An extractant for extracting iron and aluminum from wet-process phosphoric acid solution, and its preparation method and application

The acidic, bidentate organophosphorus extractant P,P'-[(alkylimine)bis(methylene)]bis[p-phenylphosphinic acid] effectively separates iron and Aluminum solves the problem of loss and poor removal effect of traditional extraction agents at high temperatures, achieving deep removal and efficient extraction of iron and aluminum.

CN118561910BActive Publication Date: 2024-10-18UNIV OF JINAN +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411037144.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-18
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

It is difficult to effectively separate iron and aluminum in a strongly acidic wet phosphoric acid system with existing technology. Traditional extraction agents suffer serious losses at high temperatures and are not effective in removing impurities.

Method used

The acidic, bidentate organophosphorus extraction agent P,P'-[(alkylimine)bis(methylene)]bis[p-phenylphosphinic acid] is used. This extraction agent is simple to synthesize, resistant to high temperatures and It is not easy to emulsify and maintains excellent ionization ability in strong acidic systems, and can effectively extract iron and aluminum in acidic solutions.

Benefits of technology

It achieves deep removal of iron and aluminum without changing the wet phosphoric acid process, has short extraction equilibrium time, fast phase separation, and has better performance than traditional phosphorus extraction agents, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561910B_ABST
    Figure CN118561910B_ABST
Patent Text Reader

Abstract

The invention discloses an extractant for extracting iron and aluminum from wet-process phosphoric acid solution, and a preparation method and application thereof. The structural formula of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution is:; The extractant for extracting iron and aluminum from wet-process phosphoric acid solution in the invention has a simple synthesis method, high yield, can be mass-produced, and has a structure without phosphate ester bonds, high temperature resistance, and is not easy to acid hydrolyze; the benzene ring strengthens the acidity of phenylphosphonic acid, promotes the cation exchange process, and the bifunctional group increases the complexing site, which is easy to form a stable chelate structure with high-valent metal ions; and it is not easy to emulsify, does not require saponification, and can achieve deep removal of iron and aluminum without changing the wet-process phosphoric acid process; the extraction equilibrium time is short, the phase separation is fast, and it has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron-aluminium separation, and in particular relates to an extractant for extracting iron and aluminium from wet-process phosphoric acid solution, and a preparation method and application thereof. Background Art

[0002] Phosphoric acid is mainly used in industries such as phosphate fertilizer, feed, food, and medicine. It is a very important chemical raw material, and its output is second only to sulfuric acid. Thermal method and wet method are two methods for preparing phosphoric acid from phosphate ore. The wet method is widely used due to its low energy consumption and low pollution. About 90% of the world's phosphoric acid is produced by wet process. The sulfuric acid process is simple and the by-product phosphogypsum is easy to separate, which can achieve large-scale industrialization. The sulfuric acid process occupies a dominant position in the production of wet phosphoric acid, so the wet phosphoric acid process usually refers to sulfuric acid phosphoric acid. During the acidolysis process, a large amount of Fe and Al impurities in the phosphate ore enter the acid solution. The high impurity content is the biggest drawback of wet phosphoric acid. Therefore, impurity removal is a key link in the wet phosphoric acid process.

[0003] At present, the hydrometallurgical industry usually uses precipitation, adsorption and solvent extraction to remove impurities from the solution. The precipitation method is simple to operate, but it consumes a large amount of precipitant and cannot introduce other impurities while deeply removing impurities. The adsorption method often uses ion exchange resin, which has high impurity removal efficiency, but the load capacity is limited. It is only economically feasible when the impurity content is very low. The solvent extraction method has a large processing capacity, high efficiency, simple operation, and is easier to achieve large-scale industrialization. In the past few decades, people have conducted a lot of research on the technology of removing iron by solvent extraction. "A method for extracting and separating iron and phosphorus from iron phosphate slag to prepare iron phosphate" (CN 114804048 A) discloses a method for extracting and separating iron from iron phosphate slag acid leaching solution using P204. The invention requires strict control of the pH of the extraction system to about 1, while the concentration of sulfuric acid and phosphoric acid in the wet phosphoric acid solution is high, so this method is not applicable. "A method for resource-based disposal of red mud" (CN 111690810 A) invented a method for extracting iron from red mud using a quaternary ammonium extractant, and the hydrogen ion concentration of the leaching system is 0.5~2 mol / L. However, quaternary ammonium extractants are easily emulsified and difficult to separate, and they also have a certain extraction effect on phosphoric acid in the acid solution, resulting in phosphorus loss. Alkaline organic amine extractants will extract phosphoric acid in the acid solution, and neutral extractants have poor coordination ability for iron and aluminum in the strong acid sulfuric acid system. Traditional acid extractants are difficult to ionize in the strong acid system, and the extraction effect becomes worse as the acidity of the aqueous phase increases. The concentration of sulfuric acid and phosphoric acid in wet-process phosphoric acid acid is high, the composition is complex, and the removal of iron and aluminum is difficult. At present, there are few reports on industrial technologies for separating iron and aluminum from wet-process phosphoric acid acid. Therefore, it is necessary to develop a new type of extractant suitable for the separation of impurities iron and aluminum in the strong acid wet-process phosphoric acid system. Summary of the invention

[0004] Aiming at the problem that traditional extraction agents cannot effectively separate iron and aluminum in wet-process phosphoric acid solution, the present invention provides an extractant for extracting iron and aluminum in wet-process phosphoric acid solution, as well as a preparation method and application thereof. The two alkyl chains not only reduce the loss of the extractant during high-temperature extraction, but also enable the extractant to have good oil solubility. The extractant still maintains excellent extraction effect on iron and aluminum ions in a strong acidic system.

[0005] The present invention is achieved through the following technical solutions:

[0006] An extractant for extracting iron and aluminum from a wet-process phosphoric acid solution, wherein the structural formula of the extractant for extracting iron and aluminum from a wet-process phosphoric acid solution is:

[0007]

[0008] R 1 and R 2 are alkyl groups with carbon number greater than or equal to 1, R 1 and R 2 The total carbon number is equal to 16.

[0009] In the present invention, the preparation method of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution comprises the following steps:

[0010] (1) Mix the solvent, secondary carbon primary amine, phenylphosphinic acid and inorganic acid, and heat until the solution is clear and transparent;

[0011] The structural formula of the secondary carbon primary amine is: , R 1 and R 2 are alkyl groups with carbon number greater than or equal to 1, R 1 and R 2 The total carbon number is equal to 16;

[0012] (2) adding formaldehyde solution or paraformaldehyde to the clear and transparent solution of step (1) to carry out a reaction;

[0013] (3) After the reaction in step (2) is completed, the aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, and the colloid is washed, rotary evaporated, and dried to obtain an extractant for extracting iron and aluminum from the wet-process phosphoric acid solution;

[0014] The preparation process of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution is as follows:

[0015] .

[0016] Furthermore, the solvent in step (1) is one or more of water and alcohol; and the inorganic acid is one of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid or acetic acid.

[0017] Furthermore, the alcohol in step (1) is one of ethanol, propanol and isopropanol; and the inorganic acid is hydrochloric acid or sulfuric acid.

[0018] Furthermore, the molar ratio of the secondary carbon primary amine to phenylphosphinic acid is 1:1-1:4; the molar ratio of the secondary carbon primary amine to inorganic acid is 10:1-1:3; and the molar ratio of the secondary carbon primary amine to formaldehyde is 1:1-1:5.

[0019] Furthermore, the heating temperature in step (1) is 50-110° C.; the reaction temperature in step (2) is 50-110° C., and the reaction time is 1-10 h.

[0020] In the present invention, the extractant for extracting iron and aluminum from wet-process phosphoric acid solution is used in extracting iron and aluminum from wet-process phosphoric acid solution.

[0021] Furthermore, the Fe 3+ The concentration is 0.1~6.5 g / L, Al 3+ The concentration is 0.1~10 g / L, the concentration of sulfuric acid is 0.01~3 mol / L, and the concentration of phosphoric acid is 1~8 mol / L.

[0022] Furthermore, the method for extracting iron and aluminum from wet-process phosphoric acid solution comprises the following steps:

[0023] (1) An extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared with a diluent is used as an organic phase, and the concentration of the extractant for extracting iron and aluminum from the wet-process phosphoric acid solution is 1-40 wt%;

[0024] (2) preheating the organic phase and the wet-process phosphoric acid solution in step (1), mixing and stirring them for extraction, and separating the mixed solution after extraction to obtain an organic phase loaded with iron and aluminum ions and a raffinate;

[0025] (3) The organic phase loaded with iron and aluminum ions is stripped with a stripping agent at a stripping temperature of 20-80 °C to obtain an aqueous solution containing iron and aluminum ions.

[0026] Furthermore, the diluent described in step (1) is one or more of aliphatic hydrocarbons, halogenated hydrocarbons, aromatic hydrocarbons, solvent oil and alcohol; the volume ratio of the wet-process phosphoric acid solution to the organic phase described in step (2) is 1:5~5:1, the extraction time is 1~120min, and the extraction temperature is 10~90°C; the stripping agent in step (3) is 0.1~1 mol / L ammonium oxalate, and the stripping time is 10~120min.

[0027] The extractant for extracting iron and aluminum from wet-process phosphoric acid is an acidic, bidentate organophosphorus extractant, referred to as P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]. The two alkyl chains not only reduce the loss of the extractant during high-temperature extraction, but also make the extractant have good oil solubility. The two phenylphosphinic acid groups enhance the ionization ability of the extractant in the acidic system, so that the extractant still maintains excellent extraction effect on iron and aluminum ions in the strong acidic system. The extractant can effectively extract iron and aluminum in the acid without changing the current wet-process phosphoric acid process.

[0028] Beneficial Effects

[0029] (1) The extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution of the present invention has a simple synthesis method, high yield, and can be produced on a large scale; the structure does not contain a phosphate ester bond, is resistant to high temperatures, and is not easily acid-lyzed; the benzene ring strengthens the acidity of phenylphosphonic acid and has a promoting effect on the cation exchange process; the bifunctional group increases the complexing site and is easy to form a stable chelate structure with high-valent metal ions.

[0030] (2) The extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution of the present invention is not easy to emulsify and does not require saponification. It can achieve deep removal of iron and aluminum without changing the wet-process phosphoric acid process; the extraction equilibrium time is short, the phase separation is fast, and the extraction performance is significantly better than traditional phosphorus (phosphine) extractants such as P204, P507, and Cyanex272. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4;

[0032] Figure 2 This is the infrared spectrum of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited by the embodiments. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.

[0034] The structural formula of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in the following examples is:

[0035]

[0036] R 1 and R 2 are alkyl groups with carbon number greater than or equal to 1, R1 and R 2 The total carbon number is equal to 16.

[0037] In the following examples and comparative examples, Fe 3+ The concentration is 1.7 g / L, Al 3+ The concentration is 7.6 g / L, the concentration of sulfuric acid is 1 mol / L, and the concentration of phosphoric acid is 6 mol / L;

[0038] The extraction rate (E) can directly show the extraction capacity of the extractant, and the stripping rate (S) can reflect the regeneration capacity of the extractant. The metal ion concentrations in the initial aqueous phase, raffinate and stripping raffinate were determined by ICP-OES, and the extraction rate E and stripping rate S were calculated by formulas (1) to (2) respectively:

[0039]

[0040] C in the formula 0 , C 1 and C 2 They represent the metal ion concentrations in the initial aqueous phase, the raffinate and the strip raffinate, respectively. In the present invention, the metal ion concentration is determined by ICP-OES.

[0041] Example 1

[0042] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, 300 mL of water, 0.5 mol of a secondary carbon primary amine, 0.5 mol of phenylphosphinic acid and 0.1 mol of hydrochloric acid were added in sequence, mixed, and heated to 70° C. The mixture became clear and transparent; the structural formula of the secondary carbon primary amine is: , where R 1 is an alkyl group with 1 carbon atom, R 2 is an alkyl group of 15 carbon atoms;

[0043] (2) Add 1 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 70°C for 4 hours;

[0044] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain an extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution.

[0045] Example 2

[0046] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, 300 mL of water, 0.5 mol of a secondary carbon primary amine, 1 mol of phenylphosphinic acid and 0.5 mol of hydrochloric acid were added in sequence, mixed, and heated to 90° C. The mixture became clear and transparent; the structural formula of the secondary carbon primary amine is: , R 1 is a 4-carbon alkyl group, R 2 is an alkyl group of 12 carbon atoms;

[0047] (2) Add 2 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 90°C for 5 hours;

[0048] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain an extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution.

[0049] Example 3

[0050] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, 300 mL of ethanol, 0.5 mol of a secondary carbon primary amine, 1 mol of phenylphosphinic acid and 0.3 mol of sulfuric acid were added in sequence, mixed, and heated to 80° C. The mixture became clear and transparent; the structural formula of the secondary carbon primary amine is: , R 1 is a 6-carbon alkyl group, R 2 is an alkyl group with 10 carbon atoms;

[0051] (2) Add 1 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 80°C for 7 hours;

[0052] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain an extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution.

[0053] Example 4

[0054] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, 300 mL of ethanol, 0.5 mol of a secondary carbon primary amine, 1.2 mol of phenylphosphinic acid and 0.2 mol of sulfuric acid were added in sequence, mixed, and heated to 100° C. The mixture became clear and transparent; the structural formula of the secondary carbon primary amine is: , R 1 is an alkyl group with 8 carbon atoms, R2 is an alkyl group of 8 carbon atoms;

[0055] (2) adding 1.5 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and reacting at 100° C. for 6 h;

[0056] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain an extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution.

[0057] Example 5

[0058] (1) In a 1000 mL three-necked round-bottom flask equipped with a mechanical stirrer and a condensation reflux device, 300 mL of ethanol, 0.5 mol of a secondary carbon primary amine, 1.5 mol of phenylphosphinic acid and 0.5 mol of sulfuric acid were added in sequence, mixed, and heated to 110° C. The mixture was clear and transparent; the structural formula of the secondary carbon primary amine was: , R 1 is a 6-carbon alkyl group, R 2 is an alkyl group with 10 carbon atoms;

[0059] (2) Add 2 mol of 37% formaldehyde solution to the clear and transparent solution of step (1), and react at 110°C for 8 hours;

[0060] (3) After the reaction in step (2) is completed, the upper aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, washed with dilute hydrochloric acid and water in turn, rotary evaporated, and vacuum dried to obtain an extractant (P,P'-[(alkylimine)di(methylene)]di[p-phenylphosphinic acid]) for extracting iron and aluminum from wet-process phosphoric acid solution.

[0061] The raw materials and yields of the extractants for extracting iron and aluminum from wet-process phosphoric acid solutions prepared in Examples 1 to 5 are shown in Table 1 below:

[0062] Table 1

[0063]

[0064] The nuclear magnetic resonance hydrogen spectrum and infrared spectrum of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 are as follows: Figure 1 and Figure 2 As shown: 1 H NMR (400 MHz, DMSO) δ 7.67 (dd, J = 11.3, 7.2 Hz, 4H, -CH=), 7.57 – 7.38 (m, 6H, -CH=), 3.06 (d,J = 9.2 Hz, 4H, N-CH 2 -P), 2.35 (s,1H, CH-N), 1.36 – 0.62 (m, 34H, -CH 2 -, -CH 3 ).IR(KBr, cm -1 ) C=C (film) / cm -1 1462;υ p=o (film) / cm -1 1192; υ C-N (film) / cm -1 1131; υ p-o (film) / cm -1 965.

[0065] Example 6

[0066] (1) 1, 2, 4-trimethylbenzene, S-150 solvent oil and S-260 solvent oil were used as diluents to prepare the extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4, as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0067] (2) 25 mL of the organic phase in step (1) and 25 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 30 min at 25 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentrations were all less than 0.055 g / L, Al 3+ The concentrations were all less than 5.81 g / L). The extraction rate (E) was calculated according to formula (1). The effect of the diluent on the extraction rate is shown in Table 2.

[0068] Table 2

[0069]

[0070] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentrations were all greater than 1.61 g / L, Al 3+ The concentrations are all greater than 1.79 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 98%.

[0071] Example 7

[0072] (1) The extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 was prepared with S-260 solvent oil as a diluent as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0073] (2) 25 mL of the organic phase in step (1) and 25 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction at a temperature of 30 min at 45°C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate; Fe in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.063 g / L, Al 3+ The concentration is 5.95 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;

[0074] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.60 g / L, Al 3+ The concentration is 1.65 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 98%.

[0075] Example 8

[0076] (1) The extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 was prepared with S-260 solvent oil as a diluent as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0077] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution (aqueous phase) were mixed and stirred for extraction at a temperature of 30 min and 55 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate; Fe in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.10 g / L, Al 3+ The concentration is 6.24 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;

[0078] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.56 g / L, Al3+ The concentration is 1.36 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 98%.

[0079] Example 9

[0080] (1) The extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 was prepared with S-260 solvent oil as a diluent as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0081] (2) 30 mL of the organic phase in step (1) and 10 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 30 min at 65 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 3.4×10 -3 g / L,Al 3+ The concentration is 3.78 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;

[0082] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 1.66 g / L, Al 3+ The concentration is 3.81 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 98%.

[0083] Example 10

[0084] (1) The extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 was prepared with S-260 solvent oil as a diluent as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0085] (2) 10 mL of the organic phase in step (1) and 30 mL of wet-process phosphoric acid solution (aqueous phase) were mixed and stirred for extraction. The extraction temperature was 30 min and the extraction temperature was 75°C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration (Fe 3+ The concentration is 0.828 g / L, Al 3+ The concentration is 7.31 g / L), and the extraction rate (E) is calculated according to formula (1). The extraction results are shown in Table 3;

[0086] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C and a stripping time of 30 min to obtain an aqueous solution containing iron and aluminum ions, wherein Fe 3+ The concentration is 0.859 g / L, Al 3+ The concentration is 0.289 g / L. The stripping rate (S) is calculated according to formula (2). The stripping rate of aluminum is greater than 99.9%, and the stripping rate of iron is greater than 98%.

[0087] Examples 7-10 Extraction of iron and aluminum in wet-process phosphoric acid solution 3+ 、Al 3+ The extraction rates are shown in Table 3 below:

[0088] Table 3

[0089]

[0090] Embodiment 11

[0091] (1) The extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 was prepared with S-260 solvent oil as a diluent as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0092] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution were mixed for extraction. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The aqueous phase after separation was mixed with 25 mL of fresh organic phase. The extraction was repeated seven times. The extraction time was 30 min each time and the extraction temperature was 25 °C. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 4;

[0093] Table 4

[0094]

[0095] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C for 30 min to obtain an aqueous solution containing iron and aluminum ions. The stripping rate (S) was calculated according to formula (2). The stripping rate of aluminum was greater than 99.9%, and the stripping rate of iron was greater than 98%.

[0096] Example 12

[0097] (1) The extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 was prepared with S-260 solvent oil as a diluent as an organic phase, and the concentration of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution was 20wt%;

[0098] (2) 25 mL of the organic phase in step (1) and 25 mL of wet phosphoric acid solution were mixed to perform secondary countercurrent extraction for deep iron removal. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate (aqueous phase). The aqueous phase after separation was then mixed with 25 mL of fresh organic phase and subjected to tertiary countercurrent aluminum removal. Each extraction time was 30 min and the extraction temperature was 25 °C. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 5;

[0099] Table 5

[0100]

[0101] (3) The organic phase loaded with iron and aluminum ions was stripped with ammonium oxalate at a stripping temperature of 40 °C for 30 min to obtain an aqueous solution containing iron and aluminum ions. The stripping rate (S) was calculated according to formula (2). The stripping rate of aluminum was greater than 99.9%, and the stripping rate of iron was greater than 98%.

[0102] Comparative Example 1

[0103] (1) Using S-260 solvent oil as a diluent, a 20 wt% solution of D2EHPA, P538, PC-88A, cyclohexane acid, CA-12, Cyanex 272, TOPO and TBP was prepared as the organic phase. The organic phase and wet phosphoric acid solution were mixed in a volume ratio of 5:1 for extraction. The extraction time was 30 min and the extraction temperature was 25 °C. After the extraction, the mixed solution was separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate. The Fe content in the raffinate was determined. 3+ 、Al 3+ The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 6;

[0104] (2) S-260 solvent oil was used as a diluent to prepare an extractant solution with a concentration of 20 wt % for extracting iron and aluminum from wet-process phosphoric acid solution prepared in Example 4 as an organic phase; the organic phase and the wet-process phosphoric acid solution were mixed in a volume ratio of 5:1 for extraction, the extraction time was 30 min, the extraction temperature was 25 ° C, and the mixed solution after the extraction was completed was phase-separated to obtain an organic phase loaded with iron and aluminum ions and a raffinate; Fe in the raffinate was determined 3+ 、Al 3+The concentration of , the extraction rate (E) was calculated according to formula (1), and the extraction results are shown in Table 6;

[0105] Table 6

[0106]

Claims

1. An extractant for extracting iron and aluminum from wet-process phosphoric acid solution, characterized in that: The structural formula of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution is: R1 and R2 are each an alkyl group having 1 or more carbon atoms, and the total carbon atoms of R1 and R2 are 16.

2. A method for preparing an extractant for extracting iron and aluminum from wet-process phosphoric acid solution according to claim 1, characterized in that: The following steps are involved: (1) Mix the solvent, secondary carbon primary amine, phenylphosphinic acid and inorganic acid, and heat until the solution is clear and transparent; The structural formula of the secondary carbon primary amine is: , R1 and R2 are alkyl groups with carbon numbers greater than or equal to 1, and the total carbon number of R1 and R2 is 16; (2) adding formaldehyde solution or paraformaldehyde to the clear and transparent solution of step (1) to carry out a reaction; (3) After the reaction in step (2) is completed, the aqueous phase is removed, and the colloid after the aqueous phase is removed is dissolved with dichloromethane, and the colloid is washed, rotary evaporated, and dried to obtain an extractant for extracting iron and aluminum from the wet-process phosphoric acid solution; The preparation process of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution is as follows: 。 3. The method for preparing the extractant for extracting iron and aluminum from wet-process phosphoric acid solution according to claim 2, characterized in that: The solvent in step (1) is one or more of water and alcohol; the inorganic acid is one of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid or acetic acid.

4. The method for preparing the extractant for extracting iron and aluminum from wet-process phosphoric acid solution according to claim 3, characterized in that: The alcohol described in step (1) is one of ethanol, propanol and isopropanol; and the inorganic acid is hydrochloric acid or sulfuric acid.

5. The method for preparing the extractant for extracting iron and aluminum from wet-process phosphoric acid solution according to claim 2, characterized in that: The molar ratio of the secondary carbon primary amine to phenylphosphinic acid is 1:1-1:4; the molar ratio of the secondary carbon primary amine to inorganic acid is 10:1-1:3; and the molar ratio of the secondary carbon primary amine to formaldehyde is 1:1-1:

5.

6. The method for preparing the extractant for extracting iron and aluminum from wet-process phosphoric acid solution according to claim 2, characterized in that: The heating temperature in step (1) is 50-110° C.; the reaction temperature in step (2) is 50-110° C., and the reaction time is 1-10 h.

7. Use of the extractant for extracting iron and aluminum from wet-process phosphoric acid solution according to claim 1 in extracting iron and aluminum from wet-process phosphoric acid solution.

8. The use according to claim 7, characterized in that The Fe 3+ The concentration is 0.1~6.5 g / L, Al 3+ The concentration is 0.1~10 g / L, the concentration of sulfuric acid is 0.01~3 mol / L, and the concentration of phosphoric acid is 1~8 mol / L.

9. The use according to claim 7, characterized in that: The method for extracting iron and aluminum from wet-process phosphoric acid solution comprises the following steps: (1) An extractant for extracting iron and aluminum from wet-process phosphoric acid solution prepared with a diluent is used as an organic phase, and the concentration of the extractant for extracting iron and aluminum from the wet-process phosphoric acid solution is 1-40 wt%; (2) preheating the organic phase and the wet-process phosphoric acid solution in step (1), mixing and stirring them for extraction, and separating the mixed solution after extraction to obtain an organic phase loaded with iron and aluminum ions and a raffinate; (3) The organic phase loaded with iron and aluminum ions is stripped with a stripping agent at a stripping temperature of 20-80 °C to obtain an aqueous solution containing iron and aluminum ions.

10. The use according to claim 9, characterized in that The diluent described in step (1) is one or more of aliphatic hydrocarbons, halogenated hydrocarbons, aromatic hydrocarbons, solvent oil and alcohol; the volume ratio of the wet-process phosphoric acid solution to the organic phase described in step (2) is 1:5~5:1, the extraction time is 1~120 min, and the extraction temperature is 10~90°C; the stripping agent in step (3) is 0.1~1 mol / L ammonium oxalate, and the stripping time is 10~120 min.

Citation Information

Patent Citations

  • Red mud resource-soil utilization treatment method

    CN111690810A

  • Method for preparing iron phosphate by extracting and separating iron and phosphorus from iron phosphate slag

    CN114804048A