A method for preparing manganese dioxide by solid phase electrooxidation and its application
Optimizing the preparation of manganese dioxide by solid-phase electrooxidation method solves the problems of single crystal form and poor electrochemical energy storage performance in the electrolytic manganese sulfate solution method, achieving efficient and low-cost large-scale production, which is suitable for supercapacitors. Cathode material.
Patent Information
- Application Number
- CN202410986492.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-23
AI Technical Summary
In the existing manganese dioxide production process, the electrolytic manganese sulfate solution method results in a single crystal form, poor electrochemical energy storage performance, high energy consumption, high chemical preparation costs, harsh production conditions, and is not suitable for large-scale production.
The solid-phase electrooxidation method is used to perform anode solid-phase electrooxidation on the anode plate, control the electrooxidation temperature, the pH value of the electrolyte and the sodium sulfate concentration. Use graphite or stainless steel plates, and the electrolyte is sodium sulfate solution to optimize the current density. and electrooxidation time to prepare manganese dioxide of different crystal forms.
It reduces the energy consumption of manganese dioxide, solves the problem of a single crystal form, improves electrochemical energy storage performance, is suitable for large-scale production, and realizes the recycling of electrolyte and recovery of precursors. The product is suitable for the positive electrode of supercapacitors. Material.
Smart Images

Figure CN118516686B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of manganese dioxide preparation and application, and in particular to a method for preparing manganese dioxide by solid phase electrooxidation and its application. Background Art
[0002] Manganese dioxide is abundant in the earth's crust and is inexpensive. It is an important battery energy storage material and is widely used in the production and development of electrochemical energy storage products such as supercapacitors, aqueous zinc-ion batteries, lithium / sodium-ion batteries, and zinc-manganese batteries. At present, the most widely used large-scale manganese dioxide production process in industry is the anode electrolysis of manganese sulfate solution process. At the same time, there are also chemical preparation processes such as template method, hydrothermal method, sol-gel method, and thin film electrochemical deposition method in the literature and patents.
[0003] The process of producing manganese dioxide by electrolytic manganese sulfate solution is relatively mature, but the manganese dioxide product produced by it has a single crystal form (γ type), poor electrochemical energy storage performance, and high energy consumption. In addition, the electrolysis temperature of this process is relatively high, 90-95°C, and the electrolyte is highly acidic. Due to the high temperature and cathode hydrogen evolution reaction, the electrolysis process inevitably produces acid mist, which harms production equipment and personnel. Chemical methods include template method, hydrothermal method, sol-gel method, and thin film electrochemical deposition method. Although they can produce manganese dioxide products with good electrochemical energy storage performance, they are costly, have harsh production conditions, and have low production efficiency. They are not suitable for large-scale production, and most of them are still in the laboratory research and development stage. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0005] To this end, the first aspect of the present invention provides a method for preparing manganese dioxide by solid phase electro-oxidation, comprising:
[0006] A manganese-containing precursor is placed on an anode plate and subjected to anode solid-phase electrooxidation to prepare manganese dioxide; the anode solid-phase electrooxidation comprises:
[0007] The electro-oxidation temperature is 20℃~95℃, the concentration of sodium sulfate in the electrolyte is 20g / L~400g / L, the pH value of the electrolyte is 0.1~14, and the current density is 10A / m 2 ~1000A / m 2 , the electro-oxidation time is 0.5h~15h.
[0008] Furthermore, the anode solid phase electro-oxidation comprises:
[0009] The anode plate is a graphite plate;
[0010] The cathode plate is a stainless steel plate or a graphite plate;
[0011] The electrolyte is one of a sodium sulfate solution, a mixed solution of sodium sulfate and sulfuric acid, and a mixed solution of sodium sulfate and sodium hydroxide.
[0012] Furthermore, the pH value of the electrolyte is 1-13.
[0013] Furthermore, the anode solid phase electro-oxidation comprises:
[0014] The electro-oxidation temperature is 28℃~32℃, the electrolyte is sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 180g / L~220g / L, and the current density is 90A / m 2 ~110A / m 2 , the electro-oxidation time is 3h~5h, the obtained manganese dioxide crystal form is amorphous, the specific capacitance is 150F / g~170F / g, and the energy consumption per ton of manganese dioxide is 2400kWh~2600kWh;
[0015] The electro-oxidation temperature is 78℃~82℃, the electrolyte is sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 180g / L~220g / L, and the current density is 90A / m 2 ~110A / m 2 The electro-oxidation time is 3h~5h, the obtained manganese dioxide crystal form is γ-type, the specific capacitance is 65F / g~75F / g, and the energy consumption per ton of manganese dioxide is 1400kWh~1600kWh.
[0016] Furthermore, the manganese-containing precursor is prepared by reacting manganese sulfate and sodium hydroxide at 20° C. to 95° C. for 0.1 h to 10 h, washing, separating and drying the obtained manganese hydroxide to obtain the manganese-containing precursor.
[0017] Furthermore, before the anode solid phase electro-oxidation, it also includes bagging;
[0018] The bagging is to wrap the anode plate with the manganese-containing precursor with filter cloth or polyester cloth bagging to fix the manganese-containing precursor on the anode plate.
[0019] Furthermore, before the bagging, the method further includes curing the paste and the coated board;
[0020] The preparation of the paste is as follows: grinding the manganese-containing precursor, adding water and stirring evenly until the mixture is in a paste state, and controlling the liquid-to-solid ratio of the manganese-containing precursor to water to be 1-5:1 mL / g to obtain a paste-like manganese-containing precursor;
[0021] The coating and curing is to evenly apply the paste-like manganese-containing precursor to the anode plate, and then dry it at 40° C. to 100° C. for 0.5 h to 5 h.
[0022] Furthermore, after the anode solid phase electro-oxidation, it also includes the recovery of stripping products, unreacted manganese-containing precursors and recycling of electrolyte;
[0023] Wherein, the unreacted manganese-containing precursor is recovered by filtering the manganese-containing precursor in the electrolyte;
[0024] The electrolyte is recycled in that after multiple electrolysis, the pH of the electrolyte gradually increases, which will lead to a decrease in current efficiency. Sulfuric acid is added to the electrolyte with a pH greater than 9 to adjust the pH of the electrolyte to 6-7 before recycling.
[0025] In a second aspect of the present invention, an application of a method for preparing manganese dioxide by solid phase electrooxidation is provided. The manganese dioxide prepared by the above-mentioned method for preparing manganese dioxide by solid phase electrooxidation is used for electrochemical energy storage materials, and the electrochemical energy storage materials include positive electrode materials for supercapacitors.
[0026] Furthermore, when the electro-oxidation temperature is 28°C to 32°C, the concentration of sodium sulfate in the electrolyte is 180 g / L to 220 g / L, and the current density is 90 A / m 2 ~110A / m 2 When the electro-oxidation time is 3h~5h, the amorphous manganese dioxide obtained has a specific capacitance of 150F / g at a discharge rate of 1 A / g, a capacity retention rate of 99% after 10,000 cycles, and a coulombic efficiency of 98%.
[0027] Compared with the prior art, the present invention has at least the following beneficial effects:
[0028] The method for preparing manganese dioxide by solid-phase electrooxidation provided by the present invention reduces energy consumption compared with traditional electrolytic preparation of manganese dioxide; and the method for preparing manganese dioxide by solid-phase electrooxidation solves the problem of single crystal form of electrolysis product in the process of producing manganese dioxide by traditional electrolysis of manganese sulfate solution, and can be adapted to traditional production equipment for preparing manganese dioxide by electrolysis, so it is suitable for large-scale production application; the manganese dioxide product prepared by solid-phase electrooxidation has electrochemical energy storage performance far superior to the manganese dioxide product prepared by electrolysis currently available on the market. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 XRD patterns of manganese dioxide prepared by solid phase electro-oxidation at different electro-oxidation temperatures provided in the examples of the present application.
[0030] Figure 2a This is a SEM photograph of manganese dioxide prepared by solid phase electrooxidation provided in Example 1 of the present application.
[0031] Figure 2b This is a TEM photograph of manganese dioxide prepared by solid phase electrooxidation provided in Example 1 of the present application.
[0032] Figure 3a This is a SEM photograph of manganese dioxide prepared by solid phase electrooxidation provided in Example 2 of the present application.
[0033] Figure 3b This is a TEM photograph of manganese dioxide prepared by solid phase electrooxidation provided in Example 2 of the present application.
[0034] Figure 4 This is a SEM photograph of manganese dioxide prepared by solid phase electrooxidation provided in Example 3 of the present application.
[0035] Figure 5a This is the cyclic voltammetry curve of the manganese dioxide product obtained in Example 1 of the present application.
[0036] Figure 5b This is the charge and discharge curve of the manganese dioxide product obtained in Example 1 of the present application.
[0037] Figure 5c This is the electrochemical impedance spectrum of the manganese dioxide product obtained in Example 1 of the present application.
[0038] Figure 6a This is the cyclic voltammetry curve of the manganese dioxide product obtained in Example 2 of the present application.
[0039] Figure 6b This is the charge and discharge curve of the manganese dioxide product obtained in Example 2 of the present application.
[0040] Figure 6c This is the electrochemical impedance spectrum of the manganese dioxide product obtained in Example 2 of the present application.
[0041] Figure 6d This is a cycle life test of the manganese dioxide product obtained in Example 2 of the present application. DETAILED DESCRIPTION
[0042] In order to better understand the above technical solution, the technical solution of the present invention is described in detail below through specific embodiments.
[0043] In a first aspect of an embodiment of the present invention, a method for preparing manganese dioxide by solid phase electro-oxidation is provided, comprising: placing a manganese-containing precursor on an anode plate, and performing anode solid phase electro-oxidation to prepare manganese dioxide; the anode solid phase electro-oxidation comprises: an electro-oxidation temperature of 20°C to 95°C, a sodium sulfate concentration in an electrolyte of 20g / L to 400g / L, a pH value of the electrolyte of 0.1 to 14, and a current density of 10A / m 2 ~1000A / m 2 , the electro-oxidation time is 0.5h~15h.
[0044] The method for preparing manganese dioxide by solid-phase electrooxidation provided in an embodiment of the present invention reduces energy consumption compared with traditional electrolytic preparation of manganese dioxide; and the method for preparing manganese dioxide by solid-phase electrooxidation solves the problem of single crystal form of electrolysis product in the process of producing manganese dioxide by traditional electrolysis of manganese sulfate solution, and can be adapted to traditional production equipment for preparing manganese dioxide by electrolysis, so it is suitable for large-scale production application; the manganese dioxide product prepared by solid-phase electrooxidation has an electrochemical energy storage performance far superior to the manganese dioxide product prepared by electrolysis currently available on the market.
[0045] In a feasible embodiment, the anode solid phase electro-oxidation includes: the anode plate is a graphite plate; the cathode plate is a stainless steel plate or a graphite plate; the electrolyte is one of a sodium sulfate solution, a mixed solution of sodium sulfate and sulfuric acid, and a mixed solution of sodium sulfate and sodium hydroxide; the pH value of the electrolyte is 0.1~14, and the pH value of the electrolyte is preferably 1~13.
[0046] Specifically, lead plates will generate lead dioxide during the electrolysis process, which will pollute the manganese dioxide product. Stainless steel plates will dissolve and pollute the electrolyte and manganese dioxide products under high potential. Graphite plates are stable and will not pollute manganese dioxide products. At the same time, their oxygen evolution overpotential is high, which can improve the current efficiency of manganese dioxide electro-oxidation. Therefore, graphite plates are selected as anode plates.
[0047] The electrolyte is a mixed solution of sodium sulfate and sulfuric acid, or a mixed solution of sodium sulfate and sodium hydroxide, or a sodium sulfate solution. When the electrolyte is a mixed solution of sodium sulfate and sulfuric acid, the manganese dioxide recovery rate decreases with the increase of sulfuric acid concentration; when the electrolyte is a mixed solution of sodium sulfate and sodium hydroxide, the current efficiency decreases with the increase of sodium hydroxide concentration. It is preferred to control the pH value of the electrolyte to 1-13, at which time the production process is green and environmentally friendly, and the operating environment is good without generating acid mist.
[0048] In a feasible embodiment, the anode solid phase electro-oxidation comprises:
[0049] The electro-oxidation temperature is 20℃~95℃, the concentration of sodium sulfate in the electrolyte is 20g / L~400g / L, and the current density is 10A / m 2 ~1000A / m 2 , the electro-oxidation time is 0.5h~15h.
[0050] Preferably, the electro-oxidation temperature is 25 to 85°C, the concentration of sodium sulfate in the electrolyte is 150 to 250 g / L, and the current density is 80 to 300 A / m 2 , the electro-oxidation time is 2 to 6 hours.
[0051] More preferably, the electro-oxidation temperature is 30±2°C, the electrolyte is a sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 200±20 g / L, and the current density is 100±10 A / m 2 , the electro-oxidation time is 3 to 5 h; or, the electro-oxidation temperature is 80 ± 2 °C, the electrolyte is a sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 200 ± 20 g / L, and the current density is 100 ± 10 A / m 2 , the electro-oxidation time is 3 to 5 hours.
[0052] Specifically, when the electro-oxidation temperature is 28°C to 32°C, the electrolyte is a sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 180g / L to 220g / L, and the current density is 90A / m 2 ~110A / m 2 When the electro-oxidation time is 3h~5h, the obtained manganese dioxide crystal form is amorphous, the specific capacitance is 150F / g~170F / g, and the energy consumption per ton of manganese dioxide is 2400kWh~2600kWh; when the electro-oxidation temperature is 78℃~82℃, the electrolyte is sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 180g / L~220g / L, and the current density is 90A / m 2 ~110A / m 2 When the electro-oxidation time is 3h~5h, the obtained manganese dioxide crystal form is γ-type, the specific capacitance is 65F / g~75F / g, and the energy consumption per ton of manganese dioxide is 1400kWh~1600kWh.
[0053] It is understandable that the temperature of electro-oxidation needs to comprehensively consider the electrolyte solubility and electrolyte evaporation. The electrolyte solubility of sodium sulfate decreases with decreasing temperature, and the electrolyte evaporation becomes more serious with increasing temperature. If the electro-oxidation temperature is lower than 20°C, it will increase energy consumption, and the sodium sulfate electrolyte solubility will also decrease; if the electro-oxidation temperature is higher than 95°C, it will cause serious electrolyte evaporation, and it will also cause equipment maintenance and heating costs to increase. Therefore, considering the electrolyte solubility and electrolyte evaporation, the electro-oxidation temperature is controlled to be 20°C to 95°C, preferably the electro-oxidation temperature is 25°C to 90°C, and further preferably the electro-oxidation temperature is 25°C to 85°C, and further preferably the electro-oxidation temperature is 30°C ± 2°C or 80°C ± 2°C.
[0054] It is understandable that the concentration of sodium sulfate in the electrolyte needs to comprehensively consider the conductivity and solubility of the sodium sulfate electrolyte. The inventor experimentally confirmed that when the electrolyte sodium sulfate solubility is lower than 200g / L, as the concentration of sodium sulfate electrolyte decreases, the conductivity of the sodium sulfate solution decreases, resulting in a gradual increase in the energy consumption of preparing manganese dioxide. When the sodium sulfate concentration is higher than 200g / L, as the concentration of sodium sulfate electrolyte increases, the energy consumption of preparing manganese dioxide is not greatly affected, but it will cause sodium sulfate precipitation to intensify. Therefore, considering the conductivity and solubility of the sodium sulfate electrolyte, the concentration of electrolyte sodium sulfate is 20g / L~400 g / L, preferably the concentration of electrolyte sodium sulfate is 100g / L~300 g / L, and further preferably the concentration of electrolyte sodium sulfate is 150g / L~250 g / L, and further preferably the concentration of electrolyte sodium sulfate is 180g / L~220 g / L.
[0055] It is understandable that the greater the current density, the more serious the oxygen evolution side reaction, and the smaller the current density, the lower the electrolysis efficiency. 2 When the current density is less than 50 A / m 2 When the current density is 10A / m 2 ~1000A / m 2 The preferred current density is 50A / m 2 ~400A / m 2 The current density is preferably 80A / m 2 ~300A / m 2 , and further preferably the current density is 90A / m 2 ~110A / m 2 .
[0056] It is understandable that the longer the electro-oxidation time is, the higher the energy consumption is. If the electro-oxidation time is too short, the manganese-containing precursor cannot react completely, and the capacitance performance of the manganese dioxide product is reduced. Therefore, the electro-oxidation time is 0.5h to 15h, preferably 1h to 10h, more preferably 2h to 6h, and more preferably 3h to 5h.
[0057] It can be understood that the larger the heteropolar pitch is, the higher the energy consumption is. If the heteropolar pitch is too low, the generated oxygen or hydrogen bubbles will diffuse to the electrode plate and reduce the current efficiency. The heteropolar pitch is 5mm to 60mm, and the preferred heteropolar pitch is 30mm to 40mm.
[0058] The method for preparing manganese dioxide by solid phase electro-oxidation provided in an embodiment of the present invention can obtain manganese dioxide products of different crystal forms by optimizing and regulating the electro-oxidation temperature. In particular, when the electro-oxidation temperature is 80°C, the obtained manganese dioxide crystal form is γ-type, the specific capacitance is above 65F / g, and the energy consumption is 1400~1600 kWh / t MnO2; when the electro-oxidation temperature is 30°C, the obtained manganese dioxide crystal form is amorphous, the specific capacitance is above 150F / g, and the energy consumption is 2400~2600kWh / t MnO2.
[0059] The electrochemical performance of the manganese dioxide products of different crystal forms obtained in the embodiment of the present invention is good, which is far superior to the manganese dioxide product (item number 10013361) sold on the market by Sinopharm Group. After testing, the manganese dioxide (item number 10013361) sold on the market by Sinopharm Group has a specific capacitance of 32.1 F / g, and the production energy consumption is about 2500 kWh / t MnO2.
[0060] In a feasible embodiment, the manganese-containing precursor is prepared by reacting manganese sulfate and sodium hydroxide at 20-95° C. for 0.1-10 h, washing, separating and drying the obtained manganese hydroxide to obtain the manganese-containing precursor.
[0061] Specifically, the preparation method of the manganese-containing precursor is as follows: dissolving a manganese sulfate solution in deionized water at 20°C to 95°C, then adding sodium hydroxide for reaction, the reaction time is 0.1 to 10 hours, obtaining a milky white manganese hydroxide solid, then washing and centrifuging the manganese hydroxide solid, and drying in an oven at 10 to 100°C for 10 to 64 hours to obtain a dark brown solid manganese-containing precursor powder. The manganese-containing precursor prepared by this method has a nanosphere structure, a small particle size, uniform dispersion, good reactivity, and relatively low cost.
[0062] In a feasible embodiment, before the anode solid phase electro-oxidation, a bag is also included;
[0063] The bagging is to wrap the anode plate with the manganese-containing precursor with filter cloth or polyester cloth bagging to fix the manganese-containing precursor on the anode plate.
[0064] Specifically, an industrial filter cloth or daily polyester cloth with an area 4 to 10 times the size of the anode plate is used to tightly wrap the anode plate with the manganese-containing precursor, and then a polyethylene string with a diameter of 0.1 to 10 mm is used to tie up the wrapped anode plate so that the manganese-containing precursor material on the anode is fixed. If the bag electrode is not used, the reactant manganese-containing precursor will fall off seriously, and the manganese dioxide yield will drop sharply.
[0065] In a feasible embodiment, before the bagging, the process also includes mixing the paste and curing the coated board;
[0066] The preparation of the paste is as follows: grinding the manganese-containing precursor, adding water and stirring evenly until the mixture is in a paste state, and controlling the liquid-to-solid ratio of the manganese-containing precursor to water to be 1-5:1 mL / g to obtain a paste-like manganese-containing precursor;
[0067] The coating and curing is to evenly apply the paste-like manganese-containing precursor to the anode plate, and then dry it at 40 to 100° C. for 0.5 to 5 hours.
[0068] Specifically, the manganese-containing precursor is ground and passed through a 50-800 mesh sieve, and then deionized water is added to the sieved manganese-containing precursor powder with a liquid-to-solid ratio of 1-5:1 ml / g, and the mixture is mixed and stirred evenly until it becomes a paste; the paste manganese-containing precursor is evenly applied to the anode plate, and then dried at 40-100° C. for 0.5-5 h to fix the manganese-containing precursor on the anode plate.
[0069] In a feasible embodiment, after the anode solid phase electro-oxidation, the process also includes stripping products, recovery of unreacted manganese-containing precursors and recycling of electrolyte; wherein,
[0070] The method for stripping the product is as follows: after the solid-phase electro-oxidation reaction of the anode is completed, the bag is opened, the product on the anode plate is stripped, and manganese dioxide is obtained after washing and drying.
[0071] The unreacted manganese-containing precursor is recovered by filtering the manganese-containing precursor in the electrolyte;
[0072] The recycling of the electrolyte is that the pH of the electrolyte gradually increases after multiple electrolysis, which will lead to a decrease in current efficiency. Sulfuric acid is added to the electrolyte with a pH greater than 9 to adjust the pH value of the electrolyte to 6~7 before recycling.
[0073] Specifically, after the reaction is completed, the anode plate is taken out and the cloth bag is opened. It can be seen that the brown-yellow manganese-containing precursor is completely electro-oxidized into black manganese dioxide. The generated manganese dioxide is peeled off with a glass slide, washed with pure water, and then dried at 50-120°C for 0.5-5 h to obtain a manganese dioxide product. Since part of the divalent manganese ions dissolve into the electrolyte during the electro-oxidation of the anode precursor, and sodium hydroxide is generated in the electrolyte during the electro-oxidation process, making the electrolyte alkaline, the generated sodium hydroxide reacts with the dissolved divalent manganese ions and dissolved oxygen to turn back into the manganese-containing precursor raw material. Therefore, after the electro-oxidation is completed, there will be a certain amount of dropped and newly generated manganese-containing precursors in the electrolytic cell. The manganese-containing precursor is recovered by filtration, and the electrolyte after filtration can continue to be used for electrolysis. Since sodium hydroxide is generated during the reaction process, the pH of the electrolyte continues to rise. After each electro-oxidation, sulfuric acid is added to the electrolyte to neutralize the generated sodium hydroxide without contaminating the electrolyte. The pH of the electrolyte is adjusted to 6-7, and then the electrolysis is continued.
[0074] In a second aspect of an embodiment of the present invention, an application of a method for preparing manganese dioxide by solid-phase electro-oxidation is provided, wherein the manganese dioxide prepared by the method for preparing manganese dioxide by solid-phase electro-oxidation is used for electrochemical energy storage materials, and the electrochemical energy storage materials include positive electrode materials for supercapacitors.
[0075] In a feasible embodiment, when the electro-oxidation temperature is 28°C to 32°C, the concentration of sodium sulfate in the electrolyte is 180 g / L to 220 g / L, and the current density is 90 A / m 2 ~110A / m 2 When the electro-oxidation time is 3-5h, the prepared amorphous manganese dioxide has a specific capacitance of 150F / g at a discharge rate of 1 A / g, a capacity retention rate of 99% after 10,000 cycles, and a coulombic efficiency of 98%.
[0076] Example 1 A method for preparing manganese dioxide by solid phase electrooxidation
[0077] A method for preparing manganese dioxide by solid phase electrooxidation comprises the following steps:
[0078] (1) Preparation of solid manganese-containing precursor material: dissolve manganese sulfate solution in deionized water at 30°C, then add sodium hydroxide to react for 1 hour to obtain a milky white manganese hydroxide solid. Then, wash the manganese hydroxide solid and centrifuge it, and dry it in an oven at 60°C for 48 hours to obtain a dark brown solid manganese-containing precursor powder.
[0079] (2) Preparation of paste: Grind the above manganese-containing precursor powder through a 200-mesh sieve, take 1.5 g of the sieved manganese-containing precursor powder, add 1.8 mL of pure water, mix and stir evenly until it becomes a paste, and obtain a paste precursor.
[0080] (3) Plate coating: Apply the paste-like manganese-containing precursor evenly onto a 4 cm × 4 cm anode plate, which is a graphite plate.
[0081] (4) Curing: Place the anode plate coated with the manganese-containing precursor into an oven and dry it at 80°C for 1 hour to fix the manganese-containing precursor on the anode plate.
[0082] (5) Bagging: Use industrial filter cloth or daily polyester cloth with an area of 10 cm × 10 cm to tightly wrap the anode plate with the precursor, and then tie it up and fix it with 1 mm polyethylene rope to fix the manganese-containing precursor material on the anode.
[0083] (6) Anodic electro-oxidation: An anode plate coated with a manganese-containing precursor and covered with a bag was used as the anode, and stainless steel was used as the cathode. A power supply was connected for constant current electro-oxidation. The distance between the electrodes during the electro-oxidation process was 35 mm and the current density was 100 A / m 2, the electro-oxidation temperature was 80 °C, the Na2SO4 electrolyte concentration was 200 g / L, and the electro-oxidation time was 5 h.
[0084] (7) Stripping the product: After the reaction is completed, take out the anode plate, untie the string and open the cloth bag. You can see that the brown-yellow manganese-containing precursor is completely transformed into black manganese dioxide. Use a glass slide to peel off the anode manganese dioxide product, wash it with 60℃ hot water for 10 minutes, and then put it in an oven at 80℃ to dry for 1 hour.
[0085] The dried product was weighed, and 0.851 g of manganese dioxide product was obtained during the electrooxidation process.
[0086] The main technical indicators of the manganese dioxide prepared in Example 1 are: the energy consumption per ton of manganese dioxide is 1807.57 kWh, the manganese dioxide yield is 97.60%, and the electrochemical energy storage performance index specific capacitance is 68.9 F / g. However, the commercially available electrolytic manganese dioxide product of Sinopharm Group has a specific capacitance of only 32.1 F / g after testing.
[0087] The manganese dioxide prepared in Example 1 is of γ-type crystal form and has a flaky nanostructure and has good electrochemical energy storage performance. Its XRD spectrum is as follows: Figure 1 As shown, SEM and TEM images are Figure 2a and Figure 2b shown.
[0088] Example 2 A method for preparing manganese dioxide by solid phase electrooxidation
[0089] A method for preparing manganese dioxide by solid phase electrooxidation comprises the following steps:
[0090] (1) Preparation of solid manganese-containing precursor material: dissolve manganese sulfate solution in deionized water at 30°C, then add sodium hydroxide to react for 1 hour to obtain a milky white manganese hydroxide solid. Then, wash the manganese hydroxide solid and centrifuge it, and dry it in an oven at 60°C for 48 hours to obtain a dark brown solid manganese-containing precursor powder.
[0091] (2) Preparation of paste: Grind the above manganese-containing precursor powder through a 200-mesh sieve, take 1.5 g of the sieved manganese-containing precursor powder, add 1.8 mL of pure water, mix and stir evenly until it becomes a paste, and obtain a paste precursor.
[0092] (3) Plate coating: Apply the paste-like manganese-containing precursor evenly onto a 4 cm × 4 cm anode plate, which is a graphite plate.
[0093] (4) Curing: Place the anode plate coated with the manganese-containing precursor into an oven and dry it at 60°C for 1 hour to fix the manganese-containing precursor on the anode plate.
[0094] (5) Bagging: Use industrial filter cloth or daily polyester cloth with an area of 10 cm × 10 cm to tightly wrap the anode plate with the precursor, and then tie it up and fix it with 1 mm polyethylene rope to fix the manganese-containing precursor material on the anode.
[0095] (6) Anodic electro-oxidation: An anode plate coated with a manganese-containing precursor and covered with a bag was used as the anode, and stainless steel was used as the cathode. A power supply was connected for constant current electro-oxidation. The distance between the electrodes during the electro-oxidation process was 35 mm and the current density was 100 A / m 2 , the electro-oxidation temperature was 30 °C, the Na2SO4 electrolyte concentration was 200 g / L, and the electro-oxidation time was 3 h.
[0096] (7) Stripping the product: After the reaction is completed, take out the anode plate, untie the string and open the cloth bag. You can see that the brown-yellow manganese-containing precursor is completely transformed into black manganese dioxide. Use a glass slide to peel off the anode manganese dioxide product, wash it with 60℃ hot water for 10 minutes, and then put it in an oven at 80℃ to dry for 1 hour.
[0097] The dried product was weighed, and 0.809 g of manganese dioxide product was obtained during the electrooxidation process.
[0098] The main technical indicators of the manganese dioxide prepared in Example 2 are: the energy consumption per ton of manganese dioxide is 2448.64 kWh, the manganese dioxide yield is 85.72%, and the electrochemical energy storage performance index specific capacitance is 162.1 F / g. However, the commercially available electrolytic manganese dioxide product of Sinopharm Group has a specific capacitance of only 32.1 F / g after testing.
[0099] The manganese dioxide prepared in Example 2 is amorphous and presents a nano-spherical particle morphology between 10nm and 100nm, which is consistent with the typical amorphous manganese dioxide morphology recorded in the literature and has good electrochemical energy storage performance. Its XRD spectrum is as follows: Figure 1 As shown, SEM and TEM images are Figure 3a and Figure 3b shown.
[0100] Example 3 A method for preparing manganese dioxide by solid phase electrooxidation
[0101] A method for preparing manganese dioxide by solid phase electrooxidation comprises the following steps:
[0102] (1) Preparation of solid manganese-containing precursor material: dissolve manganese sulfate solution in deionized water at 30°C, then add sodium hydroxide to react for 1 hour to obtain a milky white manganese hydroxide solid. Then, wash the manganese hydroxide solid and centrifuge it, and dry it in an oven at 60°C for 48 hours to obtain a dark brown solid manganese-containing precursor powder.
[0103] (2) Preparation of paste: Grind the above manganese-containing precursor powder through a 200-mesh sieve, take 1.5 g of the sieved manganese-containing precursor powder, add 1.8 mL of pure water, mix and stir evenly until it becomes a paste, and obtain a paste precursor.
[0104] (3) Plate coating: Apply the paste-like manganese-containing precursor evenly onto a 4 cm × 4 cm anode plate, which is a graphite plate.
[0105] (4) Curing: Place the anode plate coated with the manganese-containing precursor into an oven and dry it at 60°C for 1 hour to fix the manganese-containing precursor on the anode plate.
[0106] (5) Bagging: Use industrial filter cloth or daily polyester cloth with an area of 10 cm × 10 cm to tightly wrap the anode plate with the precursor, and then tie it up and fix it with 1 mm polyethylene rope to fix the manganese-containing precursor material on the anode.
[0107] (6) Anodic electro-oxidation: An anode plate coated with a manganese-containing precursor and covered with a bag was used as the anode, and stainless steel was used as the cathode. A power supply was connected for constant current electro-oxidation. The distance between the electrodes during the electro-oxidation process was 35 mm and the current density was 200 A / m 2 , the electro-oxidation temperature was 50 °C, the Na2SO4 electrolyte concentration was 200 g / L, and the electro-oxidation time was 167 min.
[0108] (7) Stripping the product: After the reaction is completed, take out the anode plate, untie the string and open the cloth bag. You can see that the brown-yellow manganese-containing precursor is completely transformed into black manganese dioxide. Use a glass slide to peel off the anode manganese dioxide product, wash it with 60℃ hot water for 10 minutes, and then put it in an oven at 80℃ to dry for 1 hour.
[0109] The dried product was weighed, and 0.707 g of manganese dioxide product was obtained during the electrooxidation process.
[0110] The main technical indicators of the manganese dioxide prepared in Example 3 are: energy consumption per ton of manganese dioxide is 4418.50 kWh, manganese dioxide yield is 80.55%, and electrochemical energy storage performance index specific capacitance is 86.4 F / g. However, the commercially available electrolytic manganese dioxide product of Sinopharm Group has a specific capacitance of only 32.1 F / g after testing.
[0111] The XRD pattern of manganese dioxide prepared in Example 3 is as follows: Figure 1 As shown, it can be seen that due to the current density of 200 A / m 2 , the temperature is 50℃, the anode polarization is aggravated, the current efficiency is reduced, so the manganese precursor is not completely reacted into manganese dioxide, so the XRD spectrum is a mixed spectrum of γ-MnO2 and manganese precursor. Figure 4As shown, it can be seen that at this time, since the current density is larger than that in Example 2 and the electro-oxidation temperature is higher than that in Example 2, the product morphology is nano-spherical, but relatively dense, resulting in its specific surface area being smaller than that of the manganese dioxide obtained in Example 2, and the capacitance performance is also worse than that in Example 2.
[0112] Example 4
[0113] The difference between Example 4 and Example 1 is that the electro-oxidation temperature is 20°C.
[0114] The main technical indicators of the manganese dioxide prepared in Example 4 are: energy consumption per ton of manganese dioxide production is 4484.50 kWh, manganese dioxide yield is 60.55%, and the electrochemical energy storage performance indicator specific capacitance is 39.4 F / g.
[0115] Example 5
[0116] The difference between Example 5 and Example 1 is that the current density is 600A / m 2 .
[0117] The main technical indicators of the manganese dioxide prepared in Example 5 are: energy consumption per ton of manganese dioxide production is 4561.19 kWh, manganese dioxide yield is 80.12%, and the electrochemical energy storage performance indicator specific capacitance is 81 F / g.
[0118] Results and Discussion of Examples 1 to 5
[0119] The XRD diffraction patterns of the manganese dioxide obtained in Examples 1 to 5 are as follows: Figure 1 As shown, it can be seen that with the decrease of temperature, the higher the proportion of amorphous manganese dioxide in the manganese dioxide generated by electro-oxidation, the lower the proportion of γ-manganese dioxide. When the electrolysis temperature is 30°C, the diffraction characteristic peak of γ-manganese dioxide almost disappears, and the product is basically all amorphous manganese dioxide.
[0120] The SEM and TEM images of the manganese dioxide prepared in Example 1 are as follows: Figure 2a and Figure 2b As shown, the SEM and TEM images of the manganese dioxide prepared in Example 2 are as follows Figure 3a and Figure 3b As shown in the figure, it can be seen that the amorphous manganese dioxide generated at low temperature has a larger specific surface area and its internal structure is relatively loose and porous, so it has better electrochemical energy storage performance as a supercapacitor, which is consistent with the results reported in the literature. However, from the perspective of energy consumption, high temperature is conducive to reducing energy consumption in both thermodynamics and kinetics. Therefore, this method can be considered from the perspectives of energy consumption and electrochemistry, and has good process flexibility.
[0121] The electro-oxidation temperature of Example 4 is 20°C. The lower the electro-oxidation temperature, the greater the resistance of the electro-oxidation reaction and the more severe the anode polarization, which will cause the anode current efficiency to decrease, anode oxygen evolution to intensify, and a large amount of reactants to fall from the anode plate, resulting in a decrease in the manganese dioxide yield and a sharp increase in energy consumption.
[0122] The current density of Example 5 is 600A / m 2 , the current density increases, the cathode polarization and the anode polarization are intensified, which increases the cathode and anode potentials and causes a sharp increase in energy consumption.
[0123] The manganese dioxide prepared in Example 1 and Example 2 is used as a positive electrode material for supercapacitors
[0124] The manganese dioxide products prepared in Example 1 and Example 2 were made into half-cells (manganese dioxide, conductive carbon black and PVDF were used as working electrodes in a mass ratio of 8:1:1) and subjected to cyclic voltammetry, charge and discharge test, electrochemical impedance spectroscopy and cycle life test and other supercapacitor electrochemical energy storage performance tests. The test results are as follows: Figure 5a , Figure 5b , Figure 5c , Figure 6a , Figure 6b , Figure 6c and Figure 6d As shown. From the cyclic voltammetry test results, it can be seen that the CV curves of the electrodes of the two manganese dioxide products show relatively symmetrical capacitance characteristics, and the manganese dioxide product of Example 2 (electrooxidation temperature 30°C) shows a shuttle shape with better symmetry, indicating that its capacitance characteristics are better. In addition, the charge and discharge test results show that the manganese dioxide product has a symmetrical triangular charge and discharge curve, and both can store and release electrical energy. By comparing the discharge time calculation, it can be obtained that at a discharge rate of 1 A / g, the specific capacitance of the manganese dioxide product of Example 2 (electrooxidation temperature 30°C) is 162.1 F / g, and the specific capacitance of the manganese dioxide product of Example 1 (electrooxidation temperature 80°C) is 68.9 F / g. This shows that the supercapacitor energy storage performance of the electro-oxidized manganese dioxide product at low temperature is better. At the same time, by comparing the electrochemical impedance spectra of the two products, it can be found that the overall electrochemical impedance corresponding to the product of Example 2 (electrooxidation temperature 30°C) is lower, which shows that the ion diffusion resistance and electron transmission resistance of the manganese dioxide product of Example 2 (electrooxidation temperature 30°C) are smaller, and its electrochemical energy storage performance is better. The battery charge and discharge performance and coulombic efficiency of the manganese dioxide product of Example 2 (electro-oxidation temperature 30°C) were tested. It can be seen that after 10,000 cycles, the battery capacitance has almost no attenuation, the capacity retention rate is 99.1%, and the coulombic efficiency is 98.2%, which proves its excellent electrochemical energy storage performance and battery cycle performance as a supercapacitor.
[0125] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.
Claims
1. A method for preparing manganese dioxide by solid phase electrooxidation, characterized in that: include: Grinding a manganese-containing precursor, adding water and stirring evenly until it becomes a paste, applying the paste-like manganese-containing precursor evenly on an anode plate, and performing anode solid-phase electrooxidation to prepare manganese dioxide; The anode solid phase electro-oxidation comprises: The electro-oxidation temperature is 20℃~95℃, the concentration of sodium sulfate in the electrolyte is 20g / L~400g / L, the pH value of the electrolyte is 0.1~14, and the current density is 10A / m 2 ~1000A / m 2 , the electro-oxidation time is 0.5h~15h; The electro-oxidation temperature is 28°C~32°C, the electrolyte is sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 180g / L~220g / L, and the current density is 90A / m 2 ~110A / m 2 , the electro-oxidation time is 3h~5h, the obtained manganese dioxide crystal form is amorphous, the specific capacitance is 150F / g~170F / g, and the energy consumption per ton of manganese dioxide is 2400kWh~2600kWh; The electro-oxidation temperature is 78℃~82℃, the electrolyte is sodium sulfate solution, the concentration of sodium sulfate in the electrolyte is 180g / L~220g / L, and the current density is 90A / m 2 ~110A / m 2 , the electro-oxidation time is 3h~5h, the obtained manganese dioxide crystal form is γ-type, the specific capacitance is 65F / g~75F / g, and the energy consumption per ton of manganese dioxide is 1400kWh~1600kWh; The manganese-containing precursor is prepared by reacting manganese sulfate and sodium hydroxide at 20° C. to 95° C. for 0.1 to 10 hours, washing, separating and drying the obtained manganese hydroxide to obtain the manganese-containing precursor.
2. The method for preparing manganese dioxide by solid phase electrooxidation according to claim 1, characterized in that: The anode solid phase electro-oxidation comprises: The anode plate is a graphite plate; The cathode plate is a stainless steel plate or a graphite plate; The electrolyte is one of a sodium sulfate solution, a mixed solution of sodium sulfate and sulfuric acid, and a mixed solution of sodium sulfate and sodium hydroxide.
3. The method for preparing manganese dioxide by solid phase electrooxidation according to claim 2, characterized in that: The pH value of the electrolyte is 1~13.
4. The method for preparing manganese dioxide by solid phase electrooxidation according to any one of claims 1 to 3, characterized in that: Before the anode solid phase electro-oxidation, it also includes bagging; The bagging is to wrap the anode plate with the manganese-containing precursor with filter cloth or polyester cloth bagging to fix the manganese-containing precursor on the anode plate.
5. The method for preparing manganese dioxide by solid phase electrooxidation according to claim 4, characterized in that: Before the bagging, it also includes mixing paste and coating the board for curing; The preparation of the paste is as follows: grinding the manganese-containing precursor, adding water and stirring evenly until the mixture is in a paste state, and controlling the liquid-to-solid ratio of the manganese-containing precursor to water to be 1-5:1 mL / g to obtain a paste-like manganese-containing precursor; The coating and curing is to evenly apply the paste-like manganese-containing precursor to the anode plate, and then dry it at 40° C. to 100° C. for 0.5 h to 5 h.
6. The method for preparing manganese dioxide by solid phase electrooxidation according to claim 5, characterized in that: After the anode solid phase electro-oxidation, the process also includes the recovery of stripping products, unreacted manganese-containing precursors and recycling of electrolyte; Wherein, the unreacted manganese-containing precursor is recovered by recovering the manganese-containing precursor in the electrolyte by a suction filtration method; The electrolyte is recycled in that after multiple electrolysis, the pH of the electrolyte gradually increases, which will lead to a decrease in current efficiency. Sulfuric acid is added to the electrolyte with a pH greater than 9 to adjust the pH of the electrolyte to 6-7 before recycling.
7. Application of a method for preparing manganese dioxide by solid phase electrooxidation, characterized in that: The manganese dioxide prepared by the method for preparing manganese dioxide by solid phase electrooxidation according to any one of claims 1 to 6 is used for electrochemical energy storage materials, and the electrochemical energy storage materials include positive electrode materials for supercapacitors.
8. The use of the method for preparing manganese dioxide by solid phase electrooxidation according to claim 7, characterized in that: When the electro-oxidation temperature is 28℃~32℃, the concentration of sodium sulfate in the electrolyte is 180g / L~220g / L, and the current density is 90A / m 2 ~110A / m 2 When the electro-oxidation time is 3h~5h, the amorphous manganese dioxide obtained has a specific capacitance of 150F / g at a discharge rate of 1 A / g, a capacity retention rate of 99% after 10,000 cycles, and a coulombic efficiency of 98%.