Solid amine honeycomb adsorbent and preparation method and application thereof

By combining modified silica sol with solid amine, a solid amine honeycomb adsorbent with high loading strength and mechanical strength is formed, which solves the problems of long diffusion path and slow adsorption kinetics of solid amine honeycomb adsorbent during CO2 adsorption. , achieving low pressure resistance and low energy consumption adsorption effect, suitable for industrial applications.

CN118527122BActive Publication Date: 2024-10-18UNIV OF SCI & TECH BEIJING
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410993636.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-18
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing solid amine honeycomb adsorbents have problems such as long diffusion paths, slow adsorption kinetics, high pressure resistance and high energy consumption during the CO2 adsorption process, resulting in limited adsorption rates.

Method used

Modified silica sol is combined with solid amine, and the aminosilane coupling agent reacts with silica sol and organic gum to form a rigid interconnected porous three-dimensional network structure, which improves the binding ability of solid amine and substrate, and prepares high load strength and mechanical properties. Strong solid amine honeycomb adsorbent.

Benefits of technology

While maintaining the adsorption performance, it significantly reduces the air flow pressure drop and energy consumption, increases the adsorption rate, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118527122B_ABST
    Figure CN118527122B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of adsorbent preparation, and specifically to a solid amine honeycomb adsorbent and its preparation method and application. The preparation method is to modify silica sol and combine it with solid amine, substrate, etc. to prepare the solid amine honeycomb adsorbent, and the modified silica sol entrains the solid amine and the substrate for better combination. The solid amine honeycomb adsorbent prepared by the preparation method has excellent mechanical strength and load strength without reducing the adsorption performance and maintaining a high load capacity, and is not easy to fly or the solid amine to fall off during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid amine honeycomb adsorbent preparation, and in particular to a solid amine honeycomb adsorbent and a preparation method and application thereof. Background Art

[0002] CO 2 As a major greenhouse gas, its emission problem is becoming increasingly serious. Carbon capture technology is currently used to control CO 2 emissions.

[0003] Carbon capture technologies mainly include amine solvent carbon capture and solid amine honeycomb adsorbent adsorption. Among them, amine solvent carbon capture still has problems such as high external heat required for solvent regeneration and equipment corrosion; while solid amine honeycomb adsorbent has the advantages of low regeneration energy consumption, environmental friendliness, and low equipment corrosion, but most solid amine honeycomb adsorbents are currently used in the form of powder or granules for various CO 2 In the adsorption capture scenario, adsorbents in powder or granular form can basically only be adsorbed and captured in a fixed bed or fluidized bed process. This will result in a longer diffusion path for such adsorbents and slow adsorption kinetics. A thicker adsorption bed is required to achieve a sufficient target gas removal rate, which increases the amount of adsorbent used. It also brings about the problem of high pressure resistance. High pressure resistance means increased energy consumption, and slow heat and mass transfer means a longer adsorption / desorption cycle time, which seriously affects the adsorption rate. Summary of the invention

[0004] In order to solve the above problems, the present application proposes a solid amine honeycomb adsorbent and a preparation method and application thereof. The preparation method is to modify the silica sol and combine it with solid amine, substrate, etc. to prepare the solid amine honeycomb adsorbent, and the modified silica sol can better combine with the substrate by entrapping the solid amine. The solid amine honeycomb adsorbent prepared by the preparation method has excellent mechanical strength and load strength without reducing the adsorption performance and maintaining a high load capacity, and is not easy to fly or the solid amine to fall off during use.

[0005] This application is implemented through the following technical solutions:

[0006] One of the purposes of the present application is to provide a method for preparing a solid amine honeycomb adsorbent, comprising the following steps:

[0007] The modified silica sol is prepared by using raw materials including aminosilane coupling agent, organic glue and silica sol;

[0008] The coating slurry is prepared by using raw materials including the modified silica sol, solid amine slurry and additives;

[0009] The coating slurry is used to load a substrate to obtain a solid amine honeycomb adsorbent.

[0010] The present application provides a method for preparing a solid amine honeycomb adsorbent, wherein the alkoxy group in the aminosilane coupling agent reacts with the surface hydroxyl group of the silica sol, and the amino group of the aminosilane coupling agent reacts with the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue, thereby obtaining a modified silica sol having an organic cross-linking function, and the aminosilane in the modified silica sol serves as a "molecular bridge" between the silica particles in the silica sol and the organic glue, so that a rigidly interconnected, porous, three-dimensional network structure is formed between the silica sol particles. In the coating slurry prepared from the modified silica sol and solid amine with a network structure, the modified silica sol reduces the internal stress and shrinkage rate during the cross-linking and curing process of the slurry, and prevents the adsorbent from cracking after drying; when preparing the modified silica sol, the aminosilane coupling agent is first hydrolyzed by the water in the silica sol, and the alkoxy group (e.g., ethoxy, -OCH 2 CH 3 ) will hydrolyze to generate silanol groups (-SiOH) in the presence of water. The generated silanol groups can further react with the hydroxyl groups (-OH) on the surface of the silica particles in the silica sol to form siloxane (Si-O-Si) bonds. After adding the organic glue, the amino group of the aminosilane coupling agent reacts with the carboxyl, aldehyde, ester or epoxy groups of the organic glue to form stable covalent bonds, and finally the modified silica sol is obtained. Then it is prepared into a coating slurry, in which the modified silica sol entrains the solid amine, so that the solid amine can be better combined with the substrate during loading. The prepared solid amine honeycomb adsorbent has high load strength and mechanical strength while maintaining the adsorption performance and high load capacity of the solid amine itself, so that the solid amine is not easy to fall off from the substrate (no powdering phenomenon occurs). The preparation method of the present application has simple steps, easy to obtain raw materials, no pollution, low cost, high stability, and easy to industrial scale production.

[0011] In some possible implementations, the step of preparing the modified silica sol includes:

[0012] Performing a first mixing reaction on the aminosilane coupling agent solution and the silica sol to obtain a hydroxyl-modified silica sol;

[0013] The hydroxyl-modified silica sol and the organic gel solution are subjected to a second mixing reaction to obtain the modified silica sol.

[0014] In the above-mentioned step of preparing the modified silica sol, the aminosilane coupling agent solution and the silica sol are first subjected to a first mixing reaction, so that the silanol formed by the hydrolysis of the alkoxy group of the aminosilane reacts with the surface hydroxyl group of the silica sol to obtain a hydroxyl-modified silica sol; in the modified silica sol, the amino group of the aminosilane coupling agent reacts with the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue to obtain a modified silica sol.

[0015] In some possible implementations, a pH adjuster is used to adjust the pH value of the coating slurry so that the pH value of the coating slurry is 8 to 14. In this case, the pH adjuster can increase the adsorption capacity of the amino group, and can ensure that the solid amine slurry is in a strong alkaline environment, thereby ensuring the stability of the slurry, and further allowing the coating slurry after the immersion treatment to be uniformly loaded on the substrate.

[0016] In some possible implementations, the loading treatment step includes repeatedly dipping the substrate in the coating slurry and then drying it. In some possible implementations, the number of times of dipping and drying is 2 to 10 times. In this case, the first dipping time can be relatively long (1 min to 15 min), and the subsequent dipping time is less than or equal to the first dipping time, and is controlled at 1 min to 10 min. This is because although the impregnated substrate has been dried, it is still in a wet state as a whole. If the subsequent dipping time is too long, it is easy to damage the substrate or the strength of the substrate is too low, and it is more likely to cause the solid amine applied previously to dissolve again in the coating slurry; the number of times of dipping and drying is 2 to 10 times, so that the solid amine raw powder on the substrate has a good loading amount, so that the solid amine inside the substrate can also participate in the adsorption of CO 2 , making it have a higher CO 2 Adsorption capacity.

[0017] Furthermore, the weight proportion of the aminosilane coupling agent solution is 6 to 15 parts. Furthermore, the weight proportion of the silica sol is 10 to 20 parts. Within this weight proportion range, the alkoxy groups in the aminosilane coupling agent can be fully hydrolyzed with the help of water in the silica sol, and the silanols generated by the hydrolysis can be completely reacted with the hydroxyl groups on the surface of the silica sol, thereby avoiding excessive aminosilane coupling agent causing slurry sedimentation, and also avoiding too little aminosilane coupling agent causing incomplete modification of the silica sol, which affects its final adhesion performance.

[0018] Furthermore, the silica sol is a neutral silica sol. This neutral silica sol can avoid the occurrence of side reactions. This is because: the active group of the aminosilane coupling agent selected is amino, so it is necessary to avoid adding any acidic substances to cause its reaction, so the silica sol cannot be acidic; secondly, in an alkaline environment, OH - Ions can act as nuclear catalysts to attack silicon atoms in silane groups, promote the breaking of Si-OR bonds, and accelerate the hydrolysis reaction. In addition, the alkaline environment can increase the contact frequency between reactants (such as water molecules and hydroxide ions) and silane groups, thereby increasing the rate of the hydrolysis reaction. During the modification process, sedimentation caused by excessive hydrolysis is unacceptable, so the silica sol must be neutral.

[0019] In some possible implementations, the mass ratio of the aminosilane coupling agent, the organic glue and the silica sol in the modified silica sol is (1-5): (1-10): (10-20). Within this mass ratio range, the silanol produced by the hydrolysis of the aminosilane coupling agent can fully react with most of the hydroxyl groups on the surface of the silica sol and the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue at the same time to obtain a modified silica sol with reliable performance.

[0020] In some possible implementations, the components and weight percentages in the solid amine slurry include: 1 to 2 parts of anti-settling agent, 90 to 120 parts of water, and 40 to 60 parts of solid amine raw powder. Within this weight percentage range, the solid amine slurry can be effectively prevented from precipitation, and the solid amine slurry will not cause problems such as pore blockage or uneven coating (impregnation) during subsequent coating (impregnation) due to excessive viscosity of the solid amine slurry.

[0021] In some possible implementations, the weight percentages of the components in the coating slurry include 10 to 20 parts of modified silica sol, 100 to 180 parts of the solid amine slurry, and 0.2 to 2 parts of the auxiliary agent. Within these weight percentage ranges, the coating slurry can have high dispersibility, stability, rheology, and coating performance.

[0022] In some possible implementations, the solid-liquid ratio of the substrate to the coating slurry is (10 g to 20 g): (300 ml to 600 ml). Within this solid-liquid ratio range, the substrate can be completely immersed in the slurry and coated evenly.

[0023] In some possible implementations, the organic glue includes at least one of polyvinyl alcohol, polyurethane, polyacrylate, cyanoacrylate, silicone, phenolic resin, polyvinyl acetate, polyamide, polyvinyl chloride, polyvinylidene chloride, polybutadiene, polystyrene, polyethylene terephthalate, polylactic acid, and polyetheretherketone. The carboxyl group, aldehyde group, ester group, or epoxy group on these organic glues can react with the aminosilane coupling agent to form a stable covalent bond, that is, participate in the modification process of the silica sol.

[0024] The second purpose of the present application is to provide a solid amine honeycomb adsorbent prepared by a preparation method of a solid amine honeycomb adsorbent provided in the present application, wherein the loading amount of solid amine raw powder in the solid amine honeycomb adsorbent is 70kg / m³~240kg / m³.

[0025] In some possible implementations, the weight fractions of the components in the solid amine honeycomb adsorbent include:

[0026] 10 to 20 parts of modified silica sol, 131 to 182 parts of solid amine slurry and 0.2 to 2 parts of auxiliary agent. Under the weight percentage range of each component in this solid amine honeycomb adsorbent, the solid amine loading of the solid amine honeycomb adsorbent is 70 kg / m³ to 240 kg / m³, which is effective for CO 2 The adsorption capacity is 70mg / g~120mg / g.

[0027] The third object of the present application is to provide a method for preparing a solid amine honeycomb adsorbent provided in the present application, wherein the solid amine honeycomb adsorbent prepared by the method or the solid amine honeycomb adsorbent provided in the present application contains CO 2 Application in the field of gas adsorption separation, purification and / or capture.

[0028] The solid amine honeycomb adsorbent provided in the embodiment of the present application is 2 In the application of capture field, the solid amine honeycomb adsorbent has small airflow pressure drop, good heat and mass transfer performance, and good thermal conductivity. It can not only reduce the energy consumption of current carbon capture but also is very suitable for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the preparation method of the solid amine honeycomb adsorbent according to the embodiment of the present application;

[0030] Figure 2 This is a schematic diagram of the structure of the solid amine honeycomb adsorbent according to an embodiment of the present application;

[0031] Figure 3 The CO of the solid amine honeycomb adsorbent of the embodiment of the present application and the adsorbent of the comparative example is 2 Adsorption isotherms;

[0032] Figure 4 The solid amine honeycomb adsorbent of Example 1 of the present application is used for direct air capture of CO 2 Penetration curve. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present application clearer, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0034] On the contrary, the present application covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present application as defined by the claims. Further, in order to make the public have a better understanding of the present application, some specific details are described in detail in the detailed description of the present application below. Those skilled in the art can fully understand the present application without the description of these details.

[0035] The following examples serve to illustrate the present application. In the examples, unless otherwise indicated, parts are by weight, percentages are by weight, and temperatures are in degrees Celsius. The relationship between parts by weight and parts by volume is the same as the relationship between grams and cubic centimeters.

[0036] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0037] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0038] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0039] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0040] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also indicate the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as µg, mg, g, kg, etc.

[0041] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0042] Solid amines in powder or granular form can only be used for adsorption capture in fixed bed or fluidized bed processes, which will result in a longer diffusion path for such adsorbents, slow adsorption kinetics, and a thicker adsorption bed layer is required to achieve a sufficient removal rate of the target gas, which increases the amount of adsorbent used and also brings about the problem of high pressure resistance, which means increased energy consumption, and slow heat and mass transfer means a longer adsorption / desorption cycle time, which seriously affects the adsorption rate. Therefore, solid amines need to be made into honeycomb adsorbents.

[0043] At present, for honeycomb adsorbents, the impregnation method is used to coat the raw adsorbent powder on the substrate; the honeycomb adsorbent is covered with honeycomb ordered pores, which greatly reduces the airflow resistance; the honeycomb adsorbent generally uses a high thermal conductivity substrate, which greatly improves the thermal desorption efficiency; this makes the honeycomb adsorbent full of advantages in large-scale applications.

[0044] However, the structure of solid amine contains amino groups, which are usually linear or cyclic chain molecules. Its structure is relatively complex, and different types of solid amines have different chemical structures. However, if the solid amine is directly coated on the substrate, the loading amount, loading strength, mechanical strength and adsorption performance of the honeycomb adsorbent cannot achieve the ideal effect, because the solid amine is an organic amine loaded on the mesoporous channels of the porous material, and then dried and crushed to obtain a powdered solid. This solid material has a very large surface energy due to the characteristics of the organic amine, and the surface tension is very large after being configured into a slurry. It is almost impossible to penetrate into the interior of the substrate like adsorbents such as zeolite, and only a thin film can be formed on the surface of the substrate. Therefore, if the traditional slurry configuration method is used, it is almost impossible to form a uniform coating on the substrate. Even if a coating is formed, it cannot bring benefits to the mechanical strength and loading strength of the substrate itself. In addition, since the formed coating is too thin, the loading amount of the solid amine is extremely low, and thus the adsorption capacity of the adsorbent is extremely low.

[0045] In order to effectively make solid amine into honeycomb adsorbent to solve the problems of slow adsorption kinetics, high pressure resistance, high energy consumption, etc. of powder or granular solid amine. The embodiment of the present application proposes a method for preparing a solid amine honeycomb adsorbent, firstly using silane coupling agent and organic glue to modify silica sol, so that the silica sol particles of the modified silica sol form a rigid interconnected, porous, three-dimensional network structure, so that the binding ability of the modified silica sol and the solid amine is effectively improved; after the modified silica sol and the solid amine are prepared into a slurry, the modified silica sol entrains the solid amine, so that the solid amine is better combined with the substrate, and the prepared solid amine honeycomb adsorbent has high load strength and mechanical strength while maintaining the adsorption performance of the solid amine itself.

[0046] For the convenience of description, the following embodiments of the present application are described by taking the preparation, solid amine honeycomb adsorbent and application of the solid amine honeycomb adsorbent as examples.

[0047] [Preparation method of solid amine honeycomb adsorbent]

[0048] One of the purposes of the embodiments of the present application is to provide a method for preparing a solid amine honeycomb adsorbent, such as Figure 1 As shown, the following steps are included:

[0049] S1. Prepare modified silica sol using raw materials including aminosilane coupling agent, organic glue and silica sol.

[0050] S2. Prepare coating slurry using raw materials including modified silica sol, solid amine slurry and additives.

[0051] S3. The substrate is loaded with the coating slurry to obtain a solid amine honeycomb adsorbent.

[0052] The preparation method of the solid amine honeycomb adsorbent provided in the embodiment of the present application is that the alkoxy group in the aminosilane coupling agent reacts with the surface hydroxyl group of the silica sol, and the amino group of the aminosilane coupling agent reacts with the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue, thereby obtaining a modified silica sol with organic cross-linking function. The aminosilane in the modified silica sol serves as a "molecular bridge" between the silica particles in the silica sol and the organic glue, so that a rigidly interconnected, porous, three-dimensional network structure is formed between the silica sol particles. In the coating slurry prepared from the modified silica sol and solid amine with a network structure, the modified silica sol reduces the internal stress and shrinkage rate during the cross-linking and curing process of the slurry, and prevents the adsorbent from cracking after drying; when preparing the modified silica sol, the aminosilane coupling agent is first hydrolyzed by the water in the silica sol, and the alkoxy group (such as ethoxy, -OCH 2 CH 3) will hydrolyze to generate silanol groups (-SiOH) in the presence of water. The generated silanol groups can further react with the hydroxyl groups (-OH) on the surface of the silica particles in the silica sol to form siloxane (Si-O-Si) bonds. After adding the organic glue, the amino group of the aminosilane coupling agent reacts with the carboxyl, aldehyde, ester or epoxy groups of the organic glue to form stable covalent bonds, and finally obtain the modified silica sol. Then it is prepared into a coating slurry, in which the modified silica sol entrains the solid amine, so that the solid amine can be better combined with the substrate during loading. The prepared solid amine honeycomb adsorbent has high load strength and mechanical strength while maintaining the adsorption performance and high load of the solid amine itself. The solid amine is not easy to fall off from the substrate (no powdering phenomenon occurs). The preparation method of the embodiment of the present application has simple steps, easy to obtain raw materials, no pollution, low cost, high stability, and easy to industrial scale production.

[0053] [Step S1]

[0054] In some embodiments, in the above step S1, the aminosilane coupling agent includes 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldichlorosilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldichlorosilane, N-(2-aminoethyl)-3-amino At least one of propyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyldichlorosilane, 3-aminopropyltri(methoxyethoxy)silane, 3-aminopropyltri(ethoxyethoxy)silane, 3-aminopropyltri(ethoxyethoxy)vinylsilane, N-(2-aminoethyl)-3-aminopropyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyldichlorosilane, 3-aminopropylmethyldiisopropoxysilane, N-(3-triaminopropyl)triaminopropyltriethoxysilane, and di(triaminopropyl)tetraaminosilane. These aminosilane coupling agents contain amino and alkoxy groups. The silanol formed after the hydrolysis of the alkoxy groups reacts with the surface hydroxyl groups of the silica sol, and the amino group of the aminosilane coupling agent reacts with the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue to obtain modified silica sol. The aminosilane in the modified silica sol acts as a "molecular bridge" between the silica nanoparticles in the silica sol and the organic glue, so that a rigidly interconnected, porous, three-dimensional network structure is formed between the silica sol particles.

[0055] In some embodiments, in the above step S1, the organic glue includes at least one of polyvinyl alcohol, polyurethane, polyacrylate, cyanoacrylate, silicone, phenolic resin, polyvinyl acetate, polyamide, polyvinyl chloride, polyvinylidene chloride, polybutadiene, polystyrene, polyethylene terephthalate, polylactic acid, and polyetheretherketone. The carboxyl group, aldehyde group, ester group, or epoxy group on these organic glues can react with the aminosilane coupling agent to form a stable covalent bond, that is, participate in the modification process of the silica sol.

[0056] In some embodiments, in the above step S1, the relative molecular weight of the organic glue is 10 4 ~10 5 , in this example, it can be 10 4 , 10 5 Typical but non-restrictive relative molecular weights or the range between any two relative molecular weights. In this relative molecular weight range, the organic glue exhibits a lower viscosity. In the entire slurry formula, more organic matter is added. One of the key factors for successful coating is viscosity. Only by ensuring a lower viscosity can the slurry flow smoothly in the pores of the honeycomb substrate and avoid pore blockage.

[0057] In some embodiments, in the above step S1, the particle size of the silica sol is 10 nm to 300 nm. In the exemplary embodiment, it can be 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, etc., which are typical but non-limiting particle sizes, or a range between any two particle sizes. In this particle size range, the silica sol has a larger specific surface area and a larger number of surface hydroxyl groups, and is generally better able to form a stable colloidal dispersion system.

[0058] In some embodiments, in the above step S1, the mass concentration of silicon dioxide in the silica sol is 30% to 60%. In the exemplary embodiment, it can be a typical but non-limiting mass concentration of 30%, 40%, 50%, 60%, or a range between any two mass concentrations. In this mass concentration range, = 1 \* GB3 ① the silica sol has a lower viscosity, better fluidity, and is easy to process and handle, = 2 \* GB3 ② it has higher dispersion stability because the lower solid content reduces the possibility of interaction and agglomeration between particles, = 3 \* GB3 ③ it can increase the mechanical strength and thermal stability of the final adsorbent.

[0059] In some embodiments, in the above step S1, the specific surface area of ​​the silica sol is 100 m 2 / g~300m 2 / g, in the example, it can be 100m 2 / g, 150m 2 / g, 200m 2 / g, 250m2 / g、300m 2 / g or any range between two specific surface areas. In this specific surface area range, the rheological properties of silica sol are good and the stability is good.

[0060] In some embodiments, in the above step S1, the pore size of the silica sol is 2 nm to 50 nm, and in the exemplary embodiment, it can be a typical but non-limiting pore size such as 2 nm, 3 nm, 4 nm, 5 nm, or a range between any two pore sizes. Within this pore size range, a large amount of physical adsorption of the porous silica formed after the silica sol is dried can be avoided, thereby causing a decrease in the separation performance of the entire adsorbent.

[0061] In some embodiments, in the above step S1, the pore volume of the silica sol is 0.5 mL / g to 1 mL / g. In the exemplary embodiment, it can be 0.5 mL / g, 0.6 mL / g, 0.7 mL / g, 0.8 mL / g, 0.9 mL / g, 1 mL / g, etc., which are typical but non-limiting pore volumes, or a range between any two pore volumes. In this pore volume range, the silica sol has good dispersibility and stability. The unit mL / g represents the total volume of pores contained in each gram of silica sol.

[0062] In some embodiments, in the above step S1, the step of preparing the modified silica sol includes:

[0063] S1-1. Perform a first mixing reaction on the aminosilane coupling agent solution and the silica sol to obtain a hydroxyl-modified silica sol.

[0064] S1-2. The hydroxyl-modified silica sol and the organic gel solution are subjected to a second mixing reaction to obtain a modified silica sol.

[0065] In the above-mentioned steps of preparing the modified silica sol, the aminosilane coupling agent solution and the silica sol are first subjected to a first mixing reaction, so that the silanol formed by the hydrolysis of the alkoxy group of the aminosilane reacts with the surface hydroxyl group of the silica sol to obtain a hydroxyl-modified silica sol; in the modified silica sol, the amino group of the aminosilane coupling agent reacts with the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue to obtain the modified silica sol.

[0066] In some embodiments, in the above step S1-1, the preparation step of the aminosilane coupling agent solution includes: mixing the aminosilane coupling agent and the first solvent, stirring at a speed of 200r / min~280r / min for 10min~30min at room temperature to obtain a fully dispersed aminosilane solution; in the exemplary embodiment, the speed can be 200r / min, 230r / min, 250r / min, 260r / min, 280r / min, etc. typical but non-limiting speeds or a range between any two speeds, and the stirring time can be 10min, 15min, 20min, 25min, 30min, etc. typical but non-limiting stirring times or a range between any two stirring times. At this rotation speed, not only can the solution be mixed evenly, but also the volatilization of the alcohol solution caused by too fast stirring speed can be prevented; in this case, the aminosilane coupling agent and the first solvent are made into an aminosilane coupling agent solution, and the first solvent can not only dissolve the aminosilane coupling agent into a solution, but also inhibit the hydrolysis reaction of the aminosilane coupling agent, thereby avoiding the solution sedimentation problem caused by large-scale hydrolysis of the aminosilane coupling agent.

[0067] In some embodiments, the weight proportions of each component in the aminosilane coupling agent solution are: 1 to 5 parts of aminosilane coupling agent, 5 to 10 parts of the first solvent; in the exemplary embodiment, the aminosilane coupling agent can be 1, 2, 3, 4, 5, etc. typical but non-limiting weight proportions or a range between any two weight proportions, and the first solvent can be 5, 6, 7, 8, 9, 10, etc. typical but non-limiting weight proportions or a range between any two weight proportions. In this case, the aminosilane coupling agent can be completely dissolved into a solution state, and the alcohol solution at this proportion can well control the speed of hydrolysis. After the silica sol is subsequently added, the speed of pure solvent evaporation can be controlled by controlling the stirring speed, thereby achieving the purpose of controlling the hydrolysis reaction speed of the aminosilane coupling agent.

[0068] In some embodiments, the first solvent includes at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, dichloromethane, chloroform, and toluene. These first solvents are commonly used small molecule alcohol solvents, which can not only dissolve the aminosilane coupling agent into a solution, but also inhibit the hydrolysis reaction of the aminosilane coupling agent, thereby avoiding the problem of solution sedimentation caused by a large amount of hydrolysis of the aminosilane coupling agent.

[0069] In some embodiments, in the above step S1-1, the weight of the aminosilane coupling agent solution is 6 to 15 parts; the weight of the silica sol is 10 to 20 parts; in the exemplary embodiment, the aminosilane coupling agent solution can be 6, 8, 10, 12, 15, etc. typical but non-limiting weights or a range between any two weights, and the silica sol can be 10, 15, 20, etc. typical but non-limiting weights or a range between any two weights. Within this weight range, the alkoxy group in the aminosilane coupling agent can be fully hydrolyzed with the help of water in the silica sol, and the silanol generated by the hydrolysis is ensured to react completely with the hydroxyl group on the surface of the silica sol, avoiding excessive aminosilane coupling agent causing slurry sedimentation, and also avoiding too little aminosilane coupling agent, resulting in incomplete modification of the silica sol, affecting its final adhesion performance.

[0070] In some embodiments, in the above step S1-1, the silica sol is a neutral silica sol. This neutral silica sol can avoid the occurrence of side reactions, because: the active group of the selected aminosilane coupling agent is an amino group, so it is necessary to avoid adding any acidic substances to cause its reaction, so the silica sol cannot be acidic; secondly, in an alkaline environment, OH⁻ ions can act as nuclear catalysts to attack the silicon atoms in the silane group, promote the breaking of the Si-OR bond, and accelerate the hydrolysis reaction. In addition, the alkaline environment can increase the contact frequency between the reactants (such as water molecules and hydroxide ions) and the silane group, thereby increasing the rate of the hydrolysis reaction. In the modification process, the sedimentation caused by excessive hydrolysis cannot be accepted, so the silica sol must be neutral.

[0071] In some embodiments, in the above step S1-1, the first mixing reaction step includes: adding the aminosilane coupling agent solution to the silica sol under a stirring condition of 600 r / min to 800 r / min to obtain a mixed solution;

[0072] The mixed solution is stirred at a temperature of 40° C. to 60° C. at a rotation speed of 300 r / min to 400 r / min for 6 h to 8 h, and then cooled at room temperature to obtain a hydroxyl-modified silica sol.

[0073] In the first mixing reaction step, a mixed solution is first prepared, and the aminosilane coupling agent solution and the silica sol are fully contacted and mixed to obtain a uniformly mixed mixed solution; the mixed solution is then heated and stirred for reaction, which not only allows the solvent therein to completely volatilize, but also allows the silanol generated by the hydrolysis of the alkoxy groups of the aminosilane coupling agent to fully react with the surface hydroxyl groups of the silica sol to obtain a hydroxyl-modified silica sol.

[0074] In some embodiments, in the above step S1-2, the preparation of the organic glue solution includes the steps of: mixing the organic glue and the second solvent for 10 min to 30 min at room temperature and a stirring speed of 200 r / min to 280 r / min to obtain an organic glue solution. Stirring the organic glue and the second solvent for 10 min to 30 min at a stirring speed of 200 r / min to 280 r / min can fully disperse the organic glue in the second solvent to form a homogeneous organic glue solution.

[0075] In some embodiments, the weight proportions of each component in the organic glue solution are: 1 to 10 parts of organic glue, 5 to 15 parts of the second solvent; in the exemplary embodiment, the aminosilane coupling agent solution can be 1, 3, 5, 7, 10, etc. typical but non-limiting weight proportions or a range between any two weight proportions, and the second solvent can be 5, 7, 10, 13, 15, etc. typical but non-limiting weight proportions or a range between any two weight proportions. In this case, the organic glue can be completely dissolved into a homogeneous solution state, reducing the reaction time of the organic glue and the hydroxyl-modified silica sol.

[0076] In some embodiments, the second solvent includes at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, dichloromethane, chloroform, and toluene. These second solvents can fully dissolve the organic glue, so that the organic glue can fully react with the hydroxyl-modified silica sol, shortening the reaction time.

[0077] In some embodiments, in the above step S1-2, the second mixing reaction step includes: mixing the organic glue solution and the hydroxyl-modified silica sol for 4h to 6h under stirring conditions at a temperature of 40°C to 60°C to obtain a modified silica sol. In this case, the organic glue solution and the hydroxyl-modified silica sol are mixed and stirred at 40°C to 60°C to completely volatilize the second solvent, and the amino group in the hydroxyl-modified silica sol can fully react with the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue to obtain the modified silica sol.

[0078] In some embodiments, in the above steps S1-1 and S1-2, when the modified silica sol is prepared, the weight proportions of the aminosilane coupling agent solution are 6 to 15 parts, the weight proportions of the organic glue solution are 6 to 20 parts, and the weight proportions of the silica sol are 10 to 20 parts.

[0079] In some embodiments, in the above step S1, the mass ratio of the aminosilane coupling agent, the organic glue and the silica sol in the modified silica sol is (1-5): (1-10): (10-20), and in the exemplary embodiment, it can be a typical but non-limiting mass ratio such as 2:6:12, 1:1:10, 5:10:20, or a range between any two mass ratios. Within this mass ratio range, the silanol produced by the hydrolysis of the aminosilane coupling agent can fully react with most of the surface hydroxyl groups of the silica sol and the carboxyl group, aldehyde group, ester group or epoxy group of the organic glue at the same time, thereby obtaining a modified silica sol with reliable performance.

[0080] [Step S2]

[0081] In some embodiments, in the above step S2, the components and weight proportions in the solid amine slurry include: 1 to 2 parts of anti-settling agent, 90 to 120 parts of water, and 40 to 60 parts of solid amine raw powder; in the exemplary embodiment, the anti-settling agent can be 1 part, 1.5 parts, 2 parts, etc., typical but non-limiting weight proportions or a range between any two weight proportions, the water can be 90 parts, 100 parts, 110 parts, 120 parts, etc., typical but non-limiting weight proportions or a range between any two weight proportions, and the solid amine raw powder can be 40 parts, 50 parts, 60 parts, etc., typical but non-limiting weight proportions or a range between any two weight proportions. Within this weight proportion range, the solid amine slurry can be effectively prevented from precipitation, and the subsequent coating (impregnation) will not cause problems such as pore plugging or uneven coating (impregnation) due to excessive viscosity of the solid amine slurry.

[0082] In some embodiments, in the above step S2, the step of preparing the solid amine slurry comprises:

[0083] S2-1. Prepare an anti-precipitation solution including an anti-precipitation agent.

[0084] S2-2. Prepare a solid amine slurry by using an anti-precipitation solution and solid amine raw powder.

[0085] In the above-mentioned steps of preparing solid amine slurry, an anti-sedimentation solution is first prepared, and then the solid amine raw powder and the anti-sedimentation solution are used to prepare the solid amine slurry. The anti-sedimentation solution can prevent the subsequently added solid amine raw powder from agglomerating into clumps quickly, and ensure that no solid sedimentation occurs in the subsequent slurry preparation process.

[0086] In some embodiments, in the above step S2-1, the step of preparing the anti-precipitation solution includes: mixing the anti-precipitation agent and water under the stirring condition of room temperature and a rotation speed of 600r / min~800r / min for 10min~30min. In this case, since the anti-precipitation agent is a polymer and is not easily soluble in water, it is necessary to stir it to fully dissolve it, and the anti-precipitation agent in the prepared anti-precipitation solution is fully dispersed, and the obtained solution is a clear and transparent solution.

[0087] In some embodiments, the anti-precipitation agent includes at least one of sodium polyacrylate, hydroxymethyl cellulose, sodium carboxymethyl cellulose, polyvinyl pyrrolidone, and polysulfonate. The anti-precipitation principle of these anti-precipitation agents is to increase the viscosity of the suspension and slow down the sedimentation rate of solid particles; or to prevent particle aggregation and sedimentation through electrostatic repulsion.

[0088] In some embodiments, the water includes at least one of deionized water, distilled water, and ultrapure water. These waters do not contain metal ion impurities, and will not cause other side reactions when mixed into a solution.

[0089] In some embodiments, in the above step S2-2, the weight percentages of each component in the anti-precipitation solution include: 1 to 2 parts of anti-precipitation agent, 90 to 120 parts of water. In some embodiments, in the above step S2-2, the weight percentages of each component of the solid amine slurry include: 91 to 122 parts of anti-precipitation solution, 40 to 60 parts of solid amine raw powder; in the exemplary embodiment, the anti-precipitation solution can be 91 parts, 100 parts, 110 parts, 120 parts, etc., typical but non-limiting weight percentages or a range between any two weight percentages, and the solid amine raw powder can be 40 parts, 50 parts, 60 parts, etc., typical but non-limiting weight percentages or a range between any two weight percentages. Within this weight percentage range, the slurry can be effectively prevented from precipitating, and the slurry viscosity will not be too large, resulting in problems such as pore plugging or uneven coating during subsequent coating.

[0090] In some embodiments, in the above step S2-2, the organic amine in the solid amine raw powder includes at least one of monoethanolamine, diethanolamine, polyethyleneimine (PEI), amide, tetraethylenepentamine, and diethylenetriamine. These solid amines usually contain multiple amino groups, can provide more active sites, and have higher adsorption capacity; these solid amines remain stable at higher temperatures, are not easily degraded, and can be used for a long time; these solid amines are effective in adsorbing CO 2 Afterwards, it can be regenerated by temperature or vacuum to restore the adsorption capacity and is suitable for cyclic use.

[0091] In some embodiments, in the above step S2-2, the specific step of preparing the solid amine slurry using the anti-precipitation solution and the solid amine raw powder includes: mixing the anti-precipitation solution and the solid amine raw powder for 30min to 60min at a temperature of 40°C to 60°C and a rotation speed of 1000r / min to 1200r / min to obtain the solid amine slurry. In this case, in the prepared solid amine slurry, the solid amine raw powder is completely dissolved and uniformly dispersed in the anti-precipitation solution, and the solid amine slurry is a white suspension.

[0092] In some embodiments, in the above step S2, the auxiliary agent includes a dispersant and / or a defoamer. When the auxiliary agent is a dispersant and a defoamer, the weight portion of the dispersant in the coating slurry is 0.1 to 1 part, and the weight portion of the defoamer in the coating slurry is 0.1 to 1 part.

[0093] In some embodiments, the dispersant includes at least one of Disperbyk-111, Disperbyk-190, Disperbyk-2016, Disperbyk-2150, Disperbyk-2200 and Disperbyk-191 of Arkema. These dispersant molecules of Arkema usually have a long chain structure or a branched chain, and can form an adsorption layer on the surface of the particles. This adsorption layer forms a physical barrier on the surface of the particles, increases the spatial distance between the particles, and prevents the particles from aggregating due to van der Waals forces or other attractive forces.

[0094] In some embodiments, the defoamer includes at least one of BYK-022, BYK-024, BYK-025, BYK-028, BYK-032, and BYK-060 from BYK. These defoamers from BYK can be inserted into the bubble membrane through their hydrophobic components, causing the bubble membrane to lose stability and break. This bubble breaking mechanism is usually through the contact between the hydrophobic particles or droplets in the defoamer and the bubble membrane, causing the bubble membrane to become thinner or break locally; it can also form a layer of hydrophobic film in the liquid to inhibit the formation of new foam, thereby preventing the slurry from generating more foam during the stirring process, thereby affecting the coating effect.

[0095] In some embodiments, in the above step S2, the step of preparing the coating slurry using modified silica sol, solid amine slurry, dispersant and defoamer includes: mixing the modified silica sol, solid amine slurry, dispersant and defoamer for 30min to 60min at a temperature of 40°C to 60°C and a rotation speed of 1000r / min to 1200r / min to obtain the coating slurry. The components in the coating slurry prepared at a temperature of 40°C to 60°C and a rotation speed of 1000r / min to 1200r / min are uniformly and fully mixed, and the prepared coating slurry is a milky white slurry.

[0096] In some embodiments, in the above step S2, the weight proportions of the components in the coating slurry include 10 to 20 parts of modified silica sol, 131 to 182 parts of solid amine slurry, 0.1 to 1 part of dispersant and 0.1 to 1 part of defoaming agent; in the exemplary embodiment, the modified silica sol can be 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, etc., typical but non-limiting weight proportions or ranges between any two weight proportions, the solid amine slurry can be 100 parts, 120 parts, 150 parts, 180 parts, etc., typical but non-limiting weight proportions or ranges between any two weight proportions, the dispersant can be 0.1 parts, 0.5 parts, 0.8 parts, 1 parts, etc., typical but non-limiting weight proportions or ranges between any two weight proportions, and the defoaming agent can be 0.1 parts, 0.5 parts, 0.8 parts, 1 parts, etc., typical but non-limiting weight proportions or ranges between any two weight proportions. Within these weight ranges, the dispersibility, stability, rheology and coating performance of the coating slurry can be higher.

[0097] In some embodiments, in the above step S2, a pH adjuster is used to adjust the pH value of the coating slurry so that the pH value of the coating slurry is 8 to 14; in the exemplary embodiment, it can be a typical but non-limiting pH value such as 8, 10, 12, 14, or a range between any two pH values. In this case, the pH adjuster can increase the adsorption capacity of the amino group, and can ensure that the solid amine slurry is in a strong alkaline environment, thereby ensuring the stability of the slurry, and then the coating slurry can be evenly loaded on the substrate after the immersion treatment.

[0098] In some embodiments, the step of adjusting the pH value of the coating slurry with a pH adjuster includes: adding the pH adjuster to the coating slurry and stirring for 8h to 12h at room temperature and a rotation speed of 1000r / min to 1200r / min to obtain a coating slurry with a pH value of 8 to 14. In this case, the addition of the pH adjuster is stopped when the pH value of the coating slurry is 8 to 14, but stirring is continued until the components in the coating slurry are evenly dispersed and the pH value remains unchanged at 8 to 14.

[0099] In some embodiments, the pH regulator includes at least one of ammonia water, triethylamine, dimethylformamide, dimethyl sulfoxide, ethylenediamine, triethylamine hydrochloride, dimethyl malonate, tripropylamine, methyl carbamate, tert-butylamine, pyridine, and pyridine derivatives. These pH regulators can create a strong alkaline environment for the slurry to ensure the stability of the slurry, and can also bring more amino groups to increase the adsorption capacity of the adsorbent after molding.

[0100] In some embodiments, in the above step S2, the viscosity of the coating slurry is 10 mPa·s~100 mPa·s; in the exemplary embodiment, it can be 10 mPa·s, 20 mPa·s, 30 mPa·s, 40 mPa·s, 50 mPa·s, 60 mPa·s, 70 mPa·s, 80 mPa·s, 90 mPa·s, 100 mPa·s, etc. Typical but non-limiting viscosity values ​​or a range between any two viscosity values. In this case, the appropriate viscosity can ensure that the coating slurry forms a uniform coating on the substrate, avoid uneven coating, and improve the quality and consistency of the product; this viscosity range can balance the fluidity and adhesion of the coating slurry, which helps the coating slurry to be firmly attached to the substrate after coating, reducing the chance of falling off or bubbling; while too high a viscosity makes the coating slurry poor in fluidity and uneven coating; too low a viscosity is likely to cause sagging (coating dripping or flowing).

[0101] [Step S3]

[0102] In some embodiments, in the above step S3, the substrate is pretreated before being loaded with the coating slurry. In some embodiments, the step of pretreating the substrate includes: calcining the substrate for 5h~10h at a temperature of 100°C~800°C and an inert gas protective gas (nitrogen, argon, helium, neon, etc.). In this case, in the pretreated substrate, calcining at a low oxygen content can prevent the organic components in the substrate from reacting too quickly with oxygen during the calcination process, and the generated reactants cause a greater impact on the substrate and destroy the substrate structure. The calcined substrate has sufficient coating channels, which is conducive to the entry of the coating slurry and increases the loading amount.

[0103] In some embodiments, in the above step S3, the substrate includes at least one of cordierite, mullite, aluminum titanate, silicon carbide, zirconium oxide, silicon nitride, ceramic fiber, glass fiber, cordierite-mullite composite matrix, cordierite-aluminum titanate composite matrix. These substrates have rich porous structures, can accommodate sufficient solid amines, and are chemically stable and do not participate in the reaction.

[0104] In some embodiments, in the above step S3, the solid-liquid ratio of the substrate and the coating slurry is (10g~20g): (300ml~600ml), and in exemplary examples, it can be 10g:300ml, 10g:400ml, 10g:500ml, 10g:600ml, 15g:300ml, 15g:400ml, 15g:500ml, 15g:600ml, 20g:300ml, 20g:400ml, 20g:500ml, 20g:600ml, etc. Typical but non-limiting solid-liquid ratios or ranges between any two solid-liquid ratios. In this solid-liquid ratio range, the substrate can be completely immersed in the slurry and coated evenly.

[0105] In some embodiments, in the above step S3, the load processing step includes:

[0106] S3-1. After immersing the substrate in the coating slurry, take it out and dry it, then put it into the coating slurry again and repeat the immersion and drying steps to obtain a wet material after immersion.

[0107] S3-2. The wet material is dripped, purged, and then dried to obtain a solid amine honeycomb adsorbent.

[0108] In the above-mentioned impregnation treatment step, the substrate is repeatedly immersed in the coating slurry to increase the loading amount of the solid amine; the wet material is purged from the top to make all the pores at the bottom of the wet material transparent, so that the liquid film formed by the surface tension is blown away by the air flow, which will not cause the pores at the bottom of the substrate to be blocked.

[0109] In some embodiments, in the above step S3-1, the single immersion time of immersing the substrate in the coating slurry is 1 min to 15 min, the single drying treatment time is 4 h to 8 h, and the number of immersions is 2 to 10 times; in the exemplary embodiment, the single immersion time can be 1 min, 5 min, 10 min, 15 min, etc. typical but non-limiting time or a range between any two times, the single drying treatment time can be 4 h, 5 h, 6 h, 7 h, 8 h, etc. typical but non-limiting time or a range between any two times, and the number of immersions can be 2 times, 4 times, 6 times, 8 times, 10 times, etc. typical but non-limiting times or a range between any two numbers. In this case, the first impregnation time can be longer (1min~15min), and the subsequent impregnation time is less than or equal to the first impregnation time, which is controlled within 1min~10min. This is because the substrate after impregnation is dried, but the whole is still in a wet state. If the subsequent impregnation time is too long, it is easy to damage the substrate or the substrate strength is too low, and it is more likely to cause the solid amine applied previously to dissolve again in the coating slurry; the number of drying treatments after impregnation is 2~10 times, which can make the solid amine original powder on the substrate have a good loading capacity, so that the solid amine inside the substrate can also participate in the adsorption of CO 2 , making it have a higher CO 2 Adsorption capacity.

[0110] In some embodiments, in the above step S3-1, in the post-immersion drying step, the drying method is natural drying, breeze drying, or drying at a temperature below 70°C. In this case, natural drying can not only save energy, but also make the substrate dry evenly. Breeze drying and drying at a temperature below 70°C can speed up the drying process.

[0111] In some embodiments, in the above step S3-2, the dripping time is 10 min to 30 min, and the dripping condition is a natural condition. In the exemplary embodiment, the dripping time can be a typical but non-limiting time such as 10 min, 15 min, 20 min, 25 min, 30 min, or a range between any two times. In this case, there is no obvious coating slurry dripping out from the bottom of the substrate after dripping, which can ensure that the pores of the substrate will not be blocked by excess coating slurry.

[0112] In some embodiments, in the above step S3-2, compressed air is used to purge the wet material, and the purge time is 5s~20s. In the exemplary example, it can be 5s, 10s, 15s, 20s, etc., typical but non-limiting time or a range between any two times. In some embodiments, the pressure of the compressed air is 0.2MPa~0.8MPa. In the exemplary example, it can be 0.2MPa, 0.4MPa, 0.6MPa, 0.8MPa, etc., typical but non-limiting time or a range between any two times. In this case, the use of compressed air to purge the wet material can blow out the excess slurry in the pores to avoid clogging the pores of the substrate; purge until all the pores at the bottom of the wet material are completely transparent, so that the slurry will not form a liquid film at the bottom due to surface tension, thereby clogging the pores.

[0113] In some embodiments, in the above step S3-2, the drying step includes: drying the purged wet material naturally for 4 hours to 8 hours, and then drying it under vacuum conditions at 70°C to 100°C for 6 hours to 15 hours to obtain a solid amine honeycomb adsorbent. In this case, the wet material is naturally dried for 4 hours to 8 hours until there is no excess slurry on the surface of the wet material and it is no longer in an obviously wet state, so that the solid amine is tightly bonded to the substrate; the wet material is dried under vacuum conditions at 70°C to 100°C, and vacuum drying prevents the solid amine from being oxidized in large quantities above 100°C.

[0114]

Solid amine honeycomb adsorbent

[0115] The second purpose of the embodiment of the present application is to provide a solid amine honeycomb adsorbent prepared by a preparation method of a solid amine honeycomb adsorbent provided in the embodiment of the present application, such as Figure 2 As shown, the loading amount of solid amine raw powder in the solid amine honeycomb adsorbent is 70kg / m³~240kg / m³.

[0116] The solid amine honeycomb adsorbent provided in the embodiment of the present application has the advantages of low pressure resistance, low energy consumption, low replacement rate, etc., and has high load strength and mechanical strength while maintaining the adsorption performance of the solid amine itself. In addition, the solid amine honeycomb adsorbent is not easy to fall off from the substrate during use to reduce the adsorption performance.

[0117] In the embodiment, the loading amount of the solid amine raw powder in the solid amine honeycomb adsorbent can be 70 kg / m 3 , 100kg / m 3 , 130kg / m 3 , 160kg / m 3 、190kg / m 3 , 210kg / m 3 , 220kg / m 3 , 230kg / m 3 , 240kg / m3 Typical but non-limiting loads or ranges between any two loads.

[0118] In some embodiments, the solid amine honeycomb adsorbent is cylindrical or cubic in shape to adapt to different adsorption device structures, and its size varies with the size of the adsorption device. In this case, the airflow passing through the honeycomb adsorbent will not produce a large pressure resistance, and it is easy to operate in industrial production, and stress fracture will not occur due to the large size of the adsorbent.

[0119] In some embodiments, the weight fractions of the components in the solid amine honeycomb adsorbent include:

[0120] 10 to 20 parts of modified silica sol, 100 to 180 parts of solid amine slurry and 0.2 to 2 parts of auxiliary agent; in the exemplary embodiment, the modified silica sol can be 10, 12, 14, 16, 18, 20 parts, etc., typical but non-limiting weight parts or a range between any two weight parts, the solid amine slurry can be 100, 120, 140, 160, 180 parts, etc., typical but non-limiting weight parts or a range between any two weight parts, and the auxiliary agent can be 0.2, 0.4, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2 parts, etc., typical but non-limiting weight parts or a range between any two weight parts. Under the weight parts range of each component in this solid amine honeycomb adsorbent, the solid amine loading of the solid amine honeycomb adsorbent is 70 kg / m 3 ~240kg / m 3 , for CO 2 The adsorption capacity is 70mg / g~120mg / g.

[0121]

Application of solid amine honeycomb adsorbent

[0122] The third purpose of the embodiment of the present application is to provide a method for preparing a solid amine honeycomb adsorbent provided in the embodiment of the present application, wherein the solid amine honeycomb adsorbent prepared by the method or the solid amine honeycomb adsorbent provided in the embodiment of the present application is subjected to CO 2 Applications in the capture field.

[0123] The solid amine honeycomb adsorbent provided in the embodiment of the present application is 2 In the application of capture field, solid amine honeycomb adsorbent has small airflow pressure drop, good heat and mass transfer performance, and good thermal conductivity. It can not only reduce the current energy consumption of carbon capture, but also is very suitable for industrialization.

[0124] In some embodiments, CO 2 The gas adsorption separation, purification and / or capture fields include flue gas CO 2Capture, VOCs purification, desulfurization and denitrification, etc.

[0125] In some embodiments, solid amine honeycomb adsorbents can be used in rotary wheel adsorption capture technology to achieve low energy consumption gas separation.

[0126] The following describes the invention in conjunction with specific embodiments.

[0127] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, comprising the following steps:

[0128] (1) Pretreatment of substrate: Take a piece of honeycomb substrate (12 mm × 12 mm × 20 mm) made of glass fiber, calcine it at 800 °C for 10 h, and maintain the oxygen content at 5% to obtain the pretreated substrate.

[0129] (2) Preparation of an alcohol solution of a silane coupling agent: 2 parts by weight of N-aminoethyl-3-aminopropyltriethoxysilane was added to 10 parts of methanol, and the mixture was stirred at 280 r / min at room temperature for 30 min to obtain a fully dispersed N-aminoethyl-3-aminopropyltriethoxysilane solution.

[0130] (3) Preparation of hydroxy-modified silica sol: 12 parts by weight of neutral silica sol and 12 parts by weight of N-aminoethyl-3-aminopropyltriethoxysilane solution were obtained, and the neutral silica sol containing 30% by mass of silicon dioxide was stirred at 800 r / min, and then the N-aminoethyl-3-aminopropyltriethoxysilane solution was slowly poured in. After the addition was completed, the mixed solution was stirred in an oil bath at 60°C and a speed of 400 r / min for 6 h, and then cooled at room temperature to obtain hydroxy-modified silica sol.

[0131] (4) Preparing an organic glue solution: obtaining 6 parts by weight of polyacrylate and 10 parts by weight of methanol; mixing the polyacrylate and methanol, and stirring at a speed of 280 r / min at room temperature for 30 min to obtain a fully dispersed polyacrylate solution.

[0132] (5) Preparation of modified silica sol: 16 parts by weight of a polyacrylate solution and 14 parts by weight of a hydroxyl-modified silica sol are obtained, the polyacrylate solution and the hydroxyl-modified silica sol are mixed, and then stirred at 60° C. and 400 r / min for 6 h to obtain a modified silica sol.

[0133] (6) Preparation of solid amine slurry:

[0134] ① Preparation of an anti-precipitation solution: obtain 1.5 parts by weight of hydroxymethyl cellulose and 110 parts by weight of deionized water, mix the hydroxymethyl cellulose and the deionized water, stir the mixture at a speed of 800 r / min for 30 minutes after mixing, and obtain a transparent anti-precipitation solution.

[0135] ② Preparation of solid amine slurry: 111.5 parts by weight of an anti-precipitation solution and 50 parts by weight of tetraethylenepentamine were obtained by mixing to obtain a mixed solution, and then the mixed solution was stirred in an oil bath at 60° C. at a speed of 1000 r / min for 60 minutes to obtain a solid amine slurry.

[0136] (7) Preparation of coating slurry:

[0137] ① Obtain 161.5 parts by weight of solid amine slurry, 20 parts by weight of modified silica sol, 0.8 parts by weight of Disperbyk-191 and 0.5 parts by weight of BYK-028, mix them to obtain a mixed slurry, and stir and disperse the mixed slurry in an oil bath at 60° C. at a speed of 1000 r / min for 60 minutes to obtain a milky white slurry;

[0138] ② Use ethylenediamine to adjust the pH value of the milky white slurry to 10, and continue stirring at a speed of 1000 r / min at room temperature for 8 hours to obtain a coating slurry with a viscosity of 50 mPa·s.

[0139] (8) Preparation of solid amine honeycomb adsorbent:

[0140] ① Place the pretreated substrate into the coating slurry for the first immersion for 10 minutes.

[0141] ② Take out the substrate after the first immersion and dry it under natural conditions for 4 hours.

[0142] ③ The dried substrate was placed in the coating slurry again and the dipping and drying steps were repeated twice, with the dipping time being 5 minutes and the drying time being 4 hours. That is, the pretreated substrate was dipped 3 times in total.

[0143] ④ Take out the substrate after repeated immersion (i.e. wet material), let it drip for 30 minutes under natural conditions, blow the substrate with 0.5MPa compressed air, and continue to dry it under natural conditions for 8 hours after blowing.

[0144] ⑤ Dry the naturally dried wet material under vacuum conditions at 90° C. for 12 h to obtain a solid amine honeycomb adsorbent.

[0145] This embodiment also provides a solid amine honeycomb adsorbent, which is prepared by the above-mentioned preparation method of the solid amine honeycomb adsorbent, wherein the loading amount of the solid amine raw powder is 154.6 kg / m³;

[0146] The size of the solid amine honeycomb adsorbent is 12 mm×12 mm×20 mm.

[0147] This embodiment provides a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, comprising steps that are substantially the same as those of embodiment 1, except that the number of portions of solid amine raw powder in step (6) is 40 portions.

[0148] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, which comprises steps that are basically the same as those in Embodiment 1, except that: the number of portions of solid amine raw powder in step (6) is 60 portions.

[0149] This embodiment provides a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Embodiment 1, except that: in the impregnation step, the number of impregnations is 2 times.

[0150] This embodiment provides a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Embodiment 1, except that: in the impregnation step, the number of impregnations is 8 times.

[0151] This embodiment provides a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Embodiment 1, except that the weight portion of the neutral silica sol is 20 parts.

[0152] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, which includes steps that are basically the same as those in Embodiment 1, except that the weight fraction of the neutral silica sol is 10 parts.

[0153] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, which includes steps that are basically the same as those in Embodiment 1, except that the weight portion of N-aminoethyl-3-aminopropyltriethoxysilane (aminosilane coupling agent) is 1 part.

[0154] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, which includes steps that are basically the same as those in Embodiment 1, except that the weight portion of N-aminoethyl-3-aminopropyltriethoxysilane (aminosilane coupling agent) is 5 parts.

[0155] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, which includes steps that are basically the same as those in Embodiment 1, except that the weight portion of polyacrylate (organic glue) is 1 part.

[0156] This embodiment provides a method for preparing a solid amine honeycomb adsorbent, which includes steps that are basically the same as those in Embodiment 1, except that: the amount of polyacrylate (organic glue) is 10 parts.

[0157] Comparative Example 1

[0158] This comparative example provides 50 parts by weight of solid amine powder of tetraethylenepentamine as CO 2 Adsorbent.

[0159] Comparative Example 2

[0160] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, which comprises steps that are substantially the same as those of Example 1, except that the step (1) of pretreating the substrate is not included.

[0161] Comparative Example 3

[0162] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, which comprises steps that are basically the same as those in Example 1, except that in point ⑤ of step (8), the drying of the wet material is not carried out under vacuum conditions.

[0163] Comparative Example 4

[0164] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, which comprises steps that are basically the same as those in Example 1, except that: in point (4) of step (8), the substrate is not purged after impregnation.

[0165] Comparative Example 5

[0166] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Example 1, except that the weight portion of tetraethylenepentamine (solid amine raw powder) is 30 parts.

[0167] Comparative Example 6

[0168] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, comprising steps that are substantially the same as those of Example 1, except that the weight fraction of tetraethylenepentamine (solid amine raw powder) is 100 parts.

[0169] Comparative Example 7

[0170] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Example 1, except that the weight portion of the neutral silica sol is 30 parts.

[0171] Comparative Example 8

[0172] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Example 1, except that the weight portion of the neutral silica sol is 5 parts.

[0173] Comparative Example 9

[0174] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, comprising steps that are basically the same as those in Example 1, except that the weight portion of N-aminoethyl-3-aminopropyltriethoxysilane (aminosilane coupling agent) is 10 parts.

[0175] Comparative Example 10

[0176] This comparative example proposes a method for preparing a solid amine honeycomb adsorbent and the solid amine honeycomb adsorbent prepared therefrom, and the steps are basically the same as those in Example 1, except that the weight portion of the polyacrylate is 12 parts.

[0177] Comparative Example 11

[0178] This comparative example provides a spherical solid amine CO 2 The adsorption material is formed by cross-linking and curing with polyethyleneimine as the matrix, and the matrix includes a thermosensitive group introduced by Michael addition; a spherical solid amine CO 2 The particle size D50 of the adsorption material is 2 μm~5 μm, and the swelling rate is 110%~270%; the provider of the thermosensitive group includes N-isopropyl acrylamide; the cross-linking agent includes ethylene glycol diglycidyl ether; and the molecular weight of polyethyleneimine is 70000.

[0179] In order to verify the progress of the embodiments of the present application, the following solid amine honeycomb adsorbents prepared by the preparation methods of the solid amine honeycomb adsorbents provided in the above embodiments 1 to 11 and the solid amine raw powder provided in Comparative Example 1, the solid amine honeycomb adsorbents provided in Comparative Examples 2 to 10, and the spherical solid amine CO provided in Comparative Example 11 are compared. 2 The adsorption materials were subjected to the following verification tests, including the following steps:

[0180] 1: After the adsorbent is dry, take it out and observe whether there is any hole blockage at the bottom. If there is a hole blockage, cut off 0.5 cm to see if it is not blocked. If it is still blocked, continue to cut off in increments of 0.5 cm until it is no longer blocked.

[0181] 2: Cut some small pieces of the monolithic adsorbent prepared in the examples, and use a BET machine (autosorb iQ) to perform carbon dioxide adsorption isotherm characterization tests on the adsorbents of all the examples and comparative examples. The static adsorption method was used to measure the CO2 adsorption isotherm at 90°C. 2 Adsorption isotherms: all samples were vacuum degassed at 100 °C for 8 h before adsorption. To reflect the adsorption capacity, the mass of the adsorbent was converted into the mass of pure solid amine.

[0182] 3: The adsorbents of the examples and comparative examples were placed in CO 2 Dynamic adsorption platform for CO 2Adsorption evaluation: Before adsorption, the adsorbent was activated with nitrogen (1L / min) at 120°C for 30 min. After activation, it was cooled to the adsorption temperature of 90°C and then switched to the raw gas. 2 The concentration is 40% (volume fraction), and the rest is N 2 The raw gas flow rate is 100ml / min; part of the tail gas after adsorption is passed into the analyzer to detect CO 2 concentration, the remaining part is sent to the tail gas treatment device and then discharged, the tail gas CO 2 When the concentration returns to the initial concentration and stabilizes, it can be considered that the adsorption has penetrated.

[0183] 4: During CO 2 During the dynamic adsorption test, a pressure sensor is used to detect the pressure difference before and after the adsorbent to test the piezoresistance of the adsorbent. According to the gas flow rate and the cross-sectional area of ​​the adsorption column, the gas flow rate is 0.01m / s.

[0184] 5: Cut off a section of the adsorbent in the embodiment and record the mass at this time. Put white paper on the bottom and let the honeycomb adsorbent do free fall at a distance of 40 cm from the white paper. Then weigh it and observe whether there is powder left on the white paper.

[0185] 6: The adsorbent of Example 1 was placed in a direct air capture platform for adsorption evaluation. Before adsorption, the adsorbent was activated with nitrogen (1 L / min) at 120°C for 30 min. After activation, it was purged with nitrogen and cooled to the adsorption temperature of 25°C, and then switched to air with an air intake flow rate of 40 L / min. A portion of the tail gas after adsorption was passed into an analyzer to detect CO 2 concentration, the remaining part is sent to the tail gas treatment device and then discharged, the tail gas CO 2 When the concentration returns to the initial concentration and stabilizes, it is considered that the adsorption has penetrated. The adsorbent after adsorption saturation is heated to 120°C for desorption. The desorbed gas is collected by a vacuum pump into a gas bag and CO is introduced. 2 Gas analyzer for analysis.

[0186] For the convenience of comparison, the parameters of the above embodiments 1 to 11 and comparative examples 1 to 11 are listed in Table 1. The solid amine honeycomb adsorbent prepared by the preparation method of the solid amine honeycomb adsorbent provided in embodiments 1 to 11 obtained in the above experiment and the solid amine raw powder provided in comparative example 1, the solid amine honeycomb adsorbent provided in comparative examples 2 to 14, and the spherical solid amine CO provided in comparative example 15 are shown in Table 1. 2 Adsorption of CO 2The unit equilibrium adsorption capacity, total equilibrium adsorption capacity, loading capacity, piezoresistance, powder loss and adsorbent pore blocking conditions are shown in Table 2. The CO 2 absorption rate of the solid amine honeycomb adsorbent prepared by the preparation method of Examples 1 to 11 is higher than that of the solid amine raw powder provided in Comparative Example 1 and the solid amine granular adsorbent prepared by Comparative Examples 2 to 11. 2 The adsorption isotherm is Figure 3 The solid amine honeycomb adsorbent obtained in the above-mentioned test step 6 directly captures carbon dioxide in the air to obtain CO 2 The penetration adsorption curve is as follows Figure 4 shown.

[0187] Table 1

[0188]

[0189] Table 2

[0190]

[0191] Note: In Table 1 and Table 2, “-” indicates that the content of the physical quantity is the same as that in Example 1; “\” indicates that the physical quantity does not exist.

[0192] From Table 2 above and Figure 3 , 4 It can be seen that:

[0193] (1) The solid amine honeycomb adsorbents in Example 1 and Comparative Example 1 were used to adsorb CO 2 The adsorption capacity of the solid amine raw powder is not much different, indicating that the solid amine honeycomb adsorbent prepared by the preparation method of the embodiment of the present application will not reduce CO too much. 2 adsorption capacity.

[0194] (2) The piezoresistance of the solid amine honeycomb adsorbent in Example 1 and Comparative Examples 1 and 11 is much lower than that of the solid amine raw powder and the spherical adsorbent, indicating that the solid amine honeycomb adsorbent prepared by the preparation method of the embodiment of the present application has a lower piezoresistance.

[0195] (3) From the comparison between Example 1 and Comparative Example 2, it can be seen that most of the organic matter in the pretreated substrate volatilizes and a large number of macropores appear, which is beneficial to the loading of the solid amine honeycomb adsorbent. The loading amount of the pretreated substrate is greater than that of the unpretreated substrate, which is ultimately reflected in the advantage of the pretreated substrate in terms of total adsorption amount.

[0196] (4) From the comparison between Example 1 and Comparative Example 3, it can be seen that the solid amine honeycomb adsorbent of the present invention must be isolated from oxygen at high temperature, otherwise the adsorbent will be oxidized and inactivated, resulting in a sharp drop in the unit adsorption amount.

[0197] (5) From the comparison between Example 1 and Comparative Example 4, it can be seen that if no purging is performed after impregnation, part of the excess slurry will accumulate at the bottom of the solid amine honeycomb adsorbent due to surface tension, causing deeper pore blockage and increasing the cost of industrial application.

[0198] (6) From the comparison between Examples 1 to 11 and Comparative Examples 5 to 6, it can be seen that reducing the number of solid amines will lead to a decrease in the loading amount of the solid amines. Although it will not have a significant impact on the unit adsorption amount of the solid amine honeycomb adsorbent, the reduction in loading amount will lead to a significant reduction in the total adsorption amount. Even if an excessive increase in the amount of solid amine powder increases the loading amount, it will also cause the solid amine inside to be unable to react with CO. 2 Contact, a large amount of solid amine honeycomb adsorbents are not fully utilized, resulting in a decrease in unit adsorption capacity, and an excessive increase in solid amine powder will cause a sharp increase in slurry viscosity, resulting in an increase in pore wall thickness, an increase in piezoresistance, and a significant increase in pore plugging depth. Due to the mismatch between the number of solid amines and the number of binders, the load strength is greatly reduced and the powder loss rate is increased.

[0199] (7) From the comparison between Examples 1 to 11 and Comparative Examples 7 to 8, it can be seen that even if the amount of silica sol is increased excessively, a large amount of solid amine powder will be blocked by the sol, resulting in a decrease in the unit adsorption amount, and an excessive increase in silica sol will lead to an increase in the viscosity of the slurry, resulting in an increase in the wall thickness of the pores, resulting in an increase in the piezoresistance and a greatly increased pore blocking depth. However, a reduction in the amount of silica sol will lead to a decrease in the load, and the powder loss rate will increase due to insufficient bonding ability. After a part of the silane is hydrolyzed, there is not enough silica sol to cross-link with it, resulting in a small part of the silane being in a paste state after hydrolysis, resulting in an increase in the viscosity of the slurry. Not only will the pores of a part of the solid amine powder be blocked, resulting in a decrease in the unit adsorption amount, but also due to the excessive viscosity, the problem of increased pore blocking depth will occur. Further reducing the content of silica sol will result in a lack of sufficient silica sol to react and cross-link with most of the aminosilane coupling agents after hydrolysis, resulting in hard sedimentation of the slurry, resulting in the consequence that it cannot be coated.

[0200] (8) By comparing Examples 1 to 11 with Comparative Example 9, it can be seen that reducing the amount of aminosilane coupling agent results in part of the silica sol and organic being unable to form crosslinks with the aminosilane coupling agent, and failing to form a sufficient three-dimensional network, resulting in a decrease in the loading amount and an increase in the powder loss rate. Increasing the amount of aminosilane coupling agent will lead to a violent hydrolysis of the silane, and after a part of the silane is hydrolyzed, there is not enough silica sol and organic glue to crosslink with it, resulting in a paste-like state after the hydrolysis of part of the silane or causing the slurry to solidify, resulting in an increase in the viscosity of the slurry and making it impossible to apply. Not only will the pores of a part of the solid amine powder be blocked, resulting in a decrease in the unit adsorption amount, but also due to the excessive viscosity, the problem of increased pore blocking depth will occur, and the solid amine will be unevenly coated on the substrate, resulting in an increase in piezoresistance.

[0201] (9) By comparing Examples 1 to 11 with Comparative Example 10, it can be seen that reducing the amount of organic glue results in a decrease in the loading amount, and the powder loss rate increases due to insufficient bonding ability. The increase in organic glue will lead to an increase in the loading amount, but excessive organic glue will block part of the pores of the solid amine powder, resulting in a decrease in the unit adsorption amount, and excessive organic glue will increase the viscosity of the slurry, ultimately leading to an increase in the piezoresistance and pore blocking depth of the solid amine honeycomb adsorbent.

[0202] (10) The direct air capture experiment of Example 1 and Figure 4 It can be seen that the solid amine honeycomb adsorbent prepared by the present invention can be used for direct air capture and can maintain a long adsorption time, and the breakthrough begins after 170 minutes. Analysis of the gas table after desorption shows that CO 2 The concentration can reach 95%, and the CO 2 The recovery rate is 93%, that is, the present invention can be used for direct air capture, has a large adsorption capacity, and can be desorbed at a relatively low temperature, so that the enriched gas concentration and the recovery rate reach "double 90%".

[0203] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a solid amine honeycomb adsorbent, characterized in that: The steps include: The modified silica sol is prepared by using raw materials including an aminosilane coupling agent, an organic glue and a silica sol. The steps of preparing the modified silica sol include: performing a first mixing reaction on an aminosilane coupling agent solution and a silica sol to obtain a hydroxyl-modified silica sol; performing a second mixing reaction on the hydroxyl-modified silica sol and the organic glue solution to obtain the modified silica sol; The preparation step of the aminosilane coupling agent solution includes: mixing the aminosilane coupling agent and the first solvent, stirring at a speed of 200 r / min to 280 r / min for 10 min to 30 min at room temperature to obtain a fully dispersed aminosilane solution; The first solvent comprises: at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, ethylene glycol, propylene glycol, dichloromethane, chloroform, and toluene; The coating slurry is prepared by using raw materials including the modified silica sol, solid amine slurry and additives; The coating slurry is used to load a substrate to obtain a solid amine honeycomb adsorbent.

2. The method for preparing a solid amine honeycomb adsorbent according to claim 1, characterized in that: In the loading treatment step, a pH adjuster is used to adjust the pH value of the coating slurry so that the pH value of the coating slurry is 8 to 14; And / or, the loading treatment step includes repeatedly immersing the substrate in the coating slurry and then drying it.

3. The method for preparing a solid amine honeycomb adsorbent according to claim 2, characterized in that: The weight proportion of the aminosilane coupling agent solution is 6 to 15 parts; And / or, the weight proportion of the silica sol is 10 to 20 parts.

4. The method for preparing a solid amine honeycomb adsorbent according to claim 1, characterized in that: The silica sol is neutral silica sol.

5. The method for preparing a solid amine honeycomb adsorbent according to claim 2, characterized in that: The number of drying treatments after dipping is 2 to 10 times.

6. The method for preparing a solid amine honeycomb adsorbent according to claim 1, characterized in that: The mass ratio of the aminosilane coupling agent, the organic glue and the silica sol in the modified silica sol is (1-5): (1-10): (10-20); And / or, the components and weight proportions in the solid amine slurry include: 1 to 2 parts of anti-settling agent, 90 to 120 parts of water, and 40 to 60 parts of solid amine raw powder; And / or, the weight proportions of the components in the coating slurry include 10 to 20 parts of modified silica sol, 100 to 180 parts of the solid amine slurry, and 0.2 to 2 parts of the auxiliary agent; And / or, the solid-liquid ratio of the substrate and the coating slurry is (10g~20g): (300ml~600ml).

7. The method for preparing a solid amine honeycomb adsorbent according to any one of claims 1 to 6, characterized in that: The organic glue includes at least one of polyvinyl alcohol, polyurethane, polyacrylate, cyanoacrylate, silicone, phenolic resin, polyvinyl acetate, polyamide, polyvinyl chloride, polyvinylidene chloride, polybutadiene, polystyrene, polyethylene terephthalate, polylactic acid, and polyetheretherketone.

8. A solid amine honeycomb adsorbent prepared by the method for preparing a solid amine honeycomb adsorbent according to any one of claims 1 to 7, characterized in that: The loading amount of the solid amine raw powder in the solid amine honeycomb adsorbent is 70kg / m³~240kg / m³.

9. The solid amine honeycomb adsorbent according to claim 8, characterized in that: The weight proportions of the components in the solid amine honeycomb adsorbent include: 10 to 20 parts of modified silica sol, 131 to 182 parts of solid amine slurry and 0.2 to 2 parts of auxiliary agent.

10. Use of the solid amine honeycomb adsorbent according to any one of claims 8 to 9 in the field of adsorption, separation, purification and / or capture of gases containing CO2.

Citation Information

Patent Citations

  • Integral structure adsorbent based on amine functionalized silica sol, and preparation method and application of integral structure adsorbent

    CN113209951A

  • Solid amine adsorbent for adsorbing CO2 as well as preparation method and application of solid amine adsorbent

    CN117680106A

  • Hierarchically porous amine-silica monolith and preparation method thereof

    US20150251160A1