A kind of cable resistant to ultraviolet aging and preparation method thereof
By using nano titanium dioxide and calcium carbonate composites in the cable to form a crosslinking network structure with anti-aging agents, the problem of degradation of existing cables in high temperature and high ultraviolet environments is solved, and the efficient anti-aging and mechanical performance of the cables are achieved.
Patent Information
- Application Number
- CN202411055224.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The performance of existing cable materials deteriorates under high temperature and high ultraviolet irradiation environments, is prone to cracking or brittleness, poses safety hazards, and has poor UV resistance.
Using a combination of PVC resin, plasticizer, linear low-density polyethylene, ethylene-octene copolymer, filler, flame retardant, calcium-zinc stabilizer, lubricant, anti-aging agent and cross-linking additive, through nanotitanium dioxide and Calcium carbonate composite material forms a hybrid crosslinking network structure with anti-aging agents to improve the UV resistance and mechanical properties of the cable.
It significantly improves the thermal oxygen aging resistance, UV aging resistance and mechanical properties of the cable, ensuring the long-term stability and safety of the cable in harsh environments.
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electric wires and cables, and in particular, relates to an anti-ultraviolet aging cable and a preparation method thereof. Background Art
[0002] Cable material is a polymer material used for insulation and protection of wires and cables, mainly divided into rubber, plastic, nylon and other categories. With the rapid development of the economy, wires and cables have been widely used in various industries and fields. PVC (polyvinyl chloride) cable is low in price and has excellent performance. It has long occupied an important position in the insulation and protection materials of wires and cables.
[0003] The research and development of cable materials usually needs to take into account the use environment of the cable, especially in areas with harsh environments. Cables are laid outdoors and are affected by direct sunlight, high and low temperatures, and corrosion. This makes the requirements for cable materials different from those of polymer materials used in daily necessities. Existing cable materials generally have good flame retardant properties, but poor UV resistance and heat resistance. Under long periods of time and in high temperature and high UV radiation environments outdoors, the performance of cable materials is significantly reduced, and they are prone to cracking or brittleness, posing a safety hazard. Therefore, PVC wires and cables must have good aging resistance. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a cable resistant to ultraviolet aging and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A cable resistant to ultraviolet aging comprises an insulating core and a sheath wrapped around the core.
[0007] Furthermore, the sheath comprises the following raw materials in parts by weight: 80-90 parts of PVC resin, 25-30 parts of plasticizer, 10-20 parts of linear low-density polyethylene, 10-20 parts of ethylene-octene copolymer, 12-18 parts of filler, 6-12 parts of flame retardant, 3-4 parts of calcium zinc stabilizer, 2-3 parts of lubricant, 1-2 parts of anti-aging agent, and 0.05-0.1 parts of cross-linking aid.
[0008] Furthermore, the plasticizer is one or more of dioctyl phthalate, epoxy soybean oil, diisononyl cyclohexane 1,2-dicarboxylate, and dioctyl sebacate.
[0009] Furthermore, the filler is prepared by the following steps:
[0010] Nano-titanium dioxide and calcium carbonate were placed in a beaker, mixed with deionized water, and concentrated hydrochloric acid was added to the beaker to adjust the pH value to 5. The mixture was then poured into a three-necked flask, stirred and heated to keep the mixture temperature at 55-75°C. Next, anhydrous ethanol and a coupling agent were mixed evenly and slowly added dropwise to the three-necked flask. After the addition was completed, heating and stirring were continued at 55-75°C for 10 hours, and finally cooled to room temperature. The mixture was filtered and washed with anhydrous ethanol for 5 times. After washing, the product was vacuum dried at 80°C for 12 hours to obtain a filler.
[0011] Furthermore, the mass ratio of the nano titanium dioxide to calcium carbonate is 1-3:1.
[0012] Furthermore, the coupling agent is one or more of vinyltrimethoxysilane, vinyltriethoxysilane, and 3-(methacryloyloxy)propyltrimethoxysilane.
[0013] Furthermore, the mass ratio of the total mass of the nano-titanium dioxide and calcium carbonate to the mass ratio of the coupling agent is 10-15:1.
[0014] Nano titanium dioxide has a small particle size and high activity. It can reflect and scatter ultraviolet rays, as well as absorb ultraviolet rays, thus having a stronger ability to block ultraviolet rays. Calcium carbonate can effectively improve the hardness and mechanical properties of the sheath. The mechanical properties and anti-ultraviolet ability of the sheath can be jointly improved by compounding and modifying nano titanium dioxide and calcium carbonate.
[0015] The silaneoxy end of the coupling agent is hydrolyzed and condensed, and cross-linked with the hydroxyl groups on the surface of nano-titanium dioxide and calcium carbonate, which greatly reduces the surface energy of the two inorganic materials, so that they are evenly dispersed in the cable sheath. The double bond end of the coupling agent can react chemically with the carbon-carbon double bond at the end of the antioxidant and the unreacted carbon-carbon double bond at the end of the matrix resin under the action of the cross-linking auxiliary agent, which forms a hybrid cross-linked network structure between the filler, the antioxidant, and the matrix resin, further promoting the high dispersion of the filler and the dispersion and stability of the antioxidant, so that the filler and the antioxidant can fully play their own role and improve the comprehensive performance of the cable sheath.
[0016] Furthermore, the flame retardant is one or more of melamine cyanurate, ammonium polyphosphate, and flame retardant FRC-2.
[0017] Furthermore, the lubricant is one or more of stearic acid, butyl stearate, zinc stearate, calcium stearate, and magnesium stearate.
[0018] Furthermore, the anti-aging agent is prepared by the following steps:
[0019] S1. Add 3,5-di-tert-butyl-4-hydroxycinnamic acid and DMSO (dimethyl sulfoxide) to a dry brown three-necked flask at room temperature, stir thoroughly to form a uniform solution, then slowly add 2-methylene-1,3-propanediol and concentrated sulfuric acid in turn, raise the temperature to 100-130°C after the addition is complete, and keep the temperature to react for 3-6 hours. Pour the reaction mixture into deionized water, stir and stand to separate until the pH of the aqueous phase is neutral, take the organic phase and dry it with anhydrous magnesium sulfate, filter it, and finally distill it under reduced pressure to obtain intermediate 1; the amount ratio of 3,5-di-tert-butyl-4-hydroxycinnamic acid, 2-methylene-1,3-propanediol, concentrated sulfuric acid and DMSO is 0.06mol:0.066mol:0.65mL:130mL;
[0020] Under heating and acidic conditions, the carboxyl group of 3,5-di-tert-butyl-4-hydroxycinnamic acid reacts with a hydroxyl group of 2-methylene-1,3-propanediol to undergo esterification. The reaction process is shown below:
[0021] ;
[0022] S2, dissolving intermediate 1 in DMF (N,N-dimethylformamide), stirring evenly, adding a mixed solution of UV-327 [2-(5-chloro-2H-benzotriazole-2-yl)-4,6-bis(1,1-dimethylethyl)phenol] and DMF, and then heating to 30-60°C and stirring for 4-6 hours. During this period, the pH value of the system was adjusted to 7 by 10wt% sodium carbonate solution. After the reaction was completed, it was cooled to room temperature and distilled under reduced pressure. It was first centrifuged and washed 3 times with deionized water, and then centrifuged and washed 3 times with anhydrous ethanol, and finally dried at 80°C for 12 hours to obtain intermediate 2; the amount ratio of intermediate 1, UV-327 and DMF was 0.054mol:0.05mol:200mL;
[0023] Under heating conditions, the -OH of intermediate 1 and the -Cl of UV-327 undergo a substitution reaction, and the reaction process is as follows:
[0024] ;
[0025] S3. Add intermediate 2, DBU (1,8-diazobispiro[5.4.0]undec-7-ene) and DMF to a fully dried three-necked flask, stir evenly, and then slowly add 2,2,6,6-tetramethylpiperidinamine. After the addition is complete, heat to 50-70°C and react for 36-48 hours. After the reaction is completed, distill under reduced pressure to obtain an antioxidant. The dosage ratio of intermediate 2, 2,2,6,6-tetramethylpiperidinamine, DBU and DMF is 0.049 mol: 0.045 mol: 1.35 mL: 180 mL.
[0026] Under the catalytic action of DBU, intermediate 2 undergoes Michael addition reaction with 2,2,6,6-tetramethylpiperidinamine. The reaction process is shown below:
[0027] ;
[0028] The anti-aging agent contains benzotriazole structure, hindered phenol structure and hindered amine structure. The benzotriazole structure can absorb 270-400nm ultraviolet light, with an absorption peak of 353nm, and has the characteristics of good compatibility, low volatility, good thermal stability, and high absorption efficiency; the hindered phenol structure has excellent antioxidant ability. Since the hydroxyl group of the hindered phenol structure is restricted by spatial barriers, the hydrogen atom can easily fall off from the original molecular structure, thereby achieving the effect of donating protons and combining with peroxyl radicals, alkyl radicals, hydroxyl radicals, etc., causing them to lose their original activity, resulting in the termination of the oxygen aging reaction; the hindered amine structure achieves light protection effect by capturing free radicals, decomposing hydroperoxides, quenching singlet oxygen, and capturing heavy metal ions, and the hindered amine structure has high light stability efficiency.
[0029] The antioxidant structure in the antioxidant - hindered phenol structure, hindered amine structure and ultraviolet absorption structure - benzotriazole structure can produce a good synergistic effect, giving the antioxidant excellent anti-ultraviolet aging and anti-thermal oxygen aging effects.
[0030] The benzene ring, heterocyclic ring and ester group in the anti-aging agent make the anti-aging agent compatible with other raw materials, and the anti-aging agent can be evenly dispersed in the sheath; the carbon-carbon double bonds in the anti-aging agent can react chemically with the double bonds on the surface of the filler and the double bonds at the end of the matrix resin that have not reacted completely under the action of the cross-linking auxiliary agent, and a hybrid cross-linking network structure is formed between the anti-aging agent, the filler and the matrix resin, so that the anti-aging agent can be further dispersed in the sheath and stably exist in the sheath, and it is not easy to migrate and fall out, and it can play an excellent anti-aging effect for a long time. At the same time, the benzotriazole structure of the anti-aging agent and the nano-titanium dioxide in the filler play an organic-inorganic synergistic role, giving the sheath a more excellent and stable anti-ultraviolet aging performance.
[0031] Furthermore, the cross-linking aid is one or more of dicumyl peroxide, benzoyl peroxide, and azobisisobutyronitrile.
[0032] A method for preparing a cable resistant to ultraviolet aging comprises the following steps:
[0033] PVC resin, linear low-density polyethylene, ethylene-octene copolymer, calcium zinc stabilizer and filler are mixed by weight at 70-80°C for 8-12 minutes, and the temperature is continued to rise to 105-115°C. Plasticizer, flame retardant, lubricant, anti-aging agent and cross-linking aid are added, and mixed at a high speed of 2000rpm for 5 minutes. The mixture is extruded, cooled and pelletized to obtain a mixed masterbatch, which is then extruded and coated on the surface of the insulating core through a twin-screw extruder to form a sheath. After cooling, a UV-resistant cable is obtained.
[0034] The beneficial effects of the present invention are as follows: the antioxidant, filler and matrix resin of the present invention interact with each other, thereby forming a relatively stable hybrid cross-linked network structure; the antioxidant containing benzotriazole structure, hindered phenol structure and hindered amine structure and the filler containing nano titanium dioxide and calcium carbonate can be highly dispersed and stably present in the sheath, and fully exert their functions, thereby giving the sheath of the present invention excellent and stable resistance to thermal oxidation aging, resistance to ultraviolet aging and mechanical properties, and thus the cable of the present invention has efficient and lasting anti-aging and mechanical properties. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1, preparation of an anti-aging agent, the specific steps are as follows:
[0037] S1. Add 16.6 g of 3,5-di-tert-butyl-4-hydroxycinnamic acid and 130 mL of DMSO to a dry 250 mL brown three-necked flask at room temperature, stir thoroughly until a uniform solution is obtained, then slowly add 5.4 mL of 2-methylene-1,3-propanediol and 0.65 mL of concentrated sulfuric acid in sequence, heat to 100 °C after the addition is completed, and keep the temperature to react for 5 h. Pour the reaction mixture into deionized water, stir and stand to separate until the pH of the aqueous phase is neutral, take the organic phase, dry it with anhydrous magnesium sulfate, filter it, and finally distill it under reduced pressure to obtain intermediate 1.
[0038] S2, 18.7g of intermediate 1 was dissolved in 100mL DMF, and after stirring evenly, a mixed solution of 17.9g UV-327 and 100mL DMF was added, and then the temperature was raised to 30°C and stirred for reaction for 5h. During this period, the pH value of the system was adjusted to 7 by 10wt% sodium carbonate solution. After the reaction was completed, the solution was cooled to room temperature and distilled under reduced pressure. The solution was first centrifuged and washed 3 times with deionized water, then centrifuged and washed 3 times with anhydrous ethanol, and finally dried at 80°C for 12h to obtain intermediate 2;
[0039] S3. Add 32.7 g of intermediate 2, 1.35 mL of DBU and 180 mL of DMF into a fully dried 500 mL three-necked flask, stir evenly, and then slowly add 7.7 mL of 2,2,6,6-tetramethylpiperidinamine. After the addition is complete, heat to 50°C and react for 42 hours. After the reaction is completed, distill under reduced pressure to obtain an anti-aging agent.
[0040] Example 2, preparing an anti-aging agent, the specific steps are as follows:
[0041] S1. Add 16.6 g of 3,5-di-tert-butyl-4-hydroxycinnamic acid and 130 mL of DMSO to a dry 250 mL brown three-necked flask at room temperature, stir thoroughly until a uniform solution is obtained, then slowly add 5.4 mL of 2-methylene-1,3-propanediol and 0.65 mL of concentrated sulfuric acid in sequence, heat to 130°C after the addition is completed, and keep the temperature to react for 3 hours. Pour the reaction mixture into deionized water, stir and stand to separate layers until the pH of the aqueous phase is neutral, take the organic phase, dry it with anhydrous magnesium sulfate, filter it, and finally distill it under reduced pressure to obtain intermediate 1.
[0042] S2, 18.7g of intermediate 1 was dissolved in 100mL DMF, and after stirring evenly, a mixed solution of 17.9g UV-327 and 100mL DMF was added, and then the temperature was raised to 60°C and stirred for 4h. During this period, the pH value of the system was adjusted to 7 by 10wt% sodium carbonate solution. After the reaction was completed, the solution was cooled to room temperature and distilled under reduced pressure. The solution was first centrifuged and washed 3 times with deionized water, then centrifuged and washed 3 times with anhydrous ethanol, and finally dried at 80°C for 12h to obtain intermediate 2;
[0043] S3. Add 32.7g of intermediate 2, 1.35mL of DBU and 180mL of DMF into a fully dried 500mL three-necked flask, stir evenly, and then slowly add 7.7mL of 2,2,6,6-tetramethylpiperidinamine. After the addition is complete, heat to 70°C and react for 36 hours. After the reaction is completed, distill under reduced pressure to obtain an anti-aging agent.
[0044] Example 3, preparing an anti-aging agent, the specific steps are as follows:
[0045] S1. Add 16.6 g of 3,5-di-tert-butyl-4-hydroxycinnamic acid and 130 mL of DMSO to a dry 250 mL brown three-necked flask at room temperature, stir thoroughly until a uniform solution is obtained, then slowly add 5.4 mL of 2-methylene-1,3-propanediol and 0.65 mL of concentrated sulfuric acid in sequence, heat to 110°C after the addition is completed, and keep the temperature to react for 4 hours. Pour the reaction mixture into deionized water, stir and stand to separate layers until the pH of the aqueous phase is neutral, take the organic phase, dry it with anhydrous magnesium sulfate, filter it, and finally distill it under reduced pressure to obtain intermediate 1.
[0046] S2, 18.7g of intermediate 1 was dissolved in 100mL DMF, and after stirring evenly, a mixed solution of 17.9g UV-327 and 100mL DMF was added, and then the temperature was raised to 50°C and stirred for 6h. During this period, the pH value of the system was adjusted to 7 by 10wt% sodium carbonate solution. After the reaction was completed, the solution was cooled to room temperature and distilled under reduced pressure. The solution was first centrifuged and washed 3 times with deionized water, then centrifuged and washed 3 times with anhydrous ethanol, and finally dried at 80°C for 12h to obtain intermediate 2;
[0047] S3. Add 32.7 g of intermediate 2, 1.35 mL of DBU and 180 mL of DMF into a fully dried 500 mL three-necked flask, stir evenly, and then slowly add 7.7 mL of 2,2,6,6-tetramethylpiperidinamine. After the addition is complete, heat to 60°C and react for 48 hours. After the reaction is completed, distill under reduced pressure to obtain an anti-aging agent.
[0048] Example 4, preparing an anti-aging agent, the specific steps are as follows:
[0049] The remaining steps remain unchanged, only step S3 of Example 3 is removed to prepare the anti-aging agent.
[0050] Example 5, preparing filler, the specific steps are as follows:
[0051] 16g of nano titanium dioxide and 8g of calcium carbonate were put into a 500mL beaker, mixed evenly with 200mL of deionized water, and concentrated hydrochloric acid was added to the beaker to adjust the pH value to 5. The mixture was then poured into a 500mL three-necked flask, stirred and heated to keep the mixture temperature at 65°C; then, 10mL of anhydrous ethanol and 2g of vinyltrimethoxysilane were mixed evenly and slowly added dropwise to the above three-necked flask. After the addition was completed, heating and stirring were continued at 65°C for 10h, and finally cooled to room temperature. The mixture was filtered and washed with anhydrous ethanol 5 times. After washing, the product was vacuum dried at 80°C for 12h to obtain a filler.
[0052] Example 6, preparing filler, the specific steps are as follows:
[0053] 18g of nano titanium dioxide and 6g of calcium carbonate were put into a 500mL beaker, mixed with 200mL of deionized water, and concentrated hydrochloric acid was added to the beaker to adjust the pH value to 5. The mixture was then poured into a 500mL three-necked flask, stirred and heated to keep the mixture temperature at 55°C. Next, 10mL of anhydrous ethanol and 1.6g of vinyltriethoxysilane were mixed and slowly added dropwise to the three-necked flask. After the addition was completed, heating and stirring were continued at 55°C for 10h, and finally cooled to room temperature. The mixture was filtered and washed with anhydrous ethanol for 5 times. After washing, the product was vacuum dried at 80°C for 12h to obtain a filler.
[0054] Example 7, preparing filler, the specific steps are as follows:
[0055] 12g of nano titanium dioxide and 12g of calcium carbonate were put into a 500mL beaker, mixed evenly with 200mL of deionized water, and concentrated hydrochloric acid was added to the beaker to adjust the pH value to 5. The mixture was then poured into a 500mL three-necked flask, stirred and heated to keep the mixture temperature at 75°C; then, 10mL of anhydrous ethanol and 2.4g of 3-(methacryloyloxy)propyltrimethoxysilane were mixed evenly and slowly added dropwise to the above three-necked flask. After the addition was completed, heating and stirring were continued at 75°C for 10h, and finally cooled to room temperature, the mixture was filtered, washed with anhydrous ethanol 5 times, and after washing, the product was vacuum dried at 80°C for 12h to obtain a filler.
[0056] Example 8, preparing a cable resistant to ultraviolet aging, the specific steps are as follows:
[0057] 80 parts of PVC resin, 10 parts of linear low-density polyethylene, 10 parts of ethylene-octene copolymer, 3 parts of calcium zinc stabilizer and 12 parts of filler prepared in Example 7 were mixed at 70°C for 8 minutes, and the temperature was continued to rise to 105°C. 12 parts of dioctyl phthalate, 13 parts of diisononyl cyclohexane 1,2-dicarboxylate, 6 parts of melamine cyanurate, 2 parts of zinc stearate, 1 part of the antioxidant prepared in Example 3 and 0.05 parts of azobisisobutyronitrile were added, and the mixture was mixed at a high speed of 2000 rpm for 5 minutes. The mixture was extruded, cooled and pelletized to obtain a mixed masterbatch, which was then extruded and coated on the surface of the insulating core through a twin-screw extruder to form a sheath to obtain a cable resistant to ultraviolet aging.
[0058] Example 9, preparing a cable resistant to ultraviolet aging, the specific steps are as follows:
[0059] 85 parts of PVC resin, 18 parts of linear low-density polyethylene, 16 parts of ethylene-octene copolymer, 3.5 parts of calcium zinc stabilizer and 15 parts of filler prepared in Example 6 were mixed at 75°C for 10 minutes by weight, and the temperature was continued to rise to 110°C. 28 parts of epoxidized soybean oil, 6 parts of ammonium polyphosphate, 5 parts of flame retardant FRC-2, 2.3 parts of stearic acid, 1.5 parts of anti-aging agent prepared in Example 3 and 0.08 parts of diisopropylbenzene peroxide were added, and the mixture was mixed at a high speed of 2000 rpm for 5 minutes. The mixture was extruded, cooled and pelletized to obtain a mixed masterbatch, which was then extruded and coated on the surface of the insulating core through a twin-screw extruder to form a sheath. After cooling, a cable resistant to ultraviolet aging was obtained.
[0060] Example 10: Preparation of a cable resistant to ultraviolet aging, the specific steps are as follows:
[0061] 90 parts of PVC resin, 20 parts of linear low-density polyethylene, 20 parts of ethylene-octene copolymer, 4 parts of calcium zinc stabilizer and 18 parts of filler prepared in Example 5 were mixed at 80°C for 12 minutes by weight, and the temperature was continued to rise to 115°C. 20 parts of cyclohexane 1,2-dicarboxylic acid diisononyl ester, 10 parts of dioctyl sebacate, 4 parts of melamine cyanurate, 4 parts of ammonium polyphosphate, 4 parts of flame retardant FRC-2, 1 part of butyl stearate, 2 parts of calcium stearate, 2 parts of the anti-aging agent prepared in Example 3 and 0.1 part of benzoyl peroxide were added, and the mixture was mixed at a high speed of 2000 rpm for 5 minutes, extruded, cooled, and pelletized to obtain a mixed masterbatch, which was then extruded and coated on the surface of the insulating core through a twin-screw extruder to form a sheath. After cooling, a cable resistant to ultraviolet aging was obtained.
[0062] Comparative Example 1: preparing a cable, the specific steps are as follows:
[0063] The remaining steps remain unchanged, only the anti-aging agent in Example 10 is replaced by the anti-aging agent prepared in Example 4, thereby preparing a cable.
[0064] Comparative Example 2: preparing a cable, the specific steps are as follows:
[0065] The remaining steps remain unchanged, except that the filler in Example 10 is replaced by 12 parts of untreated nano titanium dioxide and 6 parts of untreated calcium carbonate, thereby preparing a cable.
[0066] Comparative Example 3: preparing a cable, the specific steps are as follows:
[0067] The remaining steps remain unchanged, only the anti-aging agent in Comparative Example 2 is replaced by 1 part of ultraviolet absorber UV-327 and 1 part of antioxidant 1010, thereby preparing a cable.
[0068] Performance testing;
[0069] In order to facilitate the testing of the protective effect of the sheath on the insulated wire core, the mixed masterbatch prepared in Examples 8-10 and Comparative Examples 1-3 was extruded into a die groove coated with a release agent during the extrusion coating process. The die groove specification was 200×200×3mm, and a vertical pressure of 1.2MPa was applied at the same time. After spray cooling, the mold was demolded to make a film, and the samples were cut from the film for the following performance tests;
[0070] In order to verify the anti-aging property of the sample, a xenon lamp aging test chamber was used to conduct dry and wet accelerated aging tests. The aging test parameters were set as follows: the irradiation intensity was 75W / m 2 , the black mark temperature is 60±2℃, the dry-wet cycle is 100min illumination + 20min illumination and spraying, and the total test time is 720h; take out the samples after dry-wet accelerated aging and conduct relevant tests again.
[0071] The test results of all items are shown in Table 1:
[0072] Table 1
[0073] ;
[0074] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0075] The above contents are merely examples and explanations of the present invention. Any modifications or additions made by technicians in the technical field to the described specific embodiments or replacements with similar methods shall all fall within the protection scope of the present invention.
Claims
1. A UV-resistant cable, comprising an insulating core and a sheath wrapped around the core, characterized in that: The sheath comprises the following raw materials in parts by weight: 80-90 parts of PVC resin, 25-30 parts of plasticizer, 10-20 parts of linear low-density polyethylene, 10-20 parts of ethylene-octene copolymer, 12-18 parts of filler, 6-12 parts of flame retardant, 3-4 parts of calcium zinc stabilizer, 2-3 parts of lubricant, 1-2 parts of anti-aging agent, and 0.05-0.1 parts of cross-linking aid; The filler is prepared by the following steps: Add nano titanium dioxide, calcium carbonate and deionized water into a beaker, adjust the pH value to 5, pour into a flask, and keep the temperature at 55-75°C; add anhydrous ethanol and a coupling agent into the flask, stir at 55-75°C for 10 hours, cool, filter, wash, and dry to obtain a filler; The coupling agent is one or more of vinyl trimethoxy silane, vinyl triethoxy silane, and 3-(methacryloyloxy)propyl trimethoxy silane; The anti-aging agent is prepared by the following steps: S1. Add 3,5-di-tert-butyl-4-hydroxycinnamic acid and DMSO into a flask, stir, add 2-methylene-1,3-propanediol and concentrated sulfuric acid, react at 110° C. for 4 h, pour into deionized water, separate, take the organic phase, dry, filter, and distill under reduced pressure to obtain intermediate 1; S2, dissolving intermediate 1 in DMF, adding UV-327 and DMF, reacting at 50°C for 6h, during which the pH value of the system was adjusted to 7, cooling, distilling under reduced pressure, washing, and drying to obtain intermediate 2; S3, adding intermediate 2, DBU and DMF into a flask, stirring, adding 2,2,6,6-tetramethylpiperidinamine, reacting at 60° C. for 48 h, and distilling under reduced pressure to obtain an antioxidant; The chemical formula of the anti-aging agent is as follows: 。 2. The cable resistant to ultraviolet aging according to claim 1, characterized in that: The usage ratio of 3,5-di-tert-butyl-4-hydroxycinnamic acid, 2-methylene-1,3-propanediol, concentrated sulfuric acid and DMSO in step S1 is 0.06 mol: 0.066 mol: 0.65 mL: 130 mL; the usage ratio of intermediate 1, UV-327 and DMF in step S2 is 0.054 mol: 0.05 mol: 200 mL; the usage ratio of intermediate 2, 2,2,6,6-tetramethylpiperidinamine, DBU and DMF in step S3 is 0.049 mol: 0.045 mol: 1.35 mL: 180 mL.
3. The cable resistant to ultraviolet aging according to claim 1, characterized in that: The mass ratio of the nano titanium dioxide to calcium carbonate is 1-3:
1.
4. The cable resistant to ultraviolet aging according to claim 1, characterized in that: The mass ratio of the total mass of the nano-titanium dioxide and calcium carbonate to the mass of the coupling agent is 10-15:
1.
5. The cable resistant to ultraviolet aging according to claim 1, characterized in that: The plasticizer is one or more of dioctyl phthalate, epoxy soybean oil, diisononyl cyclohexane 1,2-dicarboxylate, and dioctyl sebacate.
6. The cable resistant to ultraviolet aging according to claim 1, characterized in that: The flame retardant is one or more of melamine cyanurate, ammonium polyphosphate, and flame retardant FRC-2.
7. The cable resistant to ultraviolet aging according to claim 1, characterized in that: The lubricant is one or more of stearic acid, butyl stearate, zinc stearate, calcium stearate, and magnesium stearate; the crosslinking aid is one or more of dicumyl peroxide, benzoyl peroxide, and azobisisobutyronitrile.
8. The method for preparing a UV-resistant cable according to claim 1, characterized in that: The following steps are involved: PVC resin, linear low-density polyethylene, ethylene-octene copolymer, calcium zinc stabilizer and filler are mixed by weight at 70-80°C for 8-12 minutes, and the temperature is continued to rise to 105-115°C. Plasticizer, flame retardant, lubricant, anti-aging agent and cross-linking aid are added, mixed for 5 minutes, extruded, cooled and pelletized to obtain a mixed masterbatch, which is then extruded and coated on the surface of the insulating core through a twin-screw extruder to form a sheath. After cooling, a UV-resistant cable is obtained.