A method for preparing modified ceramics
By using modified ceramic binders, the sintering and electrical performance issues of lead-free KNN-based piezoelectric ceramics were resolved, achieving efficient ceramic performance improvement and cost control.
Patent Information
- Application Number
- CN202410716047.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-04
AI Technical Summary
Existing technologies struggle to improve the sintering and electrical properties of lead-free KNN-based piezoelectric ceramics by modifying the use of binders, and the complexity of the dopant system leads to poor reproducibility and stability, resulting in high production costs.
Modified ceramic binders, including PAA-based binders and modifiers such as nonionic polyacrylamide, citric acid and sodium citrate buffer, neutral hydroxypropyl methylcellulose, and 2-ethylhexyl ester, are used to prepare modified ceramics through specific process steps. By utilizing carboxyl functional groups to bind with K, Na, and Nb ions, particle size and agglomeration are controlled to form dense electrodes.
The modified ceramics exhibited improved piezoelectric constant d33 and breakdown strength Eb, enhanced bonding and electrical stability, and reduced production costs.
Smart Images

Figure CN118495967B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic technology, and more particularly to a method for preparing modified ceramics. Background Technology
[0002] In industry, polyacrylic acid (PAA) is widely used in textiles, papermaking, construction, pharmaceuticals, hygiene and environmental protection. PAA can also be copolymerized with other monomers to form polymers with different functions. These materials can be used to prepare polymer hydrogels, pressure-sensitive adhesives, ion exchange resins, ultra-high molecular weight polymers, etc., and have broad and far-reaching application prospects. The application of PAA and its derivatives in the preparation of ceramic slurries is well-known. PAA-based binders can improve the mechanical properties, sintering density and compositional uniformity of ceramics, playing an important role in improving the overall performance of ceramics. The low thermal decomposition temperature of PAA makes it easy to completely decompose during the debonding process of ceramics, leaving minimal residues and reducing the introduction of impurities. By using various modification techniques to control the mechanical and chemical properties of the bonding phase, the effectiveness of the binder can be further improved. Studies have shown that PAA-based binders can improve the strength of ceramics at low concentrations (<5.0 vol%), thereby resulting in more uniform density and composition. For example, using only 2.5 vol% PAA-based binder, the strength of oxides such as SiO2, TiO2, and Al2O3 can increase by at least 8 times, and the strength of Al2O3 can increase by approximately 24 times (0.3 to 7.6 MPa). Furthermore, the addition of PAA-based binder improves the toughness of ceramics, with SiO2 toughness increasing by 2.8 × 10⁻⁶. -3 ~4.4×10 -2 Compared to polyvinyl alcohol (PVA), PAA-based adhesives exhibit a more uniform distribution, lower particle yield stress, and smaller interparticle gaps at MPa·m1 / 2, resulting in a more uniform internal structure in green bodies and ceramics. Piezoelectric ceramics are widely used functional materials that can convert mechanical energy into electrical energy and vice versa. Problems associated with lead-free KNN-based piezoelectric ceramics include poor sintering performance and low density, making it challenging to improve their electrical properties. Doping can be used to address this issue, but the complexity of dopant systems leads to poor reproducibility and stability. Advanced fabrication techniques that can significantly improve ceramic properties also result in higher production costs. Instead of these methods, modifying the use of binders to achieve improved sintering performance, and significantly improving ceramic properties by reducing defects generated during sintering, makes this a cost-effective fabrication technique. However, current research on PAA-based binders and their role in enhancing the properties of KNN-based ceramics is limited. To address the aforementioned problems, the inventors proposed a modified ceramic preparation process to solve these issues. Summary of the Invention
[0003] The technical problem to be solved by this invention is: A method for preparing modified ceramics was developed. By using a modified ceramic binder, the final modified ceramic exhibits optimal performance: the KNN ceramic synthesized from AcPAA possesses the best composite properties, with a piezoelectric constant of d. 33 ~108pC / N, the breakdown strength of PAA-DM is E b ~3.93kV / cm, the above effect was achieved through the synergistic effect of particle size and thermal behavior of the adhesive.
[0004] To achieve the above objectives, the present invention adopts the following technical solution: A modified ceramic adhesive comprises the following components: a PAA-based adhesive and a modifier.
[0005] As a further improvement to this scheme, the modifier is any one or more of nonionic polyacrylamide, citric acid and sodium citrate buffer, neutral hydroxypropyl methylcellulose, and 2-ethylhexyl ester.
[0006] A method for preparing modified ceramics includes the following preparation steps: S1. Add K2CO3, Na2CO3 and Nb2O5 into a planetary ball mill, add ZrO2 balls and anhydrous ethanol for one grinding to obtain a slurry; S2. Add the slurry obtained in S1 into the dryer and dry the slurry to obtain dried slurry; S3. Add the dried slurry obtained in S2 into the calcination equipment and calcine the dried slurry to obtain fine powder; S4. Add the fine powder obtained in S3 to a planetary ball mill for secondary ball milling. Then add the modified PAA-based binder and the fine powder after secondary ball milling to a mixing device to mix the fine powder and the modified PAA-based binder to obtain granulated particles. S5. Press the granules obtained in S4 into discs with a diameter of 12-15mm. Then, heat the discs to 600℃ and keep them at that temperature for 3 hours to fully remove the binder from the disc blanks. Then raise the temperature to 1080-1110℃ to allow the blanks to be completely ceramicized. S6. Finally, apply silver paste to the upper and lower surfaces of the ceramic and keep it at 600℃ for 30 minutes. The silver paste will solidify on the surface of the ceramic, forming a dense electrode, thus obtaining the modified ceramic.
[0007] As a further improvement to this scheme, the purity of K2CO3 is 99%, the purity of Na2CO3 is 99.8%, the purity of Nb2O5 is 99.5%, and the grinding time for one cycle is 12-20 hours.
[0008] As a further improvement to this scheme, the calcination temperature of the dried slurry is 800-1000℃, the calcination time is 6-10h, and in S4, the secondary ball milling time is 12-18h.
[0009] As a further improvement to this scheme, the pressing pressure of the disc is 10-20 MPa, and the sintering time of the disc is 5-8 h.
[0010] As a further improvement to this scheme, the sintering temperature of the ceramic blank is 1080-1110℃, and the sintering time is 5-8h.
[0011] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The modified ceramic prepared by the modified ceramic binder in this invention and the preparation process of S1-S6, wherein the functional group of PAA is a carboxyl group (-COOH), and its dissociation equation is R-COOH H2O-R-COO-H2O. As the pH value (4.5-5) increases, the negatively charged carboxylic acid group (COO-) formed by dissociation will combine with the K, Na and Nb ions in KNN and gather around the powder by electrostatic attraction, so the bonding effect is good. 2. The modified ceramics prepared by the modified ceramic binder and the preparation processes of S1-S6 in this invention can shield the potential layer generated by the partially ionized PAA backbone by neutral polymers or functional groups that are insensitive to changes in pH or ion concentration, thereby reducing agglomeration and controlling particle size. The KNN mixed raw materials are located in the impurity charge region and contain a variety of non-equivalent ions, resulting in a wide pH range and severe particle agglomeration. Therefore, the modification of PAA functional groups can reduce the impurity charge region during the granulation process and also enhance the granulation effect of ceramic powder. Attached Figure Description
[0012] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0013] Figure 1 This is a schematic diagram showing the shrinkage rate and density of samples synthesized with different modified binders according to the present invention, as well as the piezoelectric constant and breakdown strength of the samples.
[0014] Figure 2 This is a schematic diagram showing the viscosity of the adhesive of the present invention, the median particle size (D50) of the granulated powder, and the cumulative distribution.
[0015] Figure 3 This is a schematic diagram showing the particle size distribution of the powder after granulation using different binders according to the present invention.
[0016] Figure 4 This is a schematic diagram of the complex impedance spectrum of the ceramic of the present invention.
[0017] Figure 5 This is a schematic diagram of the activation energy Ea and the relaxation time of the sample in this invention.
[0018] Figure 6 This is a schematic diagram of the thermal analysis of the adhesive of the present invention.
[0019] Figure 7 This is a schematic diagram illustrating the mechanism analysis of the binder of the present invention. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described below with reference to embodiments: Example 1: This invention provides a modified ceramic binder comprising the following components: PAA-based adhesives and modifiers.
[0021] The modifier is any one or more of nonionic polyacrylamide, citric acid and sodium citrate buffer, neutral hydroxypropyl methylcellulose, and 2-ethylhexyl ester.
[0022] A process for preparing modified ceramics for use as modified ceramic binders includes the following steps: S1. Add K2CO3, Na2CO3 and Nb2O5 into a planetary ball mill, add ZrO2 balls and anhydrous ethanol for one grinding, the grinding time is 12h, and a slurry is obtained. S2. Add the slurry obtained in S1 into the dryer and dry the slurry to obtain dried slurry; S3. Add the dried slurry obtained in S2 into the calcination equipment and calcine the dried slurry. The calcination temperature of the dried slurry is 800℃ and the calcination time is 6h to obtain fine powder. S4. Add the fine powder obtained in S3 to a planetary ball mill for secondary ball milling. The secondary grinding time is 12 hours. Then add the PAA-based binder and the fine powder after secondary ball milling to a mixing device to mix the fine powder and PAA-based binder to obtain granulated particles. S5. Press the particles obtained in S4 into a disc with a diameter of 12 mm and press the disc under a pressure of 12 MPa. Then, heat the disc to 600°C and hold it for 3 hours to completely remove the binder from the disc blank. Then raise the temperature to 1080°C and sinter for 5 hours to allow the blank to be completely ceramicized. S6. Finally, apply silver paste to the upper and lower surfaces of the ceramic and keep it at 600℃ for 30 minutes. The silver paste will solidify on the surface of the ceramic, forming a dense electrode, thus obtaining the modified ceramic.
[0023] Example 2: This invention provides a modified ceramic binder comprising the following components: PAA-based adhesives and modifiers.
[0024] The modifier is any one or more of nonionic polyacrylamide, citric acid and sodium citrate buffer, neutral hydroxypropyl methylcellulose, and 2-ethylhexyl ester.
[0025] A process for preparing modified ceramics for use as modified ceramic binders includes the following steps: S1. Add K2CO3, Na2CO3 and Nb2O5 into a planetary ball mill, add ZrO2 balls and anhydrous ethanol for one grinding, the grinding time is 15h, and a slurry is obtained. S2. Add the slurry obtained in S1 into the dryer and dry the slurry to obtain dried slurry; S3. Add the dried slurry obtained in S2 into the calcination equipment and calcine the dried slurry. The calcination temperature of the dried slurry is 900℃ and the calcination time is 8h to obtain fine powder. S4. Add the fine powder obtained in S3 to a planetary ball mill for secondary ball milling. The secondary grinding time is 16 hours. Then add the PAA-based binder and the fine powder after secondary ball milling to a mixing device to mix the fine powder and PAA-based binder to obtain granulated particles. S5. Press the particles obtained in S4 into a disc with a diameter of 12 mm and press the disc under a pressure of 15 MPa. Then, heat the disc to 600°C and hold it for 3 hours to completely remove the binder from the disc blank. Then raise the temperature to 1110°C and sinter for 6 hours to allow the blank to be completely ceramicized. S6. Finally, apply silver paste to the upper and lower surfaces of the ceramic and keep it at 600℃ for 30 minutes. The silver paste will solidify on the surface of the ceramic, forming a dense electrode, thus obtaining the modified ceramic.
[0026] Example 3: This invention provides a modified ceramic binder comprising the following components: PAA-based adhesives and modifiers.
[0027] The modifier is any one or more of nonionic polyacrylamide, citric acid and sodium citrate buffer, neutral hydroxypropyl methylcellulose, and 2-ethylhexyl ester.
[0028] A process for preparing modified ceramics for use as modified ceramic binders includes the following steps: S1. Add K2CO3, Na2CO3 and Nb2O5 into a planetary ball mill, add ZrO2 balls and anhydrous ethanol for one grinding, the grinding time is 18h, and a slurry is obtained. S2. Add the slurry obtained in S1 into the dryer and dry the slurry to obtain dried slurry; S3. Add the dried slurry obtained in S2 into the calcination equipment and calcine the dried slurry. The calcination temperature of the dried slurry is 1000℃ and the calcination time is 9h to obtain fine powder. S4. Add the fine powder obtained in S3 to a planetary ball mill for secondary ball milling. The secondary grinding time is 18 hours. Then add the PAA-based binder and the fine powder after secondary ball milling to a mixing device to mix the fine powder and PAA-based binder to obtain granulated particles. S5. Press the particles obtained in S4 into discs with a diameter of 12 mm and press them at a pressure of 20 MPa. Then, heat the discs to 600°C and hold them for 3 hours to remove the binder from the disc blanks. Then, raise the temperature to 1090°C and sinter for 8 hours to allow the blanks to become completely ceramic. S6. Finally, apply silver paste to the upper and lower surfaces of the ceramic and keep it at 600℃ for 30 minutes. The silver paste will solidify on the surface of the ceramic, forming a dense electrode, thus obtaining the modified ceramic.
[0029] The adhesive products modified with PAA-based adhesives and modifiers are shown in Tables 1-1 to 1-2 below: Table 1-1 Acidic adhesives and their dosage Table 1-2 Neutral adhesives and their dosage Sodium polyacrylate (PAANa) preparation process: Neutralization of acrylic acid with sodium hydroxide: First, acrylic acid is neutralized with sodium hydroxide to produce sodium acrylate monomer.
[0030] Chemical reaction equation: CH2=CH-COOH + NaOH → CH2=CH-COONa + H2O Polymerization: Under the action of an initiator, sodium acrylate monomers undergo a polymerization reaction to produce sodium polyacrylate.
[0031] The hydroxyl groups of PAA are partially replaced by ethylene-ethylene (-C=CH2): A vinylizing agent was added to the PAA solution, and the mixture was stirred at 680 rpm for half an hour at 65°C to allow some of the hydroxyl groups of the PAA to be replaced by vinyl groups. After the reaction was complete, the acid in the reaction system was neutralized using a base (sodium hydroxide).
[0032] The remaining adhesives are prepared by mixing: The specific process is as follows: stirring time 1 hour; stirring rate: 450 r / min.
[0033] The phase structure of the ceramic was analyzed by X-ray diffraction (XRD) using Cu Kα radiation. Scanning electron microscopy (SEM) images for microstructure analysis were obtained using a Zeiss Sigma300 scanning electron microscope. Dielectric properties and impedance spectra were determined using an LCR analyzer (E4991A, Agilent, USA). Particle size distribution was measured using a Baibaxter laser particle size analyzer (BT-9300S, Dandong). Thermogravimetric analysis (TG), differential thermal analysis (DTA), and derivative thermogravimetric analysis (DTG) showed abrupt changes. refer to Figure 1 It was found that PAA-DM, PAA-HPMC, and PAA-2-EHA promoted the shrinkage of KNN sintered ceramics, while PAANa resulted in the lowest shrinkage rate. Similar changes were observed in the density of the ceramics. The results indicate that ceramics prepared by PAA-APAANa have less shrinkage, and the basic group -NH2 is superior to the alkaline environment. In addition, the low molecular weight (MW) of the binder (e.g., PAANa) is not conducive to the bonding effect, resulting in poor shrinkage and density of the ceramics. Conversely, acidic binders buffered with citrate buffer solution, such as PAA-PAANa, PAA-PAM, and AcPAA, have little effect on shrinkage but have a positive effect on the density of KNN ceramics. refer to Figure 1 In (a), it was observed that ceramics synthesized from PAA-APAANa or AcPAA had the highest d values of 103 or 108 pC / N. 33 The smallest d was detected in ceramics by PAANa. 33 This is due to the low density; the maximum d of PAA-APAANa or AcPAA is... 33 This is attributed to the reduction of carboxylic acid groups (-COO-) through pH adjustment; refer to Figure 2In (b), it was found that PAA-DM and PAA-2-EHA achieved maximum E values of 3.93 kV / mm and 3.73 kV / mm in ceramics, respectively. b Notably, DM and 2-EHA possess neutral diethyl (-C=CH2) and ester (-COO-) groups, which shield the electrostatic attraction of -COO- to K and Na, thereby reducing particle aggregation that could degrade ceramic properties. Furthermore, the lowest dg was simultaneously achieved in ceramics prepared from PAANa. 33 and E b This is also because of the worst density; refer to Figure 2 The study found that, except for the powders granulated from PAA-HPMC and PAA-C=CH2, the D50 values of other powders were approximately 0.771 μm to 0.863 μm, with the corresponding cumulative D50 distribution ranging from 50.05% to 57.62%. The results indicate that the powders are mainly composed of particles of moderate size, and the particle size distribution is normal. For PAA-HPMC and PAA-C=CH2, the particle size is approximately twice that of other particles, suggesting that the modified binder promotes particle aggregation. refer to Figure 3 As can be seen, PAA-APAANa has the highest viscosity, while PAA-PAANa has the lowest viscosity. The reason why PAA-APAANa has the highest viscosity is that PAANa undergoes flocculation after ammonia treatment. This flocculation does not affect the binding effect, and the binding effect plays an indispensable role in enhancing electrical properties. refer to Figure 4 The complex impedance spectra of the ceramics measured at different temperatures and frequencies from 100 Hz to 1 MHz are presented. The fitting circuit is also shown in the figure. All samples were found to exhibit an arc pattern, indicating that the samples have single-particle polarization behavior. It can be seen that the resistance of the samples gradually decreases with increasing temperature, resulting in a decrease in the insulation of the samples. In addition, the resistance of PAANa ceramics is much lower than that of other ceramics, which is consistent with low density. There are no other polarizations, such as space charge polarization caused by pores, indicating that there are fewer pores in the ceramics. refer to Figure 5 , Figure 5 The activation energy (Ea) is based on the Z'-Z" curve, and Ea can be evaluated using the Arrhenius equation: Where ω0, kB, and T are the exponential pre-factor, Boltzmann constant, and absolute temperature, respectively. Based on the calculation results, it can be inferred that the relaxation polarization in ceramics originates from the migration of oxygen vacancies in the grains, because according to the calculation of ion transport in perovskite oxides, the Ea of oxygen vacancies migration is about 1 eV. To observe the relaxation time τ, the Z′~Z′′ curves at 500℃, 550℃ and 600℃ were used, and the equation 2πfτ=1 was used, where f corresponds to the frequency at the maximum value of the arc. refer to Figure 5 Ea and τ are like Figure 5 As shown, PAA-DM and PAA-2-EHA exhibited maximum Ea and minimum τ, while PAANa detected minimum Ea and τ. This implies that the ceramics synthesized from PAANa have strong oxygen vacancy migration, leading to large leakage current and poor d... 33 As mentioned above; refer to Figure 6 To study the removal process, thermal analysis of PAA and PAANa was performed, such as... Figure 7 As shown, due to the drastic changes in thermogravimetric (TG) analysis and derivative thermogravimetric (DTG), PAA removal occurs within a temperature range of -88℃, while the removal initiation temperature range of PAANa is -56℃. This is beneficial for the complete removal of the adhesive. In addition, the removal temperature of PAA is 271℃, which is lower than that of PAANa (307℃), which is also beneficial for removal. Combining the narrower removal temperature range of PAANA with the lower PAA initiation temperature improves the bonding effect of the mixed adhesive and enhances the overall performance.
[0034] In a method for preparing modified ceramics according to the present invention, the following aspects are studied: alkaline, acidic, and neutral PAA-based binders. Alkaline and neutral PAA-based binders are beneficial for increasing ceramic density. Except for the calcined powders granulated from PAA-HPMC and PAA-C=CH2, the median particle size (D50) of the other powders is approximately 0.771 μm–0.863 μm, with a corresponding cumulative D50 distribution ranging from 50.05% to 57.62%. Furthermore, ceramic density and binder pyrolysis play indispensable roles in piezoelectric and breakdown properties. Overall, the KNN ceramic synthesized from AcPAA exhibits the best combined properties, with a piezoelectric constant of d... 33 ~108pC / N, the breakdown strength of PAA-DM is E b ~3.93kV / cm, the above-mentioned optimal effect is achieved through the synergistic effect of particle size and thermal behavior of adhesive.
[0035] The above description is only a preferred embodiment of the present invention and does not limit the patent scope of the present invention. All equivalent modifications made using the present invention are within the patent protection scope of the present invention.
Claims
1. A method for preparing modified ceramics, characterized in that, The preparation method of modified ceramics includes the following preparation steps: S1. Add K2CO3, Na2CO3 and Nb2O5 into a planetary ball mill, add ZrO2 balls and anhydrous ethanol for one grinding to obtain a slurry; S2. Add the slurry obtained in S1 into a dryer to dry the slurry and obtain a dried slurry. S3. Add the dried slurry obtained in S2 into the calcination equipment and calcine the dried slurry to obtain fine powder; S4. Add the fine powder obtained in S3 to a planetary ball mill for secondary ball milling. Then add the modified PAA-based binder and the fine powder after secondary ball milling to a mixing device to mix the fine powder and the modified PAA-based binder to obtain granulated particles. S5. Press the granules obtained in S4 into discs with a diameter of 12-15mm. Then, heat the discs to 600℃ and keep them at that temperature for 3 hours to fully remove the binder from the disc blanks. Then raise the temperature to 1080-1110℃ to allow the blanks to be completely ceramicized. S6. Finally, apply silver paste to the upper and lower surfaces of the ceramic and keep it at 600℃ for 30 minutes. The silver paste will solidify on the surface of the ceramic and form a dense electrode, thus obtaining the modified ceramic. in, The modified PAA-based adhesive comprises the following components: PAA-based adhesive and modifier; The modifier is any one or more of the following: nonionic polyacrylamide, citric acid and sodium citrate buffer, neutral hydroxypropyl methylcellulose, and 2-ethylhexyl ester.
2. The method for preparing modified ceramics according to claim 1, characterized in that, In S1, the purity of K2CO3 is 99%, the purity of Na2CO3 is 99.8%, the purity of Nb2O5 is 99.5%, and the grinding time for one grinding cycle is 12-20 hours.
3. The method for preparing modified ceramics according to claim 2, characterized in that, In S3, the calcination temperature of the dried slurry is 800-1000℃ and the calcination time is 6-10h. In S4, the secondary ball milling time is 12-18h.
4. The method for preparing modified ceramics according to claim 2, characterized in that, In S5, the pressing pressure of the disc is 10-20 MPa, and the sintering time of the disc is 5-8 h.
5. The method for preparing modified ceramics according to claim 2, characterized in that, In S5, the sintering temperature of the ceramic blank is 1080-1110℃, and the sintering time is 5-8h.
Citation Information
Patent Citations
Ceramic granulation powder, preparation method thereof, ceramic material and mobile phone backboard
CN113045293A
Ceramic slurry for green sheat products