A carbon-based negative electrode material for sodium ion battery and its preparation method and application
By using a combination of a surface-activated hard carbon core with an organic coating and a sulfur-selenium doped layer in the sodium-ion battery negative electrode material, the problem of low sodium storage capacity of the sodium-ion battery negative electrode material during the carbonization process is solved and significantly improved. It improves the conductivity and cycle stability and improves the overall performance of sodium-ion batteries.
Patent Information
- Application Number
- CN202410932081.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing sodium-ion battery anode materials are prone to graphitization reactions during the carbonization process, resulting in low sodium storage capacity, or the hard carbon precursor is difficult to graphitize at high temperatures, resulting in low carbon yield, which cannot effectively improve the performance of sodium-ion batteries. performance.
The surface-activated hard carbon core is mixed with an organic coating solution, and a metal salt and sulfur-selenium mixed solution is added for hydrothermal reaction to form a sulfur-selenium metallide doped layer, which is combined with the soft carbon precursor to form a composite material to improve conductivity. and structural stability.
It significantly improves the conductivity and cycle stability of sodium-ion battery anode materials, reduces the first irreversible capacity loss, enhances the adsorption and diffusion capabilities of sodium ions, and improves the rate performance and cycle performance of sodium-ion batteries.
Smart Images

Figure CN118472229B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery negative electrode materials, and in particular to a carbon-based negative electrode material for a sodium ion battery and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries have a similar working principle to the widely used lithium-ion batteries. Their energy density and cycle life are close to those of lithium-ion batteries. In addition, sodium sources are widely distributed, low-cost, safe, and easy to maintain. Sodium-ion batteries have great technical advantages in cost-sensitive and safety-demanding application scenarios such as energy storage power stations. As early as the 1980s, research on sodium-ion batteries began at the same time as lithium-ion batteries. So far, sodium-ion battery positive electrode materials such as layered oxides, polyanions, and Prussian blue have been developed to meet basic application needs, but the performance of negative electrode materials still restricts the further improvement of sodium-ion battery performance.
[0003] Among the common sodium ion negative electrode materials, amorphous carbon materials have high energy density and long cycle life, and are one of the most promising sodium ion negative electrode materials. The precursors for preparing amorphous carbon mainly include hard carbon precursors and soft carbon precursors. The carbon materials prepared from soft carbon precursors have high electrical conductivity. However, soft carbon precursors are prone to graphitization during the carbonization process, and the obtained carbon materials present a more ordered microstructure, resulting in a lower sodium storage capacity. Hard carbon precursors are difficult to graphitize at high temperatures, and the obtained carbon materials have a higher degree of disorder in the microstructure, a higher sodium storage capacity, but a lower carbon yield. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention
[0004] The object of the present invention is to provide a carbon-based negative electrode material for a sodium ion battery and a preparation method and application thereof.
[0005] In a first aspect, the present invention provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, comprising the following steps:
[0006] The hard carbon core after surface activation treatment is mixed and dispersed with an organic coating solution to prepare a coating dispersion;
[0007] The metal salt is stirred and dissolved in the coating dispersion, and the coating material is obtained by separation after stirring and reacting;
[0008] The coating material is mixed and dispersed with a sulfur-selenium mixed solution, and then hydrothermally reacted at 150° C. to 180° C. for 3 h to 5 h, and then cooled to room temperature, separated, dried, and then carbonized to obtain a doping material;
[0009] The doping material is impregnated into a soft carbon precursor, mixed and separated, and carbonized to obtain a composite material;
[0010] The composite material is immersed in a pre-sodium solution for mixing and separation, and then dried to obtain a carbon-based negative electrode material.
[0011] The hard carbon core used in the preparation method provided by the present invention has a disordered structure and a high specific surface area on its surface. After surface activation treatment, it is conducive to coating the surface with organic matter, thereby forming an organic coating layer on the surface of the hard carbon core. After impregnation with a metal salt solution, it is conducive to the metal salt to penetrate into the organic coating layer. At the same time, a hydrothermal reaction is carried out in a sulfur-selenium mixed solution, which is conducive to the mutual dispersion of sulfur-containing compounds, selenium-containing compounds and metal salts in the organic coating layer, thereby improving the uniformity of dispersion, thereby jointly forming a metal carbonized skeleton after carbonization. In addition, metal salts, sulfur elements and selenium elements jointly form sulfur-selenium metal compounds, which is conducive to improving the overall structural stability. The method provided by the present invention is simple and easy to operate, does not require complex equipment, and is conducive to large-scale industrial production.
[0012] Optionally, the mass ratio of the hard carbon core to the solute in the organic coating solution is 1:(0.1-0.5).
[0013] Optionally, the mass ratio of the metal salt to the hard carbon core is (0.05-0.15):1, and the metal element of the metal salt includes at least one of tungsten, cobalt, titanium, tin, antimony and molybdenum.
[0014] Optionally, the solutes of the sulfur-selenium mixed solution include soluble sulfur salts and soluble selenium salts.
[0015] Optionally, the mass ratio of the soluble sulfur salt, the soluble selenium salt and the coating material is (0.05-0.15):(0.05-0.15):1.
[0016] Optionally, in the process of mixing the hard carbon core after the surface activation treatment with the organic coating solution: the hard carbon core is formed by carbonization of at least one of glucose, sucrose, starch, lignin and cellulose.
[0017] Optionally, in the process of mixing the hard carbon core after the surface activation treatment with the organic coating solution: the solute of the organic coating solution includes at least one of melamine and hexamethylenetetramine and at least one of benzoic acid and terephthalic acid.
[0018] Optionally, in the process of mixing the hard carbon core after surface activation treatment with the organic coating solution: the hard carbon core is preliminarily subjected to surface activation treatment, including immersing the hard carbon core in a silane surfactant solution, stirring and dispersing, and then separating and drying.
[0019] Optionally, the soluble sulfur salt includes at least one of sodium sulfide, thiourea, thiol, and thioether.
[0020] Optionally, the soluble selenium salt includes at least one of selenious acid, selenic acid, and sodium selenite.
[0021] Optionally, during the process of mixing and dispersing the coating material with the sulfur-selenium mixed solution: selenium sulfide is also dispersed in the sulfur-selenium mixed solution.
[0022] Optionally, the doping material is immersed in the soft carbon precursor during the mixing and separation process: the soft carbon precursor includes at least one of asphalt tar and petroleum asphalt.
[0023] Optionally, the process of stirring and dissolving the metal salt in the coating dispersion and stirring the reaction includes: heating the coating dispersion to 70°C-80°C, adding the metal salt to the coating dispersion under stirring, stirring and cooling to 30°C-40°C and then keeping warm.
[0024] Optionally, the process of mixing and dispersing the coating material with the sulfur-selenium mixed solution and subjecting it to a hydrothermal reaction at 150°C-180°C includes: ultrasonically dispersing the coating material in benzyl alcohol to prepare a coating material dispersion, and heating the coating material dispersion to 150°C-180°C, and then dropping the sulfur-selenium mixed solution dropwise into the coating material dispersion for a hydrothermal reaction.
[0025] Optionally, the composite material is immersed in a pre-sodium solution for mixing and separation: the solute of the pre-sodium solution includes at least one of sodium carbonate, sodium sulfate, sodium chloride, sodium phosphate, sodium acetate, sodium formate, and sodium benzoate.
[0026] In the second aspect, the present invention also provides a carbon-based negative electrode material prepared by any of the above-mentioned optional preparation methods, comprising a hard carbon core and a sulfur-selenium doped layer and a sodium-doped carbon layer sequentially coated on the outside of the hard carbon core, and the sulfur-selenium doped layer comprises a metal carbide skeleton and sulfur elements and selenium elements doped in the metal carbide skeleton; wherein the thickness of the sulfur-selenium doped layer is 200nm-300nm, and the thickness of the sodium-doped carbon layer is 100nm-150nm.
[0027] The hard carbon core used in the carbon-based negative electrode material provided by the present invention has a disordered structure and a high specific surface area on the surface, can withstand a large volume change without being easily broken during the charge and discharge process, and the sulfur-selenium doped layer on the surface of the hard carbon core has a metal carbide skeleton with high electrical conductivity, which can significantly improve the electrical conductivity of the negative electrode material, reduce the internal resistance of the negative electrode, and improve the rate performance of the sodium ion battery. The doping of sulfur and selenium elements can provide more active sites, thereby promoting the adsorption and diffusion of sodium ions. At the same time, sulfur-selenium doping can also improve the structural stability of the negative electrode material, reduce the volume expansion and contraction of the negative electrode material during the cycle process, thereby improving the cycle performance of the sodium ion battery; the sodium-doped carbon layer outside the sulfur-selenium doped layer can effectively reduce the first irreversible capacity loss of the negative electrode material, thereby improving the initial coulomb efficiency of the sodium ion battery, and can also form a solid electrolyte interface (SEI) film on the surface of the negative electrode to prevent the decomposition of the electrolyte and the occurrence of side reactions, which is beneficial to improving the cycle stability of the sodium ion battery, and the thin layer of sodium-doped carbon layer is beneficial to the rapid diffusion and uniform distribution of sodium ions, thereby further improving the rate performance and cycle performance of the sodium ion battery.
[0028] Optionally, the metal carbide skeleton includes at least one of a tungsten carbide skeleton, a cobalt carbide skeleton, a titanium carbide skeleton, a tin carbide skeleton, an antimony carbide skeleton, and a molybdenum carbide skeleton.
[0029] Optionally, the sodium-doped carbon layer comprises a soft carbon skeleton and organic sodium and / or inorganic sodium doped in the soft carbon skeleton.
[0030] In a third aspect, the present invention also provides an application of a carbon-based negative electrode material in a sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic structural diagram of a carbon-based negative electrode material for a sodium ion battery provided by the present invention;
[0032] Figure 2 A flow chart of a carbon-based negative electrode material for a sodium ion battery provided by the present invention.
[0033] Description of reference numerals:
[0034] 1. Hard carbon core; 2. Sulfur-selenium doped layer; 3. Sodium-doped carbon layer. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0036] See also Figure 1 The present invention provides a carbon-based negative electrode material for a sodium ion battery, comprising a hard carbon core and a sulfur-selenium doped layer and a sodium-doped carbon layer sequentially coated on the outside of the hard carbon core. The hard carbon core as a matrix material has a good sodium storage capacity, and the sulfur-selenium doped layer is attached to the outside of the hard carbon core, and the sulfur and selenium doped therein have good conductivity, and the sodium storage carbon layer is not only pre-sodiumized, but also can play a good protective role on the sulfur-selenium doped layer.
[0037] Specifically, the thickness of the sulfur-selenium doped layer coated on the outside of the hard carbon core is 200nm-300nm; specifically, the thickness of the sodium-doped carbon layer coated on the outside of the sulfur-selenium doped layer is 100nm-150nm.
[0038] In fact, the sulfur-selenium doped layer also includes a metal carbide skeleton and sulfur and selenium elements doped in the metal carbide skeleton. The metal carbide skeleton not only has a good skeleton support effect, but also can provide more active sites for the doping of sulfur and selenium elements. At the same time, the pore structure in the metal carbide skeleton can provide sufficient space for volume expansion.
[0039] In some embodiments, the metal carbide skeleton in the sulfur-selenium doped layer includes at least one of a tungsten carbide skeleton, a cobalt carbide skeleton, a titanium carbide skeleton, a tin carbide skeleton, an antimony carbide skeleton, and a molybdenum carbide skeleton. In fact, the metal carbide skeleton has a high structural strength, which can effectively improve the structural stability of the sulfur-selenium doped layer, thereby ensuring the structural stability of the negative electrode material as a whole during the cycle.
[0040] In some embodiments, the sodium-doped carbon layer includes a soft carbon skeleton and organic sodium and / or inorganic sodium doped in the soft carbon skeleton. In fact, the soft carbon skeleton can be intertwined with the sulfur-selenium doped layer, that is, a composite structure of the sodium-doped carbon layer and the sulfur-selenium doped layer is formed at the connection between the sodium-doped carbon layer and the sulfur-selenium doped layer, thereby improving the tightness of the connection between the sodium-doped carbon layer and the sulfur-selenium doped layer.
[0041] See also Figure 2The present invention also provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, comprising the following steps:
[0042] S1, mixing and dispersing the hard carbon core after surface activation treatment with an organic coating solution to prepare a coating dispersion;
[0043] S2, stirring and dissolving the metal salt in the coating dispersion, stirring and reacting, and separating to obtain the coating material;
[0044] S3, mixing and dispersing the coating material and the sulfur-selenium mixed solution, and hydrothermally reacting them at 150° C.-180° C. for 3 h-5 h, cooling them to room temperature, separating, drying, and carbonizing them to obtain a doping material;
[0045] S4, impregnating the doping material into the soft carbon precursor, mixing and separating, and carbonizing to obtain a composite material;
[0046] S5. Immerse the composite material in a pre-sodium solution for mixing and separation, and obtain a carbon-based negative electrode material after drying.
[0047] In fact, in the process of preparing carbon-based negative electrode materials, after the hard carbon core is pre-activated, it is beneficial to coat the surface of the hard carbon core with organic matter, and form an organic coating layer on the surface of the hard carbon core. At the same time, after the organic coating layer is mixed and dispersed with the metal salt solution, the metal salt in the mixed dispersion penetrates into the organic coating layer, which is beneficial to improve the uniformity of the dispersion of the metal salt in the organic coating layer, and then immerse it in a sulfur-selenium mixed solution for hydrothermal reaction, which is beneficial to the infiltration of sulfur-containing compounds and selenium-containing compounds into the organic coating layer, and the sulfur-containing compounds, selenium-containing compounds and metal salts are mutually dispersed, so that after carbonization, the metal salt and the organic coating layer jointly form a metal carbonization skeleton, and the metal salt and sulfur and selenium jointly form sulfur-selenium metal compounds, which is beneficial to improve the structural stability of sulfur and selenium in the doping layer, and then immerse it in the soft carbon precursor, the surface is coated to form a soft carbon precursor layer and carbonized, so that a soft carbon skeleton is formed on the surface, which is beneficial to load the pre-sodium agent.
[0048] In some embodiments, during the execution of step S1, the hard carbon core is pre-treated with a surface activation treatment, for example, the hard carbon core can be immersed in a silane surfactant solution for stirring and dispersion, and then separated and dried. In fact, the solute in the silane surfactant solution can be γ-aminopropyltriethoxysilane. In fact, when the hard carbon core is subjected to a surface activation treatment, the hard carbon core can also be immersed in an alkaline activation solution such as a sodium hydroxide solution for separation, washing, and drying.
[0049] In some embodiments, during the execution of step S1, the average particle size of the hard carbon core after the surface activation treatment is 10 μm-20 μm, so that the hard carbon core has a better specific surface area, which is conducive to forming a more uniform organic coating layer on the surface.
[0050] In some embodiments, during the execution of step S1, the hard carbon core used is formed by carbonization of at least one of glucose, sucrose, starch, lignin, and cellulose. Specifically, the method for preparing the hard carbon core comprises the following steps: drying the bamboo board in an inert atmosphere at 80°C-90°C to remove moisture, transferring the bamboo board to an inert atmosphere at 700°C-800°C for carbonization treatment, and then crushing and sieving to obtain the hard carbon core.
[0051] In some embodiments, during the execution of step S1, the solute in the organic coating solution used includes at least one of melamine and hexamethylenetetramine and at least one of benzoic acid and terephthalic acid. In fact, after coating the surface of the hard carbon core with nitrogen-containing organic substances such as melamine and hexamethylenetetramine and subsequent carbonization, the sulfur-selenium doping layer can be in-situ nitrogen-doped, which can change the element composition of the doping layer and improve the electrochemical performance.
[0052] In some embodiments, during the execution of step S1, the hard carbon core after surface activation treatment is mixed with the organic coating solution, and then reacted at 40°C-50°C under ultrasonic dispersion for 0.5h-1h to obtain a coating dispersion. In fact, the mass ratio of the hard carbon core to the solute in the organic coating solution is 1:(0.1-0.5). By adjusting the mixing ratio of the hard carbon core and the organic solute, the thickness and density of the organic coating layer on the surface of the hard carbon core can be effectively controlled.
[0053] Specifically, during the execution of step S2, the metal salt used includes at least one of tungsten, cobalt, titanium, tin, antimony, and molybdenum. In fact, the metal salt used during the execution of step S2 must be completely soluble, for example, metal nitrates can be used. Specifically, the mass ratio of the metal salt to the hard carbon core is (0.05-0.15): 1. By adjusting the amount of the metal salt, the amount of the metal salt infiltrated into the organic coating layer can be adjusted, thereby adjusting the structural strength of the metal carbide skeleton formed during the subsequent carbonization process.
[0054] In some embodiments, during the execution of step S2, the coating dispersion is heated to 70°C-80°C, the metal salt is added to the coating dispersion under stirring and dissolved, and then the temperature is cooled to 30°C-40°C under stirring and kept for 2h-3h to obtain the coating material.
[0055] In fact, during the execution of step S2, the coating dispersion liquid is heated to 70°C-80°C at 3°C / min-5°C / min under ultrasonic dispersion, and then the metal salt is added and ultrasonically dispersed and dissolved, and then kept warm for 5min-10min. Then, the temperature is lowered to 30°C-40°C at 3°C / min-5°C / min and kept warm for 2h-3h, and then the filtered solid is obtained by suction filtration, and the filtered solid is centrifuged and washed with deionized water to obtain the coating material.
[0056] In some embodiments, during the execution of step S3, the solute in the sulfur-selenium mixed solution used includes soluble sulfur salts and soluble selenium salts, and the coating material is immersed in the sulfur-selenium mixed solution, and the soluble sulfur salts and soluble selenium salts are immersed in the surface organic coating layer of the coating material, and the organic coating layer captures the metal salt, soluble sulfur salt, and soluble selenium salt, and makes the metal salt, soluble sulfur salt, and soluble selenium salt uniformly distributed in the organic coating layer. Specifically, during the execution of step S3, the mass ratio of the soluble sulfur salt, the soluble selenium salt, and the coating material is (0.05-0.15): (0.05-0.15): 1.
[0057] Specifically, during the execution of step S3, the soluble sulfur salt used includes at least one of sodium sulfide, thiourea, mercaptan, and thioether. Specifically, during the execution of step S2, the soluble selenium salt used includes at least one of selenous acid, selenic acid, and sodium selenite.
[0058] In some embodiments, during the execution of step S3, selenium sulfide is also dispersed in the sulfur-selenium mixed solution. Since selenium sulfide is insoluble in water, after being dispersed, the selenium sulfide can directly enter the organic coating layer on the surface of the coating material and form binding sites for sulfur salts and selenium salts. At the same time, during the carbonization process, it will be directly decomposed into sulfur element and selenium element by heat.
[0059] In fact, when selenium sulfide is dispersed in the sulfur-selenium mixed solution and the coating material is mixed and dispersed with the sulfur-selenium mixed solution, ultrasonic treatment is performed under ultrasonic dispersion to promote selenium sulfide to enter the pores of the organic coating layer.
[0060] In some embodiments, during the execution of step S3, the process of mixing and dispersing the coating material with the sulfur-selenium mixed solution and performing a hydrothermal reaction includes: ultrasonically dispersing the coating material in benzyl alcohol to prepare a coating material dispersion, and heating the coating material dispersion to 150°C-180°C in an inert atmosphere and then keeping it warm for 1 hour, and then adding the sulfur-selenium mixed solution dropwise into the coating material dispersion for a hydrothermal reaction.
[0061] In some embodiments, the process of executing step S3 includes:
[0062] Ultrasonic dispersion of the coating material in benzyl alcohol to prepare a coating material dispersion;
[0063] Under an inert atmosphere, the coating material dispersion liquid is heated to 150-180°C at a rate of 3-5°C / min and then kept at this temperature for 1 hour;
[0064] The sulfur-selenium mixed solution is added dropwise into the coating material dispersion at a rate of 5 mL / min-6 mL / min, and an ultrasonic treatment environment is maintained to promote uniform dispersion;
[0065] After the addition is completed, the mixture is subjected to ultrasonic treatment and kept warm for 3 h to 5 h, then cooled to room temperature, separated, dried, and carbonized to obtain the doped material.
[0066] In some embodiments, the soft carbon precursor used in the process of performing step S4 includes at least one of asphalt tar and petroleum asphalt. In fact, the doping material is impregnated in the soft carbon precursor, and the soft carbon precursor forms a soft carbon precursor coating layer on the surface of the doping material, and then the soft carbon precursor can be carbonized to form a soft carbon skeleton after carbonization treatment. The soft carbon skeleton has a large pore structure and can also play a good protective role for the sulfur-selenium doping layer. At the same time, the doping material is impregnated in the soft carbon precursor, and the soft carbon precursor can also penetrate into the sulfur-selenium doping layer, thereby improving the tightness of the connection between the formed soft carbon skeleton and the sulfur-selenium doping layer.
[0067] In some embodiments, the solute of the pre-sodium solution used in the process of performing step S5 includes at least one of sodium carbonate, sodium sulfate, sodium chloride, sodium phosphate, sodium acetate, sodium formate, and sodium benzoate. In fact, after the composite material is immersed in the pre-sodium solution, the solute in the pre-sodium solution penetrates into the soft carbon skeleton on the surface of the composite material, thereby converting the soft carbon skeleton into a sodium-doped carbon layer.
[0068] Preparation Example
[0069] This preparation example provides a preparation and activation method for a hard carbon core, comprising the following steps: drying a bamboo tube in an argon atmosphere at 85°C until the mass does not change to obtain a hard carbon precursor, transferring the hard carbon precursor to an atmosphere furnace, carbonizing it in an argon atmosphere at 750°C, and grinding it to obtain a hard carbon core with an average particle size of 15 μm, and transferring the hard carbon core to an active solution containing γ-aminopropyltriethoxysilane and ultrasonically dispersing it for 1 hour, followed by filtering, washing, and drying to obtain a hard carbon core after surface activation treatment. Example 1
[0070] This embodiment 1 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, comprising the following steps:
[0071] S1. After mixing the hard carbon core prepared in the preparation example with the organic coating solution, the mixture is dispersed at 45° C. under ultrasonic conditions for 1 hour to obtain a coating dispersion; wherein the organic coating solution contains melamine and benzoic acid in a molar ratio of 2:1, and the mass ratio of the hard carbon core to the organic solute in the organic coating solution is 1:0.3;
[0072] S2. After heating the coating dispersion liquid from 45°C to 75°C at a rate of 5°C / min under ultrasonic dispersion, add cobalt nitrate to the coating dispersion liquid under ultrasonic state, dissolve by ultrasonic dispersion, cool to 35°C at a rate of 5°C / min, and keep warm for 3 hours, filter and wash the solid with deionized water, and centrifuge the filtered solid with deionized water at a speed of 2500rpm to obtain a coating material; wherein the mass ratio of cobalt nitrate to hard carbon core is 0.1:1;
[0073] S3, after ultrasonically dispersing the coating material in a benzyl alcohol solution to prepare a coating material dispersion, the coating material dispersion is heated from room temperature to 160°C at a rate of 5°C / min under an argon atmosphere, and then kept warm for 1 hour, the sulfur-selenium mixed solution is dripped into the coating material dispersion at a rate of 5 mL / min, and ultrasonic treatment is maintained to promote uniform dispersion, after the dripping is completed, ultrasonic treatment is performed and kept warm for 4 hours, and then cooled to room temperature, filtered, separated, washed with deionized water, and then dried, and carbonized in an argon atmosphere at 500°C to obtain a doping material; wherein, thiourea and selenic acid are dissolved in a mass ratio of 1:1 in the sulfur-selenium mixed solution, and the mass ratio of the solute in the sulfur-selenium mixed solution to the coating material is 0.2:1;
[0074] S4, adding the doping material into the asphalt tar, and impregnating it under pressure at 3.5 standard atmospheric pressure for 3 hours, and then centrifuging it at a speed of 2000 rpm to remove the excess soft carbon precursor on the surface, and then keeping it in an air atmosphere at 200° C. and cooling it to room temperature to obtain a composite material;
[0075] S5. Immerse the composite material in a sodium sulfate solution at 40° C. for 1 hour of ultrasonic dispersion, separate by filtration, wash the filtered solid with deionized water, and dry until the weight does not change to obtain a carbon-based negative electrode material. Example 2
[0076] This embodiment 2 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, which is different from the embodiment 1 in that: in step S1, hexamethylenetetramine and benzoic acid are dissolved in a molar ratio of 2:1 in the organic coating solution. Example 3
[0077] This embodiment 3 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, which is different from embodiment 1 in that: in step S2, bismuth tungstate is added to the coating dispersion under ultrasonic conditions, and the mass ratio of bismuth tungstate to hard carbon core is 0.2:1. Example 4
[0078] This embodiment 4 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, which is different from the embodiment 1 in that: in step S3, selenium sulfide with an average particle size of 5 nm is also dispersed in the sulfur-selenium mixed solution, and the mass ratio of selenium sulfide to the coating material is 0.05:1.
[0079] Comparative Example 1
[0080] This comparative example 1 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, comprising the following steps:
[0081] D1. The hard carbon core prepared in the preparation example was added into asphalt tar and impregnated under pressure at 3.5 standard atmospheric pressure for 3 hours, then centrifuged at 2000 rpm to remove excess soft carbon precursor on the surface, and then kept warm at 200°C in air atmosphere and cooled to room temperature to obtain a composite material;
[0082] D2. Immerse the composite material in a sodium sulfate solution and ultrasonically disperse it at 40° C. for 1 hour, then separate it by filtration, wash the filtered solid with deionized water, and dry it until the weight does not change to obtain a carbon-based negative electrode material.
[0083] Comparative Example 2
[0084] This comparative example 2 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, which is different from Example 1 in that in step S3, the thiourea solution is added dropwise to the coating material dispersion at a rate of 5 mL / min, and the mass ratio of the solute thiourea in the thiourea solution to the coating material is 0.2:1.
[0085] Comparative Example 3
[0086] This comparative example 3 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, which is different from Example 1 in that in step S3, the selenic acid solution is added dropwise to the coating material dispersion at a rate of 5 mL / min, and the mass ratio of the solute selenic acid in the selenic acid solution to the coating material is 0.2:1.
[0087] Comparative Example 4
[0088] This comparative example 4 provides a method for preparing a carbon-based negative electrode material for a sodium ion battery, which is different from Example 1 in that in step S3, the coating material is directly carbonized in an argon atmosphere at 500° C. to obtain a carbonized material, and in step S4, the carbonized material is added to asphalt tar.
[0089] Performance Testing
[0090] The carbon-based negative electrode materials prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were used as active materials, mixed with sodium carboxymethyl cellulose and acetylene black in a ratio of 90:5:5, and coated on the current collector copper foil, vacuum dried and rolled into a composite sheet, which was cut into a circular electrode sheet with a diameter of 10 mm, metallic sodium was used as the counter electrode and reference electrode, sodium hexafluorophosphate was used as the electrolyte, and assembled into CR2032 button batteries in an argon atmosphere glove box, and the following tests were performed:
[0091] First coulombic efficiency test: at room temperature, discharge at a constant current of 0.1C to 0.01V, then discharge at a constant current of 0.02C to 0.005V, and finally charge at a constant current of 0.1C to 2.0V. The capacity when charged to 2.0V is measured as the first reversible specific capacity, and the first coulombic efficiency is calculated. The results are shown in Table 1.
[0092] Cycle performance test: constant current charge and discharge were performed at room temperature with a current density of 0.1C, the charge and discharge voltage was limited to 0.005-2.0V, and the charge specific capacity after 100 cycles was measured, and the capacity retention rate after 100 cycles was calculated. The results are shown in Table 1.
[0093] Table 1
[0094] ,
[0095] In combination with Example 1 and Comparative Example 1, the doping of sulfur and selenium elements in Example 1 can significantly improve the conductivity and electrochemical activity of the negative electrode material, and the sulfur-selenium doping layer provides more active sites for the storage of sodium ions. It can be seen from Table 1 that the negative electrode material prepared in Example 1 has a higher charge capacity, and the cobalt carbide skeleton improves the mechanical strength and structural stability of the negative electrode material, and can accommodate the volume change during the charge and discharge process, thereby improving the capacity retention rate of the sodium ion battery.
[0096] In combination with Example 1 and Example 2, the hexamethylenetetramine used in Example 2 can form a more uniform and denser organic coating layer on the surface of the hard carbon core, and after forming the cobalt carbide skeleton, it can more stably coat the sulfur and selenium elements, and can form a more uniform sulfur-selenium coating layer after calcination, which can provide more active sites and better conductivity, thereby improving the charge capacity and first coulombic efficiency of the sodium ion battery.
[0097] In combination with Example 1 and Example 3, the bismuth salt used in Example 3 to make a bismuth carbide skeleton has an impact on the overall active sites and conductive properties of the negative electrode material, which causes the conductivity and resulting stability of the sulfur-selenium doped layer to be slightly worse than that of Example 1, resulting in a slight decrease in the charge capacity and first coulombic efficiency. This can illustrate that different metal carbide skeletons have an impact on the electrochemical properties of the negative electrode material.
[0098] In combination with Example 1 and Example 4, since selenium sulfide is doped in the sulfur-selenium mixed solution in Example 4, the active sites of the electrochemical reaction can be further increased, and the conductivity of the negative electrode material is improved, and the overall electrochemical activity of the sulfur-selenium doped layer is improved, thereby providing the sodium ion battery with a higher charge capacity, first coulombic efficiency and cycle performance.
[0099] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for preparing a carbon-based negative electrode material for a sodium ion battery, characterized in that: The following steps are involved: The hard carbon core is immersed in a silane surfactant solution, stirred and dispersed, and then separated and dried for surface activation treatment. The hard carbon core after the surface activation treatment is mixed and dispersed with an organic coating solution to obtain a coating dispersion, wherein the mass ratio of the hard carbon core to the solute in the organic coating solution is 1:(0.1-0.5); the solute in the organic coating solution includes at least one of melamine and hexamethylenetetramine and at least one of benzoic acid and terephthalic acid; The metal salt is stirred and dissolved in the coating dispersion, and the coating material is obtained by separation after stirring and reacting, wherein the mass ratio of the metal salt to the hard carbon core is (0.05-0.15):1, and the metal element of the metal salt includes at least one of tungsten, cobalt, titanium, tin, antimony, and molybdenum; The coating material is mixed and dispersed with a sulfur-selenium mixed solution, and the mixture is subjected to a hydrothermal reaction at 150° C.-180° C. for 3 h-5 h, and then cooled to room temperature, separated, dried, and then carbonized to obtain a doping material, wherein the solute of the sulfur-selenium mixed solution includes a soluble sulfur salt and a soluble selenium salt, and the mass ratio of the soluble sulfur salt, the soluble selenium salt, and the coating material is (0.05-0.15):(0.05-0.15):1; The doping material is impregnated into a soft carbon precursor, mixed and separated, and carbonized to obtain a composite material; The composite material is immersed in a pre-sodium solution for mixing and separation, and then dried to obtain a carbon-based negative electrode material.
2. The preparation method according to claim 1, characterized in that: In the process of mixing the hard carbon core after the surface activation treatment with the organic coating solution: the hard carbon core is formed by carbonization of at least one of glucose, sucrose, starch, lignin and cellulose.
3. The preparation method according to claim 1, characterized in that: In the process of mixing and dispersing the coating material with the sulfur-selenium mixed solution: the soluble sulfur salt includes sodium sulfide.
4. The preparation method according to claim 1, characterized in that: The soluble selenium salt includes sodium selenite.
5. The preparation method according to claim 1, characterized in that: Selenium sulfide is also dispersed in the sulfur-selenium mixed solution.
6. The preparation method according to claim 1, characterized in that: The doping material is immersed in the soft carbon precursor during the mixing and separation process: the soft carbon precursor includes at least one of asphalt tar and petroleum asphalt.
7. The preparation method according to claim 1, characterized in that: The process of stirring and dissolving the metal salt in the coating dispersion and stirring the reaction includes: heating the coating dispersion to 70°C-80°C, adding the metal salt to the coating dispersion under stirring, stirring and cooling to 30°C-40°C and then keeping the temperature.
8. The preparation method according to claim 1, characterized in that: The process of mixing and dispersing the coating material with the sulfur-selenium mixed solution and performing a hydrothermal reaction at 150° C.-180° C. includes: ultrasonically dispersing the coating material in benzyl alcohol to prepare a coating material dispersion liquid, heating the coating material dispersion liquid to 150° C.-180° C., and then dropwise adding the sulfur-selenium mixed solution into the coating material dispersion liquid for a hydrothermal reaction.
9. The preparation method according to claim 1, characterized in that: The composite material is immersed in a pre-sodium solution for mixing and separation: the solute of the pre-sodium solution includes at least one of sodium carbonate, sodium sulfate, sodium chloride, sodium phosphate, sodium acetate and sodium formate.
10. A carbon-based negative electrode material prepared by the preparation method according to any one of claims 1 to 8.
11. Use of a carbon-based negative electrode material prepared by the preparation method according to any one of claims 1 to 8 in a sodium ion battery.