A method for preparing LiFePO4 / C composite material doped with metal ions

By introducing metal ion doping into lithium iron phosphate materials and adjusting the calcination curve, the problems of electronic conductivity and slow lithium ion diffusion in lithium iron phosphate materials were solved, and a LiFePO4/C composite material with high sphericity and compaction density was achieved, which improved the rate performance and particle size distribution uniformity of the battery.

CN118529714BActive Publication Date: 2026-11-10EAST CHINA UNIV OF SCI & TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410699710.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2026-11-10
Estimated Expiration
2044-05-31

AI Technical Summary

Technical Problem

In existing technologies, lithium iron phosphate materials have slow electronic conductivity and lithium-ion diffusion rate, resulting in poor rate performance of batteries. Furthermore, the uneven particle size distribution and insufficient sphericity affect the compaction density, which is difficult to effectively control using existing methods.

Method used

By introducing metal ion doping during the calcination process and adjusting the calcination curve according to the type and amount of doped ions, including temperature control during the heating, cooling, and isothermal stages, the crystal growth and particle size distribution of lithium iron phosphate are regulated, resulting in a LiFePO4/C composite material with high sphericity and compaction density.

Benefits of technology

High electronic conductivity and lithium-ion diffusion rate of lithium iron phosphate materials were achieved, improving the rate performance and compaction density of batteries, and obtaining excellent electrical properties and uniform particle size distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118529714B_ABST
    Figure CN118529714B_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing a LiFePO4 / C composite material doped with metal ions. The LiFePO4 / C composite material comprises lithium iron phosphate particles doped with metal ions and a carbon layer coating the surface of the lithium iron phosphate particles. One or both of the iron and lithium sites in the lithium iron phosphate are partially substituted. Compared with existing technologies, this invention regulates the heating and cooling rates at different stages of precursor calcination based on the different effects of different doping ions on the lattice distortion and crystal growth rate of lithium iron phosphate. This alters the residence time of particles at different temperature ranges, thereby regulating the nucleation rate and crystal growth rate of lithium iron phosphate. The LiFePO4 / C composite material prepared using this method exhibits good sphericity, reasonable particle size distribution, high compaction density, and high specific capacity and capacity retention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium iron phosphate preparation technology, and in particular relates to a method for preparing a LiFePO4 / C composite material doped with metal ions. Background Technology

[0002] Lithium iron phosphate (LiFePO4) has an olivine crystal structure, exhibiting good stability and safety. LiFePO4 boasts a high theoretical lithium storage capacity (170 mAh / g), a high and stable operating voltage, and good high-temperature performance. Its raw materials are free of precious elements, widely available, and have low production costs, making it one of the most widely used cathode materials for lithium-ion batteries. However, LiFePO4 has a low theoretical density, resulting in a lower volumetric capacity ratio compared to other lithium-ion cathode materials such as lithium cobalt oxide and lithium manganese oxide. Its olivine structure leads to slow electronic conductivity and lithium-ion diffusion rate, resulting in poor rate performance of the battery.

[0003] Methods to optimize the performance of lithium iron phosphate batteries mainly include metal ion doping, coating the particle surface with conductive materials, and particle miniaturization. Particle miniaturization can shorten the lifespan of lithium iron phosphate batteries. + While ion migration distance is significant, the large particle surface area can also lead to reduced dispersibility and decreased material processability. Carbon coating can improve the electrical conductivity between the carbon layer surface and particles, reduce reaction impedance, and inhibit particle agglomeration and growth. Ion doping, without disrupting the lithium iron phosphate crystal structure, utilizes a small amount of impurities to improve the electrochemical performance of the product by introducing them into the crystal lattice. In recent years, significant progress has been made in the research of metal ion doping modification and carbon coating modification.

[0004] Compaction density is one of the important indicators of lithium iron phosphate cathode materials, and it is directly related to the volumetric energy density of lithium batteries. It is generally believed that factors such as particle size distribution, sphericity, and carbon coating will have varying degrees of influence on the compaction density of lithium iron phosphate materials, and these factors are all affected by the material preparation process.

[0005] The solid-state synthesis method for producing lithium iron phosphate involves mixing, grinding, and spray-drying a phosphorus source, lithium source, iron source, and carbon source, followed by high-temperature reaction under inert gas protection. During the grinding process, metal compounds and carbon sources are often added as modifiers. During calcination, as the temperature rises, the reactants decompose, forming intermediate products that further react to form lithium iron phosphate. The heat and mass transfer mechanisms of the high-temperature solid-state reaction are complex, influenced by factors such as the composition and particle size of the precursor impurities, calcination temperature, and residence time distribution at different temperatures. This makes process control difficult, resulting in significant batch-to-batch product quality variations.

[0006] Chinese patent CN 117558915A discloses a method for preparing lithium iron phosphate material with controlled particle size. The method involves calcining a precursor under different conditions to obtain two intermediate materials with different particle sizes. The first intermediate has a particle size range of 1.0 ≤ (D90m - D10m) / D50m ≤ 2.0, and the second intermediate has a particle size range of 1.0 ≤ (D90n - D10n) / D50n ≤ 1.5. The two intermediates are then mixed in a certain proportion and calcined again to obtain the lithium iron phosphate material. This method regulates crystal growth by adding sodium chloride or potassium chloride and calcining at different heating rates and temperatures. Ultimately, the particle size of the product is controlled by compounding a mixture of lithium iron phosphate with different particle sizes.

[0007] Chinese patent CN117263157A discloses a method for preparing lithium iron phosphate cathode material. The method uses any one or a combination of at least two of TiO2, WO3, and MgO as dopants. The particle size of the precursor is adjusted by wet milling, and then the wet abrasive is spray-dried and calcined to prepare the lithium iron phosphate cathode material. This method improves the compaction density of the lithium iron phosphate cathode material by optimizing the milling particle size and particle gradation.

[0008] Chinese patent CN117080436A discloses a method for preparing lithium iron phosphate cathode material. It uses any one or a combination of at least two of Ti, Mg, V and Al as dopants and organic polymers and small organic molecules as carbon sources. By limiting the relationship between the specific surface area, particle size and mass fraction of carbon coating layer of the material: 5≤S×(D90-D50) / WC≤15, the lithium iron phosphate cathode material can simultaneously meet the requirements of high electronic conductivity and high compaction performance.

[0009] Regular crystal morphology, suitable intermediate grain size, and reasonable grain size distribution are key to optimizing the compaction density of lithium iron phosphate (LFP). Some patents disclose methods to improve the tap density and volumetric capacity of LFP materials by spherizing LFP particles, providing explanations for improved particle sphericity through particle morphology observation, but without specifying a measurement for particle sphericity. The accumulation of slightly larger spherical particles creates voids, requiring smaller particles to fill them, thus increasing the material's compaction density. In other words, compaction density is closely related to grain size distribution and gradation. For LFP, when discussing the gradation of particles of different sizes, the range of particle size difference must be considered simultaneously. During charge and discharge, the migration distance of lithium ions within large and small particles differs, resulting in different degrees of lithium insertion / extraction at the same voltage. Over long-term use, smaller particles exhibit a higher decay rate than larger particles; larger particles have poor intrinsic kinetic performance, increasing the battery's DC internal resistance and reducing rate performance.

[0010] Existing technologies for optimizing the performance of lithium iron phosphate materials mainly employ methods such as controlling the particle size of the precursor, stepwise calcination followed by mixing, or using different temperature rise rates in stages. For ion doping, the focus is primarily on optimizing the electrical properties of the material; existing technologies have not addressed the simultaneous influence of ion doping on crystal growth and particle size distribution. Summary of the Invention

[0011] Given the lack of existing technologies regarding the influence of ion doping on the reaction of calcined precursors under high-temperature reducing atmospheres and on the nucleation and growth of lithium iron phosphate crystals, this invention provides a method for preparing LiFePO4 / C composite materials doped with metal ions.

[0012] This invention adjusts the calcination curve of the precursor based on the type and amount of dopant compound and the dopant ions, changing the heating or cooling rates at different calcination temperature ranges, and regulating the residence time of particles at different temperature ranges. This allows for the control of the precursor's solid-state chemical reaction rate, phase transition, and crystal growth rate, ultimately yielding a LiFePO4 / C composite material doped with metal ions that exhibits regular morphology, high sphericity, high compaction density, good rate performance, and high charge / discharge energy efficiency. The process is convenient to operate, highly efficient, and easily scalable for continuous industrial production.

[0013] The objective of this invention can be achieved through the following technical solutions:

[0014] This invention first provides a method for preparing LiFePO4 / C composite material doped with metal ions, the specific steps of which are as follows:

[0015] The precursor of lithium iron phosphate doped with metal ions was calcined to obtain a LiFePO4 / C composite material doped with metal ions with high sphericity and compaction density.

[0016] The calcination process involves sequentially going through a heating stage, a cooling stage, and a isothermal stage under an inert or reducing atmosphere.

[0017] (1) Heating section: The temperature rises from room temperature to the calcination endpoint temperature. The heating rate from room temperature to 450℃ is 5-10℃ / min. The heating rate from 450℃ to the calcination endpoint temperature is 10-30℃ / min. After reaching the calcination endpoint temperature, the temperature is held for 200-80 minutes.

[0018] (2) Cooling section: The temperature drops from the calcination endpoint temperature to the calcination intermediate temperature, and the cooling rate is 10-50℃ / min;

[0019] (3) Constant temperature section, the temperature is maintained at the medium temperature of calcination, and the residence time is 200-600 min;

[0020] The room temperature is 25°C, the calcination endpoint temperature is 700-810°C, and the calcination intermediate temperature is 500-650°C.

[0021] The LiFePO4 / C composite material doped with metal ions includes lithium iron phosphate particles doped with metal ions and a carbon layer coated on the surface of the lithium iron phosphate particles.

[0022] The metal ions are selected from one or more of Mg, Mn, Zr, Co, V, Zn, Nb, Al, or Ti.

[0023] In one embodiment of the present invention, in the LiFePO4 / C composite material doped with metal ions, one or both of the iron and lithium sites of lithium iron phosphate are partially replaced by doped metal ions; the molecular formula of the LiFePO4 / C composite material doped with metal ions is: Li 1-x A x Fe 1-y B y PO4 / C; wherein A and B are independently selected from one or more of Mg, Mn, Zr, Co, V, Zn, Nb, Al or Ti, 0≤x<1%, 0≤y<1%, and x and y are not simultaneously 0.

[0024] In one embodiment of the present invention, the molecular formula of the LiFePO4 / C composite material doped with metal ions is represented as: Li 1-x Al x Fe 1-y-z M y N z PO4 / C, M and N are independently selected from one or more of Mg, Mn or Ti, Al is aluminum, 0≤x≤1.5%, 0≤y≤1%, 0≤z≤1%.

[0025] In one embodiment of the present invention, the precursor of lithium iron phosphate is obtained by mixing a metal ion dopant with a phosphorus source, a lithium source, an iron source and a carbon source in the following proportions, with an elemental molar ratio of Li:Al:Fe:M:N:P:O=(1-x):x:(1-yz):y:z:1:4, adding a grinding media for grinding, and then spray drying to form a precursor of lithium iron phosphate doped with metal ions.

[0026] In one embodiment of the present invention, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, lithium phosphate, lithium acetate, or lithium oxalate; the iron source is selected from at least one of iron phosphate, iron oxide, iron pyrophosphate, or ferrous oxalate; the phosphorus source is selected from at least one of phosphoric acid, iron phosphate, iron pyrophosphate, or lithium dihydrogen phosphate; and the carbon source is selected from at least one of sucrose, glucose, starch, or polyvinyl alcohol.

[0027] The metal ion dopant is selected from oxides, phosphates, sulfates, or organic compounds containing one or more of the elements Mg, Mn, Zr, Co, V, Zn, Nb, Al, or Ti. Preferably, the doping cation of the metal ion dopant is Mg. 2+ Mn 4+ Zr 4+ Co 2+ V 5+ Zn 2+ Nb 5+ Al 3+ Ti 4+ And so on, anions have F - S 2- Cl - wait.

[0028] In one embodiment of the present invention, during the process of obtaining the lithium iron phosphate precursor doped with metal ions, the average particle size of the primary particles after grinding ranges from 200 to 600 nm; preferably from 300 to 450 nm; and the average particle size of the spherical precursor obtained after spray drying ranges from 5 to 20 μm, preferably from 5 to 15 μm.

[0029] In one embodiment of the present invention, the gas flow rate of the inert atmosphere or reducing atmosphere is 1-5 L / min.

[0030] In one embodiment of the present invention, the average particle size of the obtained LiFePO4 / C composite material doped with metal ions ranges from 300 to 500 nm, and the compaction density is 2.2 to 2.5 g / cm³. 3 .

[0031] The present invention further provides a LiFePO4 / C composite material doped with metal ions with high sphericity and compaction density prepared by the above method.

[0032] The present invention further provides the application of the LiFePO4 / C composite material with high sphericity and compaction density prepared by the above method in the preparation of lithium-ion batteries, wherein the LiFePO4 / C composite material with metal ions is used as a positive electrode material.

[0033] The present invention calcines a lithium iron phosphate precursor doped with specific metal ions. The calcination process provided by the present invention sequentially goes through a heating stage, a cooling stage and a isothermal stage, and finally obtains a LiFePO4 / C composite material doped with metal ions with reasonable particle size distribution and high compaction density.

[0034] This invention introduces metal ions into the lithium iron phosphate lattice. The resulting lattice distortion and bonding effect of the dopant ions alter the nucleation and crystal growth activation energy of lithium iron phosphate, thereby affecting the heat and mass transfer rates of the precursor at various temperatures during calcination, and consequently influencing the crystal nucleation and growth rates. Therefore, by designing calcination temperature curves based on the mechanism of action of the dopant ions, it is possible to control the high-temperature solid-state reaction rate and the nucleation and growth rates of lithium iron phosphate, resulting in a LiFePO4 / C composite material doped with metal ions that exhibits a reasonable particle size distribution, high compaction density, and excellent electrical properties.

[0035] This invention studies the influence of ion doping on the growth law of lithium iron phosphate crystals, reveals the correlation between the influence of ion doping on the morphology of lithium iron phosphate and its influence on electrical properties, and formulates a calcination curve control scheme to achieve the control of the particle size and distribution of lithium iron phosphate during calcination, thereby obtaining a LiFePO4 / C composite material doped with metal ions with high compaction density and good electrical properties.

[0036] The method for preparing LiFePO4 / C composite materials with high sphericity and compaction density doped with metal ions provided by this invention has the following significant characteristics:

[0037] 1. The method of this invention adjusts the calcination curve of the precursor according to the type and amount of doped ions. The calcination process involves heating, cooling, and holding stages, changing the residence time distribution of particles with temperature changes at each stage, thereby adjusting the solid-phase reaction rate of the precursor, the nucleation rate of lithium iron phosphate, and the crystal growth rate, and achieving the control of the morphology and particle size distribution of lithium iron phosphate.

[0038] 2. This invention does not simply regulate the heating rate during calcination based on segmented calcination at different temperatures. Instead, it is based on the type of dopant ions in the calcination precursor and their influence on the reaction, phase transition, and crystal growth during calcination, while also considering the precursor particle size range to design the sintering curve. Notably, it incorporates a rapid cooling process from a high-temperature range (700-810℃) to a medium-temperature range (500-650℃), followed by a isothermal calcination step within the medium-temperature range. During the heating phase, in the 25-450℃ range, iron phosphate reacts with lithium carbonate to form lithium iron phosphate, while the carbon source (e.g., glucose) decomposes to form carbon coatings on the particle surface. In the 450-(700-810)℃ range, rapid heating accelerates the crystal growth rate, increasing the particle size difference. Subsequently, in the (700-810)-(500-650)℃ range, rapid cooling is used to reduce the crystal growth rate, preventing further rapid particle growth and increasing the proportion of micron-sized large particles. Isothermal calcination at a moderate temperature (500-650)℃ is more conducive to the fusion and growth of small-diameter particles. This solid-phase crystallization aging process can further regulate the particle morphology and optimize the particle size distribution of LiFePO4 / C composite materials doped with metal ions, based on the particle size differences formed during the heating process.

[0039] This invention is based on the influence of doping ions on the lattice distortion and bonding of lithium iron phosphate, which changes the solid-state reaction, crystal nucleation and growth rate of the precursor during calcination. It correlates and controls ion doping with particle size and distribution optimization. While introducing metal ions to improve electrical performance, it further improves the morphology of the metal ion-doped LiFePO4 / C composite material and increases its compaction density. It is a preparation process method that can directionally control the material morphology, which is different from the existing technology.

[0040] Compared with existing technologies, this invention links the calcination temperature setting with the metal ions doped in the lithium iron phosphate precursor. Rapid cooling after high-temperature calcination followed by isothermal calcination further regularizes the particle morphology and optimizes the particle size distribution of lithium iron phosphate, building upon the particle size differences formed during the heating process. Based on the process control method of this invention, particles with a diameter range of 300-500 nm and a compaction density of 2.2-2.5 g / cm³ can be prepared. 3 The optimized particle size distribution and high compaction density of the metal-doped LiFePO4 / C composite material enable the regulation of lithium iron phosphate particle size and distribution during calcination. When assembled into a button cell, the metal-doped LiFePO4 / C composite material achieves a specific capacity of 162.6 mAh / g at 0.1C discharge and 155.8 mAh / g at 1C discharge. Attached Figure Description

[0041] Figure 1 LiFe in Example 11-y Ti y Relationship between PO4 / C particle size and CSD value and titanium doping content;

[0042] Figure 2 LiFe in Example 1 1-y Ti y Rate performance of PO4 / C samples;

[0043] Figure 3 Example 2 LiFe 1-y Mn y Relationship between PO4 / C particle size and CSD value and manganese doping amount;

[0044] Figure 4 Example 2 LiFe 1-y Mn y Rate performance of PO4 / C samples;

[0045] Figure 5 Example 3 LiFe 1-y Mg y Relationship between PO4 / C particle size and CSD value and magnesium doping amount;

[0046] Figure 6 Example 3 LiFe 1-y Mg y Rate performance of PO4 / C samples;

[0047] Figure 7 Example 4 Li 1-x Al x Relationship between FePO4 / C particle size and CSD value and aluminum doping amount;

[0048] Figure 8 Example 4 Li 1-x Al x Rate performance of FePO4 / C samples;

[0049] Figure 9 Li in Examples 5, 6, and 7 1-x Al x Fe 1-y-z Mn y Ti z Rate performance of PO4 / C;

[0050] Figure 10 Li in Examples 5, 6, and 7 1-x Al x Fe 1-y-z Mn y Ti z Impedance properties of PO4 / C. Detailed Implementation

[0051] The main procedures for preparing LiFePO4 / C composite materials doped with metal ions using the high-temperature solid-state method include: preparation and mixing of reactants, spray drying of the reaction slurry to obtain a calcination precursor, calcination of the precursor to obtain LiFePO4 / C composite materials doped with metal ions with high sphericity and compaction density; performance testing, and fabrication of button batteries using the LiFePO4 / C composite materials doped with metal ions to test their electrical performance.

[0052] This invention provides a method for preparing LiFePO4 / C composite materials with controlled morphology. Based on the type and amount of doped ions, a calcination curve is set, and temperature control is used during the heating and cooling processes to regulate the solid-phase chemical reaction, crystal nucleation, and crystal growth rate, thereby achieving the adjustment of the particle size and particle size distribution of lithium iron phosphate particles.

[0053] The specific steps are as follows:

[0054] Take 0.4 mol of iron phosphate and mix the metal ion dopant with phosphorus source, lithium source, iron source and carbon source according to the elemental molar ratio Li:Al:Fe:M:N:P:O=(1-x):x:(1-yz):y:z:1:4. Add 250 ml of ultrapure water to a zirconium oxide ball mill jar and ball mill at 450 r / min for 3-5 h in a planetary ball mill. After ball milling, spray dry the slurry to obtain precursor powder.

[0055] The precursor was placed in a tube furnace, N2 protection was turned on, and the flow rate was adjusted to 1-5 L / min. After standing for 0.5 h, the temperature was first increased to 400-450 °C at a heating rate of 5-10 °C / min, and then increased to 750-810 °C at a heating rate of 10-30 °C / min, held for 80-200 min. Then the calcination temperature was reduced to 500-650 °C at a rate of 20-50 °C / min, and calcined at a constant temperature of 500-650 °C for 300-600 min. After calcination, the product powder was allowed to cool to room temperature before being removed, thus obtaining the LiFePO4 / C composite material sample doped with metal ions.

[0056] The LiFePO4 / C composite material doped with metal ions was pulverized and then subjected to SEM, particle size and compaction density determination.

[0057] The electrical performance of button cells was determined by assembling them: The prepared LiFePO4 / C sample doped with metal ions was mixed with acetylene black and polyvinylidene fluoride (PVDF) in a mass ratio of 90:5:5, along with an appropriate amount of N-methylpyrrolidone (NMP) in a homogenizer to obtain an electrode slurry. Cut aluminum foil was laid flat on a coater, wiped clean with alcohol, ensuring no air bubbles between the foil and the coater. The electrode slurry was then evenly coated onto the flat aluminum foil using the coater. The positive electrode sheet was placed in a vacuum drying oven and dried at 120°C for 3 hours. It was then cut into 14mm diameter circles using a cutting machine, and the weight of the electrode active material was recorded. Finally, the electrodes were transferred to a glove box under argon atmosphere protection for button cell assembly. In the following examples, CR2032 coin cells were used, with a lithium metal sheet as the negative electrode and 1 mol / L LiPF6 dissolved in a 1:1 volume ratio of ethylene carbonate (EC) and dimethyl carbonate (DMC) as the electrolyte. The assembled coin cells were compacted and sealed on a packaging machine, and electrochemical tests were performed after standing for 2 hours.

[0058] The voltage range for the electrochemical tests in Examples 1-3 was 2.5-4.2V, the test rates were 0.1C, 0.2C, 0.5C and 1C respectively, and the current range was 0.126-1.26mA.

[0059] The voltage range for the electrochemical tests in Examples 4-6 was 2.0-4.0V, the test rates were 0.1C, 0.2C, 0.5C and 1C respectively, and the current range was 0.135-1.35mA.

[0060] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.

[0061] Example 1: Lithium iron phosphate was prepared from a TiO2-doped lithium iron phosphate precursor using a calcination curve with controlled heating rate. The calcination endpoint temperature was 800℃.

[0062] Example 2: Lithium iron phosphate was prepared from a lithium iron phosphate precursor doped with manganese ammonium phosphate using a calcination curve with controlled heating rate, and the calcination endpoint temperature was 800℃.

[0063] Example 3: Lithium iron phosphate was prepared from a magnesium oxide-doped lithium iron phosphate precursor using a calcination curve with controlled heating rate, and the calcination endpoint temperature was 800℃.

[0064] Example 4: Lithium iron phosphate was prepared from a lithium iron phosphate precursor doped with aluminum stearate using a calcination curve with controlled heating rate, and the calcination endpoint temperature was 800℃.

[0065] Examples 5-8 describe the preparation of lithium iron phosphate from lithium iron phosphate precursors doped with titanium, magnesium, aluminum, and manganese using calcination curves with controlled heating and cooling rates.

[0066] Example 1:

[0067] The effect of titanium dioxide doping.

[0068] 0.4 mol of ferric phosphate was mixed with ferric phosphate, lithium carbonate, and titanium dioxide in a Li:Fe:Ti:P molar ratio of 1:(1-y):y:1 (y = 0, 0.5%, 0.75%, 1%, 2%). Anhydrous glucose (10% by mass of FePO4) and 250 ml of ultrapure water were added and mixed. The mixture was then ball-milled in a planetary ball mill at 450 r / min for 4.0 h to obtain a ball-milled material with an average particle size of 460 nm. The ball-milled slurry was spray-dried to obtain a precursor powder with an average particle size of 13.8 μm. The precursor was placed in a tube furnace, N2 protection was turned on, and the flow rate was adjusted to 2.8 L / min for calcination. The calcination program was as follows: 25-400℃, heating rate 9℃ / min; 400-800℃, heating rate 15℃ / min; and holding at 800℃ for 300 min. After calcination, the LiFe was removed after the temperature had cooled to room temperature. 1-y Ti y The PO4 / C sample powders were designated as LFP (i.e., LiFePO4 / C material, hereinafter the same), 0.5% Ti-LFP, 0.75% Ti-LFP, 1% Ti-LFP, and 2% Ti-LFP, respectively. After pulverization, the samples were subjected to SEM, particle size analysis, and compaction density determination. LiFe... 1-y Ti y Using PO4 / C as the positive electrode, a CR2032 coin cell was assembled, and its electrical performance was measured.

[0069] The LiFe obtained by calcination 1-y Ti y XRD analysis was performed on PO4 / C, and the diffraction data were fitted to the unit cell parameters. The results are shown in Table 1. With the increase of Ti doping concentration, the a and b axis parameters decreased, while the c axis parameter increased. The overall unit cell volume showed a decreasing trend. This is because Ti has a relatively small ionic radius. 4+ As Fe sites are gradually replaced, the cell volume of the material gradually decreases.

[0070] Table 1. LiFe 1-y Ti y Unit cell parameters of PO4 / C sample

[0071]

[0072]

[0073] Titanium doping amount and LiFe 1-y Ti y The relationship between PO4 / C particle size and CSD value is shown in the figure. Figure 1With increased titanium doping, LiFe 1-y Ti y PO4 / C's D 10 D 50 D 90 Simultaneously, the CSD value also decreased, indicating that appropriate titanium doping is beneficial for improving LiFe. 1-y Ti y The uniformity of PO4 / C particle distribution. This is because Ti 4+ Fe replacement 2+ The shrinkage of the unit cell volume leads to a reduction in particle size; simultaneously, Ti 4+ The metallic bond is slightly stronger than that of Fe. 2+ The metallic bonds strengthen the lattice forces, resulting in smaller particle sizes. With a titanium addition of 0.75%, the particle size distribution is relatively narrow, and the compaction density reaches 2.3701 g / cm³. 3 .

[0074] LiFe with different titanium doping contents 1-y Ti y Rate performance testing was performed on PO4 / C, and the results are as follows: Figure 2 As shown in the figure. The left figure is the 0.5C single-rate cycling graph. After 30 cycles, the discharge specific capacities of LFP, 0.5%Ti-LFP, 0.75%Ti-LFP, 1%Ti-LFP, and 2%Ti-LFP are 143.8 mAh / g, 146.2 mAh / g, 150.4 mAh / g, 147.8 mAh / g, and 143.2 mAh / g, respectively, among which 0.75%Ti-LFP exhibits the best cycling stability. The right figure is the multi-rate cycling graph. Appropriate titanium doping (≤1%) can improve the discharge specific capacity of lithium iron phosphate under fast charge and discharge conditions while maintaining low capacity decay.

[0075] Example 2:

[0076] The effect of manganese doping with ammonium phosphate.

[0077] 0.4 mol of ferric phosphate was mixed with lithium carbonate and manganese ammonium phosphate in a Li:Fe:Mn:P molar ratio of 1:(1-y):y:1 (y = 0.5%, 1%, 1.5%, 2%). Anhydrous glucose (10% by mass of FePO4) and 250 ml of ultrapure water were added and mixed. The mixture was then ball-milled at 450 r / min for 4.0 h in a planetary ball mill to obtain a ball-milled material with an average particle size of 430 nm. The ball-milled slurry was spray-dried to obtain a precursor powder with an average particle size of 15.2 μm. The precursor was placed in a tube furnace, N2 protection was turned on, and the flow rate was adjusted to 2.8 L / min for calcination. The calcination program was as follows: 25-400℃, heating rate 9℃ / min; 400-800℃, heating rate 15℃ / min; and holding at 800℃ for 300 min. After calcination, the LiFe was removed after the temperature had cooled to room temperature. 1- y Mn y PO4 / C sample powders were designated as 0.5% Mn-LFP, 1% Mn-LFP, 1.5% Mn-LFP, and 2% Mn-LFP, respectively. After pulverization, the samples were subjected to SEM, particle size analysis, and compaction density determination. LiFe... 1-y Mn y Using PO4 / C as the positive electrode, a CR2032 coin cell was assembled, and its electrical performance was measured.

[0078] For LiFe 1-y Mn y XRD diffraction data of PO4 / C were fitted to the unit cell parameters (Table 2). It was found that with increasing manganese content, the unit cell parameters a, b, and c, as well as the volume V, showed an increasing trend. This is caused by the unit cell expansion resulting from Mn occupying Fe sites, due to the ionic radius of manganese. Slightly larger than the ionic radius of iron or the ionic radius of lithium

[0079] Table 2. LiFe 1-y Mn y Unit cell parameters of PO4 / C sample

[0080]

[0081] The relationship between manganese doping amount and changes in particle size and CSD value of lithium iron phosphate samples is shown in the figure. Figure 3 LiFe 1-y Mn y The particle size of PO4 / C initially increases and then decreases with increasing manganese content. When the manganese content is 1%, the particle size is relatively larger than that of lithium iron phosphate with other doping amounts, the particle size distribution is relatively narrow, and the compaction density reaches 2.3873 g / cm³. 3 .

[0082] Analysis of LiFe 1-y Mn y The electrical performance of PO4 / C shows that appropriate manganese doping is beneficial to improving the discharge specific capacity and cycle stability of lithium iron phosphate under fast charge-discharge conditions. The charge-discharge performance of the battery is significantly improved at 0.5C and 1C. The cell expansion caused by Mn substitution at Fe sites provides more migration space for lithium ions, reducing the possibility of blockage. The discharge specific capacities of LFP, 0.5% Mn-LFP, 1% Mn-LFP, and 1.5% Mn-LFP after 5 cycles at 1C are 120.07 mAh / g, 125.23 mAh / g, 131.49 mAh / g, and 119.97 mAh / g, respectively. However, at high Mn content, LiFe... 1-y Mn y The PO4 / C composite material has poor kinetics and large lattice distortion, which can easily cause the collapse of lithium-ion migration channels, resulting in excessively rapid capacity decay of the battery.

[0083] Example 3:

[0084] The effect of magnesium oxide doping.

[0085] 0.4 mol of ferric phosphate was mixed with ferric phosphate, lithium carbonate, and magnesium oxide in a Li:Fe:Mg:P molar ratio of 1:(1-y):y:1 (x = 0.5%, 1%, 1.5%, 10%). Anhydrous glucose (10% by mass of FePO4) and 250 ml of ultrapure water were added and mixed. The mixture was then ball-milled at 450 r / min for 3.8 h in a planetary ball mill to obtain a ball-milled material with an average particle size of 470 nm. The ball-milled slurry was spray-dried to obtain a precursor powder with an average particle size of 14.6 μm. The precursor was placed in a tube furnace, N2 protection was turned on, and the flow rate was adjusted to 2.8 L / min for calcination. The calcination program was as follows: 25-400℃, heating rate 9℃ / min; 400-800℃, heating rate 15℃ / min; and holding at 800℃ for 300 min. After calcination, the LiFe was removed after the temperature had cooled to room temperature. 1-y Mg y PO4 / C sample powders were designated as 0.5% Mg-LFP, 1% Mg-LFP, 1.5% Mg-LFP, and 10% Mg-LFP, respectively. After pulverization, the samples were subjected to SEM, particle size analysis, and compaction density determination. LiFe... 1-y Mg y Using PO4 / C as the positive electrode, a CR2032 coin cell was assembled, and its electrical performance was measured.

[0086] Using X-ray diffractometer to study LiFe 1-y Mg yCrystal structure analysis of PO4 / C was performed, and the results are shown in Table 3. Ionic radius of Mg. Compared to the ionic radius of Fe Small, when Mg substitutes for Fe or Li sites, LiFe 1-y Mg y PO4 / C cell shrinks, and the cell volume decreases.

[0087] Table 3. LiFe 1-y Mg y Unit cell parameters of PO4 / C sample

[0088]

[0089] LiFe 1-y Mg y The relationship between PO4 / C particle size and CSD value as a function of magnesium doping is shown in the figure. Figure 5 As the magnesium content in lithium iron phosphate increases, the particle size initially increases and then decreases. Generally, the particle size decreases after adding magnesium because magnesium substitution causes lattice distortion in lithium iron phosphate, reducing the crystal surface energy and thus inhibiting crystal growth. When the magnesium content is 1%, the particle compaction density reaches 2.4035 g / cm³. 3 .

[0090] Depend on Figure 6 Rate cycling performance analysis shows that low magnesium content doping helps delay capacity decay of lithium iron phosphate (LFP) under high-rate conditions, maintaining a high capacity retention rate. The coin cell assembled with 1.5% Mg-LFP material maintained a relatively low internal resistance during cycling, but its discharge specific capacity showed a slow upward trend. After 30 cycles at 0.5C, the capacity retention rate reached 101.1%, surpassing the discharge specific capacity data of the LFP sample after 30 cycles. The multi-rate cycling performance graph shows that as the rate increases, the difference in discharge specific capacity between samples widens. After 5 cycles at 1C, the discharge specific capacities of LFP, 0.5% Mg-LFP, 1% Mg-LFP, 1.5% Mg-LFP, and 10% Mg-LFP were 120.1, 124.0, 128.2, 118.4, and 75.1 mAh / g, respectively, with corresponding capacity retention rates of 76.2%, 78.5%, 81.0%, 76.9%, and 51.2%.

[0091] Example 4:

[0092] The effect of aluminum stearate doping.

[0093] 0.4 mol of ferric phosphate was mixed with ferric phosphate, lithium carbonate, and aluminum stearate in a Li:Al:Fe:P molar ratio of (1-x):x:1:1 (x = 0.5%, 1%, 1.5%, 10%). Anhydrous glucose (10% by mass of FePO4) and 250 ml of ultrapure water were added and mixed. The mixture was then ball-milled at 450 r / min for 3.8 h in a planetary ball mill to obtain a ball-milled material with an average particle size of 450 nm. The ball-milled slurry was spray-dried to obtain a precursor powder with an average particle size of 13.5 μm. The precursor was placed in a tube furnace, N2 protection was turned on, and the flow rate was adjusted to 2.8 L / min for calcination. The calcination program was as follows: 25-400℃, heating rate 9℃ / min; 400-800℃, heating rate 15℃ / min; and holding at 800℃ for 300 min. After calcination, the Li was removed after the temperature had cooled to room temperature. 1-x Al x FePO4 / C sample powders were designated as 0.5% Al-LFP, 1% Al-LFP, 1.5% Al-LFP, and 10% Al-LFP, respectively. After pulverization, the samples were subjected to SEM, particle size analysis, and compaction density determination. Li 1-x Al x FePO4 / C was used as the positive electrode to assemble a CR2032 coin cell, and its electrical performance was measured.

[0094] Table 4 shows the data based on Li 1-x Al x The lattice constants a, b, and cell volume V calculated from the X-ray diffraction data of FePO4 / C all decreased to varying degrees with the increase of aluminum content, indicating that aluminum ions were doped into the lithium iron phosphate lattice.

[0095] Table 4. Li 1-x Al x Lattice parameters of FePO4 / C sample

[0096]

[0097] Li 1-x Al x The relationship between FePO4 / C particle size and aluminum doping concentration is shown in the figure. Figure 7 With increased aluminum content, Li 1- x Al x FePO4 / C D 10 D 50 and D 90 They all decrease sequentially, especially D. 90The decrease in CSD was more significant, indicating that particle growth was significantly suppressed. When the aluminum addition was below 1.5%, the CSD value decreased with increasing aluminum ion doping content, and the particle size distribution tended to be more uniform. When the aluminum addition was 1%, the particle compaction density reached 2.1435 g / cm³. 3 .

[0098] Figure 8 It is Li 1-x Al x The electrical performance test results of FePO4 / C showed that when Al ≤ 1.5%, the capacity decay rate of Al-LFP was slower than that of LFP, indicating that aluminum doping is beneficial to maintaining the cycle performance of the battery. The smaller ionic radius of Al... 3+ It entered the material lattice and replaced Li + The generation of vacancies increases the interstitial space in the crystal lattice, which facilitates the migration of electrons and ions, thereby increasing the electrical conductivity of the material and thus improving the discharge specific capacity. The 1% Al-LFP sample maintained the best electrical performance, with a final discharge specific capacity of 144.8 mAh / g at 0.5C. After 5 cycles at 1C, the electrical performance of pure LFP declined significantly. The discharge specific capacities of LFP, 0.5% Al-LFP, 1% Al-LFP, 1.5% Al-LFP, and 10% Al-LFP were 103.4, 124, 126.6, 123.7, and 121.4 mAh / g, respectively, with corresponding 1C cycle capacity retention rates of 94.68%, 97.79%, 97.23%, 98.33%, and 96.27%.

[0099] Example 5:

[0100] The effect of TiO2 and AlPO4 composite doping.

[0101] 0.4 mol of ferric phosphate was mixed with lithium carbonate, anhydrous glucose (10% of the FePO4 mass), and 250 ml of ultrapure water at a FePO4:Li2CO3 (Fe:Li molar ratio) ratio of 1:1.05. Cations were introduced using TiO2 (0.75% of the FePO4 molar weight) and AlPO4 (0.0067% of the FePO4 molar weight). The mixture was ball-milled at 450 r / min for 5.0 h in a planetary ball mill to obtain a ball-milled material with an average particle size of 362 nm. The ball-milled slurry was spray-dried to obtain a precursor powder with an average particle size of 12 μm. The precursor was then placed in a tube furnace, protected with N2, and calcined at a flow rate of 2.3 L / min. The calcination procedure is as follows: 25-450℃, heating rate 10℃ / min; 450-780℃, heating rate 12℃ / min, holding for 240 min; 780-600℃, cooling rate 25℃ / min, holding for 320 min. After calcination, wait for the temperature to drop to room temperature before removing the Li.0.999933 Al 0.000067 Fe 0.9925 Ti 0.0075 PO4 / C powder was pulverized and then subjected to SEM, particle size analysis, and compaction density determination. Li 0.99993 3Al 0.000067 Fe 0.9925 Ti 0.0075 Using PO4 / C as the positive electrode, a CR2032 coin cell was assembled, and its electrical performance was measured.

[0102] In this embodiment, the average particle size of the precursor after grinding was 460 nm. Calcination was performed using a segmented controlled heating and cooling rate mode: 25-450℃, heating rate 10℃ / min; 450-780℃, heating rate 12℃ / min, holding time 240 min; 780-600℃, cooling rate 25℃ / min, holding time 320 min. The prepared LiFePO4 / C had an average particle size of 360 nm, a sphericity of 0.9714, and a compaction density of 2.3031 g / cm³. 3 .

[0103] This embodiment Li 0.999933 Al 0.000067 Fe 0.9925 Ti 0.0075 The coin cell assembled with PO4 / C material has a discharge capacity of 162.6 mAh g at 0.1C under voltages of 2.0-4.0V. -1 The 0.2C discharge capacity is 161.5 mAh g. -1 The 0.5C discharge capacity is 158.9 mAh g. -1 The 1C discharge capacity is 155.8 mAh g. -1 The capacity retention rate of 1C 4-cycle reached 99.93%.

[0104] Example 6:

[0105] The effect of TiO2 and AlPO4 composite doping.

[0106] 0.4 mol of ferric phosphate was mixed with lithium carbonate, anhydrous glucose (10% of the FePO4 mass), and 250 ml of ultrapure water at a FePO4:Li2CO3 (Fe:Li molar ratio) ratio of 1:1.2. Cations were introduced using TiO2 (0.375% of the FePO4 molar weight) and AlPO4 (0.75% of the FePO4 molar weight). The mixture was ball-milled at 450 r / min for 5.0 h in a planetary ball mill to obtain a ball-milled material with an average particle size of 415 nm. The ball-milled slurry was spray-dried to obtain a precursor powder with an average particle size of 12.5 μm. The precursor was then placed in a tube furnace, protected with N2, and calcined at a flow rate of 2.5 L / min. The calcination procedure is as follows: 25-450℃, heating rate 8℃ / min; 450-800℃, heating rate 15℃ / min, holding for 240min; 800-550℃, cooling rate 30℃ / min, holding for 280min. After calcination, wait for the temperature to drop to room temperature before removing the Li. 0.9925 Al 0.0075 Fe 0.99625 Ti 0.00375 PO4 / C product powder was pulverized and then subjected to SEM, particle size analysis, and compaction density determination. Li 0.9925 Al 0.0075 Fe 0.99625 Ti 0.00375 Using PO4 / C as the positive electrode, a CR2032 coin cell was assembled, and its electrical performance was measured.

[0107] In this embodiment, the average primary particle size of the precursor after grinding was 415 nm. Calcination was performed using a segmented controlled heating and cooling rate mode: 25-450℃, heating rate 8℃ / min; 450-800℃, heating rate 15℃ / min, holding time 240 min; 800-550℃, cooling rate 30℃ / min, holding time 280 min. The prepared Li... 0.9925 Al 0.0075 Fe 0.99625 Ti 0.00375 The average particle size of PO4 / C is 390 nm, the sphericity is 0.9542, and the compacted density is 2.2861 g / cm³. 3 .

[0108] This embodiment Li 0.9925 Al 0.0075 Fe 0.99625 Ti 0.00375 The coin cell assembled with PO4 / C material has a 0.1C discharge capacity of 161.4 mAh g at a voltage of 2.0-4.0V. -1 The 0.2C discharge capacity is 159.6 mAh g. -1 The 0.5C discharge capacity is 157.7 mAh g.-1 The 1C discharge capacity is 153.6 mAh g. -1 The capacity retention rate of 1C 4-cycle was 100%.

[0109] Example 7:

[0110] The effect of MnHPO4, TiO2, and AlPO4 composite doping (the average particle size of the mixture in the first stage is 390 nm, and the average particle size of the precursor powder after spray drying is 14.0 μm) includes cooling and mid-stage heat preservation.

[0111] 0.4 mol of ferric phosphate was mixed with lithium carbonate, anhydrous glucose (10% of the mass of FePO4), and 250 ml of ultrapure water at a FePO4:Li2CO3 (Fe:Li molar ratio) ratio of 1:1.1. Cations were introduced using dopants MnHPO4 (0.5% of the molar mass of FePO4), TiO2 (0.375% of the molar mass of FePO4), and AlPO4 (0.75% of the molar mass of FePO4). The mixture was ball-milled at 450 r / min for 5.0 h in a planetary ball mill to obtain a ball-milled material with an average particle size of 390 nm. The ball-milled slurry was then spray-dried to obtain a precursor powder with an average particle size of 14.0 μm.

[0112] The precursor was placed in a tube furnace, N2 protection was turned on, and the flow rate was adjusted to 2.2 L / min for calcination. The calcination program was as follows: 25-450℃, heating rate 10℃ / min; 400-800℃, heating rate 20℃ / min, holding time 280 min; 800-600℃, cooling rate 35℃ / min, holding time 400 min. After calcination, the LiFePO4 / C product powder was removed after the temperature had cooled to room temperature. The sample was then pulverized and subjected to SEM, particle size, and compaction density determination. (The text abruptly ends here, likely due to an incomplete sentence or missing information.) 0.9925 Al 0.0075 Fe 0.99125 Mn 0.005 Ti 0.0037 Using 5PO4 / C as the positive electrode, a CR2032 coin cell was assembled, and its electrical performance was measured.

[0113] In this embodiment, the average primary particle size of the precursor after grinding was 390 nm. Calcination was performed using a segmented controlled heating and cooling rate mode: 25-450℃, heating rate 10℃ / min; 450-800℃, heating rate 20℃ / min, holding time 280 min; 800-600℃, cooling rate 35℃ / min, holding time 400 min. The prepared Li... 0.9925 Al 0.0075 Fe 0.99125 Mn 0.005 Ti 0.00375The average particle size of PO4 / C is 395 nm, the sphericity is 0.9603, and the compacted density is 2.3556 g / cm³. 3 .

[0114] This embodiment Li 0.9925 Al 0.0075 Fe 0.99125 Mn 0.005 Ti 0.00375 The coin cell assembled with PO4 / C material has a discharge capacity of 160.5 mAh g at 0.1C under voltages of 2.0-4.0V. -1 The 0.2C discharge capacity is 158.7 mAh g. -1 The 0.5C discharge capacity is 157.6 mAh g. -1 The 1C discharge capacity is 154.2 mAh / g. -1 The capacity retention rate of 1C 4-cycle reached 99.61%.

[0115] Li in Examples 5, 6 and 7 1-x Al x Fe 1-y-z Mn y Ti z PO4 / C rate cycle capacity performance such as Figure 9 As shown, Examples 5, 6, and 7 demonstrate the improvement of the discharge specific capacity of LFP materials (i.e., LiFePO4 / C materials) by dopants to varying degrees, with Example 5 showing the best gain.

[0116] Impedance properties such as Figure 10 As shown, the impedances of Examples 5 and 6 are both less than that of the LFP, while the impedance of Example 7 is slightly greater than that of the LFP. This data also confirms the improvement in discharge specific capacity of Examples 5 and 6.

[0117] The calcination temperature control methods of the above different embodiments and Li 1-x Al x Fe 1-y-z Mn y Ti z The average particle size, compaction density, and 1C discharge specific capacity of PO4 / C are summarized in Table 5.

[0118] Table 5. Calcination temperature control methods and Li in different embodiments 1-x Al x Fe 1-y-z Mn y Ti z Table of average particle size, compaction density, and 1C discharge specific capacity data for PO4 / C

[0119]

[0120]

[0121] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a LiFePO4 / C composite material doped with metal ions, characterized in that, The specific steps are as follows: The precursor of lithium iron phosphate doped with metal ions was calcined to obtain a LiFePO4 / C composite material doped with metal ions with high sphericity and compaction density. The calcination process involves sequentially going through a heating stage, a cooling stage, and a isothermal stage under an inert or reducing atmosphere. (1) Heating section: The temperature rises from room temperature to the calcination endpoint temperature. The heating rate from room temperature to 450 ℃ is 5-10 ℃ / min. The heating rate from 450 ℃ to the calcination endpoint temperature is 10-30 ℃ / min. After reaching the calcination endpoint temperature, the temperature is held for 240 min, 280 min or 300 min. In the 25-450 ℃ section, iron phosphate reacts with lithium carbonate to generate lithium iron phosphate. At the same time, the carbon source decomposes to form carbon coating on the surface of the particles. In the 450 ℃ to calcination endpoint temperature section, the crystal growth rate is accelerated by rapid heating, which increases the particle size difference between particles. (2) Cooling section: The temperature is reduced from the calcination endpoint temperature to the calcination intermediate temperature. The cooling rate is 10-50 ℃ / min. The cooling section adopts rapid cooling to reduce the growth rate of crystals in order to avoid further rapid growth of particles and increase the proportion of micron-sized large particles. (3) Constant temperature section, the temperature is maintained at the medium temperature of calcination, and the residence time is 200-600 min. Constant temperature calcination is conducive to the fusion and growth of particles with small particle size. This solid-phase crystallization aging process can further regulate the particle morphology and optimize the particle size distribution of LiFePO4 / C composite material doped with metal ions based on the particle size difference formed during the heating process. The room temperature is 25 ℃, the calcination endpoint temperature is 700-810 ℃, and the calcination intermediate temperature is 500-650 ℃; The precursor of lithium iron phosphate is obtained by mixing a metal ion dopant with a phosphorus source, a lithium source, an iron source and a carbon source in the following proportions, with an elemental molar ratio of Li:Al:Fe:M:N:P:O=(1-x):x:(1-yz):y:z:1:4, adding a grinding media for grinding, and then spray drying to form a precursor of lithium iron phosphate doped with metal ions. The LiFePO4 / C composite material doped with metal ions includes lithium iron phosphate particles doped with metal ions and a carbon layer coated on the surface of the lithium iron phosphate particles. The metal ions are selected from one or more of Mg, Mn, Zr, Co, V, Zn, Nb, Al or Ti; In the LiFePO4 / C composite material doped with metal ions, One or both of the iron and lithium sites in lithium iron phosphate are partially replaced by doped metal ions. The molecular formula of the LiFePO4 / C composite material doped with metal ions is: Li 1-x A x Fe 1-y B y PO4 / C; wherein A and B are independently selected from one or more of Mg, Mn, Zr, Co, V, Zn, Nb, Al or Ti, 0≤x<1%, 0≤y<1%, and x and y are not simultaneously 0; The resulting LiFePO4 / C composite materials doped with metal ions had an average particle size range of 300-500 nm and a compaction density of 2.2-2.5 g / cm³. 3 .

2. The method for preparing a LiFePO4 / C composite material doped with metal ions according to claim 1, characterized in that, The molecular formula of the LiFePO4 / C composite material doped with metal ions is: Li 1-x Al x Fe 1-y-z M y N z PO4 / C, M and N are independently selected from one or more of Mg, Mn or Ti, Al is aluminum, 0≤x≤1.5%, 0≤y≤1%, 0≤z≤1%.

3. The method for preparing a LiFePO4 / C composite material doped with metal ions according to claim 1, characterized in that, The lithium source is selected from at least one of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, lithium phosphate, lithium acetate, or lithium oxalate; the iron source is selected from at least one of iron phosphate, iron oxide, iron pyrophosphate, or ferrous oxalate; the phosphorus source is selected from at least one of phosphoric acid, iron phosphate, iron pyrophosphate, or lithium dihydrogen phosphate; and the carbon source is selected from at least one of sucrose, glucose, starch, or polyvinyl alcohol. The metal ion dopant is selected from oxides, phosphates, sulfates, or organic compounds containing one or more of the elements Mg, Mn, Zr, Co, V, Zn, Nb, Al, or Ti.

4. The method for preparing a LiFePO4 / C composite material doped with metal ions according to claim 1, characterized in that, In the process of obtaining the lithium iron phosphate precursor doped with metal ions, the average particle size of the primary particles after grinding ranges from 200 to 600 nm; the average particle size of the spherical precursor obtained after spray drying ranges from 5 to 20 μm.

5. The method for preparing a LiFePO4 / C composite material doped with metal ions according to claim 4, characterized in that, In the process of obtaining the lithium iron phosphate precursor doped with metal ions, the average particle size of the primary particles after grinding ranges from 300 to 450 nm; the average particle size of the spherical precursor obtained after spray drying ranges from 5 to 15 μm.

6. The method for preparing a LiFePO4 / C composite material doped with metal ions according to claim 1, characterized in that, The gas flow rate of the inert or reducing atmosphere is 1-5 L / min.

7. A LiFePO4 / C composite material with high sphericity and compaction density doped with metal ions, prepared by the method according to any one of claims 1-6.

8. The application of the high sphericity and compaction density LiFePO4 / C composite material doped with metal ions, prepared by the method according to any one of claims 1-7, in the preparation of lithium-ion batteries, characterized in that, The LiFePO4 / C composite material doped with metal ions is used as the positive electrode material.

Citation Information

Patent Citations

  • Lithium iron phosphate positive electrode material and preparation method and application thereof

    CN117080436A

  • Preparation method of lithium iron phosphate positive electrode material, positive electrode material and battery

    CN117263157A

  • Lithium iron phosphate material and preparation method thereof, positive pole piece and secondary battery

    CN117558915A

  • Method for preparing spherical LFP (lithium iron phosphate) / carbon doped composite powder