Detection method and application of surface coating uniformity of battery positive electrode materials
By reacting the battery cathode material with an acidic solution, separating and detecting the dissolution amount, the problem of slow detection speed and high cost in the existing technology is solved, and a rapid and economical evaluation of the surface coating uniformity of the lithium-ion battery cathode material is achieved.
Patent Information
- Application Number
- CN202410912944.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The existing methods used to detect the uniformity of carbon coating on the surface of lithium-ion battery cathode materials have the problems of slow detection speed and high cost.
By mixing the battery cathode material with an acidic solution, reacting and performing solid-liquid separation, the iron and carbon content in the filtrate and insoluble powder is detected, and the carbon and iron dissolution amounts are calculated to evaluate the coating uniformity.
It improves the detection speed, reduces the detection cost, and realizes the quantification of surface coating uniformity evaluation, which can accurately evaluate the distribution uniformity of the coating layer.
Smart Images

Figure CN118465195B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion battery positive electrode materials, and in particular to a method for detecting the uniformity of surface coating of battery positive electrode materials and its application. Background Art
[0002] With the development of new energy, lithium-ion batteries are widely used as a secondary battery. They mainly rely on the movement of lithium ions between the positive and negative electrodes to work. During the charging and discharging process, lithium ions are embedded and de-embedded between the two electrodes: when charging, lithium ions are de-embedded from the positive electrode and embedded in the negative electrode through the electrolyte, and the negative electrode is in a lithium-rich state; the opposite is true during discharge.
[0003] In order to improve the cycle life of lithium-ion batteries, it is usually necessary to carbon-coat the core of the positive electrode material to prepare the positive electrode material of lithium-ion batteries. To determine the coating effect, precision instruments are generally used for analysis. Different instruments have different precision levels and different analysis principles, and the corresponding determination results also have certain differences.
[0004] At present, the commonly used detection methods for carbon coating are: ①C 13 Nuclear magnetic resonance uses the resonance transition of atomic nuclei in an external magnetic field to analyze molecular structure. Its advantage is sp 2 and sp 3 The peak separation is obvious, but the disadvantage is that it requires a relatively large sample; ② The Raman method uses the change in polarizability caused by lattice vibration to produce light scattering, obtain information such as molecular vibration and rotation, and study the molecular structure. The sp 2 / sp 3 ③ The infrared spectrum uses Gaussian function to fit the absorption peak of CH mode and decomposes sp 2 CH n and sp 3 CH n The peak area is calculated to obtain sp 2 / sp 3 value, and low cost, but this method is cumbersome to interpret and has low accuracy; ④ X-ray photoelectron spectroscopy uses photoelectron energy to determine binding energy and analyze element composition, with high sensitivity, but sp 2 and sp 3 The peaks differ by only 0.9 eV; ⑤ Electron energy loss spectrum The electron beam is inelastically scattered on the carbon surface, resulting in an energy loss region, sp 2 / sp 3 The above detection methods in the prior art are not conducive to improving the detection speed and reducing the detection cost. Summary of the invention
[0005] In view of the above problems, the present application provides a method and application for detecting the uniformity of the surface coating of a battery positive electrode material to solve the above-mentioned technical problems that are not conducive to improving the detection speed and reducing the detection cost.
[0006] In a first aspect, the present application provides a method for detecting the uniformity of the surface coating of a positive electrode material of a battery, comprising:
[0007] The carbon content of the positive electrode material of the battery is detected to obtain a first carbon content; wherein the positive electrode material of the battery comprises a core and a coating layer coated on the outer surface of the core, the core comprises lithium iron phosphate or lithium iron manganese phosphate, and the coating layer comprises carbon;
[0008] The battery positive electrode material is mixed with a first acidic solution to react and obtain a reaction mixture; the reaction mixture is subjected to solid-liquid separation to obtain a filtrate and an insoluble powder respectively;
[0009] Testing the iron content of the filtrate to obtain the amount of iron dissolved;
[0010] Detecting the carbon content of the insoluble powder to obtain a second carbon content, and obtaining a carbon dissolution amount according to the first carbon content and the second carbon content;
[0011] The surface coating uniformity of the battery positive electrode material is evaluated based on the iron element dissolution amount and the carbon element dissolution amount.
[0012] Optionally, the molar concentration of hydrogen ions in the first acidic solution is 0.1-1 mol / L.
[0013] Optionally, the first acidic solution is one of hydrochloric acid solution, sulfuric acid solution, acetic acid solution or oxalic acid solution.
[0014] Optionally, the mass ratio of the battery positive electrode material to the first acidic solution is 1:1.42-2.6.
[0015] Optionally, the battery positive electrode material is mixed with the first acidic solution and reacted under stirring, wherein the stirring speed is 75 to 250 r / min, the reaction temperature is 35 to 85° C., and the reaction time is 1 to 5 h.
[0016] Optionally, the amount of iron element dissolved is the mass concentration of iron element in the filtrate, and the amount of carbon element dissolved is the mass ratio of dissolved carbon element to the carbon element in the coating layer of the battery positive electrode material;
[0017] The evaluating the surface coating uniformity of the battery positive electrode material according to the iron element dissolution amount and the carbon element dissolution amount includes:
[0018] If the amount of iron element dissolved is less than or equal to 1800 ppm and the amount of carbon element dissolved is greater than or equal to 0.2%, the surface coating uniformity of the battery positive electrode material is qualified.
[0019] Optionally, the evaluating the surface coating uniformity of the battery positive electrode material according to the iron element dissolution amount and the carbon element dissolution amount further includes:
[0020] If the amount of iron element dissolved is less than or equal to 800 ppm and the amount of carbon element dissolved is greater than or equal to 0.4%, the surface coating uniformity of the battery positive electrode material is better.
[0021] Optionally, the iron content of the filtrate is detected by at least one of inductively coupled plasma emission spectroscopy, ultraviolet spectrometry, electrochemical method, atomic absorption method or atomic emission method.
[0022] Optionally, a high-frequency infrared carbon-sulfur analyzer is used to detect the carbon content of the battery positive electrode material or the insoluble powder.
[0023] In a second aspect, the present application provides a method for comparing the cycle life of multiple battery positive electrode materials, comprising:
[0024] According to the above-mentioned method for detecting the uniformity of the surface coating of the battery positive electrode material, a plurality of the battery positive electrode materials are respectively detected to obtain a plurality of detection results, wherein the detection results include the amount of iron element dissolution and the amount of carbon element dissolution;
[0025] The plurality of detection results are compared to compare the cycle life of a plurality of battery positive electrode materials.
[0026] The present application provides a method and application for detecting the uniformity of the surface coating of a positive electrode material of a battery, wherein the carbon content of the positive electrode material of the battery is detected to obtain a first carbon content; wherein the positive electrode material of the battery comprises a core and a coating layer coated on the outer surface of the core, the core comprises lithium iron phosphate or lithium iron manganese phosphate, and the coating layer comprises carbon; the positive electrode material of the battery is mixed with a first acidic solution for reaction to obtain a reaction mixture; the reaction mixture is subjected to solid-liquid separation to obtain a filtrate and an insoluble powder respectively; the iron content of the filtrate is detected to obtain the amount of iron dissolved; the carbon content of the insoluble powder is detected to obtain a second carbon content, and the amount of carbon dissolved is obtained according to the first carbon content and the second carbon content; the surface coating uniformity of the positive electrode material of the battery is evaluated according to the amount of iron dissolved and the amount of carbon dissolved; in the above manner, the positive electrode material of the battery is mixed with the first acidic solution for reaction, and the coating layer is subjected to a certain degree of corrosion damage, wherein the area with a thinner thickness of the coating layer may be completely corroded and damaged, exposing the core In an acidic environment; for multiple battery positive electrode materials of the same batch obtained by the same preparation method, the coating content is almost the same, the more uniform the coating is distributed on the outer surface of the core, the larger the area of the outer surface of the core is, the smaller the area of the outer surface of the core is not coated, and the smaller the area of the area with thin coating thickness; therefore, the more uniform the coating is distributed on the outer surface of the core, the larger the contact area between the coating itself and the first acidic solution, and the higher the amount of carbon element dissolution; and the more uniform the coating is distributed on the outer surface of the core, the larger the area of the outer surface of the core is not coated. The smaller the area, the smaller the contact area between the core and the first acidic solution before the coating is corroded and damaged. At the same time, the smaller the area of the thinner coating layer, the smaller the area of the outer surface of the core that is completely corroded and damaged. The smaller the contact area between the core and the first acidic solution after the coating is corroded and damaged, the smaller the amount of iron dissolved. The amount of iron dissolved and the amount of carbon dissolved during the reaction are used as the basis for evaluating the uniformity of the surface coating, which is conducive to improving the detection speed and reducing the detection cost. At the same time, the quantification of the evaluation index of the uniformity of the surface coating is achieved. These aspects or other aspects of the present application will be more concise and easy to understand in the description of the following embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic flow chart of a method for detecting the uniformity of the surface coating of a battery positive electrode material provided in an embodiment of the present application is shown. DETAILED DESCRIPTION
[0028] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0029] In order to enable those skilled in the art to better understand the solutions of the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application.
[0030] In the embodiments of the present application, it should be noted that, in this article, relational terms such as first and second, etc. are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations.
[0031] Moreover, the terms "comprises," "comprising," or any other variation thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of additional identical elements in the process, method, article, or apparatus that includes the element.
[0032] In the description of the embodiments of the present application, words such as "example" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "example" or "for example" in the embodiments of the present application is not to be interpreted as being more preferred or having more advantages than another embodiment or design. The use of words such as "example" or "for example" is intended to present relative concepts in a clear manner.
[0033] In addition, the "plurality" in the embodiments of the present application refers to two or more than two. In view of this, in the embodiments of the present application, "plurality" can also be understood as "at least two". "At least one" can be understood as one or more, for example, one, two or more. For example, including at least one means including one, two or more, and there is no limit on which ones are included. For example, including at least one of A, B and C, then A, B, C, A and B, A and C, B and C, or A, B and C can be included.
[0034] It should be noted that, in the embodiments of the present application, "and / or" describes the association relationship of the associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / ", unless otherwise specified, generally indicates that the associated objects before and after are in an "or" relationship.
[0035] As used herein, the term "lithium iron phosphate" generally has the formula Li x Fe y PO4, wherein x is 0.8 to 1.2 and y is 0.8 to 1.2. And wherein up to 10 atomic % (e.g., up to 3 atomic % or up to 5 atomic % or up to 8 atomic %) of the iron may be substituted by the dopant metal, up to 10 atomic % (e.g., up to 3 atomic % or up to 5 atomic % or up to 8 atomic %) of the phosphate may be substituted by SO4 and / or SiO4, and up to 10 atomic % of the Li may be substituted by Na and / or K.
[0036] Exemplarily, “lithium iron phosphate” may have the formula LiFePO4, wherein up to 10 atomic % (e.g., up to 3 atomic % or up to 5 atomic % or up to 8 atomic %) of Fe may be substituted by dopant metal, and up to 10 atomic % (e.g., up to 3 atomic % or up to 5 atomic % or up to 8 atomic %) of phosphate may be substituted by SO4 and / or SiO4, and up to 10 atomic % of Li may be substituted by Na and / or K.
[0037] For example, "lithium iron phosphate" may have the formula Li x Fe y PO4, wherein x is from 0.8 to 1.2 and y is from 0.8 to 1.2.
[0038] Illustratively, “lithium iron phosphate” may have the formula LiFePO 4 .
[0039] Exemplarily, the dopant metal may be one or more selected from Mn, Co, Ni, Al, Mg, Sn, Pb, Nb, B, Cu, Cr, Mo, Ru, V, Ga, Ca, Sr, Ba, Ti, Zr, and Cd.
[0040] Exemplarily, the dopant metal may be one or more selected from Mn, Al, Ti and Zr. For example, when the dopant metal is Mn, the lithium iron phosphate doped with Mn may be referred to as "lithium iron manganese phosphate", which generally has the formula Li x Fe y Mn z PO4, wherein x is from 0.8 to 1.2 and the sum of y and z is from 0.8 to 1.2.
[0041] The lithium iron phosphate may be undoped.
[0042] In the case where "lithium iron phosphate" is doped, a precursor containing the dopant is usually added during the milling step.
[0043] As used herein, the description of “a1-a2” means “greater than or equal to a1” and “less than or equal to a2”, for example, x is 0-1, that is: 0≤x≤1.
[0044] An embodiment of the present application provides a method for detecting the uniformity of the surface coating of a positive electrode material of a battery. Figure 1 As shown, the method for detecting the uniformity of the surface coating of the battery positive electrode material comprises the following steps:
[0045] a) detecting the carbon content of the positive electrode material of the battery to obtain a first carbon content; wherein the positive electrode material of the battery comprises a core and a coating layer coated on the outer surface of the core, the core comprises lithium iron phosphate or lithium iron manganese phosphate, and the coating layer comprises carbon.
[0046] Among them, the battery positive electrode material is a lithium-ion battery positive electrode material, and its core includes lithium iron phosphate (Li x Fe y PO4) or lithium iron manganese phosphate (Li x Fe y Mn z PO4).
[0047] Therein, the coating layer may comprise only carbon.
[0048] Among them, the coating layer can be based on positive electrode lithium replenishment technology, including carbon and lithium oxalate. Among them, the lithium replenishment technology is to provide an additional portion of lithium to offset the lithium consumed by the SEI film, thereby increasing the capacity of the lithium-ion battery. Lithium replenishment technology includes positive electrode lithium replenishment and negative electrode lithium replenishment. Positive electrode lithium replenishment mainly includes adding high-charge and low-discharge materials or lithium compounds that decompose at high potential to release lithium and gas. Common lithium compounds used for lithium replenishment include lithium azide, square acid lithium salts, lithium oxalate, etc.
[0049] The first carbon element content is the carbon element content in the coating layer of the battery positive electrode material before reacting with the first acidic solution.
[0050] b) mixing the positive electrode material of the battery with the first acidic solution to react and obtain a reaction mixture; performing solid-liquid separation on the reaction mixture to obtain a filtrate and an insoluble powder respectively.
[0051] Among them, the battery positive electrode material is mixed and reacted with the first acidic solution, and the first acidic solution has an acidic corrosive effect on the battery positive electrode material. First, the coating layer of the battery positive electrode material is corroded and destroyed, resulting in the dissolution of carbon elements in the coating layer; after the coating layer is corroded and damaged to a certain extent, part of the core is exposed to the first acidic solution so that the core is corroded and damaged to a certain extent, resulting in the dissolution of the main components in the core. The main components in the core can be, for example, at least one of lithium, iron and phosphate.
[0052] The carbon elements dissolved from the coating layer enter into the filtrate of the reaction mixture, and the main components dissolved from the inner core enter into the filtrate of the reaction mixture.
[0053] c) The iron content of the filtrate is tested to obtain the amount of iron dissolved.
[0054] The first acidic solution does not contain iron, and all the iron in the filtrate is derived from the iron dissolved from the inner core. Therefore, the result of detecting the iron content of the filtrate is the amount of iron dissolved from the inner core.
[0055] The iron content of the filtrate is detected by at least one of inductively coupled plasma (ICP) emission spectroscopy, ultraviolet spectrometry, electrochemical method, atomic absorption method or atomic emission method. For example, the iron content of the filtrate can be detected by inductively coupled plasma emission spectroscopy.
[0056] d) detecting the carbon content of the insoluble powder to obtain a second carbon content, and obtaining a carbon dissolution amount according to the first carbon content and the second carbon content.
[0057] The second carbon content is the carbon content in the coating layer of the positive electrode material after the battery reacts with the first acidic solution. The difference between the first carbon content and the second carbon content is the amount of carbon dissolved in the positive electrode material during the mixing reaction with the first acidic solution.
[0058] For example, a high-frequency infrared carbon-sulfur analyzer can be used to detect the carbon content of the battery positive electrode material or the insoluble powder.
[0059] e) Evaluate the surface coating uniformity of the battery positive electrode material based on the amount of iron and carbon dissolution.
[0060] Among them, in the battery positive electrode material, the more evenly the coating layer is distributed on the outer surface of the core, the larger the contact area between the coating layer itself and the first acidic solution, therefore, the better the coating uniformity of the coating layer, the greater the amount of carbon element dissolved from the coating layer.
[0061] Among them, in the battery positive electrode material, the more uniformly the coating layer is distributed on the outer surface of the core, the smaller the contact area between the core and the first acid solution before the coating layer is corroded and damaged; the core will only contact the first acid solution after part of the structure of the coating layer is corroded and damaged, and the more uniformly the coating layer is distributed on the outer surface of the core, the shorter the contact time between the core and the first acid solution after the coating layer is corroded and damaged; therefore, the better the coating uniformity of the coating layer, the smaller the amount of iron element dissolution in the core.
[0062] In this embodiment, the battery positive electrode material is mixed with the first acidic solution for reaction, and the amount of iron element and carbon element dissolved during the reaction is used as the basis for evaluating the surface coating uniformity, which is beneficial to improving the detection speed and reducing the detection cost; at the same time, the quantification of the surface coating uniformity evaluation index is achieved.
[0063] In step b), if the first acidic solution corrodes the positive electrode material of the battery too lightly, the coating layer and the core cannot be corroded, and the corresponding elements in the coating layer and the core cannot be dissolved, thereby affecting the detection effect. If the first acidic solution corrodes the positive electrode material of the battery too heavily, the coating layer can be completely corroded and destroyed regardless of whether the coating layer is evenly coated on the outer surface of the core, which will cause a large amount of corresponding elements in the coating layer and the core to be dissolved, thereby affecting the detection effect.
[0064] As an embodiment, in step b), the molar concentration of hydrogen ions in the first acidic solution is 0.1 to 1 mol / L. In this embodiment, the hydrogen ion content in the first acidic solution is controlled within the above range, which can have a certain corrosive effect on the coating layer but cannot completely destroy it in a short time, which is conducive to improving the detection effect.
[0065] In some embodiments, the first acidic solution is one of a hydrochloric acid solution, a sulfuric acid solution, an acetic acid solution, or an oxalic acid solution.
[0066] In some embodiments, in step b), the mass ratio of the positive electrode material of the battery to the first acidic solution is 1:1.42-2.6. For example, the mass ratio of the positive electrode material of the battery to the first acidic solution can be 1g:1.5g, 1g:1.6g, 1g:1.7g, 1g:1.8g, 1g:1.9g, 1g:2g, 1g:2.1g, 1g:2.2g, 1g:2.3g, 1g:2.4g or 1g:2.5g, etc., but is not limited to the listed values, and other values not listed in the above numerical range are also applicable.
[0067] In some embodiments, in step b), the battery positive electrode material is mixed with the first acidic solution and reacted under stirring, wherein the stirring speed is 75 to 250 r / min, the reaction temperature is 35 to 85° C., and the reaction time is 1 to 5 h.
[0068] Illustratively, in step b), the temperature of heating and stirring is 35-85°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0069] Illustratively, in step b), the heating and stirring time is 1 to 5 h, for example, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h or 4 h, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0070] Illustratively, in step b), magnetic stirring can be adopted, and the stirring rate of heating stirring (the set speed of the magnetic stirrer) can be 75 to 250 r / min, for example, 80 r / min, 100 r / min, 120 r / min, 140 r / min, 160 r / min, 180 r / min or 200 r / min, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0071] Exemplarily, in step b), heating and stirring are performed in a beaker.
[0072] As an embodiment, the amount of iron dissolved is the mass concentration of iron in the filtrate. The amount of carbon dissolved is the mass ratio of dissolved carbon to the carbon in the coating layer of the positive electrode material of the battery; for example, if is the first carbon element content, is the second carbon element content, then the carbon element dissolution amount .
[0073] In step e), the surface coating uniformity of the battery positive electrode material is evaluated according to the amount of iron element dissolution and the amount of carbon element dissolution, including:
[0074] e-1) If the amount of iron element dissolved is less than or equal to 1800 ppm and the amount of carbon element dissolved is greater than or equal to 0.2%, the surface coating uniformity of the battery positive electrode material is qualified.
[0075] In some embodiments, in step e), the surface coating uniformity of the battery positive electrode material is evaluated according to the amount of iron element dissolution and the amount of carbon element dissolution, and further includes:
[0076] e-2) If the amount of iron element dissolved is less than or equal to 800 ppm and the amount of carbon element dissolved is greater than or equal to 0.4%, the surface coating uniformity of the battery positive electrode material is better.
[0077] Exemplarily, the battery positive electrode material can be prepared as follows:
[0078] S101, adding a lithium source, an iron source and a phosphorus source to a first solvent to obtain a first mixture;
[0079] Among them, the lithium source is selected from one or more of lithium carbonate, lithium hydroxide, lithium acetate, lithium citrate, and lithium dihydrogen phosphate; the iron source is selected from one or more of iron oxide, ferric oxide, ferric citrate, ferric phosphate, and ferrous oxalate; the phosphorus source is selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, phosphoric acid, and lithium dihydrogen phosphate.
[0080] The first solvent is an organic solvent or water, and the organic solvent is selected from one of methanol, ethanol, acetone and N-methyl-2-pyrrolidone.
[0081] S102, grinding the first mixture using a grinder to obtain a first slurry;
[0082] The abrasive particle size D50 of the first slurry can be controlled to be 0.25-0.5 μm.
[0083] S103, spray drying the first slurry to obtain a first powder;
[0084] S104, calcining the first powder under a protective gas atmosphere to obtain lithium iron phosphate;
[0085] The calcination temperature of the first powder is 650-795° C., and the first powder is calcined under a protective atmosphere, wherein the protective gas is selected from one or more of argon, helium, nitrogen, and carbon dioxide.
[0086] The lithium iron phosphate obtained in step S104 is the core of the battery positive electrode material.
[0087] S105, adding lithium iron phosphate (core) and the first carbon source into the second solvent and mixing them to obtain a second mixture;
[0088] The second solvent is water, and the first carbon source is selected from one or more of glucose, sucrose, citric acid, polyethylene glycol, polyvinyl butyral, polyvinyl alcohol, polyacrylonitrile, starch, and cellulose.
[0089] S106, spray drying the second mixture to obtain a second powder;
[0090] S107, calcining the second powder under a protective gas atmosphere to obtain a modified lithium iron phosphate composite material;
[0091] The second powder is calcined at a temperature of 350-450° C. and is calcined in a protective atmosphere, wherein the protective gas is selected from one or more of argon, helium, nitrogen and carbon dioxide.
[0092] Through steps S105 to S107, carbon is coated on the outer surface of the lithium iron phosphate obtained in step S104 to form a coating layer. The mass ratio of the residual amount of carbon element in the first carbon source after roasting to the lithium iron phosphate core is (1.0-5.0): (92-100).
[0093] Those skilled in the art should understand that the battery positive electrode material can be prepared according to other methods described in the prior art.
[0094] An embodiment of the present application provides a method for comparing the cycle life of multiple battery positive electrode materials, comprising the following steps:
[0095] 1) According to the above-mentioned method for detecting uniformity of surface coating of battery positive electrode materials, multiple battery positive electrode materials are respectively detected to obtain multiple detection results, including the amount of iron element dissolution and the amount of carbon element dissolution;
[0096] 2) Compare multiple test results to compare the cycle life of multiple battery positive electrode materials;
[0097] Among them, the greater the amount of carbon element dissolved from the battery positive electrode material and the smaller the amount of iron element dissolved from the battery positive electrode material, the longer the cycle life of the battery made using the battery positive electrode material.
[0098] In this embodiment, the cycle life of the battery made of the battery positive electrode material is indirectly determined based on the comparison results of the carbon element dissolution amount and the iron element dissolution amount of the battery positive electrode material.
[0099] Example
[0100] The present embodiment provides a method for detecting the uniformity of the surface coating of the battery positive electrode material. The battery positive electrode material to be detected is divided into four equal parts, each with a mass of 5 g. Each part of the battery positive electrode material is detected according to the following steps:
[0101] Step (1): Take 5g of battery positive electrode material and perform high-frequency red sulfur carbon analyzer test and analysis to obtain the first carbon element content ;
[0102] Step (2): 5 g of the above-mentioned battery positive electrode material is placed in a beaker, 30 mL of 0.5 mol / L HCL solution is added, a magnetic bar is placed in the beaker, the speed is set to 100 r / min on the magnetic stirrer, and stirring is performed for 2 h. After the reaction is completed, the solution is quickly filtered to obtain a filtrate and a powder. The powder is repeatedly washed with ethanol to remove electrolyte impurities, and then dried in a vacuum oven for 8 h;
[0103] Step (3): The filtrate obtained in step (2) is subjected to ICP testing to obtain the amount of iron dissolved in the positive electrode material of the battery; the obtained powder is tested and analyzed by a high-frequency red sulfur carbon analyzer to obtain the second carbon content. ,Will As the amount of carbon element dissolved.
[0104] Embodiment 1 to Embodiment 3
[0105] According to the above steps, the first battery positive electrode material (sample 1, embodiment 1), the second battery positive electrode material (sample 2, embodiment 2) and the third battery positive electrode material (sample 3, embodiment 3) were tested respectively. The results are shown in Table 1.
[0106] Comparative Example 1
[0107] The method for detecting the uniformity of the surface coating of the positive electrode material of the battery provided in this comparative example is to divide the non-carbon-coated lithium iron phosphate positive electrode material (sample 4) to be detected into four equal portions, each with a mass of 5g, and each portion of the non-carbon-coated lithium iron phosphate positive electrode material is detected according to the following steps:
[0108] Step (1): Take 5g of lithium iron phosphate positive electrode material that has not been carbon-coated and perform a high-frequency red sulfur carbon analyzer test and analysis to obtain the first carbon element content ;
[0109] Step (2): 5 g of the above-mentioned lithium iron phosphate positive electrode material that has not been carbon-coated is placed in a beaker, 30 mL of a 0.5 mol / L HCL solution is added, a magnetic bar is placed, the speed is set to 100 r / min on a magnetic stirrer, and stirring is performed for 2 h. After the reaction is completed, the solution is quickly filtered to obtain a filtrate and a powder. The powder is repeatedly washed with ethanol to remove electrolyte impurities, and then dried in a vacuum oven for 8 h;
[0110] Step (3): The filtrate obtained in step (2) is subjected to ICP testing to obtain the amount of iron dissolved in the positive electrode material of the battery; the obtained powder is tested and analyzed by a high-frequency red sulfur carbon analyzer to obtain the second carbon content. ,Will As the amount of carbon element dissolved.
[0111] The results of Comparative Example 1 are shown in Table 1.
[0112] Battery positive electrode material cycle life test
[0113] According to the mass ratio of battery positive electrode material (lithium iron phosphate): conductive carbon black: PVDF (Polyvinylidene fluoride) = 95%: 3%: 2%, a certain amount of materials are weighed, and PVDF is dissolved in a certain amount of NMP (N-methyl-2-pyrrolidone), which specifically includes the following steps:
[0114] The battery positive electrode material and conductive carbon black were added, put into a blender and stirred for 40 minutes to obtain a first mixture; PVDF was then added to the first mixture and mixed evenly to prepare a uniform positive electrode slurry.
[0115] The prepared positive electrode slurry is evenly coated on aluminum foil to make a pole piece, and then dried in an oven at 115°C to make a positive electrode sheet for standby use; the positive electrode sheet is assembled with a separator, a lithium sheet, and an electrolyte into a button-type full battery.
[0116] The button-type full battery was subjected to 0.1C and 1C rate tests with a test voltage of 3-3.65V; a storage test was performed with a test voltage of 3-3.65V, 55°C, fully charged storage, and a storage time of 7 days (7D).
[0117] According to the steps of the above battery positive electrode material cycle life test, the battery positive electrode materials used in Example 1, Example 2, Example 3 and Comparative Example 1 were made into button-type full batteries, and rate tests and storage tests were performed respectively. The results are shown in Table 1.
[0118] Table 1 Experimental results
[0119]
[0120] Carbon coating the inner core of the positive electrode material of the battery can improve the conductivity of the positive electrode material of the battery on the one hand, and can provide a stable chemical and electrochemical reaction interface on the other hand, thereby improving its storage performance. The uniformity of the coating layer on the outer surface of the inner core also has a great influence on the conductivity and interface stability of the positive electrode material of the battery. In other words, the uniformity of the coated carbon is positively correlated with the rate performance and storage performance of the positive electrode material of the battery, which can reversely verify the coating uniformity of the positive electrode material of the battery, thereby judging the accuracy of the detection method of the surface coating uniformity of the positive electrode material of the battery of the embodiment of the present application.
[0121] As shown in the data in Table 1, the smaller the amount of iron element dissolved, the larger the amount of carbon element dissolved, the better the coating uniformity, and at the same time, the better the test rate performance and storage performance; the larger the amount of iron element dissolved, the smaller the amount of carbon element dissolved, the worse the coating uniformity, and at the same time, the test rate performance and storage performance are also worse.
[0122] It can be seen from Table 1 that the experimental results of the method for detecting the uniformity of the surface coating of the battery positive electrode material of the embodiment of the present application and the experimental results of the battery positive electrode material cycle life detection test are able to correspond to each other. The method for detecting the uniformity of the surface coating of the battery positive electrode material of the embodiment of the application has high accuracy and is reliable.
[0123] The above is only an implementation method of the present application. It should be pointed out that a person skilled in the art can make improvements without departing from the inventive concept of the present application, but these improvements are within the scope of protection of the present application.
Claims
1. A method for detecting the uniformity of the surface coating of a battery positive electrode material, characterized in that: include: The carbon content of the positive electrode material of the battery is detected to obtain a first carbon content; wherein the positive electrode material of the battery comprises a core and a coating layer coated on the outer surface of the core, the core comprises lithium iron phosphate or lithium iron manganese phosphate, and the coating layer comprises carbon; The battery positive electrode material is mixed with a first acidic solution to react and obtain a reaction mixture; the reaction mixture is solid-liquid separated to obtain a filtrate and an insoluble powder respectively; the molar concentration of hydrogen ions in the first acidic solution is 0.1 to 1 mol / L, the reaction temperature is 35 to 85° C., and the reaction time is 1 to 5 hours; Testing the iron content of the filtrate to obtain the amount of iron dissolved; Detecting the carbon content of the insoluble powder to obtain a second carbon content, and obtaining a carbon dissolution amount according to the first carbon content and the second carbon content; The surface coating uniformity of the battery positive electrode material is evaluated based on the iron element dissolution amount and the carbon element dissolution amount.
2. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 1, characterized in that: The first acidic solution is one of hydrochloric acid solution, sulfuric acid solution, acetic acid solution or oxalic acid solution.
3. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 2, characterized in that: The mass ratio of the battery positive electrode material to the first acidic solution is 1:1.42-2.
6.
4. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 1, characterized in that: The battery positive electrode material is mixed with the first acidic solution and reacted under stirring, wherein the stirring speed is 75 to 250 r / min.
5. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 1, characterized in that: The amount of iron element dissolved is the mass concentration of iron element in the filtrate, and the amount of carbon element dissolved is the mass ratio of dissolved carbon element to the carbon element in the coating layer of the battery positive electrode material; The evaluating the surface coating uniformity of the battery positive electrode material according to the iron element dissolution amount and the carbon element dissolution amount includes: If the amount of iron element dissolved is less than or equal to 1800 ppm and the amount of carbon element dissolved is greater than or equal to 0.2%, the surface coating uniformity of the battery positive electrode material is qualified.
6. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 5, characterized in that: The evaluating the surface coating uniformity of the battery positive electrode material according to the iron element dissolution amount and the carbon element dissolution amount further includes: If the amount of iron element dissolved is less than or equal to 800 ppm and the amount of carbon element dissolved is greater than or equal to 0.4%, the surface coating uniformity of the battery positive electrode material is better.
7. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 1, characterized in that: The iron content of the filtrate is detected by at least one of inductively coupled plasma emission spectrometry, ultraviolet spectrometry, electrochemical method, atomic absorption method or atomic emission method.
8. The method for detecting the uniformity of the surface coating of the positive electrode material of a battery according to claim 1, characterized in that: A high-frequency infrared carbon-sulfur analyzer is used to detect the carbon content of the battery positive electrode material or the insoluble powder.
9. A method for comparing the cycle life of multiple battery positive electrode materials, characterized in that: include: According to the method for detecting the uniformity of the surface coating of the battery positive electrode material as described in any one of claims 1 to 8, a plurality of the battery positive electrode materials are respectively detected to obtain a plurality of detection results, wherein the detection results include the dissolution amount of iron element and the dissolution amount of carbon element; and the plurality of the detection results are compared to compare the cycle life of the plurality of battery positive electrode materials.
Citation Information
Patent Citations
Low-gas-production high-capacity ternary positive electrode material
CN112151775A
Method for testing carbon coating integrity of silicon-carbon coated negative electrode material
CN115575278A
Rapid detection method for cycle life of positive electrode material
CN117330725A
Method and device for comparing coating integrity of positive electrode active material
CN117969742A
Device for detecting integrity and thickness uniformity of nano coating layer