2 g of succinic anhydride was added at 30°C for reaction for 24 hours. After the reaction, the anhydrous ethanol was removed at 60°C, and the mixture was washed twice with dichloromethane and dried by spin drying to obtain a binder of formula 1. The number average molecular weight was 1670 as measured by gel permeation chromatography, and its H 1 -NMR characterization data are as follows:

[0052] H 1 -NMR(DMSO): d(ppm) = 8.01-7.94 (2H); 1.55-1.44 (7H); 3.46-3.30(12H); 3.14-3.01(14H); 2.89-2.64 (20H); 2.53-2.39(18H).

[0053] (2) Preparation of positive electrode slurry

[0054] 0.1 g of the binder prepared in this example, 0.8 g of lithium iron phosphate and 0.1 g of acetylene black were mixed evenly, and the mixture was added into 4 g of water and stirred for 4 hours to obtain a binder.

[0055] (3) Preparation of positive electrode

[0056] The positive electrode slurry prepared in this embodiment was scraped onto the surface of the aluminum foil current collector by a solution scraping method using an Elcometer 4340 coating machine. The scraper height was set to 200 μm and the scraping speed was 0.2 inches per second. After the scraping was completed, it was dried at 65° C. for 3 hours and then dried at 100° C. for 12 hours, and then cut into positive electrode sheets.

[0057] (4) Preparation of lithium-ion batteries

[0058] A lithium-ion battery was assembled with a metal lithium sheet as the negative electrode, LiPF6 as the electrolyte, a PP separator and the positive electrode sheet prepared in this embodiment.

[0059] Example 2

[0060] (1) Preparation of binder

[0061] 5 g of polyethyleneimine PEI (Mn=3500) was dissolved in 50 mL of butanone, and 1 g of 1,8-naphthalenesulfonate was added at 40°C for 16 hours. After the reaction, butanone was removed at 40°C, washed twice with ethyl acetate, and dried by spin drying to obtain a binder shown in Formula 2. The number average molecular weight was 4320 as measured by gel permeation chromatography, and its H 1 -NMR characterization data are as follows:

[0062] H 1 -NMR(DMSO): d(ppm) =9.48-9.35(3H); 8.37-8.10(16H); 7.54-7.45(4H); 7.34-7.20(4H); 3.58-3.45(10H); 2.33-2.20(34H); 1.54-1.48(7H).

[0063] (2) Preparation of positive electrode slurry

[0064] 0.1 g of the binder prepared in this example, 0.8 g of lithium iron phosphate and 0.1 g of acetylene black were mixed evenly, and the mixture was added into 4 g of water and stirred for 4 hours to obtain a binder.

[0065] The preparation method of the positive electrode sheet and the lithium ion battery of this embodiment is the same as that of embodiment 1.

[0066] Example 3

[0067] (1) Preparation of binder

[0068] 5 g of ethylenediamine core dendritic polyamidoamine (G=2.0, Mn=3250) was dissolved in 50 mL of methanol, and 2 g of propylene carbonate was added at 30°C for reaction for 24 hours. After the reaction, methanol was removed at 60°C, washed twice with ethyl acetate, and dried by spin drying to obtain a binder shown in Formula 3. The number average molecular weight was 4580 as measured by gel permeation chromatography, and its H 1 -NMR characterization data are as follows:

[0069] H 1 -NMR(DMSO): d(ppm)=8.10-7.99(30H); 6.70-6.55(14H); 5.47-5.30(14H); 4.41-4.35(14H); 4.28-4.19(28H); 3.66-3.52(32H); 3.49-3.29(84H); 3.14-3.02(24H); 2.69-2.50(68H); 2.48-2.36(24H); 1.31-1.22(42H).

[0070] (2) Preparation of positive electrode slurry

[0071] 0.1 g of the binder prepared in this example, 0.8 g of lithium iron phosphate and 0.1 g of acetylene black were mixed evenly, and the mixture was added into 4 g of water and stirred for 4 hours to obtain a binder.

[0072] The preparation method of the positive electrode sheet and the lithium ion battery of this embodiment is the same as that of embodiment 1.

[0073] Comparative Example 1

[0074] 0.1 g of PVDF (HSV900), 0.8 g of lithium iron phosphate and 0.1 g of acetylene black were mixed, 4 g of NMP was added and stirred for 4 hours to obtain a positive electrode slurry.

[0075] The positive electrode slurry prepared in this comparative example was coated on an aluminum foil current collector, dried at 65° C. for 3 hours, then dried at 100° C. for 12 hours, and cut into positive electrode sheets.

[0076] A lithium-ion battery was assembled with a metal lithium sheet as the negative electrode, LiPF6 as the electrolyte, a PP separator and the positive electrode sheet prepared in this comparative example.

[0077] Comparative Example 2

[0078] 0.1 g of ethylenediamine core dendritic polyamidoamine (G=2.0), 0.8 g of lithium iron phosphate and 0.1 g of acetylene black were mixed, added into 4 g of water and stirred for 4 hours to obtain a positive electrode slurry.

[0079] The positive electrode slurry prepared in this comparative example was coated on an aluminum foil current collector, dried at 65° C. for 3 hours, then dried at 100° C. for 12 hours, and cut into positive electrode sheets.

[0080] Charge and discharge performance test

[0081] The lithium ion batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to charge and discharge cycle tests using a small current button cell tester (CT-4000). The specific test method is as follows:

[0082] (1) The lithium ion batteries prepared in Examples 1-2 and Comparative Example 1 were placed in a constant temperature environment (25°C), and the program was set as follows: charging to 3.8 V with a current of 0.1C, then discharging to 2.5 V with a current of 0.1C, for 3 cycles; charging to 3.8 V with a current of 0.5C, then discharging to 2.5 V with a current of 0.5C, for 3 cycles; charging to 3.8 V with a current of 1C, then discharging to 2.5 V with a current of 1C, for 3 cycles; charging to 3.8 V with a current of 2C, then discharging to 2.5 V with a current of 2C, for 3 cycles; charging to 3.8 V with a current of 3C, then discharging to 2.5 V with a current of 3C, for 3 cycles.

[0083] (2) The lithium-ion batteries prepared in Example 3 and Comparative Examples 1-2 were placed in a constant temperature environment (25°C) and programmed to charge to 3.8 V at 6C current and then discharge to 2.5 V at 6C current for 100 cycles.

[0084] (3) The lithium-ion batteries prepared in Example 1, Example 3 and Comparative Example 1 were placed in a constant temperature environment (25° C.) and the program was set as follows: charging at 1C current to 3.8V; then discharging at 1C current to 2.5V.

[0085] Figure 2 The charge and discharge cycle test results of the lithium ion batteries prepared in Examples 1-2 and Comparative Example 1 at currents of 0.1C, 0.5C, 1C, 2C, and 3C, respectively. The lithium ion batteries prepared in Examples 1-2 have a higher specific capacity (Capacity) at a large current (3C), while the specific capacity of the lithium ion battery prepared in Comparative Example 1 decreases significantly at a large current (3C). It can be seen that compared with the PVDF binder, the lithium ion battery assembled with the positive electrode sheet prepared by the binder of the embodiment of the present application has a higher specific capacity at a large current.

[0086] Figure 3The test results of the charge and discharge cycles of the lithium-ion batteries prepared in Example 3 and Comparative Examples 1-2 at 6C current are shown. The lithium-ion battery assembled with the positive electrode sheet prepared with the PVDF binder of Comparative Example 1 cannot perform normal charge and discharge process at 6C current, while the lithium-ion battery assembled with the positive electrode sheet prepared with the binder having cations and anions of Example 3 of the present application has excellent cycle charge and discharge performance at 6C current, and is far superior to Comparative Example 2. It can be seen that the present application can well regulate the movement of lithium ions by introducing anions into the binder molecular chain, making the transmission of lithium ions faster and more uniform.

[0087] Figure 4 The charge and discharge test results of the lithium-ion batteries prepared in Example 1, Example 3 and Comparative Example 1 at 1C current are shown. The specific capacity of the lithium-ion battery assembled with the positive electrode sheet prepared with the PVDF binder of Comparative Example 1 is less than 120 mAh·g -1 , while the lithium-ion battery assembled with the positive electrode sheet prepared by the binder of the embodiment of the present application has a higher specific capacity, among which the specific capacity of embodiment 1 is as high as 160 mAh·g -1 , Example 3 up to 140 mAh g -1 .

[0088] Impedance performance test

[0089] The EIS impedance performance test was performed on the lithium ion batteries prepared in Examples 1-2 and Comparative Example 1 using a CHI660E electrochemical workstation. The test voltage was the open circuit voltage of the lithium ion battery, and the frequency was 0.11-100000 Hz. Figure 5 The impedance performance test results of the lithium ion battery prepared in Comparative Example 1 are shown. Figure 6 The impedance performance test results of the lithium ion batteries prepared in Examples 1 and 2 are shown.

[0090] Combination Figure 5 and Figure 6 It can be seen that the impedance of the lithium ion battery prepared in Comparative Example 1 is 90Ω, and the impedance of the lithium ion battery prepared in Examples 1 and 2 is 15Ω. Therefore, the lithium ion battery assembled with the positive electrode sheet prepared by the binder of the present application has a lower impedance.

[0091] In summary, when the binder of the present application is formulated into a positive electrode slurry to prepare a positive electrode sheet, not only can water be used as a dispersion medium to meet the needs of green environmental protection, but it can also significantly improve the transmission process of lithium ions, thereby greatly improving the electrochemical performance of lithium-ion batteries.

[0092] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.

Claims

1. A positive electrode slurry, characterized in that: The binder of the positive electrode slurry is obtained by an ionization reaction between a first reactant and a second reactant in a solvent, wherein: The first reactant is polyethyleneimine, and the second reactant is succinic anhydride, and the reaction obtains a binder shown in Formula 1, and the number average molecular weight is 1670: ; Alternatively, the first reactant is polyethyleneimine, and the second reactant is 1,8-naphthalenesulfonate, and the reaction obtains a binder shown in Formula 2, and the number average molecular weight is 4320: ; Alternatively, the first reactant is ethylenediamine core dendritic polyamidoamine, and the second reactant is propylene carbonate, and the reaction obtains a binder shown in Formula 3, and the number average molecular weight is 4580: 。 2. The positive electrode slurry according to claim 1, characterized in that The number average molecular weight of the first reactant is 1000-5000.

3. The positive electrode slurry according to claim 1, characterized in that The reaction conditions of the first reactant and the second reactant at least satisfy at least one of the following: (1) The molar ratio of the first reactant to the second reactant is 1:1 to 1:50; (2) The reaction temperature of the first reactant and the second reactant is 30° C. to 100° C., and the reaction time is 1 hour to 40 hours.

4. The positive electrode slurry according to claim 1, characterized in that: The solvent is selected from at least one of water, methanol, ethanol, toluene, xylene, acetonitrile, pyridine, cyclohexane, petroleum ether, n-hexane, ethyl ether, acetone, butanone, ethyl acetate, butyl acetate, dichloromethane, tetrahydrofuran, dimethyl sulfoxide, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.

5. The positive electrode slurry according to any one of claims 1 to 4, characterized in that: The positive electrode slurry also includes an active material, a conductive agent and a dispersion medium, and the mass ratio of the binder, the active material, the conductive agent and the dispersion medium is (0.05~0.15):(0.6~1.0):(0.05~0.15):(3~5).

6. The positive electrode slurry according to claim 5, characterized in that The active material includes at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, and lithium manganese oxide; the conductive agent includes at least one of conductive carbon black, conductive graphite, and carbon nanotubes; and the dispersion medium includes water and / or an organic solvent.

7. A method for preparing a positive electrode slurry according to any one of claims 1 to 6, characterized in that: The method comprises: adding a dispersion medium into a mixture of a binder, an active material and a conductive agent and stirring the mixture to obtain the positive electrode slurry.

8. A positive electrode sheet, characterized in that: include: A current collector and a positive electrode material layer located on the surface of the current collector, wherein the positive electrode material layer is formed by coating and drying the positive electrode slurry prepared by the positive electrode slurry according to any one of claims 1 to 6 or the positive electrode slurry prepared by the method for preparing the positive electrode slurry according to claim 7.

9. A lithium ion battery, characterized in that: Including the positive electrode sheet as claimed in claim 8.

Citation Information

Patent Citations

  • Method for preparing cross-linking waterborne adhesive for lithium ion batteries

    CN107793967A