A multi-component, long-life, dual-phase La-Mg-Ni-based hydrogen storage alloy and its preparation method

By preparing a multi-component La-Mg-Ni based hydrogen storage alloy, using the chemical composition La0.65Nd0.1Mg0.25Ni3.1Co0.15Al0.01 and segmented heat treatment technology, an A2B7-A7B23 dual-phase structure was formed, which solved the problem of insufficient cycle life of La-Mg-Ni superlattice hydrogen storage alloys and achieved high capacity and stable electrochemical performance.

CN118497553BActive Publication Date: 2026-11-10BAOTOU ZHONGKE XUANDA NEW ENERGY TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410583741.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2026-11-10
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

Existing La-Mg-Ni superlattice hydrogen storage alloys exhibit a trade-off in their electrochemical performance: high capacity but poor cycle life. The single composition of multi-element alloys leads to insufficient cycle stability, making it difficult to improve performance through adjustments to the alloy structure and the synergistic effect of surface passivation films.

Method used

A multi-component, long-life, dual-phase La-Mg-Ni based hydrogen storage alloy was prepared using a chemical composition of La0.65Nd0.1Mg0.25Ni3.1Co0.15Al0.01. The A2B7 and A7B23 phase structures were formed through induction melting and segmented heat treatment. The Nd, Co, and Al were used to form a surface oxide film to slow down electrode corrosion and reduce lattice hydrogen absorption expansion.

Benefits of technology

It significantly improves the discharge capacity and cycle stability of the alloy, with a capacity retention rate of 87.3% after 100 cycles. It has excellent high-rate discharge performance and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497553B_ABST
    Figure CN118497553B_ABST
Patent Text Reader

Abstract

This invention discloses a multi-component, long-life, dual-phase La-Mg-Ni-based hydrogen storage alloy and its preparation method. The molecular formula of the hydrogen storage alloy is La. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 , consisting of A2B7 phase and A7B 23 The phase composition is a two-phase structure. Nd, Co and Al can respectively mitigate electrode corrosion by forming a surface oxide film and reduce lattice hydrogen absorption expansion to slow down structural damage, thereby improving the cycle performance of the alloy to a certain extent. The alloy is prepared by induction melting and segmented heat treatment. The preparation method is simple and the process is easy to control. Its discharge capacity and cycle stability are significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hydrogen storage materials technology, specifically relating to a multi-component long-life dual-phase La-Mg-Ni based hydrogen storage alloy and its preparation method. Background Technology

[0002] Human activities and social development have led to the massive consumption of fossil fuels, causing severe environmental problems and an energy crisis affecting the entire globe. Therefore, at the 75th United Nations General Assembly, the Chinese government solemnly declared to the world that hydrogen energy, due to its abundant resources, environmental friendliness, and good combustion performance, is considered the most promising clean energy source of the 21st century. Nickel / metal hydride (Ni / MH) batteries are one of the important areas of hydrogen energy application and still hold a significant market share. However, traditional AB5-type hydrogen storage alloy electrode materials cannot meet market demands due to capacity limitations. A new type of La-Mg-Ni superlattice hydrogen storage alloy, composed of [A2B4] and [AB5] sublattices, has been developed and combines the high capacity of AB2-type alloys with the easy activation of AB5-type alloys. It is being promoted to the market as a new generation of Ni / MH battery anode materials. However, the overall electrochemical performance of this type of alloy, especially its hydrogen storage capacity and cycle life, still needs further improvement.

[0003] In the research process of improving the above-mentioned performance, an important problem exists: different electrochemical properties tend to have a "trade-off" phenomenon. For example, AB3 type superlattice hydrogen storage alloys have high capacity but poor cycle life, while A2B7 and A5B... 19 The AB3 type alloy has a relatively good cycle life, but its capacity is significantly lower than that of the AB3 type alloy. A7B 23 The A2B7 phase is a recently discovered superlattice structure alloy phase, consisting of six [AB5] subunits and four [A2B4] subunits stacked along the c-axis in the order [AB5]-[A2B4]-2[AB5]-[A2B4]-[AB5]-[A2B4]-2[AB5]-[A2B4]. Our previous research showed that a certain amount of A7B appears in the A2B7 single-phase alloy. 23 The phase can significantly improve the discharge capacity of alloy electrodes, and the rate discharge performance is also improved to some extent, but its cycle stability is not yet ideal. The reason for this is that the existing phases are predominantly A2B7, with A7B as a secondary phase. 23 Alloys where the primary phase is a minor phase have a relatively simple elemental composition, containing only one substituent element besides La, Mg, and Ni, and their role is also relatively singular. Recent studies have found that although a series of A2B7-A7B alloys can be prepared by adjusting the elemental composition, stoichiometry, and heat treatment procedures, the specific composition of the alloy can be varied. 23Dual-phase alloys, with capacities exceeding 400 mAh / g, exhibit significantly improved cycle stability compared to AB3 alloys. However, due to their relatively simple elemental composition—containing only one substitution element besides La, Mg, and Ni (Pr, Nd, or Co)—their role in cycle stability is limited, resulting in poor stability and restricting the improvement of their cycle life. Furthermore, increasing the number of alloying elements increases instability and makes controlling the phase structure formed by the alloy more difficult. Therefore, if multi-component A2B7-A7B alloys could be prepared... 23 Dual-phase alloys, which synergistically enhance both crystal structure and surface passivation film, will contribute to further improving the alloy's cycle performance. However, multi-component A2B7-A7B... 23 There are currently no reports on dual-phase superlattice hydrogen storage alloys. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention aims to provide a multi-component, long-life, dual-phase La-Mg-Ni-based hydrogen storage alloy and its preparation method. The molecular formula of this hydrogen storage alloy is La. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 , consisting of A2B7 phase and A7B 23 The phase composition is a two-phase structure. Nd, Co and Al can respectively mitigate electrode corrosion by forming a surface oxide film and reduce lattice hydrogen absorption expansion to slow down structural damage, thereby improving the cycle performance of the alloy to a certain extent. The alloy is prepared by induction melting and segmented heat treatment. The preparation method is simple and the process is easy to control. Its discharge capacity and cycle stability are significantly improved.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] A multi-component, long-life, dual-phase La-Mg-Ni based hydrogen storage alloy, the molecular formula of which is La 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 .

[0007] As a limitation of the present invention, the hydrogen storage alloy is composed of A2B7 phase and A7B... 23 The phases form a two-phase structure.

[0008] As a further limitation of the present invention, the content of the A2B7 phase is 77.3 to 85.8 wt%.

[0009] This invention also provides a method for preparing a multi-component long-life dual-phase La-Mg-Ni based hydrogen storage alloy, which is prepared according to the following steps:

[0010] S1, Induction Melting Alloy

[0011] According to La 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The chemical composition was prepared by batching, with La in excess of 3wt%, Nd in excess of 3wt%, and Mg in excess of 10wt%, and the alloy ingot was prepared by medium-frequency induction melting.

[0012] S2, Heat Treatment

[0013] Take the smelted alloy ingot, place it in a sealed nickel shell container, and then place the nickel shell containing the alloy ingot in a vacuum tube furnace for segmented heat treatment under an argon atmosphere.

[0014] As a limitation of the preparation method of the present invention, in step S2, the segmented heat treatment is performed sequentially according to the following steps:

[0015] Warming phase:

[0016] In the first heating stage, the temperature is increased from room temperature to 600℃ at a heating rate of 5℃ / min, and held for 2 hours.

[0017] In the second heating stage, the temperature is increased from 600℃ to 700℃ at a heating rate of 1℃ / min, and held for 2 hours.

[0018] In the third heating stage, the temperature is increased from 700℃ to 800℃ at a heating rate of 1℃ / min, and held for 2 hours.

[0019] In the fourth heating stage, the temperature was increased from 800℃ to 960-970℃ at a heating rate of 1℃ / min, and held for 10 hours.

[0020] Cooling stage: The temperature is reduced to 500°C at a rate of 5°C / min, and then cooled to room temperature along with the furnace.

[0021] As a second limitation of the preparation method of the present invention, in step S2, the sealed nickel shell container satisfies the following ratio: alloy ingot mass to nickel sheet area forming the nickel shell container is (11.8~12.5) g : (55.90~59.63) cm². 2 .

[0022] The heat treatment process of this invention is crucial for the formation of the alloy's phase structure. In the first heating stage, the remaining elemental Mg undergoes a peritectic reaction with the solid phase to generate the AB2 phase. In the second heating stage, the AB2 phase undergoes a peritectic reaction with the liquid phase to generate the AB3 alloy phase. In the third heating stage, the AB3 phase undergoes a peritectic reaction with the liquid phase to generate A7B. 23 Alloy phase; fourth heating stage, A7B 23 The phase undergoes a peritectic reaction with the liquid phase to form the A2B7 phase. Depending on the ratio of the A side to the B side, a portion of A7B will be present. 23 Alloy phases remain; during this stage, the final two-phase structure can only be formed when the temperature reaches 960-970℃. At temperatures below 960℃, the AB3 phase will exist in the alloy, while at temperatures above 970℃, the A2B7 single phase will be generated.

[0023] The above-mentioned technical solution of the present invention is a whole in which each step is closely related and mutually influential, and together they determine the morphological characteristics and performance of the product.

[0024] The above technical solution has the following advantages or beneficial effects:

[0025] 1. The preparation method of this invention is simple, the process is easy to control, and the cycle is short, making it suitable for industrial production and promotion.

[0026] 2. The prepared hydrogen storage alloy exhibits significantly improved discharge capacity and cycle stability without compromising rate discharge performance. The alloy electrode achieves a capacity of 356 mAh·g after 100 cycles. -1 The corresponding capacity retention rate is 87.3% when the discharge current density is 1500 mA·g. -1 At that time, the HRD of the alloy electrode was 52.7%.

[0027] This invention is applicable to the preparation of two-phase hydrogen storage alloys. Attached Figure Description

[0028] Figure 1 This is an example of the actual preparation process of the nickel-shell container prepared according to the present invention;

[0029] Figure 2 The XRD patterns of alloy samples from Examples 1-3 and Comparative Examples 1-2 of this invention are shown below.

[0030] Figure 3 The graphs show the relationship between discharge capacity and cycle number during the activation process of alloy samples from Examples 1-3 and Comparative Examples 1-2 of the present invention during the first seven weeks of the invention.

[0031] Figure 4 The graphs show the relationship between the discharge capacity (left) and capacity retention (right) of the alloy samples in Examples 1-3 and Comparative Examples 1-2 of this invention and the number of cycles.

[0032] Figure 5 The high rate discharge (HRD) curves are for the alloy samples of Examples 1-3 and Comparative Examples 1-2 of this invention. Detailed Implementation

[0033] The following embodiments are merely some, not all, of the embodiments of the present invention. Therefore, the detailed descriptions of the embodiments provided below are not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0034] In this invention, unless otherwise specified, all equipment and raw materials are commercially available or commonly used in the industry. The methods described in the following embodiments are conventional methods in the art, unless otherwise specified.

[0035] Example 1

[0036] S1, Induction Melting Alloy

[0037] According to La 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The chemical composition was prepared by batching, with La in excess of 3wt%, Nd in excess of 3wt%, and Mg in excess of 10wt%, and the alloy ingot was prepared by medium-frequency induction melting.

[0038] A uniformly shaped La was obtained by wire cutting. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The alloy block weighed 11.8g. The sharp corners and surface oxide layer of the alloy were removed using a file and sandpaper to prevent the sharp parts from puncturing the nickel shell.

[0039] Preparation of sealed nickel shells, such as Figure 1 As shown in (a) to (d), the specific production process is as follows:

[0040] ① Cut a 6.5×8.6cm nickel sheet (the length-to-width ratio of the nickel sheet is 4:3), fold the rectangle along the center line of the long side and bend it so that the center line forms a curved surface with a certain curvature;

[0041] ② Tap the bottom of the bent edge to form a flat surface of a certain width (1-1.5cm wide). This step can create a wider cavity inside the nickel shell container. When the alloy ingot is placed in the cavity of the nickel shell container, the alloy ingot has a certain amount of room to move in the cavity of the nickel shell container, ensuring that the alloy ingot is not stuck by the inner wall of the nickel shell container.

[0042] ③ Subsequently, fold both sides of the long side to make a nickel-shell container with an opening on only one side, with the folded edge width being 0.3 to 0.5 cm;

[0043] ④ Place the alloy block of the corresponding mass into the corresponding nickel shell container, fold the remaining side, i.e. the short side, with a folded edge width of 0.3 to 0.5 cm. At the same time, ensure that the alloy ingot can be placed into the cavity of the nickel shell container without being stuck by the inner wall of the nickel shell container, so as to avoid the alloy ingot reacting with the nickel shell container at high temperature.

[0044] ⑤ Use a spot welding machine to seal the three folded edges of the nickel shell ingot.

[0045] S2, Heat Treatment

[0046] Place the sealed nickel shell containing the alloy into the small ark crucible, and position the crucible in the center of the tube furnace, inserting furnace liners at both ends. Tighten the tube furnace end cap screws simultaneously with a hex wrench to seal. Purge the tube furnace with gas, open the vacuum pump valve, and slowly turn the metal valve counterclockwise to begin evacuation. When the pressure gauge reading reaches -0.1 or evacuation stops, close the valve. Open the argon cylinder valve, and then slowly open the metal valve next to the pressure gauge counterclockwise to fill the quartz tube with argon gas until the pressure gauge reading reaches 0. Close the metal valve next to the pressure gauge and reopen the metal valve of the vacuum pump. Vacuum the valves and repeat the above operation 2-3 times. After completion, close the vacuum pump valves, and then prepare for the heat treatment process. During the heating process, first heat to 600℃ at a heating rate of 5℃ / min and hold for 2 hours. Then heat to 700℃ at a heating rate of 1℃ / min and hold for 2 hours. Then heat to 800℃ at a heating rate of 1℃ / min and hold for 2 hours. Finally, heat to 960℃ at a heating rate of 1℃ / min and hold for 10 hours. Then proceed to the cooling process, cooling to 500℃ at a cooling rate of 5℃ / min, and then cooling to room temperature with the furnace.

[0047] The sample was removed from the nickel shell, approximately 0.3g of which was used to remove the surface oxide layer with a file. The sample was then pulverized and ground to below 300 mesh. XRD analysis was performed, and the XRD data were refined using Maud software. The XRD pattern of the alloy and the phase composition obtained after refinement are shown below. Figure 2 As shown in the left figure. The results indicate that the alloy is A2B7-A7B. 23 The structure is a two-phase structure, in which the A2B7 phase content is 77.3 wt%, and the A7B phase content is 100%.23 The phase content is 22.7 wt%.

[0048] A portion of the alloy block was removed, the oxide layer was removed, and it was ground to 200-400 mesh to serve as the negative electrode active material for the battery. It was mixed evenly with nickel hydroxide powder at a ratio of 1:5, cold-pressed into sheets, and welded to the tabs to serve as the negative electrode of the nickel-metal hydride battery. Nickel hydroxide plates were used as the positive electrode of the nickel-metal hydride battery, and 6M KOH solution was used as the electrolyte. Nylon separators were used. The above materials were used to make an open-ended dual-electrode half-cell for electrochemical performance testing. Before the test, the battery system was soaked and allowed to stand for 24 hours to fully wet the separator. Then, the electrochemical performance of the battery was tested using a Xinwei CT-4008-5V6A-S1 battery tester.

[0049] The activation curve of the alloy electrode is as follows: Figure 3 As shown, the alloy electrode can be fully activated in the second week, with a maximum discharge capacity of 404 mAh g. -1 The cycle stability curves and capacity retention curves of the alloy within 100 cycles are as follows: Figure 4 As shown, the capacity of the alloy electrode after 100 cycles is 345 mAh g. -1 The corresponding capacity retention rate is 85.5%; the high rate discharge performance (HRD) of the alloy is as follows: Figure 5 As shown, when the discharge current density is 1500 mA g -1 At that time, the HRD of the alloy electrode was 49.2%.

[0050] Example 2

[0051] S1, Induction Melting Alloy

[0052] According to La 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The chemical composition was prepared by batching, with La in excess of 3wt%, Nd in excess of 3wt%, and Mg in excess of 10wt%, and the alloy ingot was prepared by medium-frequency induction melting.

[0053] A uniformly shaped La was obtained by wire cutting. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The alloy block weighs 12.5g. Use a file and sandpaper to remove the sharp corners and surface oxide layer of the alloy to prevent the sharp parts from puncturing the nickel shell.

[0054] A 6.7×8.9cm nickel sheet (with a length-to-width ratio of 4:3) was cut to make a sealing nickel shell, and the sealing nickel shell containing the alloy was prepared in the same way as in Example 1.

[0055] S2, Heat Treatment

[0056] Place the sealed nickel shell containing the alloy into the small ark crucible, and position the crucible in the center of the tube furnace, inserting furnace liners at both ends. Tighten the tube furnace end cap screws simultaneously with a hex wrench to seal. Purge the tube furnace with gas, open the vacuum pump valve, and slowly turn the metal valve counterclockwise to begin evacuation. When the pressure gauge reading reaches -0.1 or evacuation stops, close the valve. Open the argon cylinder valve, and then slowly open the metal valve next to the pressure gauge counterclockwise to fill the quartz tube with argon gas until the pressure gauge reading reaches 0. Close the metal valve next to the pressure gauge and reopen the metal valve of the vacuum pump. Vacuum the valves and repeat the above operation 2-3 times. After completion, close the vacuum pump valves, and then prepare for the heat treatment process. During the heating process, first heat to 600℃ at a heating rate of 5℃ / min and hold for 2 hours. Then heat to 700℃ at a heating rate of 1℃ / min and hold for 2 hours. Then heat to 800℃ at a heating rate of 1℃ / min and hold for 2 hours. Finally, heat to 965℃ at a heating rate of 1℃ / min and hold for 10 hours. Then enter the cooling process and cool to 500℃ at a cooling rate of 5℃ / min. Then cool to room temperature with the furnace.

[0057] The sample was removed from the nickel shell, approximately 0.3g of which was used to remove the surface oxide layer with a file. The sample was then pulverized and ground to below 300 mesh. XRD analysis was performed, and the XRD data were refined using Maud software. The XRD pattern of the alloy and the phase composition obtained after refinement are shown below. Figure 2 As shown in the left figure. The results indicate that the alloy is A2B7-A7B. 23 The structure is a two-phase structure, in which the A2B7 phase content is 81.7 wt%, and the A7B phase content is 100%. 23 The phase content is 18.3 wt%.

[0058] A portion of the alloy block was removed, the oxide layer was removed, and it was ground to 200-400 mesh to serve as the negative electrode active material for the battery. It was mixed evenly with nickel hydroxide powder at a ratio of 1:5, cold-pressed into sheets, and welded to the tabs to serve as the negative electrode of the nickel-metal hydride battery. Nickel hydroxide plates were used as the positive electrode of the nickel-metal hydride battery, and 6M KOH solution was used as the electrolyte. Nylon separators were used. The above materials were used to make an open-ended dual-electrode half-cell for electrochemical performance testing. Before the test, the battery system was soaked and allowed to stand for 24 hours to fully wet the separator. Then, the electrochemical performance of the battery was tested using a Xinwei CT-4008-5V6A-S1 battery tester.

[0059] The activation curve of the alloy electrode is as follows: Figure 3As shown, the alloy electrode can be fully activated in the second week, with a maximum discharge capacity of 407 mAh g. -1 The cycle stability curves and capacity retention curves of the alloy within 100 cycles are as follows: Figure 4 As shown, the capacity of the alloy electrode after 100 cycles is 352 mAh g. -1 The corresponding capacity retention rate is 86.5%; the high rate discharge performance (HRD) of the alloy is as follows: Figure 5 As shown, when the discharge current density is 1500 mA g -1 At that time, the HRD of the alloy electrode was 50.5%.

[0060] Example 3

[0061] S1, Induction Melting Alloy

[0062] According to La 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The chemical composition was prepared by batching, with La in excess of 3wt%, Nd in excess of 3wt%, and Mg in excess of 10wt%, and the alloy ingot was prepared by medium-frequency induction melting.

[0063] A uniformly shaped La was obtained by wire cutting. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The alloy block weighs 12.0g. Use a file and sandpaper to remove the sharp corners and surface oxide layer of the alloy to prevent the sharp parts from puncturing the nickel shell.

[0064] A 6.57×8.75cm nickel sheet (with a length-to-width ratio of 4:3) was cut to make a sealing nickel shell. The sealing nickel shell containing the alloy was prepared in the same manner as in Example 1.

[0065] Place the sealed nickel shell containing the alloy into the small ark crucible, and position the crucible in the center of the tube furnace, inserting furnace liners at both ends. Tighten the tube furnace end cap screws simultaneously with a hex wrench to seal. Purge the tube furnace with gas, open the vacuum pump valve, and slowly turn the metal valve counterclockwise to begin evacuation. When the pressure gauge reading reaches -0.1 or evacuation stops, close the valve. Open the argon cylinder valve, and then slowly open the metal valve next to the pressure gauge counterclockwise to fill the quartz tube with argon gas until the pressure gauge reading reaches 0. Close the metal valve next to the pressure gauge and reopen the metal valve of the vacuum pump. Vacuum the valves and repeat the above operation 2-3 times. After completion, close the vacuum pump valves, and then prepare for the heat treatment process. During the heating process, first heat to 600℃ at a heating rate of 5℃ / min and hold for 2 hours. Then heat to 700℃ at a heating rate of 1℃ / min and hold for 2 hours. Then heat to 800℃ at a heating rate of 1℃ / min and hold for 2 hours. Finally, heat to 970℃ at a heating rate of 1℃ / min and hold for 10 hours. Then proceed to the cooling process and cool to 500℃ at a cooling rate of 5℃ / min. Then cool to room temperature with the furnace.

[0066] The sample was removed from the nickel shell, approximately 0.3g of which was used to remove the surface oxide layer with a file. The sample was then pulverized and ground to below 300 mesh. XRD analysis was performed, and the XRD data were refined using Maud software. The XRD pattern of the alloy and the phase composition obtained after refinement are shown below. Figure 2 As shown in the left figure. The results indicate that the alloy is A2B7-A7B. 23 The structure is a two-phase structure, in which the A2B7 phase content is 85.8 wt%, and the A7B phase content is 100%. 23 The phase content is 14.2 wt%.

[0067] A portion of the alloy block was removed from its oxide layer and ground to a fineness of 200-400 mesh to serve as the negative electrode active material for the battery. This material was then mixed uniformly with nickel hydroxide powder at a 1:5 ratio, cold-pressed into sheets, and welded to electrode tabs to form the negative electrode of the nickel-metal hydride battery. Nickel hydroxide plates were used as the positive electrode, and a 6M KOH solution was used as the electrolyte. A nylon separator was employed. These materials were used to construct an open-cell dual-electrode half-cell for electrochemical performance testing. Before testing, the battery system was soaked and allowed to stand for 24 hours to fully wet the separator. The electrochemical performance of the battery was then tested using a Xinwei CT-4008-5V6A-S1 battery tester. The activation curves of the alloy electrodes are shown below. Figure 3 As shown, the alloy electrode can be fully activated in the second week, with a maximum discharge capacity of 408 mAh g. -1 The cycle stability curves and capacity retention curves of the alloy within 100 cycles are as follows: Figure 4 As shown, the capacity of the alloy electrode after 100 cycles is 356 mAh g. -1The corresponding capacity retention rate is 87.3%; the high rate discharge performance (HRD) of the alloy is as follows: Figure 5 As shown, when the discharge current density is 1500 mAg -1 At that time, the HRD of the alloy electrode was 52.7%.

[0068] Comparative Example 1

[0069] A uniformly shaped La was obtained by wire cutting. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The alloy block (obtained by induction melting in the same way as in Example 1) weighed 11.7g. The sharp corners and surface oxide layer of the alloy were removed by filing and sandpaper to prevent the sharp parts from puncturing the nickel shell.

[0070] A 6.4×8.6cm nickel sheet (with a length-to-width ratio of 4:3) was cut and a sealed nickel shell containing the alloy was prepared using the same method as in Example 1.

[0071] Place the sealed nickel shell containing the alloy into the small ark crucible, and position the crucible in the center of the tube furnace, with furnace liners placed at both ends. Tighten the end cap screws of the tube furnace simultaneously using a hex wrench to seal it. Purge the tube furnace with gas, open the vacuum pump valve, and slowly turn the metal valve counterclockwise to begin evacuation. When the pressure gauge reading reaches -0.1 or evacuation stops, close the valve, open the argon cylinder switch, and slowly open the metal valve next to the pressure gauge counterclockwise to fill the quartz tube with argon gas until the pressure gauge reading reaches 0. Close the metal valve next to the pressure gauge, and open the metal valve of the vacuum pump again to evacuate. Repeat the above operation 2-3 times. After completion, close the vacuum pump valve, and then prepare for the annealing process. During the heating process, first heat to 600℃ at a heating rate of 5℃ / min and hold for 2 hours, then heat to 900℃ at a heating rate of 1℃ / min and hold for 10 hours. Then begin the cooling process, cooling to 500℃ at a cooling rate of 5℃ / min, and then cool to room temperature with the furnace.

[0072] The sample was removed from the nickel shell, approximately 0.3g of which was used to remove the surface oxide layer with a file. The sample was then pulverized and ground to below 300 mesh. XRD analysis was performed, and the XRD data were refined using Maud software. The XRD pattern of the alloy and the phase composition obtained after refinement are shown below. Figure 2 As shown in the right figure, the results indicate that the alloy consists of A2B7 and AB3 phases, with A2B7 phase comprising 57.6 wt% and AB3 phase comprising 42.4 wt%.

[0073] A portion of the alloy block was removed from its oxide layer and ground to a fineness of 200-400 mesh to serve as the negative electrode active material for the battery. This material was then mixed uniformly with nickel hydroxide powder at a 1:5 ratio, cold-pressed into sheets, and welded to electrode tabs to form the negative electrode of the nickel-metal hydride battery. Nickel hydroxide plates were used as the positive electrode, and a 6M KOH solution was used as the electrolyte. A nylon separator was employed. These materials were used to construct an open-cell dual-electrode half-cell for electrochemical performance testing. Before testing, the battery system was soaked and allowed to stand for 24 hours to fully wet the separator. The electrochemical performance of the battery was then tested using a Xinwei CT-4008-5V6A-S1 battery tester. The activation curves of the alloy electrodes are shown below. Figure 3 As shown, the alloy electrode can be fully activated in the second week, with a maximum discharge capacity of 401 mAh g. -1 The cycle stability curves and capacity retention curves of the alloy within 100 cycles are as follows: Figure 4 As shown, the capacity of the alloy electrode after 100 cycles is 317 mAh g. -1 The corresponding capacity retention rate is 79.0%; the high rate discharge performance (HRD) of the alloy is as follows: Figure 5 As shown, when the discharge current density is 1500 mAg -1 At that time, the HRD of the alloy electrode was 47.6%.

[0074] Comparative Example 2

[0075] A uniformly shaped La was obtained by wire cutting. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The alloy block (obtained by induction melting in the same way as in Example 1) weighed 11.5g. The sharp corners and surface oxide layer of the alloy were removed by filing and sandpaper to prevent the sharp parts from puncturing the nickel shell.

[0076] A 6.4×8.6cm nickel sheet (with a length-to-width ratio of 4:3) was cut and a sealed nickel shell containing the alloy was prepared using the same method as in Example 1.

[0077] Place the sealed nickel shell containing the alloy into the small ark crucible, and position the crucible in the center of the tube furnace, with furnace liners placed at both ends. Tighten the end cap screws of the tube furnace simultaneously using a hex wrench to seal it. Purge the tube furnace with gas, open the vacuum pump valve, and slowly turn the metal valve counterclockwise to begin evacuation. When the pressure gauge reading reaches -0.1 or evacuation stops, close the valve, open the argon cylinder switch, and slowly open the metal valve next to the pressure gauge counterclockwise to fill the quartz tube with argon gas until the pressure gauge reading reaches 0. Close the metal valve next to the pressure gauge, and open the metal valve of the vacuum pump again to evacuate. Repeat the above operation 2-3 times. After completion, close the vacuum pump valve, and then prepare for the annealing process. During the heating process, first heat to 600℃ at a heating rate of 5℃ / min and hold for 2 hours, then heat to 950℃ at a heating rate of 1℃ / min and hold for 10 hours. Then begin the cooling process, cooling to 500℃ at a cooling rate of 5℃ / min, and then cool to room temperature with the furnace.

[0078] The sample was removed from the nickel shell, approximately 0.3g of which was used to remove the surface oxide layer with a file. The sample was then pulverized and ground to below 300 mesh. XRD analysis was performed, and the XRD data were refined using Maud software. The XRD pattern of the alloy and the phase composition obtained after refinement are shown below. Figure 2 As shown in the right figure, the results indicate that the alloy consists of A2B7 and AB3 phases, with A2B7 phase comprising 79.4 wt% and AB3 phase comprising 20.6 wt%.

[0079] A portion of the alloy block was removed from its oxide layer and ground to a fineness of 200-400 mesh to serve as the negative electrode active material for the battery. This material was then mixed uniformly with nickel hydroxide powder at a 1:5 ratio, cold-pressed into sheets, and welded to electrode tabs to form the negative electrode of the nickel-metal hydride battery. Nickel hydroxide plates were used as the positive electrode, and a 6M KOH solution was used as the electrolyte. A nylon separator was employed. These materials were used to construct an open-cell dual-electrode half-cell for electrochemical performance testing. Before testing, the battery system was soaked and allowed to stand for 24 hours to fully wet the separator. The electrochemical performance of the battery was then tested using a Xinwei CT-4008-5V6A-S1 battery tester. The activation curves of the alloy electrodes are shown below. Figure 3 As shown, the alloy electrode can be fully activated in the second week, with a maximum discharge capacity of 398 mAh g. -1 The cycle stability curves and capacity retention curves of the alloy within 100 cycles are as follows: Figure 4 As shown, the capacity of the alloy electrode after 100 cycles is 327 mAh g. -1 The corresponding capacity retention rate is 82.1%; the high rate discharge performance (HRD) of the alloy is as follows: Figure 5 As shown, when the discharge current density is 1500 mAg -1 At that time, the HRD of the alloy electrode was 48.8%.

Claims

1. A multi-component, long-life, dual-phase La-Mg-Ni-based hydrogen storage alloy, characterized in that, The molecular formula of this hydrogen storage alloy is La. 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The hydrogen storage alloy is composed of A2B7 phase and A7B... 23 The phase composition is a two-phase structure; the A2B7 phase content is 77.3–85.8 wt%. The preparation method of the multi-component long-life dual-phase La-Mg-Ni based hydrogen storage alloy is carried out according to the following steps: S1, Induction Melting Alloy According to La 0.65 Nd 0.1 Mg 0.25 Ni 3.1 Co 0.15 Al 0.01 The chemical composition was prepared by batching, with La in excess of 3 wt%, Nd in excess of 3 wt%, and Mg in excess of 10 wt%, and the alloy ingot was prepared by medium-frequency induction melting. S2, Heat Treatment Take the smelted alloy ingot, put it into a sealed nickel shell container, and then place the nickel shell containing the alloy ingot into a vacuum tube furnace for segmented heat treatment under an argon atmosphere. The segmented heat treatment is performed sequentially according to the following steps: Warming phase: First heating stage: The temperature is increased from room temperature to 600 ℃ at a heating rate of 5℃ / min, and held for 2 h; In the second heating stage, the temperature is increased from 600 ℃ to 700 ℃ at a heating rate of 1℃ / min, and held for 2 h. In the third heating stage, the temperature is increased from 700 ℃ to 800 ℃ at a heating rate of 1℃ / min, and held for 2 hours. In the fourth heating stage, the temperature was increased from 800 ℃ to 960~970 ℃ at a heating rate of 1℃ / min, and held for 10 h. Cooling stage: The temperature is reduced to 500 ℃ at a cooling rate of 5 ℃ / min, and then cooled to room temperature with the furnace.

2. The multi-component long-life dual-phase La-Mg-Ni based hydrogen storage alloy according to claim 1, characterized in that, In step S2, the sealed nickel shell container satisfies the ratio of alloy ingot mass to nickel sheet area forming the nickel shell container as (11.8~12.5) g : (55.90~59.63) cm². 2 .

Citation Information

Patent Citations

  • (La,Nd,)-Mg-Ni double-phase superlattice hydrogen storage alloy and preparation method thereof

    CN112501475A