Lithium ion battery positive electrode slurry and preparation method and system thereof
The ball mill stirring device is used to process carbon nanotubes and conductive carbon black, which solves the problem of conductive carbon black agglomeration during the dispersion process, achieves uniform dispersion and improved consistency of the lithium-ion battery cathode slurry, and improves battery performance.
Patent Information
- Application Number
- CN202410913072.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Conductive carbon black easily forms agglomerates during the dispersion process of lithium-ion battery cathode slurry, resulting in uneven dispersion and poor consistency of the slurry, affecting battery performance.
A ball mill stirring device is used to mix carbon nanotubes and conductive carbon black. Through cyclic stirring, ball milling and transportation, a uniformly dispersed conductive slurry is obtained. The conductive slurry is added after the main material and binder are processed to reduce conductivity. Carbon black reunion.
The uniform dispersion of conductive carbon black in the slurry is achieved, the consistency of the slurry is improved, and the battery performance is improved.
Smart Images

Figure CN118486833B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery preparation, and in particular to a lithium ion battery positive electrode slurry and a preparation method and a preparation system thereof. Background Art
[0002] With the rapid development of new energy in China, lithium-ion battery companies have higher and higher requirements for battery quality. The cathode slurry of lithium-ion batteries plays a decisive role in battery performance, so evenly dispersed cathode slurry is particularly important.
[0003] In the preparation method of lithium-ion battery positive electrode slurry in the related art, since the conductive carbon black has a small particle size, it is easy to form agglomerates when dispersed, resulting in uneven dispersion of the slurry and poor consistency of the slurry, which in turn affects the performance of the battery. Summary of the invention
[0004] The invention provides a lithium ion battery positive electrode slurry and a preparation method and a preparation system thereof, which can solve the problem of agglomeration of conductive carbon black during dispersion.
[0005] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a method for preparing a positive electrode slurry for a lithium ion battery, comprising:
[0006] Step S1: adding carbon nanotubes and conductive carbon black into a ball mill stirring device, wherein the ball mill stirring device comprises a first stirring tank, a ball milling mechanism, a second stirring tank and a conveying pipeline, wherein the outlet of the first stirring tank is connected to the inlet of the second stirring tank through the ball milling mechanism, and the outlet of the second stirring tank is connected to the inlet of the first stirring tank through the conveying pipeline;
[0007] Step S2: mixing the carbon nanotubes and the conductive carbon black in the first stirring tank to obtain a mixed material;
[0008] Step S3: the mixed material is cyclically stirred in the first stirring tank, ball-milled in the ball milling mechanism, stirred in the second stirring tank, and transported to the first stirring tank through the transport pipeline, the number of cycles is 2-5 times, and a uniformly dispersed conductive slurry is obtained;
[0009] Step S4: adding the main material and the binder into a stirring device, and sequentially performing dry mixing, a first NMP spraying, a kneading, a conductive slurry adding, a second NMP spraying, and a dispersion to obtain the positive electrode slurry for the lithium-ion battery.
[0010] According to one embodiment of the present invention, in step S2, the orbital speed of the first stirring tank is 20-30 rpm, the rotational speed is 100-600 rpm, and the mixing time is 5-10 min.
[0011] According to an embodiment of the present invention, in step S3, the revolution speed of the first stirring tank and the second stirring tank is 10 rpm.
[0012] According to one embodiment of the present invention, in step S3, the ball milling flow rate is 50-300 L / min, and the ball milling speed is 300-800 rpm.
[0013] According to an embodiment of the present invention, in step S4, the rotation speed of the dry mixing process is 100-600 rpm, the revolution speed is 20-30 rpm, and the dry mixing time is 5-15 min.
[0014] According to an embodiment of the present invention, in step S4, the kneading process is kneading for 15 minutes with the revolution turned on and the rotation turned off, and then the rotation is turned on, wherein the revolution speed is 20-30 rpm and the rotation speed is 300-600 rpm.
[0015] According to one embodiment of the present invention, in step S4, the first NMP spraying treatment is to spray N-methylpyrrolidone while the revolution is turned on and the rotation is turned off, so that the N-methylpyrrolidone and the solid powder after the dry mixing treatment are initially wetted, wherein the revolution speed is 3-10rpm, the spraying time is 3-8min, and the spraying amount of N-methylpyrrolidone is 60-75% of the added amount of N-methylpyrrolidone;
[0016] The second NMP spray treatment is to spray N-methylpyrrolidone in a state where the revolution is turned on and the rotation is turned off to dilute the slurry obtained by the kneading treatment, wherein the revolution speed is 5-10rpm, the spraying time is 3-8min, and the spraying amount of N-methylpyrrolidone is the difference between the added amount of N-methylpyrrolidone and the spraying amount of the first NMP spray treatment.
[0017] According to an embodiment of the present invention, in step S4, the conductive paste is added by adding the conductive paste with the revolution turned on and the rotation turned off, and the revolution speed is 5-10 rpm.
[0018] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a positive electrode slurry for a lithium ion battery, which is prepared by the preparation method of the positive electrode slurry for a lithium ion battery.
[0019] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a preparation system of lithium-ion battery positive electrode slurry, which is applied to the preparation method of lithium-ion battery positive electrode slurry, the preparation system comprises: a ball mill stirring device and a stirring device, the ball mill stirring device comprises a first stirring tank, a ball milling mechanism, a second stirring tank and a conveying pipeline, the outlet of the first stirring tank is connected to the inlet of the second stirring tank through the ball milling mechanism, and the outlet of the second stirring tank is connected to the inlet of the first stirring tank through the conveying pipeline.
[0020] The beneficial effects of the present invention are as follows: a method for preparing a positive electrode slurry for a lithium-ion battery comprises: step S1: adding carbon nanotubes and conductive carbon black into a ball mill stirring device, wherein the ball mill stirring device comprises a first stirring tank, a ball milling mechanism, a second stirring tank and a conveying pipeline, wherein the outlet of the first stirring tank is connected to the inlet of the second stirring tank through the ball milling mechanism, and the outlet of the second stirring tank is connected to the inlet of the first stirring tank through the conveying pipeline; step S2: mixing the carbon nanotubes and the conductive carbon black in the first stirring tank to obtain a mixed material; step S3: cyclically stirring the mixed material in the first stirring tank, ball milling in the ball milling mechanism, and the mixing process is repeated. Treatment, stirring treatment in the second stirring tank and conveying it to the first stirring tank through the conveying pipeline, the number of cycles is 2-5 times, and a uniformly dispersed conductive slurry is obtained; step S4: adding the main material and the binder into the stirring device, and sequentially performing dry mixing treatment, the first NMP spraying treatment, kneading treatment, the addition treatment of the conductive slurry, the second NMP spraying treatment and dispersion treatment to obtain the lithium ion battery positive electrode slurry; by first preparing the carbon nanotubes and conductive carbon black into a uniformly dispersed conductive slurry, and then adding the conductive slurry after the main material and the binder are kneaded, the problem of agglomeration of conductive carbon black during the dispersion process is solved, and the conductive carbon black is more evenly dispersed in the slurry and the consistency of the slurry is better. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the structure of a system for preparing positive electrode slurry for lithium-ion batteries according to an embodiment of the present invention.
[0022] Figure 2 The present invention is a schematic diagram of a process for preparing a positive electrode slurry for a lithium-ion battery according to an embodiment of the present invention.
[0023] Figure 3 This is a SEM image of the positive electrode slurry for a lithium-ion battery prepared in Example 1 of the present invention.
[0024] Figure 4 This is a SEM image of the positive electrode slurry for a lithium-ion battery prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The terms "first", "second" and "third" in the present invention are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Therefore, the features defined as "first", "second" and "third" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. All directional indications (such as up, down, left, right, front, back...) in the embodiments of the present invention are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.
[0027] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0028] Figure 1 FIG. 1 is a schematic diagram of a system for preparing a positive electrode slurry for a lithium-ion battery according to an embodiment of the present invention. Figure 1 The preparation system 100 includes a ball mill stirring device 10 and a stirring device 20 .
[0029] As an embodiment, the ball mill stirring device 10 and the stirring device 20 may be connected via a pipeline 30 .
[0030] As an embodiment, the ball mill stirring device 10 includes a first stirring tank 11, a ball mill mechanism 12, a second stirring tank 13 and a conveying pipeline 14. The first stirring tank 11 has a first outlet 111 and a first inlet 112, the second stirring tank 13 has a second outlet 131 and a second inlet 132, the first outlet 111 of the first stirring tank 11 is connected to the second inlet 132 of the second stirring tank 13 through the ball mill mechanism 12, and the second outlet 131 of the second stirring tank 13 is connected to the first inlet 112 of the first stirring tank 11 through the conveying pipeline 14.
[0031] As an embodiment, the stirring device 20 includes but is not limited to a double planetary mixer, a high-speed disperser, a twin-screw mixer, etc.
[0032] When preparing positive electrode slurry for lithium-ion batteries, carbon nanotubes and conductive carbon black are added to a ball mill stirring device 10, wherein the carbon nanotubes are purchased raw materials and are in a solution state; the carbon nanotubes and the conductive carbon black are mixed and treated in a cycle in a first stirring tank 11 to obtain a mixed material; the mixed material is sequentially stirred in the first stirring tank 11, ball milled in the ball milling mechanism 12, stirred in the second stirring tank 13 and transported to the first stirring tank 11 through a conveying pipe 14, and the number of cycles is 2-5 times to obtain a uniformly dispersed conductive slurry; the main material and the binder are added to the stirring device 20, and dry mixing, a first NMP spraying, kneading, adding of conductive slurry, a second NMP spraying and dispersion are sequentially performed to obtain positive electrode slurry for lithium-ion batteries; the preparation system 100 can reduce the agglomeration of conductive carbon black during the dispersion process, thereby improving the dispersibility of positive electrode slurry for lithium-ion batteries.
[0033] Figure 2 FIG. 1 is a flow chart of a method for preparing a positive electrode slurry for a lithium-ion battery according to an embodiment of the present invention. It should be noted that the method of the present invention is not limited to the method of preparing a positive electrode slurry according to an embodiment of the present invention if the results are substantially the same. Figure 2 The process sequence shown is limited. Figure 2 As shown, the method comprises the steps of:
[0034] Step S1: adding carbon nanotubes and conductive carbon black into a ball mill stirring device, the ball mill stirring device comprises a first stirring tank, a ball milling mechanism, a second stirring tank and a conveying pipeline, the outlet of the first stirring tank is connected to the inlet of the second stirring tank through the ball milling mechanism, and the outlet of the second stirring tank is connected to the inlet of the first stirring tank through the conveying pipeline.
[0035] Specifically, the carbon nanotubes are purchased raw materials in a solution state. The positive electrode slurry of the lithium-ion battery includes the following components by mass percentage: 94%-97% of the main material, 0.5%-2% of the conductive carbon black, 0.2%-2% of the carbon nanotubes, and 1.5%-3% of the binder. In step S1, 0.2%-2% of the carbon nanotubes and 0.5%-2% of the conductive carbon black are added to the first stirring tank.
[0036] Step S2: mixing the carbon nanotubes and the conductive carbon black in a first stirring tank to obtain a mixed material.
[0037] In step S2, the revolution speed of the first stirring tank is 20-30 rpm, preferably 25 rpm; the rotation speed is 100-600 rpm, preferably 300 rpm; the mixing time is 5-10 min, preferably 10 min.
[0038] Step S3: The mixed material is cyclically stirred in the first stirring tank, ball-milled in the ball milling mechanism, stirred in the second stirring tank and transported to the first stirring tank through the conveying pipeline, the number of cycles is 2-5 times, and a uniformly dispersed conductive slurry is obtained.
[0039] In step S3, the revolution speed of the first stirring tank and the second stirring tank is 10rpm. It can be understood that after step S2, the first stirring tank continues to turn on the revolution and turn off the rotation, the revolution speed is 10rpm, and then the mixed material is ball-milled in the ball milling mechanism, and then enters the second stirring tank for stirring. The second stirring tank is in the state of turning on the revolution and turning off the rotation, and the revolution speed is 10rpm. After the stirring is completed, it is transported to the first stirring tank through the conveying pipeline, and the above operation is repeated for 2-5 times, that is, the number of ball milling is 2-5 times. This step can produce a uniformly dispersed conductive slurry by cyclically performing the operations of stirring the first stirring tank-ball milling by the ball milling mechanism-stirring the second stirring tank, thereby avoiding agglomeration of conductive carbon black in the subsequent dispersion process.
[0040] Furthermore, the ball milling flow rate is 50-300 L / min, preferably 100 L / min; the ball milling speed is 300-800 rpm, preferably 500 rpm.
[0041] Step S4: adding the main material and the binder into a stirring device, and sequentially performing dry mixing, a first NMP spraying, a kneading, a conductive slurry adding, a second NMP spraying, and a dispersion to obtain a positive electrode slurry for a lithium-ion battery.
[0042] In step S4, 94%-97% of the main material and 1.5%-3% of the binder are added to the stirring device while the revolution is turned on and the rotation is turned off. The revolution speed is 5-10 rpm, preferably 10 rpm. This step does not require the vacuum to be turned on to avoid the extraction of solid powder.
[0043] The dry mixing process is to preliminarily mix the main material and the binder. During the dry mixing process, the revolution and rotation are started at the same time. The revolution axis can rotate forward first and then reverse or reverse first and then forward. Among them, the rotation speed is 100-600rpm, preferably 300rpm; the revolution speed is 20-30rpm, preferably 25rpm; the dry mixing time is 5-15min, preferably 10min.
[0044] The first NMP spray treatment is to spray N-methylpyrrolidone in a state where the revolution is turned on and the rotation is turned off, so that N-methylpyrrolidone and the solid powder after dry mixing are initially wetted, wherein the revolution speed is 3-10rpm, preferably 5rpm, the spraying time is 3-8min, and the spraying amount of N-methylpyrrolidone is 60-75% of the added amount of N-methylpyrrolidone. In this embodiment, the purpose of the first NMP spray treatment is to increase the N-methylpyrrolidone feeding pressure by spraying through the spray pipe, so as to flush the powder stuck on the stirring paddle in the stirring device into the tank body.
[0045] The kneading process plays the role of dispersing and mixing the materials, achieving the effect of no dry powder and complete infiltration. The kneading process is kneading for 15 minutes with the revolution turned on and the rotation turned off, and then the rotation is turned on, wherein the revolution speed is 20-30rpm, preferably 25rpm; the rotation speed is 300-600rpm, preferably 300rpm.
[0046] The conductive paste is added by adding the conductive paste prepared in step S3 while the revolution is turned on and the rotation is turned off, and the revolution speed is 5-10 rpm.
[0047] The second NMP spray treatment is to spray N-methylpyrrolidone in a state where the revolution is turned on and the rotation is turned off to dilute the slurry obtained by the kneading treatment, wherein the revolution speed is 5-10rpm, the spraying time is 3-8min, and the spraying amount of N-methylpyrrolidone is the difference between the amount of N-methylpyrrolidone added and the amount of NMP spray treatment in the first NMP spray treatment. In this embodiment, the purpose of the second NMP spray treatment is to further dilute the slurry by adding N-methylpyrrolidone.
[0048] The dispersion treatment is to preliminarily disperse the slurry to further reduce the viscosity of the slurry. The dispersion treatment needs to be carried out under vacuum conditions to remove bubbles generated during the dispersion process. The revolution speed of the dispersion treatment is 25-30rpm, preferably 30rpm; the rotation speed is 900-1200rpm, preferably 1100rpm.
[0049] In order to further reduce the viscosity of the slurry, after step S4, a step of circulating high-speed dispersion treatment of the slurry in a high-speed disperser may be added.
[0050] Furthermore, in steps S1-S4, the stirring process requires the use of circulating cooling water to ensure that the slurry temperature is controlled within 55°C throughout the process.
[0051] The method for preparing a positive electrode slurry for a lithium-ion battery according to an embodiment of the present invention prepares carbon nanotubes and conductive carbon black into a uniformly dispersed conductive slurry, and then adds the conductive slurry after the main material and the binder are kneaded, thereby solving the problem of agglomeration of the conductive carbon black during the dispersion process, making the conductive carbon black more uniformly dispersed in the slurry and improving the consistency of the slurry.
[0052] The embodiment of the present invention also provides a positive electrode slurry for a lithium ion battery, which is prepared by the above-mentioned method for preparing the positive electrode slurry for a lithium ion battery. The positive electrode slurry for a lithium ion battery has excellent dispersibility and no conductive carbon black agglomeration phenomenon occurs. Figure 3 shown.
[0053] Example 1
[0054] Step S1: adding 0.2%-2% carbon nanotubes and 0.5%-2% conductive carbon black into a first stirring tank;
[0055] Step S2: mixing the carbon nanotubes and the conductive carbon black in a first stirring tank to obtain a mixed material, with an orbital speed of 25 rpm and an autorotational speed of 300 rpm; the mixing time is 10 min;
[0056] Step S3: The mixed material is cyclically stirred in the first stirring tank, ball-milled in the ball milling mechanism, stirred in the second stirring tank, and transported to the first stirring tank through the conveying pipeline, the number of cycles is 2-5 times, and a uniformly dispersed conductive slurry is obtained;
[0057] The first stirring tank is used for stirring: the revolution speed is 10 rpm;
[0058] Ball milling treatment: ball milling flow rate is 100L / min; ball milling speed is 500rpm;
[0059] The second stirring tank is used for stirring: the revolution speed is 10 rpm;
[0060] The number of cycles is 5 times.
[0061] Step S4: adding the main material and the binder into a stirring device, and sequentially performing dry mixing, a first NMP spraying, a kneading, a conductive slurry adding, a second NMP spraying, and a dispersion to obtain a positive electrode slurry for a lithium-ion battery.
[0062] Dry mixing treatment: orbital speed is 25rpm; rotation speed is 300rpm; dry mixing time is 10min;
[0063] The first NMP spraying treatment: the revolution speed is 5 rpm, the spraying time is 5 min, and the spraying amount of N-methylpyrrolidone is 75% of the added amount of N-methylpyrrolidone;
[0064] Kneading treatment: the revolution speed is 25 rpm, the rotation speed is 300 rpm, and the kneading time is 15 min;
[0065] Conductive slurry addition process: the revolution speed is 5 rpm;
[0066] The second NMP spray treatment: the revolution speed is 5 rpm, the spray time is 5 min, and the spray amount of N-methylpyrrolidone is the difference between the added amount of N-methylpyrrolidone and the spray amount of the first spray treatment;
[0067] Dispersion treatment: orbital speed is 30rpm, rotation speed is 1100rpm.
[0068] Comparative Example 1
[0069] Different from Example 1, steps S1-S3 are omitted, and in step S4, the main material, the binder and the conductive carbon black are added into the stirring device together, and the conductive slurry is added by directly adding the carbon nanotubes.
[0070] test
[0071] The lithium-ion battery positive electrode slurries prepared in Example 1 and Comparative Example 1 were tested by scanning electron microscope (SEM) using Zeiss EVO10 to observe the agglomeration of conductive carbon black. Figure 3 As shown, in the lithium ion battery positive electrode slurry prepared in Example 1, the conductive carbon black has good dispersion in the slurry and no agglomeration phenomenon. Figure 4 As shown, in the lithium ion battery positive electrode slurry prepared in Comparative Example 1, the conductive carbon black has poor dispersion in the slurry and has serious agglomeration phenomenon.
[0072] The above are only implementation modes of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a positive electrode slurry for a lithium ion battery, It is characterized in that include: Step S1: adding carbon nanotubes and conductive carbon black into a ball mill stirring device, wherein the ball mill stirring device comprises a first stirring tank, a ball milling mechanism, a second stirring tank and a conveying pipeline, wherein the outlet of the first stirring tank is connected to the inlet of the second stirring tank through the ball milling mechanism, and the outlet of the second stirring tank is connected to the inlet of the first stirring tank through the conveying pipeline; Step S2: mixing the carbon nanotubes and the conductive carbon black in the first stirring tank to obtain a mixed material; Step S3: the mixed material is cyclically stirred in the first stirring tank, ball-milled in the ball milling mechanism, stirred in the second stirring tank, and transported to the first stirring tank through the transport pipeline, the number of cycles is 2-5 times, and a uniformly dispersed conductive slurry is obtained; Step S4: adding the main material and the binder into a stirring device, and sequentially performing dry mixing, a first NMP spraying, a kneading, an addition of the conductive slurry, a second NMP spraying, and a dispersion to obtain the positive electrode slurry for the lithium-ion battery; In the step S4, the first NMP spraying treatment is to spray N-methylpyrrolidone while the revolution is turned on and the rotation is turned off, so that the N-methylpyrrolidone and the solid powder after the dry mixing treatment are preliminarily wetted, wherein the revolution speed is 3-10rpm, the spraying time is 3-8min, and the spraying amount of N-methylpyrrolidone is 60-75% of the added amount of N-methylpyrrolidone; The second NMP spray treatment is to spray N-methylpyrrolidone in a state where the revolution is turned on and the rotation is turned off to dilute the slurry obtained by the kneading treatment, wherein the revolution speed is 5-10rpm, the spraying time is 3-8min, and the spraying amount of N-methylpyrrolidone is the difference between the added amount of N-methylpyrrolidone and the spraying amount of the first NMP spray treatment.
2. The method for preparing the positive electrode slurry for lithium-ion batteries according to claim 1, It is characterized in that In the step S2, the orbital speed of the first stirring tank is 20-30 rpm, the rotational speed is 100-600 rpm, and the mixing time is 5-10 min.
3. The method for preparing the positive electrode slurry for lithium-ion batteries according to claim 1, It is characterized in that In the step S3, the revolution speed of the first stirring tank and the second stirring tank is 10 rpm.
4. The method for preparing a positive electrode slurry for a lithium ion battery according to claim 1, It is characterized in that In the step S3, the ball milling flow rate is 50-300 L / min, and the ball milling speed is 300-800 rpm.
5. The method for preparing the positive electrode slurry for lithium-ion batteries according to claim 1, It is characterized in that In step S4, the rotation speed of the dry mixing process is 100-600 rpm, the revolution speed is 20-30 rpm, and the dry mixing time is 5-15 min.
6. The method for preparing the positive electrode slurry for lithium-ion batteries according to claim 1, It is characterized in that In step S4, the kneading process is kneading for 15 minutes with the revolution turned on and the rotation turned off, and then the rotation is turned on, wherein the revolution speed is 20-30 rpm and the rotation speed is 300-600 rpm.
7. The method for preparing a positive electrode slurry for a lithium ion battery according to claim 1, It is characterized in that In the step S4, the conductive paste is added by turning on the revolution and turning off the rotation, and the revolution speed is 5-10 rpm.
8. A positive electrode slurry for a lithium-ion battery, It is characterized in that The positive electrode slurry for a lithium-ion battery is prepared by the method for preparing the positive electrode slurry for a lithium-ion battery as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Positive electrode slurry and preparation method and stability evaluation method thereof
CN116581295A
Preparation device of oily carbon nanotube conductive paste with high solid content