A high-strength silicon carbide refractory material and preparation method thereof

By preparing composite ceramic powder and pre-modifying the surface, a stable structure and coating layer are formed, which solves the shortcomings of silicon carbide refractory materials in terms of high-temperature strength and thermal stress, improves its density and stability, and ensures that during rapid temperature changes performance stability.

CN118580089BActive Publication Date: 2024-10-11ZUNLONG NEW MATERIAL (SHANDONG) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068404.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-11
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Existing silicon carbide refractory materials have deficiencies in high-temperature strength and thermal stress, resulting in reduced density and stability, and are prone to problems such as deformation, cracks, and bubbling during rapid temperature changes.

Method used

The method of preparing composite ceramic powder, surface pre-modification and functional composite powder is used to form a stable structure through the combination of zirconium-based precursor powder, alumina, titanium oxide and silane coupling agent, and amino groups and rings are introduced on the surface. Oxygen group forms a coating layer to improve the bonding performance and fire resistance of silicon carbide materials.

Benefits of technology

It effectively eliminates the interface bonding problem between raw materials, improves the density and high-temperature stability of silicon carbide refractory materials, reduces thermal stress defects, and enhances its stability and long-term performance during rapid temperature changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a high-strength silicon carbide refractory material and a preparation method thereof, which belongs to the field of refractory materials. The preparation method of the high-strength silicon carbide refractory material consists of the following steps: preparing composite ceramic powder, surface pre-modification, preparing functional composite powder, and molding. The high-strength silicon carbide refractory material and the preparation method thereof of the present invention can effectively eliminate the interface bonding problem between the raw materials caused by the introduction of the reinforcing phase, while improving the high-temperature strength of the silicon carbide refractory material, further improving the density and overall stability of the silicon carbide refractory material; and effectively reducing the thermal stress defects of the silicon carbide refractory material, improving the stability of the silicon carbide refractory material in the process of rapid temperature change, and improving its long-term stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of refractory materials, in particular to a high-strength silicon carbide refractory material and a preparation method thereof. Background Art

[0002] Since silicon carbide was discovered by E. G. Acheson in 1891 and used in electric furnace production, it has been often used as artificial abrasives due to its high hardness; it was later used in the field of high-temperature materials in 1893. Silicon carbide refractory materials are a kind of high-quality refractory materials that people have long known, with high strength, high thermal conductivity, good shock resistance, wear resistance, erosion resistance and other excellent properties; the thermal conductivity of silicon carbide refractory materials is about 10-14 times that of clay products; it can resist the erosion of various acids, alkalis and salts, has good chemical stability, and is widely used in metallurgy, chemical industry, ceramics and other industrial fields.

[0003] The original silicon carbide refractory material is made of silicon carbide as the main raw material, clay, silicon dioxide, silicate, mullite, etc. as binders, and is made by pressing or ramming into shape and then firing at high temperature. In the existing technology, modified silicon carbide products have been widely developed, including silicon carbide materials such as silicon nitride bonded silicon carbide, silicon oxynitride bonded silicon carbide, reaction sintered silicon carbide (self-bonded silicon carbide), recrystallized silicon carbide (R-silicon carbide), silicon-infiltrated silicon carbide (Si-silicon carbide), etc., further expanding the application range of silicon carbide products.

[0004] However, the existing silicon carbide refractory materials still have poor high-temperature strength and thermal stress defects, which seriously restrict the application of silicon carbide refractory materials. In view of the above technical defects, in the prior art, reinforcing phases such as reinforcing fibers and reinforcing ceramic particles are usually added to the raw materials of silicon carbide refractory materials to improve the high-temperature strength of silicon carbide refractory materials, but the introduction of reinforcing phases will lead to interface bonding problems between the raw materials, which will lead to reduced density and overall stability of silicon carbide refractory materials. At the same time, in view of the thermal stress defects of silicon carbide refractory materials, in the process of reducing its thermal stress by heat treatment, it will further lead to a reduction in the uniformity of the organizational distribution of silicon carbide materials, which not only affects the performance stability of silicon carbide refractory materials, but also causes silicon carbide refractory materials to be prone to deformation, cracks, bubbling and other problems during rapid temperature changes, and cannot maintain ideal long-term performance.

[0005] Thus, a high-strength silicon carbide refractory material and a preparation method thereof are provided, which can effectively eliminate the interface bonding problem between the raw materials caused by the introduction of the reinforcing phase, and while improving the high-temperature performance of the silicon carbide refractory material, further improve the density and overall stability of the silicon carbide refractory material; and effectively reduce the thermal stress defects of the silicon carbide refractory material, improve the stability of the silicon carbide refractory material in the process of rapid temperature change, and improve its long-term stability, which has important technical significance. Summary of the invention

[0006] In order to solve the technical problems existing in the prior art, the present invention provides a high-strength silicon carbide refractory material and a preparation method thereof, which can effectively eliminate the interface bonding problem between the raw materials caused by the introduction of the reinforcing phase, while improving the high-temperature strength of the silicon carbide refractory material, further improve the density and overall stability of the silicon carbide refractory material; and effectively reduce the thermal stress defects of the silicon carbide refractory material, improve the stability of the silicon carbide refractory material in the process of rapid temperature change, and improve its long-term stability.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0008] A high-strength silicon carbide refractory material and a preparation method thereof, comprising the following steps: preparing composite ceramic powder, pre-modifying the surface, preparing functional composite powder, and molding.

[0009] The preparation of the composite ceramic powder comprises the following steps: preparing zirconium-based precursor powder and composite treatment.

[0010] The method for preparing the zirconium-based precursor powder is as follows: zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide are added into deionized water, ultrasonically dispersed for 10-20 minutes, and then stirred for 30-40 minutes; under stirring, ammonia water is added dropwise to adjust the pH to 8-8.5, and then the mixture is transferred into an autoclave, the autoclave is sealed, and the temperature is increased to 150-160° C. at a heating rate of 2-2.5° C. / min, and the mixture is subjected to hydrothermal treatment at the temperature for 22-24 hours, and then naturally cooled to room temperature, and solid matter is collected by centrifugation at 7000-8000 rpm, and the solid matter is washed with 2-3 times the weight of deionized water, and then placed in a vacuum drying oven, and dried to constant weight at 100-110° C. under a vacuum degree of 0.07-0.08 MPa, to obtain the zirconium-based precursor powder.

[0011] In the preparation of the zirconium-based precursor powder, the weight ratio of zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide is 90-95:1-1.3:1.8-2.1:0.8-0.9;

[0012] The mass concentration of ammonia water is 23-25wt%.

[0013] The composite treatment method comprises the following steps: putting zirconium-based precursor powder, aluminum oxide powder, titanium oxide powder, silane coupling agent A-174 and ethanol solution into a ball mill, controlling the ball-to-material ratio to be 6-6.5:1, the ball milling speed to be 250-260 rpm, and performing ball milling for 2-3 hours to obtain a ball milled product; placing the ball milled product in a drying oven, drying it at 110-120° C. to a constant weight, and crushing it into a composite powder with a particle size of 7-10 μm; then transferring the composite powder into a calcining furnace, controlling the heating rate to be 3-4° C. / min, heating it to 1300-1400° C., and calcining it at the temperature for 40-60 minutes, pouring the calcined molten liquid onto a stainless steel plate for stamping, cooling it and crushing it to 10-20 μm to obtain a composite ceramic powder.

[0014] In the composite treatment, the weight ratio of zirconium-based precursor powder, aluminum oxide powder, titanium oxide powder, silane coupling agent A-174, and ethanol solution is 22-25:42-46:3-3.5:0.4-0.5:34-35;

[0015] The volume concentration of the ethanol solution is 70-75%.

[0016] The surface pre-modification method comprises the following steps: adding composite ceramic powder, aluminum-titanium master alloy powder and sepiolite powder into an ethanol solution, stirring for 15-30 minutes, heating to 40-45° C. with stirring, and keeping the temperature; then, dripping silane coupling agent KH-560 and silane coupling agent KH-792 at the same time under stirring conditions, and controlling the dripping time of silane coupling agent KH-560 and silane coupling agent KH-792 to be 50-60 minutes; after the dripping is completed, continuing to keep the temperature and stir for 4-5 hours, filtering out solid matter, washing the solid matter with 1.2-1.8 times the weight of anhydrous ethanol, and then adding the solid matter into 7.5-8 times the weight of anhydrous ethanol, stirring evenly, and obtaining a pre-modified dispersion.

[0017] In the surface pre-modification, the weight ratio of the composite ceramic powder, the aluminum-titanium master alloy powder, the sepiolite powder, the ethanol solution, the silane coupling agent KH-560, and the silane coupling agent KH-792 is 15-17:7-7.5:4.2-4.8:105-110:2-2.3:1.2-1.4;

[0018] The titanium content in the aluminum-titanium master alloy powder is 9.5-11wt% and the particle size is 40-50μm;

[0019] The particle size of sepiolite powder is 22-30 μm.

[0020] The method for preparing the functional composite powder comprises the following steps: adding tetraethoxysilane and n-dodecyltrimethoxysilane into anhydrous ethanol, uniformly dispersing them by ultrasonication, preparing a modified liquid for standby use; adding ammonia water into an ethanol solution with a volume concentration of 89-91%, uniformly dispersing them by ultrasonication, preparing a promoting liquid for standby use; stirring the pre-modified dispersed liquid and heating it to 40-42° C. and keeping it warm; then dripping the modified liquid and the promoting liquid at 320-360 rpm at the same time, and controlling the dripping time of the modified liquid and the promoting liquid to be 15-20 min; after the dripping is completed, keeping the temperature for reaction for 4-5 hours, filtering out the solid, washing the solid with 2.5-3 times the weight of anhydrous ethanol, placing it in a vacuum drying oven, drying it to constant weight at 70-75° C. under a vacuum degree of 0.08-0.09 MPa, and crushing it to prepare the functional composite powder.

[0021] In the preparation of the functional composite powder, the weight ratio of tetraethoxysilane, n-dodecyltrimethoxysilane and anhydrous ethanol in the modified liquid is 2.4-2.7:1.6-1.9:33-35;

[0022] The weight ratio of ammonia water to ethanol solution in the promoting liquid is 5.8-6:40-41;

[0023] The mass concentration of ammonia water is 23-25wt%;

[0024] The weight ratio of the pre-modified dispersion liquid, the modified liquid and the promoting liquid is 80-83:38-40:44-45.

[0025] The molding method comprises the following steps: putting silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate into a mixer and mixing them evenly, and then pressing and molding the green body under a pressure of 150-180 MPa to obtain a green body; transferring the green body into a drying oven, drying the green body at 105-110° C. for 22-28 hours, transferring the green body into a calcining furnace, calcining the green body at 1200-1250° C. for 4-5 hours in a nitrogen atmosphere, and naturally cooling the green body to room temperature to obtain a high-strength silicon carbide refractory material.

[0026] In the molding process, the weight ratio of silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate is 84-88:10-13:3-3.5:1.8-2.3.

[0027] A high-strength silicon carbide refractory material is prepared by the above-mentioned preparation method.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The preparation method of the high-strength silicon carbide refractory material of the present invention comprises the following steps: in the step of preparing a zirconium-based precursor powder in preparing a composite ceramic powder, firstly, zirconium oxychloride is combined with magnesium salt, lanthanum salt and hexadecyltrimethylammonium bromide to prepare magnesium / lanthanum composite stabilized zirconium oxide, thereby stabilizing the crystal structure and improving the physical properties of the zirconium-based precursor powder and its compatibility with other raw materials; then, the zirconium-based precursor powder is combined with aluminum oxide and titanium oxide to obtain a composite ceramic powder with good structural stability and good mechanical properties; then, in the surface pre-modification step, an aminosilane coupling agent and an epoxysilane coupling agent are combined to prepare the composite ceramic powder; The ceramic powder, aluminum-titanium master alloy powder and sepiolite powder are pre-modified on the surface, and while improving the bonding performance of the aforementioned components, amino groups and epoxy groups are introduced on the surface to promote the subsequent step of preparing a functional composite powder and improve its subsequent bonding performance with the coating film layer; and the introduction of the aluminum-titanium master alloy and sepiolite in this step can further improve the refractory performance of the silicon carbide refractory material, improve the pore distribution of the silicon carbide refractory material, and improve the overall stability and high-temperature stability of the silicon carbide refractory material; then in the step of preparing the functional powder, tetraethoxysilane and n-dodecyl tris(III) are used to prepare the functional composite powder. Methoxysilane is hydrolyzed and condensed on the outer surface of the aforementioned composite ceramic powder, aluminum-titanium master alloy, and sepiolite composite material to form a coating layer, thereby improving the surface performance of the functional composite powder. In the subsequent process of combining with silicon carbide to prepare refractory materials, the bonding performance of the functional composite powder and silicon carbide is effectively improved, the interface bonding problem with raw materials such as silicon carbide is effectively avoided, the overall stability and density of silicon carbide refractory materials are improved, and the thermal stress defect problems such as reduced uniformity of the organizational structure of silicon carbide refractory materials caused by calcination and high-temperature working environment are effectively avoided, and the silicon carbide refractory materials are further improved in the process of rapid temperature change. stability, improve its long-term stability, and improve the overall mechanical properties of silicon carbide refractory materials; the above-mentioned technical means cooperate with each other and work synergistically to obtain high-strength silicon carbide refractory materials, which can effectively eliminate the interface bonding problem between the raw materials caused by the introduction of the reinforcing phase while obtaining high-strength mechanical properties, and further improve the density and overall stability of silicon carbide refractory materials while improving the high-temperature strength of silicon carbide refractory materials; and effectively reduce the thermal stress defects of silicon carbide refractory materials, improve the stability of silicon carbide refractory materials in the process of rapid temperature change, and improve their long-term stability.

[0030] (2) The high-strength silicon carbide refractory material of the present invention has an apparent porosity of 11.2-11.5%, a room temperature flexural strength of 63.5-64.1 MPa, a room temperature compressive strength of 274.6-275.3 MPa, a high temperature (1400°C) flexural strength of 61.1-62.0 MPa, and a pore size of less than 1 μm accounts for 92-93%.

[0031] (3) In the decarburization layer thickness test of the high-strength silicon carbide refractory material of the present invention, the test temperature is set at 1400°C, the holding time is 2.5h, and the decarburization layer thickness is 0.06-0.07mm; in the heating permanent line change test, the test temperature is set at 1300°C, and the heating permanent line change is 0.45-0.47%.

[0032] (4) The high-strength silicon carbide refractory material of the present invention is heated to 1100°C at a heating rate of 30°C / min, kept warm for 30 minutes, and then air-cooled to room temperature; after the aforementioned 20 times of rapid heating and air cooling, no deformation, cracking, or blistering occurs, and the room-temperature compressive strength of the high-strength silicon carbide refractory material can still reach 250.2-252.5MPa, and the high-temperature (1400°C) flexural strength can still reach 55.5-56.6MPa, and the high-temperature (1400°C) flexural strength retention rate is 90.8-91.3%. DETAILED DESCRIPTION

[0033] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0034] Example 1

[0035] This embodiment provides a method for preparing a high-strength silicon carbide refractory material, specifically:

[0036] 1. Preparation of composite ceramic powder

[0037] 1) Preparation of zirconium-based precursor powder

[0038] Zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide were put into deionized water, ultrasonically dispersed for 10 minutes, and stirred for 30 minutes. Under stirring, ammonia water was added dropwise to adjust the pH to 8, and then the mixture was transferred into an autoclave. The autoclave was sealed and heated to 150°C at a heating rate of 2°C / min. After heat treatment with water for 22 hours, the mixture was naturally cooled to room temperature, and solids were collected by centrifugation at 7000 rpm. The solids were washed with twice the weight of deionized water, and then placed in a vacuum drying oven. The mixture was dried to constant weight at 100°C under a vacuum degree of 0.07 MPa to obtain a zirconium-based precursor powder.

[0039] Wherein, the weight ratio of zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide is 90:1:1.8:0.8.

[0040] The mass concentration of ammonia water is 23wt%.

[0041] 2) Composite treatment

[0042] Zirconium-based precursor powder, alumina powder, titanium oxide powder, silane coupling agent A-174 and ethanol solution are put into a ball mill, the ball-to-material ratio is controlled to be 6:1, the ball mill speed is 250rpm, and the ball milling treatment is carried out for 2 hours to obtain a ball-milled product; the ball-milled product is placed in a drying oven, dried to constant weight at 110°C, and then crushed into a composite powder with a particle size of 7μm; then the composite powder is transferred into a calcining furnace, the heating rate is controlled to be 3°C / min, the temperature is raised to 1300°C, and after calcining for 40 minutes, the calcined molten liquid is poured onto a stainless steel plate for stamping treatment, and then cooled and crushed to 10μm to obtain a composite ceramic powder.

[0043] Among them, the weight ratio of zirconium-based precursor powder, aluminum oxide powder, titanium oxide powder, silane coupling agent A-174, and ethanol solution is 22:42:3:0.4:34.

[0044] The volume concentration of the ethanol solution is 70%.

[0045] 2. Surface pre-modification

[0046] Composite ceramic powder, aluminum-titanium intermediate alloy powder and sepiolite powder are put into an ethanol solution, stirred for 15 minutes, heated to 40°C with stirring, and kept warm; then, silane coupling agent KH-560 and silane coupling agent KH-792 are added dropwise at the same time under stirring, and the dropping time of silane coupling agent KH-560 and silane coupling agent KH-792 is controlled to be 50 minutes; after the dropping is completed, the stirring is continued for 4 hours, the solid matter is filtered out, the solid matter is washed with 1.2 times the weight of anhydrous ethanol, and the solid matter is put into 7.5 times the weight of anhydrous ethanol, stirred evenly, and a pre-modified dispersion is obtained.

[0047] Among them, the weight ratio of composite ceramic powder, aluminum-titanium intermediate alloy powder, sepiolite powder, ethanol solution, silane coupling agent KH-560 and silane coupling agent KH-792 is 15:7:4.2:105:2:1.2.

[0048] The titanium content in the aluminum-titanium master alloy powder is 10.5wt% and the particle size is 45μm.

[0049] The particle size of the sepiolite powder is 25 μm.

[0050] 3. Preparation of functional composite powder

[0051] Tetraethoxysilane and n-dodecyltrimethoxysilane were added to anhydrous ethanol, and ultrasonically dispersed them uniformly to obtain a modified liquid for standby use; ammonia water was added to an ethanol solution with a volume concentration of 89%, and ultrasonically dispersed them uniformly to obtain a promoting liquid for standby use; the pre-modified dispersion was stirred and heated to 40°C and kept warm; then, the modified liquid and the promoting liquid were dripped into the solution at the same time under stirring at 320rpm, and the dripping time of the modified liquid and the promoting liquid was controlled to be 15min; after the dripping was completed, the solution was kept warm for 4h, the solid was filtered out, and the solid was washed with 2.5 times the weight of anhydrous ethanol, and then placed in a vacuum drying oven, dried at 70°C to constant weight under a vacuum degree of 0.08MPa, and crushed to obtain a functional composite powder.

[0052] The weight ratio of tetraethoxysilane, n-dodecyltrimethoxysilane and anhydrous ethanol in the modified liquid is 2.4:1.6:33.

[0053] The weight ratio of ammonia water to ethanol solution in the promoting liquid is 5.8:40.

[0054] The mass concentration of ammonia water is 23wt%.

[0055] The weight ratio of the pre-modified dispersion liquid, the modified liquid and the accelerating liquid is 80:38:44.

[0056] 4. Molding

[0057] Silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate are put into a mixer and mixed evenly, and then pressed under a pressure of 150 MPa to obtain a green body; the green body is transferred to a drying oven, dried at 105°C for 22 hours, transferred to a calcining furnace, calcined at 1200°C for 4 hours in a nitrogen atmosphere, and naturally cooled to room temperature to obtain a high-strength silicon carbide refractory material.

[0058] Among them, the weight ratio of silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate is 84:10:3:1.8.

[0059] This embodiment also provides a high-strength silicon carbide refractory material, which is prepared using the aforementioned preparation method.

[0060] Example 2

[0061] This embodiment provides a method for preparing a high-strength silicon carbide refractory material, specifically:

[0062] 1. Preparation of composite ceramic powder

[0063] 1) Preparation of zirconium-based precursor powder

[0064] Zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide were put into deionized water, ultrasonically dispersed for 15 minutes, and stirred for 350 minutes. Under stirring, ammonia water was added dropwise to adjust the pH to 8.2, and then the mixture was transferred into an autoclave. The autoclave was sealed and heated to 155°C at a heating rate of 2.3°C / min. After heat treatment with water for 23 hours, the mixture was naturally cooled to room temperature, and solids were collected by centrifugation at 7500rpm. The solids were washed with 2.5 times the weight of deionized water, and then placed in a vacuum drying oven. The mixture was dried to constant weight at 105°C under a vacuum degree of 0.075MPa to obtain a zirconium-based precursor powder.

[0065] Among them, the weight ratio of zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide is 93:1.2:2:0.85.

[0066] The mass concentration of ammonia water is 24wt%.

[0067] 2) Composite treatment

[0068] Zirconium-based precursor powder, alumina powder, titanium oxide powder, silane coupling agent A-174 and ethanol solution are put into a ball mill, the ball-to-material ratio is controlled to be 6.3:1, the ball mill speed is 255 rpm, and the ball milling treatment is carried out for 2.5 hours to obtain a ball-milled product; the ball-milled product is placed in a drying oven, dried to constant weight at 115°C, and then crushed into a composite powder with a particle size of 8 μm; then the composite powder is transferred into a calcining furnace, the heating rate is controlled to be 3.5°C / min, the temperature is raised to 1350°C, and after calcining for 50 minutes, the calcined molten liquid is poured onto a stainless steel plate for stamping treatment, and then cooled and crushed to 12 μm to obtain a composite ceramic powder.

[0069] Among them, the weight ratio of zirconium-based precursor powder, aluminum oxide powder, titanium oxide powder, silane coupling agent A-174, and ethanol solution is 23.5:44:3.3:0.45:34.5.

[0070] The volume concentration of the ethanol solution is 72%.

[0071] 2. Surface pre-modification

[0072] Composite ceramic powder, aluminum-titanium intermediate alloy powder and sepiolite powder are put into an ethanol solution, stirred for 20 minutes, heated to 42°C with stirring, and kept warm; then, silane coupling agent KH-560 and silane coupling agent KH-792 are added dropwise at the same time under stirring, and the dropping time of silane coupling agent KH-560 and silane coupling agent KH-792 is controlled to be 55 minutes; after the dropping is completed, the stirring is continued for 4.5 hours, the solid matter is filtered out, the solid matter is washed with 1.5 times the weight of anhydrous ethanol, and the solid matter is put into 7.8 times the weight of anhydrous ethanol, stirred evenly, and a pre-modified dispersion is obtained.

[0073] Among them, the weight ratio of composite ceramic powder, aluminum-titanium intermediate alloy powder, sepiolite powder, ethanol solution, silane coupling agent KH-560 and silane coupling agent KH-792 is 16:7.3:4.5:108:2.2:1.3.

[0074] The titanium content in the aluminum-titanium master alloy powder is 10.5wt% and the particle size is 45μm.

[0075] The particle size of the sepiolite powder is 25 μm.

[0076] 3. Preparation of functional composite powder

[0077] Tetraethoxysilane and n-dodecyltrimethoxysilane were added to anhydrous ethanol, and ultrasonically dispersed them uniformly to obtain a modified liquid for standby use; ammonia water was added to an ethanol solution with a volume concentration of 90%, and ultrasonically dispersed them uniformly to obtain a promoting liquid for standby use; the pre-modified dispersion was stirred and heated to 41°C and kept warm; then, the modified liquid and the promoting liquid were dripped into the solution at the same time under stirring at 350rpm, and the dripping time of the modified liquid and the promoting liquid was controlled to be 18min; after the dripping was completed, the solution was kept warm for 4.5h, the solid was filtered out, and the solid was washed with 2.8 times the weight of anhydrous ethanol, and then placed in a vacuum drying oven, dried at 72°C to constant weight under a vacuum degree of 0.085MPa, and crushed to obtain a functional composite powder.

[0078] The weight ratio of tetraethoxysilane, n-dodecyltrimethoxysilane and anhydrous ethanol in the modified liquid is 2.6:1.7:34.

[0079] The weight ratio of ammonia water to ethanol solution in the promoting liquid is 5.9:40.5.

[0080] The mass concentration of ammonia water is 24wt%.

[0081] The weight ratio of the pre-modified dispersion liquid, the modified liquid, and the promoting liquid is 82:39:44.5.

[0082] 4. Molding

[0083] Silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate are put into a mixer and mixed evenly, and then pressed under a pressure of 170 MPa to obtain a green body; the green body is transferred to a drying oven, dried at 108°C for 24 hours, transferred to a calcining furnace, calcined at 1230°C for 4.5 hours in a nitrogen atmosphere, and naturally cooled to room temperature to obtain a high-strength silicon carbide refractory material.

[0084] Among them, the weight ratio of silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate is 86:12:3.3:2.1.

[0085] This embodiment also provides a high-strength silicon carbide refractory material, which is prepared using the aforementioned preparation method.

[0086] Example 3

[0087] This embodiment provides a method for preparing a high-strength silicon carbide refractory material, specifically:

[0088] 1. Preparation of composite ceramic powder

[0089] 1) Preparation of zirconium-based precursor powder

[0090] Zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide were put into deionized water, ultrasonically dispersed for 20 minutes, and stirred for 40 minutes. Under stirring, ammonia water was added dropwise to adjust the pH to 8.5, and then the mixture was transferred into an autoclave. The autoclave was sealed and heated to 160°C at a heating rate of 2.5°C / min. After heat treatment with water for 24 hours, the mixture was naturally cooled to room temperature, and solids were collected by centrifugation at 8000rpm. The solids were washed with 3 times the weight of deionized water, and then placed in a vacuum drying oven. The mixture was dried to constant weight at 110°C under a vacuum degree of 0.08MPa to obtain a zirconium-based precursor powder.

[0091] Among them, the weight ratio of zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide is 95:1.3:2.1:0.9.

[0092] The mass concentration of ammonia water is 25wt%.

[0093] 2) Composite treatment

[0094] Zirconium-based precursor powder, alumina powder, titanium oxide powder, silane coupling agent A-174 and ethanol solution are put into a ball mill, the ball-to-material ratio is controlled to be 6.5:1, the ball mill speed is 260 rpm, and the ball milling treatment is carried out for 3 hours to obtain a ball-milled product; the ball-milled product is placed in a drying oven, dried to constant weight at 120°C, and then crushed into a composite powder with a particle size of 10 μm; then the composite powder is transferred into a calcining furnace, the heating rate is controlled to be 4°C / min, the temperature is raised to 1400°C, and after calcining for 60 minutes, the calcined molten liquid is poured onto a stainless steel plate for stamping treatment, and then cooled and crushed to 20 μm to obtain a composite ceramic powder.

[0095] Wherein, the weight ratio of zirconium-based precursor powder, alumina powder, titanium oxide powder, silane coupling agent A-174 and ethanol solution is 25:46:3.5:0.5:35.

[0096] The volume concentration of the ethanol solution is 75%.

[0097] 2. Surface pre-modification

[0098] Composite ceramic powder, aluminum-titanium intermediate alloy powder and sepiolite powder are put into an ethanol solution, stirred for 30 minutes, heated to 45°C with stirring and kept warm; then, silane coupling agent KH-560 and silane coupling agent KH-792 are added dropwise at the same time under stirring, and the dropping time of silane coupling agent KH-560 and silane coupling agent KH-792 is controlled to be 60 minutes; after the dropping is completed, the stirring is continued for 5 hours, the solid matter is filtered out, the solid matter is washed with 1.8 times the weight of anhydrous ethanol, and the solid matter is put into 8 times the weight of anhydrous ethanol, stirred evenly, and a pre-modified dispersion is obtained.

[0099] Among them, the weight ratio of composite ceramic powder, aluminum-titanium intermediate alloy powder, sepiolite powder, ethanol solution, silane coupling agent KH-560 and silane coupling agent KH-792 is 17:7.5:4.8:110:2.3:1.4.

[0100] The titanium content in the aluminum-titanium master alloy powder is 11wt% and the particle size is 50μm.

[0101] The particle size of the sepiolite powder is 30 μm.

[0102] 3. Preparation of functional composite powder

[0103] Tetraethoxysilane and n-dodecyltrimethoxysilane were added to anhydrous ethanol, and ultrasonically dispersed them uniformly to obtain a modified liquid for standby use; ammonia water was added to an ethanol solution with a volume concentration of 91%, and ultrasonically dispersed them uniformly to obtain a promoting liquid for standby use; the pre-modified dispersion was stirred and heated to 42°C, and kept warm; then, the modified liquid and the promoting liquid were dripped into the solution at the same time under stirring at 360rpm, and the dripping time of the modified liquid and the promoting liquid was controlled to be 20min; after the dripping was completed, the solution was kept warm for 5h, the solid was filtered out, and the solid was washed with 3 times the weight of anhydrous ethanol, and then placed in a vacuum drying oven, dried at 75°C to constant weight under a vacuum degree of 0.09MPa, and crushed to obtain a functional composite powder.

[0104] The weight ratio of tetraethoxysilane, n-dodecyltrimethoxysilane and anhydrous ethanol in the modified liquid is 2.7:1.9:35.

[0105] The weight ratio of ammonia water to ethanol solution in the promoting liquid is 6:41.

[0106] The mass concentration of ammonia water is 25wt%.

[0107] The weight ratio of the pre-modified dispersion liquid, the modified liquid, and the accelerating liquid is 83:40:45.

[0108] 4. Molding

[0109] Silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate are put into a mixer and mixed evenly, and then pressed under a pressure of 180 MPa to obtain a green body; the green body is transferred to a drying oven, dried at 110°C for 28 hours, transferred to a calcining furnace, calcined at 1250°C for 5 hours in a nitrogen atmosphere, and naturally cooled to room temperature to obtain a high-strength silicon carbide refractory material.

[0110] Among them, the weight ratio of silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate is 88:13:3.5:2.3.

[0111] This embodiment also provides a high-strength silicon carbide refractory material, which is prepared using the aforementioned preparation method.

[0112] Comparative Example 1

[0113] The technical scheme of Example 2 is adopted, but the differences are as follows: 1) in the preparation of the composite ceramic powder, the step of preparing the zirconium-based precursor powder is omitted; and in the subsequent composite treatment step, an equal amount of zirconium oxide powder is used to replace the zirconium-based precursor powder; 2) the surface pre-modification step is omitted, and the composite ceramic powder, aluminum-titanium intermediate alloy powder, and sepiolite powder are mixed evenly, added into 7.8 times the weight of anhydrous ethanol, stirred evenly, and used as a pre-modified dispersion for subsequent steps.

[0114] Comparative Example 2

[0115] The technical solution of Example 2 is adopted, but the differences are as follows: 1) in the surface pre-modification step, the use of sepiolite powder and silane coupling agent KH-792 is omitted; 2) the step of preparing the functional composite powder is omitted, and the solid obtained by the surface pretreatment in the previous step is washed and dried to obtain a dry product; the dry product is used to replace the functional composite powder in an equal amount for use in the molding step.

[0116] The apparent porosity, room temperature flexural strength, room temperature compressive strength, high temperature (1400°C) flexural strength, decarburization layer thickness, and heating permanent line change of the silicon carbide refractory materials of Examples 1-3 and Comparative Examples 1-2 were tested respectively; and the proportion of pores with a diameter less than 1 μm in the silicon carbide refractory materials was counted.

[0117] Among them, the detection of apparent porosity refers to GB / T 2997-2015 "Test method for bulk density, apparent porosity and true porosity of dense shaped refractory products".

[0118] The test of room temperature flexural strength and high temperature flexural strength refers to GB / T 3001-2017 "Test method for flexural strength of refractory materials at room temperature".

[0119] The test of room temperature compressive strength refers to GB / T 5072-2023 "Test method for room temperature compressive strength of refractory materials".

[0120] The detection of decarburized layer thickness refers to GB / T 17732-2008 "Test method for dense shaped carbon-containing refractory products"; among them, the test temperature is set to 1400℃ and the holding time is set to 2.5h.

[0121] The detection of permanent linear changes upon heating refers to the length measuring instrument method of GB / T 5988-2022 "Test method for permanent linear changes upon heating of refractory materials", and the test temperature is set to 1300°C.

[0122] The specific results are shown in the following table:

[0123]

[0124] Further, the silicon carbide refractory materials of Examples 1-3 and Comparative Examples 1-2 were made into rectangular parallelepiped samples of 115mm×65mm×65mm, and each sample was placed in a high-temperature resistance furnace, and the heating rate was controlled to be 30℃ / min, and the temperature was raised to 1100℃. After keeping the temperature for 30 minutes, the sample was taken out and the sample was blown to room temperature with a pressure of 0.1MPa of normal temperature compressed air; after repeating the aforementioned rapid heating and air cooling process 20 times, each sample was observed for deformation, cracks, and bubbling; and the room temperature compressive strength and high temperature (1400℃) flexural strength of each sample were tested respectively, and the high temperature (1400℃) flexural strength retention rate of each sample was calculated. The specific results are shown in the following table:

[0125]

[0126] It can be seen that the preparation method of the high-strength silicon carbide refractory material of the present invention, in the step of preparing the zirconium-based precursor powder in preparing the composite ceramic powder, firstly, zirconium oxychloride is combined with magnesium salt, lanthanum salt, and hexadecyltrimethylammonium bromide to prepare magnesium / lanthanum composite stabilized zirconium oxide, so as to stabilize the crystal structure and improve the physical properties of the zirconium-based precursor powder and its compatibility with other raw materials; then, the zirconium-based precursor powder is combined with aluminum oxide and titanium oxide to obtain a composite ceramic powder with good structural stability and good mechanical properties; then, in the surface pre-modification step, an aminosilane coupling agent and an epoxysilane coupling agent are combined to The surfaces of composite ceramic powder, aluminum-titanium master alloy powder and sepiolite powder are pre-modified. While improving the bonding performance of the aforementioned components, amino groups and epoxy groups are introduced on their surfaces to promote the subsequent step of preparing a functional composite powder and improve its subsequent bonding performance with the coating film layer. In addition, the introduction of aluminum-titanium master alloy and sepiolite in this step can further improve the refractory performance of silicon carbide refractory materials, improve the pore distribution of silicon carbide refractory materials, and improve the overall stability and high-temperature stability of silicon carbide refractory materials. Then, in the step of preparing functional powders, tetraethoxysilane and n-dodecyl Trimethoxysilane is hydrolyzed and condensed on the outer surface of the aforementioned composite ceramic powder, aluminum-titanium master alloy, and sepiolite composite material to form a coating layer, thereby improving the surface performance of the functional composite powder. In the subsequent process of combining with silicon carbide to prepare refractory materials, the bonding performance of the functional composite powder and silicon carbide is effectively improved, the interface bonding problem with raw materials such as silicon carbide is effectively avoided, the overall stability and density of silicon carbide refractory materials are improved, and the thermal stress defect problems such as reduced uniformity of the organizational structure of silicon carbide refractory materials caused by calcination and high-temperature working environment are effectively avoided, and the silicon carbide refractory materials are further improved in the process of rapid temperature change. stability, improve its long-term stability, and improve the overall mechanical properties of silicon carbide refractory materials; the above-mentioned technical means cooperate with each other and work synergistically to obtain high-strength silicon carbide refractory materials, which can effectively eliminate the interface bonding problem between the raw materials caused by the introduction of the reinforcing phase while obtaining high-strength mechanical properties, and further improve the density and overall stability of silicon carbide refractory materials while improving the high-temperature strength of silicon carbide refractory materials; and effectively reduce the thermal stress defects of silicon carbide refractory materials, improve the stability of silicon carbide refractory materials in the process of rapid temperature change, and improve their long-term stability.

[0127] It can be seen from Comparative Example 1 that after omitting the preparation and addition of the zirconium-based precursor powder and omitting the surface pre-modification step, the binding performance of zirconium oxide powder with aluminum oxide and titanium oxide is reduced, and the stability of each component in the functional composite powder is reduced; at the same time, the binding performance with the coating layer in the step of preparing the functional powder is reduced, resulting in a certain degree of reduction in the long-term stability, density, and overall physical properties of the silicon carbide refractory. Specifically, the apparent porosity of the silicon carbide refractory obtained increases, and the flexural strength, compressive strength, and heating permanent line change all show a certain degree of deterioration; and after 20 rapid temperature changes, the room temperature compressive strength and high temperature flexural strength are significantly reduced.

[0128] It can be seen from Comparative Example 2 that after omitting the use of sepiolite powder and silane coupling agent KH-792 in the surface modification step and omitting the step of preparing functional composite powder, the pore distribution and overall stability of silicon carbide refractory materials cannot be further improved; at the same time, the interface bonding performance between the added reinforcing components (composite ceramic powder, aluminum-titanium intermediate alloy powder) and raw materials such as silicon carbide cannot be improved, and the overall stability and density of silicon carbide refractory materials have deteriorated to a certain extent; it cannot effectively avoid thermal stress defects in high temperature environments, the stability during rapid temperature changes is reduced, and the long-term stability and overall mechanical properties are reduced. Specifically, the apparent porosity of silicon carbide refractory materials increases, the flexural strength, compressive strength and heating permanent line changes all deteriorate to a certain extent, and the proportion of pores less than 1μm increases; at the same time, after 20 rapid temperature changes, deformation, cracks, and bubbling problems occur, and the room temperature compressive strength and high temperature flexural strength after 20 rapid temperature changes are significantly deteriorated.

[0129] Unless otherwise specified, all percentages used in the present invention are by mass.

[0130] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-strength silicon carbide refractory material, characterized in that: The method comprises the following steps: preparing composite ceramic powder, pre-modifying the surface, preparing functional composite powder, and molding; The preparation of the composite ceramic powder comprises the following steps: preparing zirconium-based precursor powder and composite treatment; The method for preparing the zirconium-based precursor powder comprises: adding zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide into deionized water and dispersing them uniformly; adjusting the pH to 8-8.5 with ammonia water, transferring the mixture into an autoclave, sealing the autoclave, heating the mixture to 150-160° C., performing hydrothermal treatment at the temperature, separating and collecting solids, washing the solids and drying them to obtain the zirconium-based precursor powder; The composite treatment method comprises the following steps: subjecting zirconium-based precursor powder, aluminum oxide powder, titanium oxide powder, silane coupling agent A-174 and ethanol solution to ball milling, drying and crushing to obtain composite powder; transferring the composite powder into a calcining furnace, heating it to 1300-1400° C., calcining it at a constant temperature, pouring the calcined molten liquid onto a stainless steel plate for stamping, and crushing it to obtain composite ceramic powder; The surface pre-modification method comprises the following steps: adding composite ceramic powder, aluminum-titanium master alloy powder and sepiolite powder into an ethanol solution, dispersing them uniformly, heating them to 40-45° C. and keeping them warm; while stirring, simultaneously dropping silane coupling agent KH-560 and silane coupling agent KH-792 into the solution; after the addition is completed, continuing to keep the temperature and stirring, filtering out solids, washing the solids with anhydrous ethanol, and then adding them into anhydrous ethanol with a weight of 7.5-8 times the weight of the solids, dispersing them uniformly, and obtaining a pre-modified dispersion; The method for preparing the functional composite powder comprises: adding tetraethoxysilane and n-dodecyltrimethoxysilane into anhydrous ethanol, dispersing them uniformly, and obtaining a modified liquid; adding ammonia water into the ethanol solution, dispersing them uniformly, and obtaining a promoting liquid; stirring the pre-modified dispersed liquid and heating it to 40-42° C., and keeping it warm; while stirring, simultaneously dropping the modified liquid and the promoting liquid; after the dropping is completed, keeping it warm for reaction, filtering out solids, and washing and drying the solids to obtain the functional composite powder; The molding method comprises the following steps: mixing silicon carbide powder, functional composite powder, dextrin and calcium lignin sulfonate uniformly, pressing and molding, drying and calcining to obtain a high-strength silicon carbide refractory material.

2. The method for preparing the high-strength silicon carbide refractory material according to claim 1, characterized in that: In the preparation of the zirconium-based precursor powder, the heating rate to 150-160° C. is 2-2.5° C. / min; The heat treatment time of the water is 22-24 hours at a temperature of 150-160°C. The weight ratio of zirconium oxychloride, magnesium nitrate, lanthanum nitrate and hexadecyltrimethylammonium bromide is 90-95:1-1.3:1.8-2.1:0.8-0.

9.

3. The method for preparing the high-strength silicon carbide refractory material according to claim 1, characterized in that: In the composite treatment, the ball milling time is 2-3h; The heating rate to 1300-1400°C is 3-4°C / min; The calcination time after heating to 1300-1400°C is 40-60 minutes.

4. The method for preparing the high-strength silicon carbide refractory material according to claim 1, characterized in that: In the composite treatment, the weight ratio of zirconium-based precursor powder, aluminum oxide powder, titanium oxide powder, silane coupling agent A-174, and ethanol solution is 22-25:42-46:3-3.5:0.4-0.5:34-35; The volume concentration of the ethanol solution is 70-75%.

5. The method for preparing the high-strength silicon carbide refractory material according to claim 1, characterized in that: In the surface pre-modification, the dropping time of the silane coupling agent KH-560 and the silane coupling agent KH-792 is controlled to be 50-60 minutes; and the heat preservation and stirring time after the dropping is completed is 4-5 hours.

6. The method for preparing the high-strength silicon carbide refractory material according to claim 1, characterized in that: In the surface pre-modification, the weight ratio of the composite ceramic powder, the aluminum-titanium master alloy powder, the sepiolite powder, the ethanol solution, the silane coupling agent KH-560, and the silane coupling agent KH-792 is 15-17:7-7.5:4.2-4.8:105-110:2-2.3:1.2-1.4; The titanium content in the aluminum-titanium master alloy powder is 9.5-11wt% and the particle size is 40-50μm; The particle size of sepiolite powder is 22-30 μm.

7. The method for preparing a high-strength silicon carbide refractory material according to claim 1, characterized in that: In the preparation of the functional composite powder, the dropwise addition time of the modifying liquid and the promoting liquid is controlled to be 15-20 minutes; and the heat preservation reaction time after the dropwise addition is completed is 4-5 hours; The weight ratio of the pre-modified dispersion liquid, the modified liquid and the promoting liquid is 80-83:38-40:44-45.

8. The method for preparing a high-strength silicon carbide refractory material according to claim 1, characterized in that: In the preparation of the functional composite powder, the weight ratio of tetraethoxysilane, n-dodecyltrimethoxysilane and anhydrous ethanol in the modified liquid is 2.4-2.7:1.6-1.9:33-35; The weight ratio of ammonia water to ethanol solution in the promoting liquid is 5.8-6:40-41; The mass concentration of ammonia water is 23-25wt%; The volume concentration of the ethanol solution is 89-91%.

9. The method for preparing a high-strength silicon carbide refractory material according to claim 1, characterized in that: During the molding, the pressure of the pressing molding is 150-180MPa; The drying temperature is 105-110℃ and the drying time is 22-28h; The calcination is carried out under nitrogen atmosphere protection, the calcination temperature is 1200-1250°C, and the calcination time is 4-5h.

10. A high-strength silicon carbide refractory material, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.