A negative electrode material, a negative electrode slurry and preparation method, a negative electrode sheet and nickel-zinc battery

By adding zinc and zinc oxide to the negative electrode material of nickel-zinc batteries, and using hectorite and polyether-modified silicone oil to form an interface protective film, combined with phosphates and organic surfactants in the electrolyte, the problem of nickel-zinc batteries was solved. The problems of short life and poor high-temperature storage performance are achieved by achieving good cycle stability and high-temperature storage performance.

CN118507731BActive Publication Date: 2024-10-15SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964078.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-15
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Nickel-zinc batteries have a short lifespan and poor high-temperature storage performance. It is difficult to find a balance between increasing lifespan and reducing self-discharge with existing technology, resulting in difficulties in mass production.

Method used

Zinc and zinc oxide are added to the negative electrode material, and through the combination of laponite and polyether-modified silicone oil, an interface protective film containing silicon and magnesium is formed to enhance the water retention and adhesion of the negative electrode slurry and slow down self-discharge. Phosphate, boric acid, and organic surfactants are added to the electrolyte to reduce the corrosion of the negative electrode active material by the electrolyte.

Benefits of technology

It significantly improves the high-temperature storage performance and cycle stability of nickel-zinc batteries, extends the cycle life of the battery, slows down the self-discharge phenomenon, and achieves uniform distribution and stability of the negative electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_56
    Figure SMS_56
Patent Text Reader

Abstract

In order to overcome the problems of short life and easy self-discharge of existing nickel-zinc batteries, the present invention provides a negative electrode material, including a negative electrode active material and a negative electrode additive, the negative electrode active material includes zinc and zinc oxide, the negative electrode additive includes hectorite and polyether modified silicone oil, and the mass ratio of hectorite to polyether modified silicone oil is 1:10-10:1; the present invention adds hectorite in the process of preparing the negative electrode material, and the hectorite forms a uniform and extremely thin silicon- and magnesium-containing interface protective film on the negative electrode sheet, thereby slowing down the corrosion of zinc and zinc oxide in the negative electrode by the alkaline electrolyte, thereby achieving the effect of slowing down the self-discharge degree of the nickel-zinc battery, so that the nickel-zinc battery exhibits good high-temperature storage performance and cycle stability performance; the ether bond of the polyether modified silicone oil enhances the water retention of the negative electrode slurry, improves the adhesion between the negative electrode active material and the negative electrode current collector in the nickel-zinc battery, and makes the distribution of the negative electrode active material in the negative electrode slurry uniform and consistent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode material, a negative electrode slurry and a preparation method thereof, a negative electrode sheet and a nickel-zinc battery. Background Art

[0002] At present, the nickel-zinc batteries with large-scale commercial applications mainly include lead-acid batteries, nickel-zinc batteries and lithium-ion batteries. However, they all have certain limitations. For example, the low energy density and environmentally harmful characteristics of lead-acid batteries make them face elimination; the low operating voltage and power density, as well as the limited service life restrict the promotion and application of nickel-zinc batteries; lithium batteries are limited by flammable and high-viscosity organic electrolytes, high manufacturing costs and limited lithium and cobalt resources, etc., and there are great safety hazards in large-scale applications, and the fast charging and discharging capabilities are poor, and the cost remains high. Among the many known battery systems, alkaline nickel-zinc batteries, as green and environmentally friendly aqueous batteries, have the advantages of long life, high voltage, and low internal resistance. They are the most likely type of battery to meet the above requirements. They have the advantages of high power, rich electrode material resources, and excellent safety performance. They are considered to be strong competitors and substitutes for lithium batteries, lead-acid batteries, and nickel-zinc batteries.

[0003] Although alkaline nickel-zinc batteries have many advantages, they have poor storage performance at high temperatures due to their high self-discharge. The self-discharge of nickel-zinc batteries occurs because of the irreversible consumption of Zn or ZnO in a strong alkaline electrolyte.

[0004] In the prior art, the self-discharge of nickel-zinc batteries is reduced by adding lead and cellulose to the negative electrode, thereby improving the storage performance of nickel-zinc batteries. Bismuth oxide, indium oxide, tin oxide, etc. can also be added to the negative electrode material to improve the life performance of nickel-zinc batteries.

[0005] However, the above-mentioned improvement methods only increase the life of nickel-zinc batteries or reduce the self-discharge phenomenon of nickel-zinc batteries by improving the negative electrode or electrolyte, but cannot achieve a balance between the two performances and realize mass production; therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be solved. Summary of the invention

[0006] In view of the problems of short life and poor high-temperature storage performance of nickel-zinc batteries, the present invention provides a negative electrode material for a nickel-zinc battery, a negative electrode slurry for a nickel-zinc battery and a preparation method, a negative electrode sheet for a nickel-zinc battery and a nickel-zinc battery.

[0007] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0008] A first aspect of the present invention provides a negative electrode material, comprising a negative electrode active material and a negative electrode additive, wherein the negative electrode active material comprises zinc and zinc oxide, and the negative electrode additive comprises hectorite and polyether modified silicone oil, and the mass ratio of the hectorite to the polyether modified silicone oil is 1:10-10:1.

[0009] Optionally, the mass ratio of the hectorite to the polyether-modified silicone oil is 5:6-8:3.

[0010] Optionally, the negative electrode additive also includes , , One or more of .

[0011] Optionally, in parts by weight, the 0.1-1 part; 0.5-3 parts; For 1-8 servings.

[0012] Optionally, it also includes a conductive agent, a thickener, a dispersant and a binder. In parts by weight, the negative electrode active material is 78-98 parts; the negative electrode additive is 1-10 parts; the conductive agent is 1-2 parts; the thickener is 0.3-0.5 parts; the dispersant is 1-2 parts; and the binder is 3-5 parts.

[0013] The dispersant includes one or more of sodium polyacrylate (PAANa), potassium polyacrylate (PAAK), and polyacrylamide (PAM);

[0014] The binder includes one or more of styrene-butadiene rubber (SBR) and polytetrafluoroethylene (PTFE);

[0015] The conductive agent includes one or more of activated carbon, conductive carbon black, carbon nanotubes, graphene, and vapor-grown carbon fibers;

[0016] The thickener includes one or more of sodium carboxymethyl cellulose (CMC), hydroxyethyl cellulose (HEC), and hydroxypropyl methyl cellulose (HPMC).

[0017] A second aspect of the present invention provides a negative electrode slurry, comprising the negative electrode material described above.

[0018] A third aspect of the present invention provides a method for preparing a negative electrode slurry, comprising the following steps performed in sequence:

[0019] Add conductive agent, thickener and dispersant into the barrel and stir;

[0020] Adding negative electrode active materials including zinc and zinc oxide into the barrel in multiple portions and stirring;

[0021] Add a binder, laponite and polyether-modified silicone oil into a barrel and stir to obtain a negative electrode slurry; the mass ratio of the laponite to the polyether-modified silicone oil is 1:10-10:1.

[0022] Optionally, the method further includes the following steps after adding the conductive agent, thickener, and dispersant into the barrel and stirring, and before adding the negative electrode active material into the barrel:

[0023] Add negative electrode additives except hectorite and polyether modified silicone oil into the barrel and stir.

[0024] A fourth aspect of the present invention provides a negative electrode plate, comprising the negative electrode slurry and a negative electrode current collector as described above, wherein the negative electrode slurry is coated on at least one surface of the negative electrode current collector.

[0025] Optionally, the negative electrode current collector is selected from any one of an obliquely stretched copper mesh, a tinned obliquely stretched copper mesh, a galvanized obliquely stretched copper mesh, a copper foil, and a tinned copper foil.

[0026] A fifth aspect of the present invention provides a nickel-zinc battery, comprising a negative electrode plate, a positive electrode plate, a separator and an electrolyte as described above, wherein the electrolyte is formed by mixing solution A and solution B, the weight ratio of solution A to solution B is 8-9:1, the solution A comprises an alkaline solution and a ZnO solution, and the solution B comprises one or more of a phosphate, a boron source, and an organic surfactant.

[0027] Optionally, the phosphate includes one or more of sodium phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate; the organic surfactant includes one or more of glycerol, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, dodecyltrimethylammonium bromide, and sorbitol.

[0028] According to the negative electrode active material provided by the present invention, hectorite is added during the preparation of the negative electrode material. The magnesium and silicon elements in the hectorite form a uniform, extremely thin silicon- and magnesium-containing interface protective film on the negative electrode sheet under weak alkaline conditions in the aqueous system, which slows down the corrosion of the alkaline electrolyte on the zinc and zinc oxide in the negative electrode, thereby achieving the effect of slowing down the self-discharge degree of the nickel-zinc battery, so that the nickel-zinc battery exhibits good high-temperature storage performance and cycle stability performance; the modified polyether-modified silicone oil has good water solubility and is applied to the preparation of the negative electrode material of the nickel-zinc battery. The ether bond of the polyether-modified silicone oil enhances the water retention of the negative electrode slurry, and the polyether-modified silicone oil has a certain viscosity, which improves the adhesion between the negative electrode active material and the negative electrode collector in the nickel-zinc battery, and can make the negative electrode active material in the negative electrode slurry dispersed evenly, ensuring the uniformity and consistency of the distribution of the negative electrode active material in the negative electrode sheet. DETAILED DESCRIPTION

[0029] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0030] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0031] In one embodiment, the first aspect of the present invention provides a negative electrode material, including a negative electrode active material and a negative electrode additive, wherein the negative electrode active material includes zinc and zinc oxide, and the negative electrode additive includes hectorite and polyether modified silicone oil, and the mass ratio of the hectorite to the polyether modified silicone oil is 1:10-10:1.

[0032] The mass ratio of the hectorite to the polyether-modified silicone oil is any point value among 1:10, 2:9, 3:8, 4:7, 5:6, 6:5, 7:4, 8:3, 9:2 or 10:1, or a range value consisting of any two point values.

[0033] The present invention adds hectorite during the preparation of the negative electrode material. The magnesium and silicon elements in the hectorite form a uniform, extremely thin interface protective film containing silicon and magnesium on the negative electrode sheet under weak alkaline conditions in the aqueous system, thereby slowing down the corrosion of zinc and zinc oxide in the negative electrode by the alkaline electrolyte, thereby achieving the effect of slowing down the self-discharge degree of the nickel-zinc battery, and making the nickel-zinc battery show good high-temperature storage performance and cycle stability performance.

[0034] The modified polyether-modified silicone oil has good water solubility and is applied to the preparation of negative electrode materials for nickel-zinc batteries. The ether bonds of the polyether-modified silicone oil enhance the water retention of the negative electrode slurry, and the polyether-modified silicone oil has a certain viscosity, which improves the adhesion between the negative electrode active material and the negative electrode collector in the nickel-zinc battery, and can make the negative electrode active material in the negative electrode slurry dispersed evenly, ensuring the uniformity and consistency of the distribution of the negative electrode active material in the negative electrode sheet; at the same time, it can avoid the shedding of the negative electrode active material, resulting in a reduction in battery capacity and slowing down the self-discharge of the nickel-zinc battery.

[0035] In one embodiment, the negative electrode active material is 78-98 parts by weight, and the total amount of the hectorite and the polyether-modified silicone oil is 1-10 parts by weight.

[0036] In a preferred embodiment, the negative electrode active material is 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts or 98 parts, or any two parts of the range. Preferably, the negative electrode active material is 80-90 parts.

[0037] In a preferred embodiment, the hectorite and polyether-modified silicone oil are any one of 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 parts or a range of any two parts. Preferably, the hectorite and polyether-modified silicone oil are 3-7 parts.

[0038] In one embodiment, the mass ratio of the hectorite to the polyether-modified silicone oil is 5:6-8:3. Preferably, the mass ratio of the hectorite to the polyether-modified silicone oil is 7:4.

[0039] In one embodiment, the negative electrode additive further includes , , One or more of .

[0040] Specifically, , , The negative electrode material can improve the hydrogen evolution overpotential of the negative electrode, inhibit the generation of hydrogen during the charge and discharge process, and improve the stability of the negative electrode. Thus, the negative electrode material can improve the hydrogen evolution overpotential of the negative electrode, inhibit the generation of hydrogen during the charge and discharge process, thereby improving the stability of the negative electrode, while improving the migration of ions inside the negative electrode and the uniformity of the dissolution / deposition of metal zinc, inhibiting the formation of dendrites, and applying it to zinc ion batteries can improve the stability and cycle life of zinc ion batteries.

[0041] In one embodiment, in parts by weight, 0.1-1 part; 0.5-3 parts; For 1-8 servings.

[0042] In a preferred embodiment, the It is any point value among 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part, or a range value consisting of any two point values. It is 0.2 parts to 0.8 parts.

[0043] In a preferred embodiment, the It is 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3 parts, or any two of them. 1-2 servings.

[0044] In a preferred embodiment, the 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6 , 4.7 parts, 4.8 parts, 4.9 parts, 5 parts, 5.1 parts, 5.2 parts, 5.3 parts, 5.4 parts, 5.5 parts, 5.6 parts, 5.7 parts, 5.8 parts, 5.9 parts, 6.0 parts, 6.1 parts, 6.2 parts, 6.3 parts, 6.4 parts, 6.5 parts, 6.6 parts, 6.7 parts, 6.8 parts, 6.9 parts, 7.0 parts, 7.1 parts, 7.2 parts, 7.3 parts, 7.4 parts, 7.5 parts, 7.6 parts, 7.7 parts, 7.8 parts, 7.9 parts or 8 parts, any point value or a range consisting of any two point values. Preferably said 3 to 5 servings.

[0045] In one embodiment, it also includes a conductive agent, a thickener, a dispersant and a binder. In terms of weight, the negative electrode active material is 78-98 parts; the negative electrode additive is 1-10 parts; the conductive agent is 1-2 parts; the thickener is 0.3-0.5 parts; the dispersant is 1-2 parts; and the binder is 3-5 parts.

[0046] In a preferred embodiment, the negative electrode active material is any one of 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts or 98 parts, or a range value consisting of any two points; preferably, the negative electrode active material is 85-90 parts.

[0047] In a preferred embodiment, the negative electrode additive is any point value among 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, or a range value consisting of any two point values.

[0048] In a preferred embodiment, the conductive agent is 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2 parts, or any two parts of the range. Preferably, the conductive agent is 1.2-1.8 parts.

[0049] In a preferred embodiment, the thickener is 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49 or 0.5, or any two of them. Preferably, the thickener is 0.35-0.45.

[0050] In a preferred embodiment, the dispersant is 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2 parts, or any two parts of the range. Preferably, the dispersant is 1.2-1.8 parts.

[0051] In a preferred embodiment, the binder is 3.0 parts, 3.1 parts, 3.2 parts, 3.3 parts, 3.4 parts, 3.5 parts, 3.6 parts, 3.7 parts, 3.8 parts, 3.9 parts, 4.0 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.4 parts, 4.5 parts, 4.6 parts, 4.7 parts, 4.8 parts, 4.9 parts or 5 parts, any one of the values ​​or a range consisting of any two points.

[0052] In one embodiment, the dispersant includes one or more of sodium polyacrylate (PAANa), potassium polyacrylate (PAAK), and polyacrylamide (PAM).

[0053] The present invention uses one or more of sodium polyacrylate (PAANa), potassium polyacrylate (PAAK), and polyacrylamide (PAM) as dispersants, all of which have high ionic conductivity, can reduce the internal resistance of the negative electrode, increase the conductivity, and improve the high-temperature storage performance and service life of the nickel-zinc battery.

[0054] In one embodiment, the binder includes one or more of styrene-butadiene rubber (SBR) and polytetrafluoroethylene (PTFE).

[0055] In one embodiment, the conductive agent includes one or more of activated carbon, conductive carbon black, carbon nanotubes, graphene, and vapor-grown carbon fibers.

[0056] In one embodiment, the thickener includes one or more of sodium carboxymethyl cellulose (CMC), hydroxyethyl cellulose (HEC), and hydroxypropyl methyl cellulose (HPMC).

[0057] A second aspect of the present invention provides a negative electrode slurry, comprising the negative electrode material mentioned above.

[0058] The third aspect of the present invention provides a method for preparing the aforementioned negative electrode slurry, comprising the following steps performed in sequence:

[0059] Step 1, add conductive agent, thickener and dispersant into the barrel and stir;

[0060] Step 3, adding negative electrode active materials including zinc and zinc oxide into the barrel in multiple times and stirring;

[0061] Step 4: Add a binder, laponite and polyether-modified silicone oil into a barrel and stir to obtain a negative electrode slurry; the mass ratio of the laponite to the polyether-modified silicone oil is 1:10-10:1.

[0062] Specifically, first add a conductive agent, a thickener, and a dispersant into the barrel and stir for 30 minutes; then add the negative electrode active material into the barrel in three times and stir zinc and zinc oxide, and continue stirring for 30 minutes; continue to add the binder styrene butadiene rubber (SBR) and polytetrafluoroethylene (PTFE) into the barrel, and continue stirring for 30 minutes; finally, add hectorite and polyether modified silicone oil into the barrel and stir for 30 minutes to obtain the negative electrode slurry.

[0063] In one embodiment, the method further includes the following steps after adding the conductive agent, thickener, and dispersant to the barrel and stirring, and before adding the negative electrode active material to the barrel:

[0064] Add negative electrode additives except hectorite and polyether modified silicone oil into the barrel and stir.

[0065] Specifically, add , , Negative electrode additive; stirring for 30 minutes.

[0066] A fourth aspect of the present invention provides a negative electrode plate, comprising the negative electrode slurry and a negative electrode current collector as described above, wherein the negative electrode slurry is coated on at least one surface of the negative electrode current collector.

[0067] Specifically, the negative electrode slurry is coated on both surfaces of the negative electrode current collector.

[0068] Furthermore, it also includes auxiliary tape. When the negative electrode slurry is coated on the surface of the negative electrode collector, the auxiliary tape is pasted on the area of ​​the negative electrode collector where the negative electrode slurry is not pre-coated. The auxiliary tape is any one of masking tape and insulating tape.

[0069] In one embodiment, the negative electrode current collector is selected from any one of an obliquely drawn copper mesh, a tinned obliquely drawn copper mesh, a galvanized obliquely drawn copper mesh, a copper foil, and a tinned copper foil.

[0070] Specifically, the thickness of the oblique copper mesh is 0.17 mm, the porosity is 61-85%, and the specification is 20-500 mesh;

[0071] In tinned oblique-stretched copper mesh and galvanized oblique-stretched copper mesh, the coating thickness is 2-10μm.

[0072] The thickness of the copper foil is 0.17 mm and the porosity is 40-60%.

[0073] In tinned copper foil, the coating thickness is 3-5 μm.

[0074] A fifth aspect of the present invention provides a nickel-zinc battery, comprising a negative electrode plate, a positive electrode plate, a separator and an electrolyte as described above, wherein the electrolyte is a mixture of solution A and solution B, the weight ratio of solution A to solution B is 8-9:1, the solution A comprises an alkaline solution and a ZnO solution, and the solution B comprises one or more of phosphate, boric acid, and an organic surfactant.

[0075] Specifically, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on the surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material and an auxiliary agent, and the positive electrode active material includes nickel hydroxide.

[0076] Specifically, the auxiliary agent includes a certain amount of conductive agent, and the conductive agent can be one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0077] Specifically, the auxiliary agent includes a certain amount of a binder, and the binder can be one or more of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, carboxymethyl cellulose (CMC), and the like.

[0078] Specifically, the auxiliary agent includes a certain amount of thickener, and the thickener may be carboxymethyl cellulose (CMC) or the like.

[0079] In some embodiments, the positive electrode current collector is selected from a metal material that can conduct electrons. Preferably, the positive electrode current collector is selected from nickel foam.

[0080] The diaphragm is placed between the positive and negative electrodes of the battery to prevent the direct contact between the positive and negative active materials and cause a short circuit in the battery. The diaphragm must not only be able to resist the penetration of zinc dendrites, but also be resistant to strong alkali, anti-oxidation, easy to be infiltrated by electrolyte, have good mechanical strength and strong flexibility, low resistance and high ionic conductivity; the diaphragm can be any diaphragm material suitable for nickel-zinc batteries in the art, for example, it can include but is not limited to glass fiber diaphragms.

[0081] The electrolyte of the present invention is formed by mixing solution A and solution B, wherein the weight ratio of solution A to solution B is 8-9:1, solution A comprises an alkaline solution and a ZnO solution, and solution B comprises one or more of phosphate, boric acid, and an organic surfactant.

[0082] Solution A is a 5-7 mol / L alkaline solution and a saturated ZnO solution, and solution B includes one or more of phosphate, boric acid, and an organic surfactant.

[0083] The pH of the electrolyte is 13-15, the specific gravity is 1.2-1.5 g / mL, and the conductivity at 25° C. is 350-500 mS / cm.

[0084] The invention adds phosphate, boric acid and organic surfactant to the electrolyte, which can slow down the corrosion of the electrolyte to the negative electrode active material, reduce the self-discharge phenomenon, and effectively improve the storage performance and cycle life of the nickel-zinc battery at high temperature.

[0085] The electrolyte of the present invention has the advantages of high ion conductivity, low cost and environmental friendliness. The negative electrode sheet prepared by the present invention and the electrolyte are assembled into a nickel-zinc battery, which slows down the self-discharge phenomenon of the nickel-zinc battery and can show excellent storage performance and cycle life even under high temperature conditions.

[0086] In the nickel-zinc battery provided by the present invention, the positive electrode sheet, the separator and the negative electrode sheet can generally be used to form a battery cell of a nickel-zinc battery. For example, the positive electrode sheet, the separator and the negative electrode sheet can each be a layer body, so that they can be cut into a target size and stacked in sequence, and can be further combined with an electrolyte to form a nickel-zinc battery. The positive electrode sheet, the separator and the negative electrode sheet can directly form a single-layer laminated battery, and can be further wound to a target size to form a battery cell, and can be further combined with an electrolyte to form a nickel-zinc battery. However, in a preferred embodiment of the present invention, the nickel-zinc battery is a single-layer laminated battery. Such a battery is easier to operate during the floating charge process on the one hand, and has a lower screening cost on the other hand. The nickel-zinc battery may also include various other components that can be used for nickel-zinc batteries. For example, applicable components may include but are not limited to packaging shells, pole ears, external electrodes, etc.

[0087] The battery disclosed in the embodiment of the present application can be used in various energy storage systems that use batteries as power sources or use batteries as energy storage elements. The electrical device can be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, and the like. The vehicle can be a fuel vehicle, a gas vehicle, or a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; the electric toy includes a fixed or mobile electric toy, for example, a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; the electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and a railway electric tool, for example, an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc.

[0088] In one embodiment, the phosphate includes one or more of sodium phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate; the organic surfactant includes one or more of glycerol, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, dodecyltrimethylammonium bromide, and sorbitol.

[0089] Specifically, solution B is one or more of 2 wt % phosphate, 2 wt % boric acid, and 2 wt % organic surfactant.

[0090] Organic surfactants are hydrophilic and can improve the solubility of the electrolyte, dissolve additives that are difficult to dissolve in alkaline solutions, and improve the conductivity of the electrolyte.

[0091] The present invention is further described below by way of examples.

[0092] Example 1

[0093] Preparation of negative electrode:

[0094] Preparation of the negative electrode slurry of the nickel-zinc battery in this embodiment: first add 1.5 parts of conductive agent, 0.4 parts of thickener, and 1.5 parts of dispersant into the barrel and stir for 30 minutes; then add 0.5 parts of , 1.5 parts , 4 servings Negative electrode additive; continue stirring for 30 minutes; then add 63 parts of ZnO and 25 parts of Zn into the barrel in 3 times, and continue stirring for 30 minutes; continue to add 4 parts of binder into the barrel, and continue stirring for 30 minutes; finally, add 8 parts of hectorite and 3 parts of polyether modified silicone oil into the barrel and stir for 30 minutes to obtain negative electrode slurry;

[0095] The conductive agent is graphite, the thickener is 1.5wt% CMC, and the binder is a mixture of 48wt% SBR and 60wt% PTFE, wherein the weight ratio of the two is 4:1;

[0096] The negative electrode slurry is coated on the negative electrode current collector, and then rolled, softened, and cut to obtain the negative electrode sheet of the nickel-zinc battery; the negative electrode current collector of this embodiment is an obliquely stretched tin-plated copper mesh.

[0097] Preparation of positive electrode:

[0098] The positive electrode comprises a positive electrode current collector and a positive electrode active material, wherein the positive electrode current collector has a surface density of 300-400 g / m 2 Nickel foam.

[0099] 85 copies , 1 part ZnO, 3 parts CoO, 2 parts Ni powder, 1 part , 2 , 2 1 part of graphite, 5 parts of CMC and 0.5 parts of PTFE are mixed in proportion, stirred evenly, coated on the positive electrode collector, and rolled, softened, cut, etc. to make the positive electrode sheet of the nickel-zinc battery; the positive electrode collector has a surface density of 300-400g / m 2 Nickel foam.

[0100] Preparation of electrolyte:

[0101] Solution A in the nickel-zinc battery electrolyte of this embodiment includes the following components: 8 parts of 5 mol / L KOH, 8 parts of 0.5 mol / L ZnO;

[0102] Solution B includes the following components: 1 part of 2 wt% disodium hydrogen phosphate, 0.5 part of 2 wt% boric acid, and 0.5 part of 2 wt% glycerol.

[0103] Preparation of the battery:

[0104] The positive electrode sheet, separator and negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrodes to play a role of isolation, and then wound to the bare battery cell. The bare battery cell is placed in the steel shell, the exposed edge of the negative electrode is welded to the negative current collector, and the negative current collector is welded to the steel shell, and then the electrolyte is injected, the cap is spot welded, and the sealing process is carried out to prepare the nickel-zinc battery.

[0105] Example 2

[0106] Example 2 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0107] Add 1 part to the barrel , 3 copies , 8 servings Negative electrode additives: Add 5 parts of hectorite and 6 parts of polyether modified silicone oil into the barrel.

[0108] Preparation of electrolyte:

[0109] Solution A in the nickel-zinc battery electrolyte of this embodiment includes the following components: 9 parts of 5 mol / L KOH, 8 parts of 0.5 mol / L ZnO;

[0110] Solution B includes the following components: 1 part of 2 wt% disodium hydrogen phosphate, 0.5 part of 2 wt% boric acid, and 0.5 part of 2 wt% glycerol.

[0111] Example 3

[0112] Example 3 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0113] Add 10 parts of laponite and 1 part of polyether-modified silicone oil to the barrel.

[0114] Preparation of electrolyte:

[0115] Solution A in the nickel-zinc battery electrolyte of this embodiment includes the following components: 9 parts of 5 mol / L KOH, 9 parts of 0.5 mol / L ZnO;

[0116] Solution B includes the following components: 1 part of 2 wt% disodium hydrogen phosphate, 0.5 part of 2 wt% boric acid, and 0.5 part of 2 wt% glycerol.

[0117] Example 4

[0118] Example 4 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0119] Add 1 part of hectorite and 10 parts of polyether-modified silicone oil to the barrel.

[0120] Example 5

[0121] Example 5 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0122] Add 0.1 parts of , 0.5 , 1 Negative electrode additives.

[0123] Example 6

[0124] Example 6 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0125] Add 1 part to the barrel , 3 copies , 8 servings Negative electrode additives.

[0126] Example 7

[0127] Example 7 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0128] Solution B includes the following components: 1 part of 2 wt % sodium phosphate, 0.5 part of 2 wt % boric acid, and 0.5 part of 2 wt % sodium dodecyl sulfate.

[0129] Example 8

[0130] Example 8 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0131] Solution B includes the following components: 1 part of 2 wt % sodium phosphate, 0.5 part of 2 wt % boric acid, and 0.5 part of 2 wt % dodecyltrimethylammonium bromide.

[0132] Comparative Example 1

[0133] Comparative Example 1 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, and includes most of the operation steps in Example 1, except that:

[0134] Does not contain hectorite and polyether modified silicone oil;

[0135] Comparative Example 2

[0136] Comparative Example 2 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0137] Does not contain polyether modified silicone oil.

[0138] Comparative Example 3

[0139] Comparative Example 3 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0140] Contains no hectorite.

[0141] Comparative Example 4

[0142] Comparative Example 4 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0143] Preparation of negative electrode:

[0144] Add 2 parts of , 4 servings , 9 copies Negative electrode additives.

[0145] Comparative Example 5

[0146] Comparative Example 5 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0147] Preparation of negative electrode:

[0148] Does not contain , and Negative electrode additives.

[0149] Comparative Example 6

[0150] Comparative Example 6 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0151] Preparation of negative electrode:

[0152] Does not contain Negative electrode additives.

[0153] Comparative Example 7

[0154] Comparative Example 7 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0155] Preparation of negative electrode:

[0156] Does not contain Negative electrode additives.

[0157] Comparative Example 8

[0158] Comparative Example 8 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0159] Preparation of negative electrode:

[0160] Does not contain Negative electrode additives.

[0161] Comparative Example 9

[0162] Comparative Example 9 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, and the difference is that:

[0163] Preparation of negative electrode:

[0164] Does not contain and Negative electrode additives.

[0165] Comparative Example 10

[0166] Comparative Example 10 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0167] Preparation of negative electrode:

[0168] Does not contain and Negative electrode additives.

[0169] Comparative Example 11

[0170] Comparative Example 11 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0171] Preparation of negative electrode:

[0172] Does not contain and Negative electrode additives.

[0173] Comparative Example 12

[0174] Comparative Example 12 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0175] Does not contain disodium hydrogen phosphate.

[0176] Comparative Example 13

[0177] Comparative Example 13 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0178] Does not contain boric acid.

[0179] Comparative Example 14

[0180] Comparative Example 14 is used to illustrate a negative electrode material, a negative electrode slurry and preparation method, a negative electrode plate and a nickel-zinc battery disclosed in the present invention, including most of the operating steps in Example 1, except that:

[0181] Does not contain glycerin.

[0182] Performance Testing:

[0183] Storage performance test:

[0184] The nickel-zinc batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 14 were charged to 1.9 V at 1C and discharged to 1.3 V at 1C. The charge and discharge were repeated until the battery capacity decreased to 60% of the initial charge. The number of charge and discharge times was recorded.

[0185] The storage performance test environment is: 45°C, 7 / 14 / 28 days; 60°C, 7 days.

[0186] Storage performance capacity test conditions: 0.2C discharge to 1.3V, 0.2C charge to 1.9V, stand for 10 minutes, and cycle the above steps three times. The test results are shown in Table 1:

[0187] Table 1 Test results of Examples 1-8 and Comparative Examples 1-14 of the present invention

[0188]

[0189] As can be seen from Table 1, by comparing Examples 1-8 with Comparative Examples 1-3, it can be seen that by adding hectorite and polyether-modified silicone oil to the negative electrode, the nickel-zinc battery exhibits a cycle life of up to 200 cycles and optimal high-temperature storage performance. This is because the magnesium and silicon elements in the hectorite form a uniform, extremely thin silicon- and magnesium-containing interface protective film on the negative electrode sheet under weakly alkaline conditions in the aqueous system, which slows down the corrosion of zinc and zinc oxide in the negative electrode by the alkaline electrolyte. The ether bond of the polyether-modified silicone oil enhances the water retention of the negative electrode slurry, and the polyether-modified silicone oil has a certain viscosity, which improves the adhesion between the negative electrode active material and the negative electrode current collector in the nickel-zinc battery, and at the same time can avoid the shedding of the negative electrode active material, slowing down the self-discharge phenomenon of the nickel-zinc battery.

[0190] As can be seen from Table 1, by comparing Example 1, Example 5, Example 6 and Comparative Examples 4-11, it can be seen that adding 0.1-1 parts of , 0.5-3 servings , 1-8 servings , Ni-Zn batteries exhibit a cycle life of up to 200 cycles and optimal high-temperature storage performance, this is because , , It can increase the hydrogen evolution overpotential of the negative electrode, inhibit the generation of hydrogen during the charge and discharge process, improve the stability of the negative electrode, and at the same time improve the migration of ions inside the negative electrode and the uniformity of metal zinc dissolution / deposition, inhibit the formation of dendrites, and apply it to zinc ion batteries to improve the stability and cycle life of zinc ion batteries.

[0191] As can be seen from Table 1, by comparing Examples 1-8 with Comparative Examples 12-14, it can be seen that by adding phosphate, boric acid and organic surfactant to the electrolyte, the nickel-zinc battery exhibits a cycle life of up to 200 cycles and optimal high-temperature storage performance. This is because adding phosphate, boric acid and organic surfactant to the electrolyte can slow down the corrosion of the electrolyte on the negative electrode active material, reduce the self-discharge phenomenon, and effectively improve the storage performance and cycle life of the nickel-zinc battery at high temperatures.

[0192] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A nickel-zinc battery, Features: It includes a negative electrode sheet, a positive electrode sheet, a separator and an electrolyte, wherein the electrolyte is formed by mixing solution A and solution B, wherein solution A includes an alkaline solution and a ZnO solution, and solution B includes one or more of phosphate, boric acid and an organic surfactant; The phosphate includes one or more of sodium phosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate; the organic surfactant includes one or more of glycerol, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, dodecyltrimethylammonium bromide, and sorbitol; The negative electrode sheet comprises a negative electrode slurry and a negative electrode current collector, wherein the negative electrode slurry is coated on at least one surface of the negative electrode current collector; The negative electrode slurry includes a negative electrode material; The negative electrode material includes a negative electrode active material and a negative electrode additive, the negative electrode active material includes zinc and zinc oxide, the negative electrode additive includes hectorite and polyether modified silicone oil, and the mass ratio of the hectorite to the polyether modified silicone oil is 1:10-10:1; In parts by weight, the negative electrode active material is 78-98 parts, and the total amount of the hectorite and the polyether-modified silicone oil is 1-10 parts; The negative electrode additive also includes One or more of; In parts by weight, the 0.1-1 part; 0.5-3 parts; For 1-8 servings.

2. The nickel-zinc battery according to claim 1, Features: The mass ratio of the hectorite to the polyether-modified silicone oil is 5:6-8:

3.

3. The nickel-zinc battery according to claim 1, Features: The negative electrode material also includes a conductive agent, a thickener, a dispersant and a binder. In terms of weight, the conductive agent is 1-2 parts; the thickener is 3-0.5 parts; the dispersant is 1-2 parts; and the binder is 3-5 parts.

4. The nickel-zinc battery according to claim 3, Features: The dispersant includes one or more of sodium polyacrylate, potassium polyacrylate and polyacrylamide.

5. The nickel-zinc battery according to claim 3, Features: The binder includes one or more of styrene-butadiene rubber and polytetrafluoroethylene.

6. The nickel-zinc battery according to claim 3, Features: The conductive agent includes one or more of activated carbon, conductive carbon black, carbon nanotubes, graphene, and vapor-grown carbon fibers.

7. The nickel-zinc battery according to claim 3, Features: The thickener includes one or more of sodium carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose.

8. The nickel-zinc battery according to claim 1, Features: The negative electrode current collector is selected from any one of an obliquely drawn copper mesh, a tinned obliquely drawn copper mesh, a galvanized obliquely drawn copper mesh, a copper foil, and a tinned copper foil.

9. The nickel-zinc battery according to claim 1, Features: The weight ratio of the solution A to the solution B is (8-9):

1.

10. The nickel-zinc battery according to any one of claims 3 to 7, Features: The method for preparing the negative electrode slurry comprises the following steps performed in sequence: Add conductive agent, thickener and dispersant into the barrel and stir; Adding negative electrode active materials including zinc and zinc oxide into the barrel in multiple portions and stirring; Add a binder, laponite and polyether-modified silicone oil into a barrel and stir to obtain a negative electrode slurry.

11. The nickel-zinc battery according to claim 10, Features: The method further includes the following steps after adding a conductive agent, a thickener, and a dispersant into the barrel and stirring, and before adding a negative electrode active material into the barrel: Add negative electrode additives except hectorite and polyether modified silicone oil into the barrel and stir.