Battery negative electrode material and preparation method thereof and lithium ion battery
By using heat treatment and vapor deposition processes containing lithium compounds and doping elements in lithium-ion batteries to prepare nano-silicon battery anode materials, and performing carbon coating and demagnetization, the problems of expansion and safety hazards of silicon-based anode materials are solved and achieved High-efficiency, long-life battery performance.
Patent Information
- Application Number
- CN202411025787.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing silicon-based negative electrode materials expand greatly during the charging process, resulting in a decrease in cycle performance, and the preparation of small nanometer silicon particles has safety hazards and performance deterioration problems.
By mixing the lithium-containing compound and the target doping element compound in a preset ratio and then performing heat treatment, a dispersed carrier precursor is obtained, which is then vapor-deposited with silicon powder in proportion to prepare the nano-silicon battery negative electrode material, and under an inert atmosphere Carry out carbon coating and demagnetization to obtain stable and evenly dispersed nano-silicon battery negative electrode materials.
It achieves high first Coulombic efficiency, long cycle performance and stable dispersion of nano-silicon battery anode materials, avoids safety hazards and performance degradation in aqueous pulping, and improves the energy density and cycle life of the battery.
Smart Images

Figure CN118545730B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a battery negative electrode material and a preparation method thereof, and a lithium ion battery. Background Art
[0002] Silicon-based negative electrode materials are ideal next-generation negative electrode materials. The specific capacity of pure Si-based negative electrode materials is 10 times that of graphite, but pure Si expands by nearly 300% during the charging process, which greatly reduces its cycle performance in the battery. Studies have shown that when the size of silicon nanoparticles is less than 50nm, its expansion during the charging and discharging process can be significantly inhibited. However, the smaller the silicon nanoparticles, the more active their chemical properties are and the easier they are to be oxidized by air, water, etc., which poses a safety hazard. In addition, the smaller the nano-silicon, the easier it is to agglomerate, resulting in performance deterioration at the battery cell level. Therefore, how to prepare smaller nano-silicon particles and disperse them stably and evenly is the technical difficulty of the current silicon negative electrode. Summary of the invention
[0003] In view of at least some of the problems and shortcomings in the prior art, the embodiments of the present invention disclose a method for preparing a battery negative electrode material, a battery negative electrode material and a lithium ion battery, which have the advantages of high initial efficiency, long cycle and uniform dispersed phase.
[0004] On the one hand, an embodiment of the present invention provides a method for preparing a negative electrode material for a battery, comprising:
[0005] Step S1: mixing lithium-containing compound powder and target doping element compound powder in a first preset ratio and then subjecting the mixture to heat treatment to obtain a dispersed carrier precursor; the target doping element compound contains lithium;
[0006] Step S2: the dispersed carrier precursor and silicon powder are mixed evenly according to a second preset ratio and then subjected to vapor deposition treatment to obtain the nano-silicon battery negative electrode material.
[0007] In one embodiment of the present invention, the doping elements in the target doping element compound include any one or more of boron, phosphorus, sulfur, molybdenum, tungsten, titanium, aluminum, bromine, fluorine, and iodine; the target doping element compound powder includes any one or more of lithium borate powder, lithium aluminate powder, lithium phosphate powder, lithium tungstate powder, and lithium sulfide powder.
[0008] In one embodiment of the present invention, the lithium-containing compound includes: one or more of lithium acetate, lithium sulfite, lithium tetrafluoroborate, lithium citrate, lithium hydroxide, lithium oxide, lithium nitride, lithium nitrate, lithium chloride, lithium bromide, lithium borate, lithium lactate, lithium sulfide, lithium sulfate, lithium iodide, lithium iodate, lithium carbonate, lithium bicarbonate, lithium oxalate, lithium peroxide, lithium tungstate, lithium aluminate, lithium tantalate, lithium chromate, lithium manganate, spodumene, lithium mica, petalite, eucryptite, lithium beryllite, lithium phosphate aluminum, hectorite, jaddarite, iron lithium mica, and lithium cryolite.
[0009] In one embodiment of the present invention, the first preset ratio is the ratio of the mass of the lithium-containing compound powder to the mass of the target doping element compound powder, and the range of the first preset ratio is 0.01% to 40%;
[0010] The second preset ratio is the mass ratio of the dispersed carrier precursor to the silicon powder, and the range of the second preset ratio is 35% to 65%.
[0011] In one embodiment of the present invention, the step S1 specifically comprises: obtaining a first mixture after the heat treatment, crushing and screening the first mixture to obtain the dispersed carrier precursor;
[0012] The step S2 specifically includes: obtaining a second mixture after the vapor deposition process, and crushing and screening the second mixture to obtain the nano-silicon battery negative electrode material.
[0013] In one embodiment of the present invention, the temperature of the heat treatment is 500°C to 950°C; the temperature of the vapor deposition treatment is 900°C to 2650°C; and the reaction time of the heat treatment and the vapor deposition treatment is 0.5h to 10h.
[0014] In one embodiment of the present invention, the average particle size of the lithium-containing compound powder, the target doping element compound powder, the dispersed carrier precursor, the silicon powder and the nano-silicon battery negative electrode material is 2um to 7um.
[0015] In one embodiment of the present invention, the preparation method further comprises S3: carbon coating the nano-silicon battery negative electrode material under an inert atmosphere and screening and demagnetizing the carbon-coated battery negative electrode material to obtain the coated battery negative electrode material.
[0016] On the other hand, an embodiment of the present invention provides a battery negative electrode material, including a nano-silicon battery negative electrode material prepared by any of the aforementioned methods.
[0017] On the other hand, an embodiment of the present invention provides a lithium-ion battery, comprising the aforementioned battery negative electrode material.
[0018] It can be seen from the above that the above technical features of the present invention can have one or more of the following beneficial effects:
[0019] 1. The nano silicon battery negative electrode material obtained by the preparation method of the target doping element compound containing lithium element comprises a doped and modified lithium silicate phase, which has the characteristic of being insoluble in water, and effectively avoids the problems generated in the aqueous phase pulping process.
[0020] 2. The preparation method in this application maximizes the capacity of the silicon negative electrode and improves the first coulombic efficiency and cycle performance of the silicon negative electrode by effectively controlling the proportional process.
[0021] 3. Nano-silicon battery negative electrode material has the characteristics of high modulus, high strength and rapid ion conductivity, which effectively realizes the stable dispersion of nano-silicon and avoids agglomeration in the later stage.
[0022] 4. The preparation process of the present application successfully achieves the preparation of low-sized nano-silicon particles, and the preparation process is low-cost, does not contain flammable and explosive substances, has high process controllability, and is easy to achieve large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0024] Figure 1 A schematic diagram of a process for preparing a negative electrode material for a battery provided by an embodiment of the present invention;
[0025] Figure 2 This is the X-ray diffraction pattern of the negative electrode material prepared in Example 1 of the present invention;
[0026] Figure 3 This is a scanning electron microscope image of the negative electrode material prepared in Example 1 of the present invention;
[0027] Figure 4 This is a scanning electron microscope cross-sectional view of the negative electrode material prepared in Example 1 of the present invention;
[0028] Figure 5 This is a scanning electron microscope cross-sectional EDS image of the negative electrode material prepared in Example 1 of the present invention;
[0029] Figure 6 This is the first charge and discharge diagram of the button-type lithium-ion secondary battery prepared in Example 1 of the present invention;
[0030] Figure 7The AC impedance comparison between Example 1 of the present invention and Comparative Examples 5 and 6;
[0031] Figure 8 Comparison of the slurry conditions at high temperature and the pH value of the powder solution of the embodiment provided in the present invention and the comparative example;
[0032] Fig. 9 The ICP test results of the embodiments and comparative examples provided in the embodiments of the present invention are as follows: doping element content, first discharge capacity, first coulomb efficiency, and capacity retention rate after 100 cycles and 300 cycles. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0035] It should also be noted that the division of multiple embodiments in the present invention is only for the convenience of description and should not constitute a special limitation. The features in various embodiments can be combined and referenced to each other without contradiction.
[0036] See also Figure 1 , a method for preparing a negative electrode material for a battery provided by an embodiment of the present invention comprises the following steps:
[0037] Step S1: mixing lithium-containing compound powder and target doping element compound powder in a first preset ratio and then subjecting the mixture to heat treatment to obtain a dispersed carrier precursor; the target doping element compound contains lithium;
[0038] Step S2: uniformly mixing the dispersed carrier precursor and silicon powder according to a second preset ratio and subjecting the mixture to a vapor deposition treatment to obtain a nano-silicon battery negative electrode material.
[0039] Exemplarily, the mixing equipment used for uniform mixing in the above steps S1 and S2 includes: a mixer with a plowshare, a V-shaped mixer, a fusion machine, and a ball mill.
[0040] In the related technology, silane is used as the silicon source, and then the generated nano-silicon is deposited on the surface or in the pores of the carbon substrate by high-temperature cracking, so as to prepare high-capacity and high-initial-efficiency silicon-carbon negative electrode materials. However, in actual operation, the selection of gases such as silane has a very high safety risk factor. Silane is flammable and explosive. During the operation, the slightest carelessness may cause a violent reaction, which can easily lead to serious safety accidents such as casualties.
[0041] It is worth mentioning that silicon powder is used as the silicon source in this scheme. The chemical properties of silicon powder are relatively stable. It is not as flammable and explosive as silane, which reduces the risk of dangerous accidents during storage, transportation and use, and effectively protects the life safety of operators and the safety of the production environment; silicon powder is usually easier to obtain and relatively cheap, which can reduce the procurement cost of raw materials, thereby improving the economic benefits of the entire production process; secondly, the composition of silicon powder is relatively simple and stable, and it is easier to control the reaction conditions during the production process, which is conducive to ensuring the stability and consistency of product quality. In large-scale production, it can effectively avoid production interruptions caused by safety issues such as silane leakage, and can reduce production costs, improve production efficiency and product quality reliability.
[0042] In an embodiment of the present application, the doping elements in the target doping element compound include: any one or more of boron (B), phosphorus (P), sulfur (S), molybdenum (Mo), tungsten (W), titanium (Ti), aluminum (Al), bromine (Br), fluorine (F), and iodine (I).
[0043] In an embodiment of the present application, the target doping element compound powder includes any one or more of lithium borate powder, lithium aluminate powder, lithium phosphate powder, lithium tungstate powder, and lithium sulfide powder.
[0044] Specifically, the target doping element compound is a compound with a non-positive molar ratio, and the doped elements cover a wide range from -1 valence state to positive 7 valence state, specifically including one or more of B, P, S, Mo, W, Ti, Al, Br, F, and I. Through the doping of elements, a structure with higher modulus and better thermal stability is successfully achieved. Among the many doping elements, the doping effects of B, Ti, and Al are particularly ideal and are preferred.
[0045] For example, the doping of B element can significantly enhance the hardness and strength of modified silicate; the addition of Ti element can improve the high temperature resistance of the material and further enhance the thermal stability; the incorporation of Al element helps to optimize the crystal structure, making its overall performance more superior.
[0046] It is worth mentioning that in the relevant technology, since lithium silicate and lithium silicate doped with alkali metal or alkaline earth metal are soluble in aqueous conditions, water can still penetrate into the interior of the carbon layer even after coating. In the slurrying process of the negative electrode material under aqueous conditions, water will corrode and dissolve lithium silicate, causing the nano-silicon in the dispersed phase to come into contact with water and react to generate hydrogen. When used in large quantities, there are safety hazards, and the oxidation of nano-silicon by water will also lead to a decrease in the initial coulomb efficiency of the material and a decrease in performance. In addition, the unstable silicate phase will become alkaline after hydrolysis. Excessive alkalinity will cause the SBR in the battery slurry to fail and reduce the suspension capacity of CMC, thereby causing the slurry to settle.
[0047] In the present application, the target doping element compound containing lithium element is subjected to the preparation method of the present invention, and the obtained nano silicon battery negative electrode material comprises a lithium silicate phase after doping modification, which has the characteristic of being insoluble in water, effectively preventing water from corroding and dissolving the dispersed phase, ensuring the structural integrity and stability of the silicate phase, thereby ensuring the consistency and reliability of the material performance. In the long-term use process, the material performance will not gradually decline due to the effect of water. The potential safety hazards caused by problems in the aqueous phase pulping process are avoided. The situation in which dangerous gases such as hydrogen are generated due to the reaction of water and the dispersed phase is avoided, which greatly improves the safety during production and use. At the same time, the first-effect coulomb efficiency of the material is significantly improved, so that the battery can store and release energy more efficiently. Secondly, the effectiveness of SBR in the battery slurry and the suspension capacity of CMC are also guaranteed, which effectively prevents the slurry from settling, thereby maintaining the uniformity and stability of the slurry, and providing good basic conditions for subsequent production processes. In large-scale battery production, the advantage of the water-insoluble dispersed phase stabilized by doping can significantly reduce the defective rate, improve production efficiency, and reduce production costs. The battery can also extend its service life during actual application.
[0048] In an embodiment of the present application, the lithium-containing compound includes: one or more of lithium acetate, lithium sulfite, lithium tetrafluoroborate, lithium citrate, lithium hydroxide, lithium oxide, lithium nitride, lithium nitrate, lithium chloride, lithium bromide, lithium borate, lithium lactate, lithium sulfide, lithium sulfate, lithium iodide, lithium iodate, lithium carbonate, lithium bicarbonate, lithium oxalate, lithium peroxide, lithium tungstate, lithium aluminate, lithium tantalate, lithium chromate, lithium manganate, spodumene, lithium mica, lithium feldspar, eucryptite, lithium beryllite, lithium phosphate aluminum stone, hectorite, jaddarite, iron lithium mica, and lithium cryolite.
[0049] Specifically, spodumene, lepidolite, petalite, eucryptite, lithium borate, and lithium aluminate are preferably selected.
[0050] It is worth mentioning that lithium ions in a variety of lithium-containing compounds can be more embedded and extracted during the charge and discharge process, thereby increasing the capacity of the battery. Some compounds such as lithium carbonate and lithium borate help to form a stable solid electrolyte interface (SEI) film, reduce the capacity decay of the electrode during the cycle, and increase the cycle life of the battery. Some compounds such as lithium tetrafluoroborate and lithium chloride can increase the ionic conductivity of the electrolyte, allowing lithium ions to be quickly transmitted during the charge and discharge process, enhancing the rate performance of the battery, that is, the rapid charge and discharge capability. Among them, the crystal structure in the preferred spodumene can give the material a better lithium ion transmission channel, improve the charge and discharge efficiency and cycle life of the battery; at the same time, compared with some more expensive lithium compounds, the priority selection of these materials can control production costs to a certain extent and improve the competitiveness of products in the market.
[0051] In an embodiment of the present application, the first preset ratio is a ratio of the mass of the lithium-containing compound powder to the mass of the target doping element compound powder, and the first preset ratio ranges from 0.01% to 40%;
[0052] Specifically, the mass ratio of the lithium-containing compound powder to the target doping element compound powder is between 0.01% and 40%, for example, but not limited to 0.25%, 1%, 10.3%, 20%, 30%, wherein the preferred ratio range is 5% to 10%.
[0053] The second preset ratio is the mass ratio of the dispersed carrier precursor to the silicon powder, and the range of the second preset ratio is 35% to 65%.
[0054] The mass ratio of the dispersed carrier precursor to the silicon powder is between 35% and 65%, for example, it can be but not limited to 40.8%, 54.0%, 64.2%, 34.5%, 44.8%, 55.0%, 55.2%, 45.5% and the like, wherein the preferred ratio range is 47% to 55%.
[0055] It is worth mentioning that the proportion of nano-silicon and its dispersed phase is effectively controlled during the process to maximize the capacity of the silicon negative electrode, thereby greatly improving the energy density of lithium-ion secondary batteries, allowing the battery to store more electrical energy at the same volume or weight. Among them, the microstructure of the electrode can be optimized to make the insertion and extraction of lithium ions during the charging and discharging process smoother, reduce capacity decay, and improve the cycle stability of the battery. At the same time, reasonable proportion control can enhance the conductivity of the electrode, reduce internal resistance, improve the rate performance of the battery, and meet the needs of fast charging and discharging.
[0056] In an embodiment of the present application, the step S1 specifically includes: obtaining a first mixture after the heat treatment, and crushing and screening the first mixture to obtain the dispersed carrier precursor.
[0057] Furthermore, the temperature of the heat treatment is 500° C. to 950° C., and the reaction time of the heat treatment is 0.5 h to 10 h.
[0058] Specifically, the heat treatment temperature is between 500°C (degrees Celsius) and 950°C, for example, but not limited to 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C, 660°C, 680°C, 700°C, 720°C, 740°C. The preferred temperature range is 600°C to 720°C.
[0059] It should be noted that the heat treatment is also applied to heat treatment equipment, which includes a tubular furnace, a box furnace, a rotary furnace, and a tunnel kiln.
[0060] The step S2 specifically includes: obtaining a second mixture after the vapor deposition process, and crushing and screening the second mixture to obtain the nano-silicon battery negative electrode material.
[0061] Furthermore, the temperature of the vapor deposition process is 900° C. to 2650° C., and the reaction time of the vapor deposition process is 0.5 h to 10 h.
[0062] The temperature of the vapor deposition process is in the range of 900°C to 2650°C, preferably 1000°C to 1500°C. The pressure during heating is 10 -10 Pa (Pa) to 30Pa, the more preferred range is 10 -5 Pa to 10 -7 Pa.
[0063] It should be noted that the vapor deposition process also uses vacuum heat treatment equipment, which includes a horizontal vacuum furnace, a vertical vacuum furnace, and a rotary vacuum furnace, and is characterized in that the internal heating material is a high-temperature graphite device.
[0064] Specifically, the first mixture and the second mixture are crushed by a pulverizing device, and then sieved according to the average particle size of the powder to obtain the dispersed carrier precursor and the nano silicon battery negative electrode material. The average particle size of the lithium-containing compound powder, the target doping element compound powder, the dispersed carrier precursor, the silicon powder and the nano silicon battery negative electrode material is 2um to 7um.
[0065] Exemplarily, the pulverizing equipment includes a roller mill, a ball mill, a sand mill, a jaw crusher, a jet mill, or a combination of two thereof.
[0066] It is worth mentioning that in the related technologies for preparing nano-silicon negative electrode materials, micron silicon is prepared into silicon nanoparticles below 100nm through sand milling or ball milling. However, the preparation of nano-silicon by ball milling or sand milling has problems such as low production capacity of single-batch equipment, easy oxidation of nano-silicon during the grinding preparation process, difficulty in preparing silicon particles below 50nm, and high energy consumption. At the same time, there is also the preparation of silicon nanoparticles below 20nm by pyrolysis of gas-phase silicon compounds at high temperature. Once the selection of materials is not well controlled, there is a high safety risk factor in the high-temperature pyrolysis, which may cause casualties.
[0067] The materials selected in this application are all in powder form. Since the powdered material has a large surface area, it can contact the reaction medium more fully, so that a better uniform reaction effect can be achieved in the equipment of the process preparation process; at the same time, the reaction material in the solid phase reaction in step S1 is in a powder state compared to the block and granular state, which can also significantly reduce the temperature required for the reaction. The powdered reactants can save energy and reduce the requirements for the high temperature resistance of the equipment. In step S2, the mixed reactants require a lower air pressure to ensure the reaction, and the uniform mixing degree of the powder state is higher than that of the granular and block state, which increases the saturated vapor pressure of the reactants, which is conducive to the acceleration of the gas phase reaction process rate, and greatly reduces the pressure on the equipment. Bearing requirements. Further reducing equipment costs and operating risks, powder mixing is conducive to lower costs and effectively reduces costs.
[0068] The mixed product is crushed and the agglomerated powder is broken up into fine particles. By controlling the same particle size, the mixing can be made more uniform. During the screening process, the powder should be controlled to have similar maximum and minimum particle sizes as much as possible to ensure the consistency and stability of the product, thereby preparing nano-silicon with the required particle size.
[0069] The heating rate of the heat treatment and the vapor deposition treatment is in the range of 1°C / min (degrees Celsius per minute) to 5.5°C / min, for example, it can be but not limited to 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, preferably 2.5°C / min to 4°C / min.
[0070] It is worth mentioning that in the related technology, a mixture of Si single substance, lithium silicate and Si oxide is used as raw material, and the reaction is carried out under reduced pressure to obtain Li-doped silicon oxide-based negative electrode materials. In addition, there are also modified silicon-based negative electrode materials prepared by vacuum evaporation using silicon, silicon dioxide, and metal single substances or metal compounds of six elements, namely lithium, sodium, potassium, magnesium, strontium and calcium, as raw materials. Although in these processes, silicon dioxide is partially treated and converted into silicates, its initial effect has been significantly improved compared to traditional silicon dioxide. However, there is still a part of the silicon dioxide phase. This situation will still cause a sudden and substantial attenuation of the cycle performance of the later silicon negative electrode material during the use of the battery cell.
[0071] In addition, the silicate in its dispersed phase is mainly composed of alkali metals or alkaline earth metals. Due to the low modulus of the dispersed phase, it is difficult to suppress the aggregation of Si atoms during the process of silicon nano-lithium extraction and insertion during cycling. The continuous growth of Si clusters, coupled with the influence of heat treatment of silicon-based negative electrode materials in the later processing technology on the thermal diffusion and agglomeration of silicon nano-structures, ultimately leads to the growth of silicon grains.
[0072] The present application adopts the heat treatment and the vapor deposition process to prepare nano silicon negative electrode powder. In the process of mixing and reacting the lithium-containing compound powder and the target doping element compound powder, and further reacting the dispersed carrier precursor with the silicon powder, the reaction conditions in the process are controlled so that the dispersed phase finally formed has high modulus, high strength, and fast ion conduction characteristics, which can significantly enhance the transmission efficiency of lithium ions in the electrode, reduce the internal resistance of the battery, and improve the energy density and cycle life of the battery. The reduction of internal resistance not only reduces the energy loss of the battery during operation and improves the energy utilization efficiency, but also helps to reduce the heating phenomenon of the battery during the charging and discharging process, further improving the safety and stability of the battery; due to the significant enhancement of lithium ion transmission efficiency and the effective reduction of internal resistance, the energy density of the battery has been greatly improved, which means that at the same volume or weight, the battery can store more energy, providing more lasting and powerful power support for various application scenarios. At the same time, the cycle life of the battery has also been significantly extended, and it can withstand more charge and discharge cycles while maintaining good performance, thereby reducing the cost of use and maintenance frequency of the battery.
[0073] In an embodiment of the present application, the preparation method further comprises step S3: carbon-coating the nano-silicon battery negative electrode material under an inert atmosphere and screening and demagnetizing the carbon-coated battery negative electrode material to obtain the coated battery negative electrode material.
[0074] Specifically, the carbon source of the carbon-coated silicon oxide powder includes one or more of methane, ethane, propane, butane, acetylene, liquefied petroleum gas, propylene, ethylene, butadiene, toluene, and styrene, preferably acetylene and butadiene.
[0075] The carbon coating mass accounts for 1.0% to 10.0% of the total mass of the silicon oxide powder product, for example, it can be but not limited to 1%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 10%, preferably 2.0% to 3.0%.
[0076] The inert atmosphere includes nitrogen, helium, argon, neon, xenon, or a mixture of one or two thereof, preferably nitrogen.
[0077] It is worth mentioning that carbon coating the material can significantly improve its electronic conduction efficiency, which helps to increase the charge and discharge rate of the battery; secondly, the carbon layer can act as a barrier to reduce the direct contact and interaction between the material and the electrolyte, thereby reducing the degree of dissolution of the electrolyte to the material and inhibiting the side reactions; at the same time, carbon coating can effectively alleviate the huge volume expansion of silicon during charging and discharging, prevent the collapse of the electrode structure, and thus significantly improve the cycle performance of the battery. Before selling the finished product, the negative electrode material of the nano-silicon battery will be demagnetized. Magnetic metal impurities will form tiny local currents inside the battery, leading to self-discharge; the magnetic field and electric field generated by the magnetic material will interact with each other, which may interfere with the normal charge and discharge process of the battery and cause loss of capacitance; reduce unnecessary magnetic field interference to ensure that the battery can maintain stable performance output under various conditions of use. Demagnetization can extend the storage and use time of the battery, help maintain the stability of the battery's capacity, and ensure its performance.
[0078] The present invention is further described in detail below in conjunction with specific embodiments. The embodiments are only used to explain the present invention but not to limit the scope of the present invention.
[0079] Example 1
[0080] First, 2 kg of spodumene powder with a D50 (median particle size) of 2 um and a Dmax (maximum particle size) of 15 um and 0.87 kg of lithium borate powder with a D50 (median particle size) of 3 um and a Dmax (maximum particle size) of 17 um were mixed evenly by a fusion machine and then reacted at 700°C in a tubular furnace for 5 hours. After the reaction, the mixture was crushed and sieved by a ball mill to obtain a dispersed carrier precursor.
[0081] Then, the dispersed carrier precursor with D50 (median particle size) of 3um and Dmax (maximum particle size) of 18um and 0.61kg of silicon powder with D50 (median particle size) of 4um and Dmax (maximum particle size) of 20um were mixed evenly by a fusion machine and then heated in a horizontal vacuum furnace at 1950℃ and a pressure of 10 -6 The reaction was continued for 10 hours, and then the reaction was cooled, discharged, crushed by a roller mill and a jet mill, and sieved to obtain the negative electrode material of the nano-silicon battery.
[0082] Finally, the nano-silicon battery negative electrode material was carbon-coated for 2 hours by passing 1L / min (liter / minute) of acetylene through a rotary kiln at 800°C in a nitrogen atmosphere. Finally, the material was discharged, sieved, and demagnetized to obtain the coated battery negative electrode material.
[0083] The battery negative electrode material prepared in Example 1 has an X-ray diffraction pattern as shown in Figure 2 .from Figure 2 It can be seen that the peak at 28° corresponds to the size of the nano-silicon grains, and other diffraction peaks correspond to different silicate phase structures. It should be noted that Figure 2 The horizontal axis is the diffraction peak intensity, and the vertical axis is the diffraction angle.
[0084] The battery negative electrode material prepared in Example 1 has a scanning electron microscope image as shown in Figure 3 .from Figure 3 The microscopic morphology of the nano silicon battery negative electrode material can be seen in FIG. Figure 3 The parameters of the scanning electron microscope image are: magnification 5K times, scale 30um.
[0085] The negative electrode material of the battery prepared in Example 1 has a scanning electron microscope cross-sectional view as shown in FIG. Figure 4 .from Figure 4 The side morphology and internal dispersion of one particle of the nano silicon battery negative electrode material can be seen in the figure, and the dispersion is uniform. It should be noted that Figure 4 The parameters of the scanning electron microscope image are: magnification 2w times, scale 2um.
[0086] The battery negative electrode material prepared in Example 1 has a scanning electron microscope cross-section EDS (Energy Dispersive Spectrometer) diagram as shown in FIG. Figure 5 , Figure 5Figure a is a diagram showing the overall distribution of boron, oxygen and silicon, Figure b is a diagram showing the distribution of boron in Figure a alone, Figure c is a diagram showing the distribution of oxygen in Figure a alone, and Figure d is a diagram showing the distribution of silicon in Figure a alone. All of them show a relatively uniform dispersion. It should be noted that Figure 5 The parameters of the scanning electron microscope image are: magnification 2w times, scale 2um.
[0087] The first charge and discharge diagram of the button-type lithium-ion secondary battery prepared in Example 1 is shown in Figure 6 ,from Figure 6 The preliminary capacity and first efficiency evaluation can be seen in the figure. The voltage increases during charging and decreases during discharge.
[0088] The AC impedance comparison diagram of Example 1 and Comparative Examples 5 and 6 is shown in Figure 7 ,from Figure 7 It can be seen that the ionic conductivity of the doped phase is better, and the ohmic value of Example 1 is smaller than that of Comparative Examples 5 and 6, and the conductivity is better, and the ability of rapid charge and discharge is high. It should be noted that Figure 7 The horizontal axis is the real part of the impedance, and the vertical axis is the imaginary part of the impedance.
[0089] Example 2
[0090] First, 2 kg of lithium mica powder with D50 (median particle size) of 2 um and Dmax (maximum particle size) of 15 um and 2.4 kg of lithium aluminate powder with D50 (median particle size) of 3 um and Dmax (maximum particle size) of 17 um were mixed evenly by a ball mill and then reacted at 800 ° C in a tube furnace for 4 hours. After the reaction, the mixture was crushed and sieved by a ball mill to obtain a dispersed carrier precursor.
[0091] Then, the dispersed carrier precursor with D50 (median particle size) of 4um and Dmax (maximum particle size) of 19.5um and 0.51kg of silicon powder with D50 (median particle size) of 4um and Dmax (maximum particle size) of 20um were mixed evenly by a fusion machine and then heated in a horizontal vacuum furnace at 1350℃ and a pressure of 10 -5 The reaction was continued for 10 hours, and then the reaction was cooled, discharged, crushed by a roller mill and a jet mill, and sieved to obtain the negative electrode material of the nano-silicon battery.
[0092] Finally, the nano-silicon battery negative electrode material was carbon-coated for 2 hours by passing 1L / min of butadiene at 800°C in a nitrogen atmosphere through a rotary kiln, and finally the material was discharged, sieved, and demagnetized to obtain the coated battery negative electrode material.
[0093] Example 3
[0094] First, 2 kg of eucryptite powder with D50 (median particle size) of 5 um and Dmax (maximum particle size) of 20 um and 0.63 kg of lithium phosphate powder with D50 (median particle size) of 5 um and Dmax (maximum particle size) of 21 um were evenly mixed in a ball mill in a certain proportion, and then reacted at 900 ° C in a tube furnace for 3 hours. After the reaction, the mixture was crushed and sieved by a ball mill to obtain a dispersed carrier precursor.
[0095] Then, the dispersed carrier precursor with D50 (median particle size) of 8um and Dmax (maximum particle size) of 27um and 0.45kg of silicon powder with D50 (median particle size) of 7.5um and Dmax (maximum particle size) of 26um were mixed evenly by a fusion machine and then heated in a horizontal vacuum furnace at 1050℃ and 10 -1 The reaction was continued for 12 hours, and then the reaction was cooled, discharged, crushed and sieved by a jet mill to obtain the negative electrode material of nano-silicon battery.
[0096] Finally, the nano-silicon battery negative electrode material was carbon coated for 3 hours by passing 1L / min of methane at 900°C in a nitrogen atmosphere through a rotary kiln, and finally the material was discharged, sieved, and demagnetized to obtain the coated battery negative electrode material.
[0097] Example 4
[0098] First, 2 kg of petalite powder with a D50 (median particle size) of 5 um and a Dmax (maximum particle size) of 20 um and 5.4 kg of lithium tungstate powder with a D50 (median particle size) of 4 um and a Dmax (maximum particle size) of 21 um were mixed evenly in a VC mixer and then reacted in a tubular furnace at 700 ° C for 6 hours. After the reaction, the mixture was crushed and sieved by a roller mill and a ball mill to obtain a dispersed carrier precursor.
[0099] Then, the dispersed carrier precursor with D50 (median particle size) of 6um and Dmax (maximum particle size) of 23um and 0.67kg of silicon powder with D50 (median particle size) of 4um and Dmax (maximum particle size) of 20um were mixed evenly by a fusion machine and then placed in a rotary vacuum furnace at 2250℃ and pressure of 10 -9 The reaction was continued for 8 hours, and then the reaction was cooled, discharged, crushed by roller mill and ball mill, and sieved to obtain the negative electrode material of nano silicon battery.
[0100] Finally, the nano silicon battery negative electrode material was carbon coated for 3.5 hours by passing 1 L / min of propylene through a rotary kiln at 750°C in a nitrogen atmosphere, and finally the coated battery negative electrode material was prepared by discharging, screening and demagnetizing.
[0101] Example 5
[0102] First, 2 kg of lithium beryllium powder with a D50 (median particle size) of 1 um and a Dmax (maximum particle size) of 15 um and 0.035 kg of lithium sulfide powder with a D50 (median particle size) of 2 um and a Dmax (maximum particle size) of 17.5 um were mixed evenly in a VC mixer and then reacted in a tubular furnace at 700 ° C for 6 hours. After the reaction, the mixture was crushed and sieved by a double-roll mill and a ball mill to obtain a dispersed carrier precursor.
[0103] Then, the dispersed carrier precursor with D50 (median particle size) of 3um and Dmax (maximum particle size) of 16um and 0.46kg of silicon powder with D50 (median particle size) of 4um and Dmax (maximum particle size) of 18um were mixed evenly by a fusion machine and then placed in a vertical vacuum furnace at 1150℃ and a pressure of 10 -2 The reaction was continued for 9 hours, and then the reaction was cooled, discharged, crushed by roller mill and ball mill, and sieved to obtain the negative electrode material of nano silicon battery.
[0104] Finally, the nano-silicon battery negative electrode material was carbon coated for 1.5 hours by passing 1L / min of butane at 900°C in a nitrogen atmosphere through a rotary kiln, and finally the material was discharged, sieved, and demagnetized to obtain the coated battery negative electrode material.
[0105] In order to better illustrate the advantages of the embodiments of the present invention, the performance of the coated battery negative electrode materials prepared in embodiments 1 to 5 of the present invention was tested. The test methods used in the following experimental examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0106] Comparative Example 1
[0107] The lithium borate powder 0.87 kg in Example 1 was replaced with lithium hydroxide powder 0.99 kg, mixed evenly in a fusion machine, and reacted in a horizontal vacuum furnace. Other conditions were the same as in Example 1.
[0108] Comparative Example 2
[0109] The lithium borate powder 0.87 kg in Example 1 was replaced with lithium hydroxide powder 0.99 kg, mixed evenly in a fusion machine, and reacted in a horizontal vacuum furnace. Other conditions were the same as in Example 1.
[0110] Comparative Example 3
[0111] Except that the temperature of the horizontal vacuum furnace for sublimation and deposition process is changed to 1000° C., other conditions are the same as those in Example 1.
[0112] Comparative Example 4
[0113] Except that the preparation temperature of the dispersed carrier precursor in the tube furnace is changed to 800° C., other conditions are the same as those in Example 1.
[0114] Comparative Example 5
[0115] Si powder, SiO2 powder and LiOH powder were mixed evenly in a molar ratio of 4:1:3 and then loaded into a tube furnace, heated to 1400°C and sintered in an Ar atmosphere at atmospheric pressure. The sintered material was then heated to 1400°C in a horizontal vacuum furnace under reduced pressure, with a vacuum degree of 5Pa for gasification and deposition, and the reaction lasted for 10 hours. After the reaction was completed, the material was cooled, discharged, crushed by a roller mill and a jet mill, and sieved to obtain a nano-silicon battery negative electrode material.
[0116] Finally, the nano-silicon battery negative electrode material was passed through a rotary kiln in a nitrogen atmosphere at 800°C and 2L / min of acetylene was introduced for carbon coating for 40 minutes. Finally, the material was discharged, sieved, and demagnetized to prepare a powder with an average particle size of 5.6um.
[0117] Comparative Example 6
[0118] 10kg silicon powder, 13.5kg silicon dioxide powder and 5.3kg magnesium oxide powder were added to the VC machine and mixed evenly. The materials were placed in a horizontal furnace and gasified and deposited at 1350℃, 800℃ at the collecting end, and 5Pa vacuum for 10 hours. After the reaction, the materials were cooled, discharged, crushed by roller mill and ball mill, and sieved to obtain a powder with an average particle size of 5um.
[0119] Finally, the powder was passed through a rotary kiln in a nitrogen atmosphere at 900°C and 2L / min of acetylene was introduced for carbon coating for 40 minutes. Finally, the powder was discharged, sieved, and demagnetized to obtain the coated battery negative electrode material.
[0120] 1. Experimental objects: the battery negative electrode materials prepared in Examples 1 to 5 of the present invention; the battery negative electrode materials prepared in Comparative Examples 1 to 6 above.
[0121] 2. Experimental methods:
[0122] ①XRD measurement conditions are as follows:
[0123] Target: Cu (Kα line) target;
[0124] Measuring range: 10° (degrees) ~ 90°;
[0125] Scanning mode: continuous scanning;
[0126] Scan rate: 0.04 o / s (degrees / second);
[0127] Scan step: 0.02 o ;
[0128] Tube voltage: 40.0KV (kilovolts);
[0129] Tube current: 30mA (milliampere).
[0130] ②pH test conditions are as follows:
[0131] Take 1g of the nano silicon battery negative electrode material in the above examples 1 to 5 and comparative examples 1 to 6, add 20g of deionized water, and ultrasonically disperse for 3min, then use a pH meter to test the pH, and read the value after it stabilizes. Figure 8 As shown, the conditions of the slurry of the embodiment and the comparative example at high temperature and the pH value of the powder solution are compared.
[0132] ③ The test conditions for button-type lithium-ion secondary batteries are as follows:
[0133] The silicon-based negative electrode powder material, SP (conductive carbon black), CMC (sodium carboxymethyl cellulose) and SBR emulsion (styrene-butadiene rubber) are mixed in a mass ratio of 75:15:5:5, and water is added to a magnetic stirrer for continuous stirring and dispersion. Then it is coated on a 10um copper foil by a coating machine, and then dried at 90℃ in vacuum (-0.1MPa) for 6h. The roller is compacted and the compaction density is controlled at 1.30g / cm 3 (g / cm2), and then use a punching machine to make a disc with a diameter of 12mm, dry it in vacuum (-0.1MPa) at 90℃ for 5h, weigh it and calculate the weight of the active material. Assemble CR2016 button cells in a glove box, use metal lithium sheets as counter electrodes, polypropylene microporous membranes as separators, 1mol / L LiPF6 (lithium hexafluorophosphate) is dissolved in EC (ethylene carbonate) and DEC (diethyl carbonate) in a volume ratio of 1:1, and an electrolyte with 5.0% FEC (fluoroethylene carbonate) is added. The battery was left to stand at room temperature for 12h, and then tested on a constant current charge and discharge test on a blue power test system, charged to 0.005V at 0.05C, and then discharged to 2.0V at 0.1C. The charge and discharge curves are shown in the figure. Figure 6 As shown, the first charge capacity was 2001.95 mAh / g (milliampere-hour / gram), the first discharge capacity was 1856.45 mAh / g, and the first efficiency was 92.73%. The remaining uncoated slurry was sealed and placed at 70°C for observation. Fig. 9 As shown, the ICP test results of the embodiment and the comparative example show the doping element content, the first discharge capacity, the first coulombic efficiency, and the capacity retention rate after 100 cycles and 300 cycles.
[0134] ④The compressive strength test process and conditions are as follows:
[0135] Test process: Powder is dispersed in liquid and dripped onto a glass slide. Single particles are located under an optical microscope. The pressure head is controlled to press down at a uniform speed. During the particle compression process, force and displacement curves are collected to calculate the mechanical properties of single particles.
[0136] Test conditions:
[0137] Magnification: up to 1200 times
[0138] Pressure test range: 0-100mN (millinewton)
[0139] Pressure test accuracy: ±0.1mN
[0140] Minimum displacement unit: 10nm (nanometer)
[0141] Data acquisition frequency: 1000Hz (Hertz)
[0142] Battery AC impedance test test conditions are as follows:
[0143] Start frequency: 10000Hz
[0144] End frequency: 0.01Hz
[0145] Amplitude: 0.005V
[0146] Measurement delay: 0S
[0147] Conclusion: If Figure 8 and Fig. 9 The data in the table show that the slurry made of the material is at 70°C. Comparative Example 1 uses lithium hydroxide powder as the target doping element compound powder, and the pH of the negative electrode material powder prepared is 9.1, and there is no abnormality within 36 hours, and its structure is the most stable. The content of the doping element in Examples 1 to 5 and Comparative Examples 1 to 6 prepared by this method is closely related to the type of the doping element, and the appropriate ratio enables a higher retention rate to be achieved.
[0148] In summary, the battery negative electrode material provided by the embodiment of the present invention has the advantages of high initial efficiency, long cycle and uniform dispersed phase.
[0149] On the other hand, an embodiment of the present invention provides a battery negative electrode material, including a nano-silicon battery negative electrode material prepared by any of the aforementioned methods.
[0150] On the other hand, an embodiment of the present invention provides a lithium-ion battery, comprising the aforementioned battery negative electrode material.
[0151] It can be understood that the aforementioned embodiments are merely exemplary descriptions of the present invention. The technical solutions of the various embodiments can be arbitrarily combined and used in combination, provided that the technical features do not conflict, the structures do not contradict, and the purpose of the present invention is not violated.
[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a negative electrode material for a battery, characterized in that: include: Step S1: mixing the lithium-containing compound powder and the target doping element compound powder in a first preset ratio and then performing heat treatment to obtain a dispersed carrier precursor; The target doping element compound contains lithium; The doping element in the target doping element compound includes any one or more of boron, phosphorus, sulfur, molybdenum, tungsten, titanium, aluminum, bromine, fluorine, and iodine; Step S2: the dispersed carrier precursor and silicon powder are mixed evenly according to a second preset ratio and then subjected to vapor deposition treatment to obtain a nano-silicon battery negative electrode material.
2. The preparation method according to claim 1, characterized in that: The target doping element compound powder includes any one or more of lithium borate powder, lithium aluminate powder, lithium phosphate powder, lithium tungstate powder, and lithium sulfide powder.
3. The preparation method according to claim 1, characterized in that: The lithium-containing compound includes: one or more of lithium acetate, lithium sulfite, lithium tetrafluoroborate, lithium citrate, lithium hydroxide, lithium oxide, lithium nitride, lithium nitrate, lithium chloride, lithium bromide, lithium borate, lithium lactate, lithium sulfide, lithium sulfate, lithium iodide, lithium iodate, lithium carbonate, lithium bicarbonate, lithium oxalate, lithium peroxide, lithium tungstate, lithium aluminate, lithium tantalate, lithium chromate, lithium manganate, spodumene, lithium mica, petalite, eucryptite, lithium beryllite, lithium phosphate aluminum oxide, hectorite, jaddarite, iron lithium mica, and lithium cryolite.
4. The preparation method according to claim 1, characterized in that: The first preset ratio is a ratio of the mass of the lithium-containing compound powder to the mass of the target doping element compound powder, and the range of the first preset ratio is 0.01% to 40%; And / or, the second preset ratio is a ratio of the mass of the dispersed carrier precursor to the silicon powder, and the range of the second preset ratio is 35% to 65%.
5. The preparation method according to claim 1, characterized in that: The step S1 specifically includes: obtaining a first mixture after the heat treatment, crushing and screening the first mixture to obtain the dispersed carrier precursor; And / or, the step S2 specifically includes: obtaining a second mixture after the vapor deposition process, and crushing and screening the second mixture to obtain the nano-silicon battery negative electrode material.
6. The preparation method according to claim 1, characterized in that: The temperature of the heat treatment is 500° C. to 950° C.; and / or the temperature of the vapor deposition treatment is 900° C. to 2650° C.; and / or the reaction time of the heat treatment and the vapor deposition treatment is 0.5 h to 10 h.
7. The preparation method according to claim 1, characterized in that: The average particle sizes of the lithium-containing compound powder, the target doping element compound powder, the dispersed carrier precursor, the silicon powder and the nano-silicon battery negative electrode material are all 2um to 7um.
8. The preparation method according to claim 1, characterized in that: The preparation method further comprises step S3: carbon coating the nano silicon battery negative electrode material under an inert atmosphere and screening and demagnetizing the carbon coated battery negative electrode material.
9. A battery negative electrode material, characterized in that: The invention comprises a nano silicon battery negative electrode material prepared by any one of the methods described in claims 1 to 8.
10. A lithium ion battery, characterized in that: The invention comprises the battery negative electrode material as claimed in claim 9.