A method for preparing reverse osmosis membrane for lithium extraction from salt lake
Through the selection of specific materials and fine process control, a reverse osmosis membrane with high stability and durability is formed, which solves the problem of insufficient stability and durability of the existing lithium extraction reverse osmosis membrane and improves the lithium extraction efficiency and membrane performance.
Patent Information
- Application Number
- CN202410750668.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Existing lithium extraction reverse osmosis membranes have problems in terms of stability and durability, causing membrane materials to easily deform, crack or age, reducing permeability and lithium extraction efficiency.
Using materials such as dimethyl sulfoxide, polyamic acid ester powder, sodium iodide powder and polysulfone imide membrane support membrane, a uniform and dense solution is formed by carefully controlling the solution temperature, standing time, soaking time and drying conditions. Membrane structure enhances membrane stability and durability.
It improves the permeability and selectivity of the reverse osmosis membrane, enhances its application effect and economic benefits in the process of extracting lithium from salt lakes, and ensures the membrane's high efficiency, stability and long-term durability.
Smart Images

Figure CN118477497B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of reverse osmosis membranes, and in particular to a method for preparing a reverse osmosis membrane for lithium extraction from a salt lake. Background Art
[0002] Lithium extraction from salt lakes refers to the process of extracting and separating lithium from salt lakes. Salt lakes are a special geological environment. Due to long-term evaporation and drying, water bodies rich in various salts and minerals are formed. Salt lakes usually contain rich lithium resources, mainly in the form of lithium sulfate and lithium chloride. Lithium extraction from salt lakes is an important way to mine lithium resources and has certain advantages.
[0003] Lithium extraction reverse osmosis membrane is an important technical means for extracting lithium from lithium resources such as salt lakes. It has the advantages of high efficiency, environmental protection, and energy saving. It is widely used in the field of lithium resource development and utilization. However, the existing lithium extraction reverse osmosis membranes have some problems in stability and durability. The existing lithium extraction reverse osmosis membranes have problems such as improper material selection and unreasonable preparation process during the preparation process, resulting in poor performance and stability of the membrane materials. Some membrane materials are prone to deformation, rupture or aging during long-term use, which reduces the membrane's permeability and selectivity, and affects the lithium extraction efficiency and product quality. To this end, we propose a method for preparing a salt lake lithium extraction reverse osmosis membrane. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a reverse osmosis membrane for extracting lithium from a salt lake.
[0005] In order to solve the problems raised in the above background technology, the present invention provides the following technical solutions: a method for preparing a reverse osmosis membrane for extracting lithium from a salt lake, wherein the specific steps of the method for preparing a reverse osmosis membrane for extracting lithium from a salt lake are as follows:
[0006] S1. It is necessary to prepare a polymer solution. A dimethyl sulfoxide solution is selected as a solvent and placed in a clean test tube without impurities. The dimethyl sulfoxide solution is heated. After the heating is completed, polyamic acid ester powder is slowly and evenly added to the dimethyl sulfoxide solution. During the process of adding the polyamic acid ester powder, it is necessary to stir evenly until the polyamic acid ester powder and the dimethyl sulfoxide solution are fully mixed, thereby completing the preparation of the polymer solution.
[0007] S2. After the polymer solution is prepared, the polymer solution is placed in a lightless environment, and then the polymer solution is filtered using a microporous filter membrane, and then sodium iodide powder is slowly and evenly added to the filtered polymer solution. During the process of adding the sodium iodide powder, the test tube is evenly shaken until the sodium iodide powder is completely dissolved in the polymer solution, thereby completing the preparation of the stabilizer solution;
[0008] S3, selecting a polysulfonimide membrane support film as a support layer, allowing the stabilizer solution to stand at room temperature, and then immersing the polysulfonimide membrane support film in the stabilizer solution, taking out the support layer after immersion, and slowly placing it in a constant temperature water bath for immersion, and solidifying on the surface of the support layer after immersion to form a dense film structure;
[0009] S4, taking out the support layer forming the thin film structure, and then placing it in a vacuum drying oven for vacuum drying, and obtaining a reverse osmosis membrane after vacuum drying.
[0010] As a further solution of the present invention: in S1, the volume of the selected dimethyl sulfoxide solution is 30 ml, the temperature of the dimethyl sulfoxide solution heating treatment is 58°C~62°C, the heating process needs to be slow and uniform heating, and the added amount of polyamic acid ester powder is 10g.
[0011] As a further solution of the present invention: in S2, after the polymer solution is prepared, it needs to be allowed to stand in a lightless environment at 24°C to 26°C for 1 hour, and sodium iodide powder is added after standing for 1 hour, and the amount of sodium iodide powder added is 100 mg.
[0012] As a further solution of the present invention: in S3, the stabilizer solution needs to be left to stand at room temperature of 24°C to 26°C for 1 hour, and then the polysulfoneimide membrane support membrane is evenly and slowly placed in the stabilizer solution for immersion for 12 hours.
[0013] As a further solution of the present invention: in S3, the temperature of the constant temperature water bath is 80° C., the water bath time is 2 hours, and after the water bath is finished, it can be observed that a uniform coating is attached to the surface of the support layer.
[0014] As a further solution of the present invention: in S3, after the immersion is completed, the support membrane should be carefully taken out to ensure that there are no bubbles or damage on the surface of the support membrane, and the support membrane without bubbles or damage on the surface is put into S4 for drying.
[0015] As a further solution of the present invention: in S2, the added sodium iodide powder needs to be filtered through a filter with a pore size of 50 μm, and the sodium iodide powder with a particle size less than 50 μm is selected.
[0016] As a further solution of the present invention: in S3, the stabilizer solution is filtered using a microporous filter membrane before use, and the pore size of the microporous filter membrane is 0.4 μm, which helps to remove the solid particles remaining in the stabilizer solution.
[0017] As a further solution of the present invention: in S4, the working temperature of the vacuum drying oven is set to 60° C., the air pressure is set to 80 Pa, and the drying time is set to 2 hours.
[0018] By adopting the above technical solution, compared with the prior art, the beneficial effects of the present invention are:
[0019] 1. The present invention uses selected materials including dimethyl sulfoxide, polyamic acid ester powder, sodium iodide powder and polysulfonimide membrane support membrane. The selection of these materials plays a vital role in the performance and stability of the membrane. First, dimethyl sulfoxide as a solvent has good solubility and thermal stability, which is conducive to the dissolution and mixing of polymers, thereby ensuring the uniformity and stability of the membrane material. Polyamic acid ester powder as a polymer raw material can form a uniform polymer structure in the solution, providing a good foundation for the formation of the membrane. Sodium iodide powder as a stabilizer can improve the salt resistance and stability of the membrane and reduce the expansion and deformation of the membrane during use. The polysulfonimide membrane support membrane as a supporting layer of the membrane has good mechanical properties and chemical stability, can effectively support the thin film structure, and enhance the stability and durability of the membrane.
[0020] 2. The present invention can optimize the preparation process of the reverse osmosis membrane and improve the performance and quality of the membrane by accurately controlling various parameters during the preparation process, such as the temperature of the solution, the standing time, the immersion time and the drying conditions. For example, during the preparation process, fine regulation of the treatment and immersion process of the dimethyl sulfoxide solution, the polymer solution and the stabilizer solution is helpful to form a uniform and dense membrane structure and improve the permeability and selectivity of the membrane. In addition, by performing precise drying treatment in a vacuum drying oven, residual solvents and moisture can be effectively removed to ensure the quality and stability of the membrane. These optimization measures help to improve the performance of the reverse osmosis membrane and enhance its application effect and economic benefits in the process of lithium extraction from salt lakes. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram for comparing the characteristics of reverse osmosis membranes in embodiments of the present invention. DETAILED DESCRIPTION
[0022] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0023] The present invention provides a method for preparing a reverse osmosis membrane for lithium extraction from a salt lake. The specific steps of the method for preparing a reverse osmosis membrane for lithium extraction from a salt lake are as follows:
[0024] S1. It is necessary to prepare a polymer solution. A dimethyl sulfoxide solution is selected as a solvent and placed in a clean test tube without impurities. The dimethyl sulfoxide solution is heated. After the heating is completed, polyamic acid ester powder is slowly and evenly added to the dimethyl sulfoxide solution. During the process of adding the polyamic acid ester powder, it is necessary to stir evenly until the polyamic acid ester powder and the dimethyl sulfoxide solution are fully mixed, thereby completing the preparation of the polymer solution.
[0025] S2. After the polymer solution is prepared, the polymer solution is placed in a lightless environment, and then the polymer solution is filtered using a microporous filter membrane, and then sodium iodide powder is slowly and evenly added to the filtered polymer solution. During the process of adding the sodium iodide powder, the test tube is evenly shaken until the sodium iodide powder is completely dissolved in the polymer solution, thereby completing the preparation of the stabilizer solution;
[0026] S3, selecting a polysulfonimide membrane support film as a support layer, allowing the stabilizer solution to stand at room temperature, and then immersing the polysulfonimide membrane support film in the stabilizer solution, taking out the support layer after immersion, and slowly placing it in a constant temperature water bath for immersion, and solidifying on the surface of the support layer after immersion to form a dense film structure;
[0027] S4, taking out the support layer forming the thin film structure, and then placing it in a vacuum drying oven for vacuum drying, and obtaining a reverse osmosis membrane after vacuum drying;
[0028] In one embodiment of the present invention: in S1, the volume of the selected dimethyl sulfoxide solution is 30 ml, the temperature of the dimethyl sulfoxide solution heating treatment is 58° C. to 62° C., the heating process needs to be slow and uniform, and the amount of polyamic acid ester powder added is 10 g.
[0029] In one embodiment of the present invention: in S2, after the polymer solution is prepared, it needs to be allowed to stand in a lightless environment at 24°C to 26°C for 1 hour, and sodium iodide powder is added after standing for 1 hour, and the amount of sodium iodide powder added is 100 mg.
[0030] In one embodiment of the present invention: in S3, the stabilizer solution needs to be left standing at room temperature of 24°C to 26°C for 1 hour, and then the polysulfoneimide membrane support membrane is evenly and slowly placed in the stabilizer solution for immersion for 12 hours.
[0031] In one embodiment of the present invention: in S3, the temperature of the constant temperature water bath is 80°C, the water bath time is 2 hours, and after the water bath is finished, it can be observed that a uniform coating is attached to the surface of the support layer.
[0032] In one embodiment of the present invention: in S3, after the immersion is completed, the support membrane should be carefully taken out to ensure that there are no bubbles or damages on the surface of the support membrane, and the support membrane without bubbles or damages on the surface is put into S4 for drying.
[0033] In one embodiment of the present invention: in S2, the added sodium iodide powder needs to be filtered through a filter with a pore size of 50 μm, and the sodium iodide powder with a particle size less than 50 μm is selected.
[0034] In one embodiment of the present invention: In S3, the stabilizer solution is filtered using a microporous filter membrane before use, and the pore size of the microporous filter membrane is 0.4 μm, which helps to remove the solid particles remaining in the stabilizer solution.
[0035] In one embodiment of the present invention: in S4, the working temperature of the vacuum drying oven is set to 60° C., the air pressure is set to 80 Pa, and the drying time is set to 2 h.
[0036] Embodiment 1
[0037] First, select 30 ml of dimethyl sulfoxide solution as a solvent and place it in a clean test tube without impurities, and heat the dimethyl sulfoxide solution evenly to 58°C~62°C. After the heating is completed, 10 g of polyamic acid ester powder is slowly and evenly added to the dimethyl sulfoxide solution. In the process of adding the polyamic acid ester powder, it is necessary to stir evenly until the polyamic acid ester powder and the dimethyl sulfoxide solution are fully mixed to obtain a polymer solution. After that, after the polymer solution is prepared, it needs to be allowed to stand in a lightless environment at 24°C~26°C for 1 hour. After standing for 1 hour, 100 g of sodium iodide powder is added. The added sodium iodide powder needs to be filtered through a filter with a pore size of 50 μm. In the process of adding the sodium iodide powder, the test tube is evenly shaken until the sodium iodide powder is completely dissolved in the polymer solution, thereby completing the preparation of the stabilizer solution. The stabilizer solution preparation After preparation, it needs to be allowed to stand at room temperature of 24℃~26℃ for 1h, and then the stabilizer solution is filtered with a microporous filter membrane before use. The pore size of the microporous filter membrane is 0.4μm, which helps to remove the residual solid particles in the stabilizer solution. After filtration, the polysulfoneimide membrane support membrane is evenly and slowly placed in the stabilizer solution for 12h. After the immersion is completed, the support layer is taken out and slowly placed in a constant temperature water bath at 80℃ for 2h. After the immersion is completed, it will solidify on the surface of the support layer to form a dense film structure. Then slowly take out the support membrane to ensure that there are no bubbles and damage on the surface of the support membrane, and then place it in a vacuum drying oven for vacuum drying. The working temperature of the vacuum drying oven is set to 60℃, the set air pressure is set to 80Pa, and the set drying time is 2h. After vacuum drying, a reverse osmosis membrane is obtained.
[0038] Embodiment 2
[0039] First, select 30 ml of diethyl sulfoxide solution as a solvent and place it in a clean test tube without impurities, and heat the diethyl sulfoxide solution evenly to 58°C~62°C. After the heating is completed, 10 g of polyimide powder is slowly and evenly added to the diethyl sulfoxide solution. In the process of adding the polyimide powder, it is necessary to stir evenly until the polyimide powder and the diethyl sulfoxide solution are fully mixed to obtain a polymer solution. After that, after the polymer solution is prepared, it needs to be allowed to stand in a lightless environment at 24°C~26°C for 1 hour. After standing for 1 hour, 100 g of sodium bromide powder is added. The added sodium bromide powder needs to be filtered through a filter with a pore size of 50 μm. In the process of adding the sodium bromide powder, the test tube is evenly shaken until the sodium bromide powder is completely dissolved in the polymer solution, thereby completing the preparation of the stabilizer solution. The stabilizer solution preparation After preparation, it needs to be allowed to stand at room temperature of 24℃~26℃ for 1h, and then the stabilizer solution is filtered with a microporous filter membrane before use. The pore size of the microporous filter membrane is 0.4μm, which helps to remove the residual solid particles in the stabilizer solution. After filtration, the polyamide membrane support membrane is evenly and slowly placed in the stabilizer solution for 12h. After the immersion is completed, the support layer is taken out and slowly placed in a constant temperature water bath at 80℃ for 2h. After the immersion is completed, it will solidify on the surface of the support layer to form a dense film structure. Then slowly take out the support membrane to ensure that there are no bubbles and damage on the surface of the support membrane, and then place it in a vacuum drying oven for vacuum drying. The working temperature of the vacuum drying oven is set to 60℃, the set air pressure is set to 80Pa, and the set drying time is 2h. After vacuum drying, a reverse osmosis membrane is obtained.
[0040] Embodiment 3
[0041] First, select 30 ml of acetone solution as the solvent and place it in a clean test tube without impurities, and heat the acetone solution evenly to 58°C~62°C. After the heating is completed, 10 g of polyamide powder is slowly and evenly added to the acetone solution. During the process of adding the polyamide powder, it is necessary to stir evenly until the polyamide powder and the acetone solution are fully mixed to obtain a polymer solution. After that, after the polymer solution is prepared, it needs to be allowed to stand in a lightless environment at 24°C~26°C for 1 hour. After standing for 1 hour, 100 g of sodium chloride powder is added. The added sodium chloride powder needs to be filtered through a filter with a pore size of 50 μm. During the process of adding the sodium chloride powder, the test tube is evenly shaken until the sodium chloride powder is completely dissolved in the polymer solution, thereby completing the preparation of the stabilizer solution. After the stabilizer solution is prepared, it needs to be stirred at 2 The stabilizer solution was allowed to stand at room temperature of 4°C to 26°C for 1 hour, and then the stabilizer solution was filtered through a microporous filter membrane before use. The pore size of the microporous filter membrane was 0.4 μm, which helped to remove the residual solid particles in the stabilizer solution. After the filtration was completed, the polycarbonate membrane support membrane was evenly and slowly placed in the stabilizer solution for 12 hours. After the immersion was completed, the support layer was taken out and slowly placed in a constant temperature water bath at 80°C for 2 hours. After the immersion was completed, it would solidify on the surface of the support layer to form a dense film structure. Then the support membrane was slowly taken out to ensure that there were no bubbles or damage on the surface of the support membrane. It was then placed in a vacuum drying oven for vacuum drying. The working temperature of the vacuum drying oven was set to 60°C, the air pressure was set to 80Pa, and the drying time was set to 2 hours. After the vacuum drying was completed, a reverse osmosis membrane was obtained.
[0042] Comparative Example 1
[0043] A double-sided polyamide membrane prepared based on a polyolefin porous base membrane is provided in a patent document with application publication number CN117160257A and titled “A double-sided polyamide membrane prepared based on a polyolefin porous base membrane and a preparation method thereof”.
[0044] The same concentration and amount of salt lake water were taken, and the membranes prepared in Example 1, Example 2, Example 3 and Comparative Example 1 were tested under the same temperature and pressure. After 50 lithium extraction experiments, the properties of the membranes prepared in Example 1, Example 2, Example 3 and Comparative Example 1 were tested.
[0045] As attached Figure 1 As shown, the multiple permeability, stability and durability of lithium extraction efficiency of the reverse osmosis membrane prepared by the present invention are higher than those of reverse osmosis membranes on the market.
[0046] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.
[0047] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0048] The above contents are merely examples and explanations of the present invention. Various modifications or additions to the specific embodiments described or replacements in similar ways by technicians in the technical field shall fall within the protection scope of the present invention as long as they do not deviate from the invention or exceed the scope defined by the claims.
[0049] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a reverse osmosis membrane for lithium extraction from a salt lake, characterized in that: The specific steps of the method for preparing a reverse osmosis membrane for lithium extraction from a salt lake are as follows: S1. It is necessary to prepare a polymer solution. A dimethyl sulfoxide solution is selected as a solvent and placed in a clean test tube without impurities. The dimethyl sulfoxide solution is heated. After the heating is completed, polyamic acid ester powder is slowly and evenly added to the dimethyl sulfoxide solution. During the process of adding the polyamic acid ester powder, it is necessary to stir evenly until the polyamic acid ester powder and the dimethyl sulfoxide solution are fully mixed, thereby completing the preparation of the polymer solution. S2. After the polymer solution is prepared, the polymer solution is placed in a lightless environment, and then the polymer solution is filtered using a microporous filter membrane, and then sodium iodide powder is slowly and evenly added to the filtered polymer solution. During the process of adding the sodium iodide powder, the test tube is evenly shaken until the sodium iodide powder is completely dissolved in the polymer solution, thereby completing the preparation of the stabilizer solution; S3, selecting a polysulfonimide membrane support film as a support layer, allowing the stabilizer solution to stand at room temperature, and then immersing the polysulfonimide membrane support film in the stabilizer solution, taking out the support layer after immersion, and slowly placing it in a constant temperature water bath for immersion, and solidifying on the surface of the support layer after immersion to form a dense film structure; S4, taking out the support layer forming the thin film structure, and then placing it in a vacuum drying oven for vacuum drying, and obtaining a reverse osmosis membrane after vacuum drying; In S1, the volume of the selected dimethyl sulfoxide solution is 30 ml, the temperature of the dimethyl sulfoxide solution heating treatment is 58° C. to 62° C., the heating process needs to be heated slowly and evenly, and the amount of polyamic acid ester powder added is 10 g; In S2, after the polymer solution is prepared, it needs to be allowed to stand in a lightless environment at 24°C to 26°C for 1 hour, and then sodium iodide powder is added after standing for 1 hour, and the amount of sodium iodide powder added is 100 mg; In S3, the temperature of the constant temperature water bath is 80° C., the water bath time is 2 h, and after the water bath is finished, it can be observed that a uniform coating is attached to the surface of the support layer; In S4, the working temperature of the vacuum drying oven is set to 60° C., the air pressure is set to 80 Pa, and the drying time is set to 2 h.
2. The method for preparing a reverse osmosis membrane for lithium extraction from a salt lake according to claim 1, characterized in that: In S3, the stabilizer solution needs to be left to stand at room temperature of 24° C. to 26° C. for 1 hour, and then the polysulfoneimide membrane support membrane is evenly and slowly placed in the stabilizer solution for immersion for 12 hours.
3. The method for preparing a reverse osmosis membrane for lithium extraction from a salt lake according to claim 1, characterized in that: In S3, after the immersion is completed, the support film should be carefully taken out to ensure that there are no bubbles or damages on the surface of the support film, and the support film without bubbles or damages on the surface is put into S4 for drying.
4. The method for preparing a reverse osmosis membrane for lithium extraction from a salt lake according to claim 1, characterized in that: In S2, the added sodium iodide powder needs to be filtered through a filter with a pore size of 50 μm, and the sodium iodide powder with a particle size less than 50 μm is selected.
5. The method for preparing a reverse osmosis membrane for lithium extraction from a salt lake according to claim 1, characterized in that: In S3, the stabilizer solution is filtered using a microporous filter membrane before use. The pore size of the microporous filter membrane is 0.4 μm, which helps to remove the solid particles remaining in the stabilizer solution.