A polycarboxylate diluent for water-based drilling fluids resistant to carbonate / bicarbonate contamination, its preparation method and application
The use of polycarboxylate diluents solves the problem of increased viscosity and shear force of drilling fluids under CO2 pollution, achieves dilution and improved stability of drilling fluids, and solves the problem of wellbore instability and large fluid loss during drilling. problem, with the characteristics of low cost and environmental protection.
Patent Information
- Application Number
- CN202411088087.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
CO2 contamination during the drilling process causes the viscosity and shear force of the drilling fluid to increase significantly, resulting in excessive pump pressure, affected mud cake quality, and wellbore instability. Existing technologies are difficult to effectively solve the problem of thick drilling fluids contaminated by HCO3- and CO32- ions. issues.
Polycarboxylate diluents are used, including acrylic acid, N-vinylpyrrolidone, sodium methacrylate sulfonate, isopentenyl alcohol polyoxyethylene ether, oxidants and reducing agents, and are formed through a specific preparation method. Reduce drilling fluid viscosity, shear force and fluid loss.
It can effectively reduce the viscosity, shear force and filter loss of drilling fluid, improve drilling efficiency, and has a simple process, low cost, safety and environmental protection. The diluent has good resistance to high temperature and salt pollution.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of drilling fluid treatment agents, and in particular to a polycarboxylate diluent for carbonate / bicarbonate pollution resistant water-based drilling fluid, and a preparation method and application thereof. Background Art
[0002] Drilling is the only way to establish a channel connecting underground oil and gas and ground engineering. As the "blood" of drilling, drilling fluid has the functions of stabilizing the well wall, suspending rock cuttings, cooling the drill bit, and increasing the mechanical drilling speed, which plays a vital role in the success or failure of drilling. Drilling fluid is mainly divided into oil-based drilling fluid, synthetic drilling fluid and water-based drilling fluid according to its composition. Oil-based drilling fluid has excellent resistance to high temperature, salt and calcium, and pollution, but its relatively high cost and serious environmental pollution limit its large-scale application. In contrast, water-based drilling fluid composed of water, bentonite, chemical additives, etc. is the mainstream direction in the current drilling fluid field.
[0003] As oil and gas exploration and development gradually expands to unconventional and deep formations, geological conditions in the formations are becoming increasingly complex. During the drilling process, various pollutants in the formation (such as salt ions, acidic gases, etc.) are often encountered, which poses a huge challenge to the performance of drilling fluids. Specifically, carbon dioxide pollution in the formation is one of the most common pollutants encountered during drilling. 2 The invasion of CO causes the drilling fluid to thicken, and the viscosity and shear force increase significantly, which can easily cause excessive pump pressure, seriously hindering safe and efficient drilling; at the same time, CO 2 The invasion of CO will also affect the quality of mud cake, forming thick and loose mud cake on the well wall, increasing the loss of drilling fluid, and eventually leading to wellbore instability and fracture leakage. 2 After entering the drilling fluid, it reacts with water to generate H 2 CO 3 , but H 2 CO 3 Unstable, easily hydrolyzed to form HCO 3 - and CO 3 2- ions. Therefore, it is urgent to develop a 3 - and CO 3 2- Drilling fluid diluent under ion contamination conditions to reduce the viscosity, shear force and filtration loss of drilling fluid during drilling. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a polycarboxylate diluent for anti-carbonate / bicarbonate contaminated water-based drilling fluid and its preparation method and application. The diluent of the present invention can solve the problem of HCO 3- and CO 3 2- The contaminated drilling fluid becomes thicker, and the viscosity, shear force, and filtration loss increase. The diluent of the present invention is applied to HCO 3 - and CO 3 2- The contaminated drilling fluid can effectively reduce the viscosity, shear force and filtration loss of the drilling fluid.
[0005] To achieve the above object, the technical solution of the present invention is as follows:
[0006] A polycarboxylate diluent for carbonate / bicarbonate pollution-resistant water-based drilling fluid is prepared by comprising the following raw materials in parts by weight: 5-10 parts of acrylic acid, 1-5 parts of N-vinyl pyrrolidone, 5-10 parts of sodium methyl propylene sulfonate, 40-50 parts of isopentanol polyoxyethylene ether, 0.02-0.6 parts of an oxidant, 45-55 parts of a reducing agent and 40-60 parts of water.
[0007] Preferably, according to the present invention, the polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is prepared by comprising the following raw materials in parts by weight: 7-8 parts of acrylic acid, 2.5-3.5 parts of N-vinyl pyrrolidone, 6.3-8.3 parts of sodium methyl methacrylate sulfonate, 45-50 parts of isopentanol polyoxyethylene ether, 0.048-0.168 parts of oxidant, 50-51 parts of reducing agent, and 45-50 parts of water.
[0008] Preferably, the polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is prepared by including the following raw materials in parts by weight: 7.2 parts of acrylic acid, 3.5 parts of N-vinyl pyrrolidone, 6.3 parts of sodium methyl methacrylate sulfonate, 48 parts of isopentanol polyoxyethylene ether, 0.168 parts of oxidant, 50.048 parts of reducing agent, and 50 parts of water.
[0009] Preferably according to the present invention, the prenol polyoxyethylene ether is TPEG-2400 or TPEG-3000.
[0010] Preferably according to the present invention, the oxidant is hydrogen peroxide with a mass concentration of 3%.
[0011] According to the present invention, the reducing agent is preferably ascorbic acid (V C ).
[0012] The method for preparing the polycarboxylate diluent for the above-mentioned anti-carbonate / bicarbonate contamination water-based drilling fluid comprises the steps of:
[0013] The isopentanol polyoxyethylene ether and the oxidant are fully dispersed in water, and a mixed solution is obtained through reaction; a mixed solution of acrylic acid (AA), N-vinyl pyrrolidone (NVP) and sodium methyl methacrylate sulfonate (SMAS) is added dropwise, and then a reducing agent aqueous solution is added dropwise, and the pH is adjusted through reaction to obtain a polycarboxylate diluent for water-based drilling fluid resistant to carbonate / bicarbonate contamination.
[0014] According to the preferred embodiment of the present invention, the reaction temperature after fully dispersing the isopentanol polyoxyethylene ether and the oxidant in water is room temperature, the reaction time is 3-5 hours, and the reaction is carried out under protective gas protection and stirring conditions. Preferably, the protective gas is nitrogen or argon.
[0015] Preferably, according to the present invention, the dropping rate of the mixed solution of acrylic acid (AA), N-vinyl pyrrolidone (NVP) and sodium methyl methacrylate sulfonate (SMAS) is 5-10 g / h; the dropping is carried out at room temperature, under protective gas protection and stirring. Preferably, the protective gas is nitrogen or argon.
[0016] According to the preferred embodiment of the present invention, the mass concentration of the reducing agent aqueous solution is 0.05%-0.1%; the dropping rate of the reducing agent aqueous solution is 10-30 g / h; the dropping of the reducing agent aqueous solution is carried out at room temperature, under protective gas protection and under stirring conditions. Preferably, the protective gas is nitrogen or argon.
[0017] According to the preferred embodiment of the present invention, the reaction temperature after adding the reducing agent aqueous solution is room temperature, the reaction time is 2-6 hours, and the reaction is carried out under the protection of protective gas and stirring. Preferably, the protective gas is nitrogen or argon.
[0018] Preferably according to the present invention, a sodium hydroxide aqueous solution with a mass concentration of 10%-30% is used to adjust the pH to 7-11, preferably 7-8.
[0019] The polycarboxylate diluent for carbonate / bicarbonate resistant water-based drilling fluid is used as a diluent in carbonate / bicarbonate resistant water-based drilling fluid to reduce viscosity, shear force and filtration loss.
[0020] The technical features and beneficial effects of the present invention are as follows:
[0021] 1. The preparation process of the present invention is simple, the synthetic monomer is common, cheap and easy to obtain, the synthesis temperature and time are easy to control, the obtained diluent is safe and environmentally friendly, has no irritating odor, and has low cost.
[0022] 2. The drilling fluid diluent of the present invention has strong dilution and viscosity reduction capabilities in the drilling fluid, and has the outstanding feature of strong resistance to carbonate / bicarbonate pollution. It can reduce the apparent viscosity, plastic viscosity, shear force and filtration loss of the drilling fluid system, thereby greatly improving the drilling efficiency.
[0023] 3. Ascorbic acid added in the present invention as a reducing agent can form a redox system with hydrogen peroxide. Ascorbic acid can promote the decomposition of hydrogen peroxide, generate free radicals, and then initiate the polymerization reaction of the monomer. The hydrogen peroxide added in the present invention as an oxidant provides oxidation ability, promotes the polymerization of monomer molecules, can make the reaction proceed more smoothly, and improve the rate and efficiency of the reaction. At the same time, by controlling the amount of hydrogen peroxide and the dripping speed, the progress of the reaction can also be adjusted. Compared with other initiation systems, the polymerization reaction is faster, which is conducive to obtaining a diluent with excellent performance.
[0024] 4. The sodium methyl methacrylate sulfonate added in the present invention can provide sulfonic acid groups to improve the temperature and salt resistance of the diluent; the addition of N-vinyl pyrrolidone can increase the stability of the drilling fluid and inhibit the hydration and dispersion of shale; the selected isopentanol polyoxyethylene ether can improve the hydration and dispersion of clay, and has good rheological adjustment and filtration loss reduction properties.
[0025] 5. The drilling fluid diluent obtained by the present invention contains -SO 3 - and -OH, etc., can be adsorbed on the clay surface through electrostatic adsorption to form a thicker hydration film, so that the clay particles repel each other, prevent the particles from agglomerating and flocculating, and form a grid structure, which has a certain stabilizing effect on the drilling fluid; the pyrrolidone ring and sulfonic acid group in the molecular chain have strong thermal stability and still have good flow stability at high temperatures. At the same time, the presence of sulfonic acid groups can also improve the drilling fluid's ability to resist electrolyte pollution.
[0026] 6. The drilling fluid diluent obtained by the present invention contains strong adsorption groups that can react with HCO 3 - and CO 3 2- The ions produce competitive adsorption, which makes the diluent have more adsorption sites on the clay surface, thereby enhancing the stability of the system and reducing the viscosity of the drilling fluid.
[0027] 7. The drilling fluid diluent obtained by the present invention disassembles the already bonded and thickened drilling fluid grid structure, preventing it from generating a new grid structure. At the same time, the presence of the adsorptive groups can form coordination bonds with clay particles, making the end-face diffusion double-layer repulsion of the particles stronger and the hydration film thickness increased, ultimately achieving the purpose of preventing the drilling fluid from thickening and improving the rheology of the drilling fluid. The raw material composition and preparation method of the present invention work together as a whole to achieve the excellent effects of the present invention; any replacement of raw materials, inappropriate proportions, and preparation conditions will reduce the performance of the resulting diluent. DETAILED DESCRIPTION
[0028] The present invention will be further described below by means of specific examples, but is not limited thereto.
[0029] The experimental methods described in the examples are conventional methods unless otherwise specified; the reagents and materials used are commercially available unless otherwise specified.
[0030] Example 1
[0031] A method for preparing a polycarboxylate diluent for a water-based drilling fluid resistant to carbonate / bicarbonate pollution, comprising the steps of:
[0032] 1) 48 g of prenol polyoxyethylene ether (TPEG-2400), 48 mg of hydrogen peroxide (3%) and 50 g of deionized water were added into a three-bottom round-mouth flask and stirred to obtain a mixed solution;
[0033] 2) The three-bottom round-mouth flask was stirred and reacted at room temperature for 4 hours under nitrogen protection;
[0034] 3) Dissolve 6.3g of sodium methyl propylene sulfonate in 7.2g of acrylic acid and 3.5g of N-vinyl pyrrolidone, and add dropwise to one side of a three-necked round-bottom flask using a constant pressure separatory funnel at room temperature under nitrogen protection and stirring for 2 hours;
[0035] 4) Mix 48 mg of ascorbic acid and 50 g of deionized water, and add dropwise to the other side of the three-necked round-bottom flask using a constant pressure separatory funnel at room temperature under nitrogen protection and stirring for 2 hours;
[0036] 5) Stir the reaction at room temperature under nitrogen protection for 4 hours;
[0037] 6) After the reaction is completed, the pH value is adjusted to 7 using a 20% sodium hydroxide aqueous solution.
[0038] It is a polycarboxylate diluent for water-based drilling fluid that is resistant to carbonate / bicarbonate contamination.
[0039] Example 2
[0040] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 1, except that the amount of hydrogen peroxide used is 96 mg; the other steps and conditions are the same as in Example 1.
[0041] Example 3
[0042] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 1, except that the amount of hydrogen peroxide used is 168 mg; the other steps and conditions are the same as in Example 1.
[0043] Example 4
[0044] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that the amount of N-vinyl pyrrolidone used is 2.5 g; the other steps and conditions are the same as those in Example 3.
[0045] Example 5
[0046] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that the amount of sodium methyl methacrylate sulfonate used is 8.3 g; the other steps and conditions are the same as those in Example 3.
[0047] Example 6
[0048] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that a 20% sodium hydroxide aqueous solution is used to adjust the pH value to 10; the other steps and conditions are the same as those in Example 3.
[0049] Example 7
[0050] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that the reaction time after adding the reducing agent is 2 hours; the other steps and conditions are the same as those in Example 3.
[0051] Example 8
[0052] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that the dripping time of the mixed solution of acrylic acid (AA), N-vinyl pyrrolidone (NVP) and sodium methyl methacrylate sulfonate (SMAS) is 3 hours; the other steps and conditions are the same as those in Example 3.
[0053] Example 9
[0054] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that the dropping time of the reducing agent aqueous solution is 3 hours; the other steps and conditions are the same as those in Example 3.
[0055] Example 10
[0056] A method for preparing a polycarboxylate diluent for carbonate / bicarbonate-resistant water-based drilling fluid is as described in Example 3, except that the isopentanol polyoxyethylene ether is TPEG-3000; the other steps and conditions are the same as those in Example 3.
[0057] Comparative Example 1
[0058] A method for preparing a diluent comprises the following steps:
[0059] 1) 48 g of prenol polyoxyethylene ether (TPEG-2400) and 50 g of deionized water were added into a three-bottom round-mouth flask and stirred to obtain a mixed solution;
[0060] 2) The three-bottom round-mouth flask was stirred and reacted at room temperature for 4 hours under nitrogen protection;
[0061] 3) Dissolve 6.3g of sodium methyl propylene sulfonate in 7.2g of acrylic acid and 3.5g of N-vinyl pyrrolidone, and add dropwise to one side of a three-necked round-bottom flask using a constant pressure separatory funnel at room temperature under nitrogen protection and stirring for 2 hours;
[0062] 4) Mix 65 mg of azobisisobutylamidine hydrochloride and 50 g of deionized water, and add dropwise to the other side of the three-necked round-bottom flask using a constant pressure separatory funnel at room temperature under nitrogen protection and stirring for 2 hours;
[0063] 5) Stir the reaction at room temperature under nitrogen protection for 4 hours;
[0064] 6) After the reaction is completed, the pH value is adjusted to 7 using a 20% sodium hydroxide aqueous solution.
[0065] That is the diluent.
[0066] Comparative Example 2
[0067] A method for preparing a diluent, as described in Comparative Example 1, except that azobisisobutylamidine hydrochloride is replaced with 65 mg of persulfate and 21 mg of sodium sulfite; other steps and conditions are the same as those in Comparative Example 1.
[0068] Comparative Example 3
[0069] A method for preparing a diluent is as described in Example 3, except that sodium methyl methacrylate sulfonate is replaced by sodium allyl sulfonate; the other steps and conditions are the same as those in Example 3.
[0070] Comparative Example 4
[0071] A method for preparing a diluent is as described in Example 3, except that sodium methyl methacrylate sulfonate is replaced by sodium p-styrene sulfonate; the other steps and conditions are the same as those in Example 3.
[0072] Comparative Example 5
[0073] A method for preparing a diluent is as described in Example 3, except that acrylic acid is replaced by acrylamide; the other steps and conditions are the same as those in Example 3.
[0074] Comparative Example 6
[0075] A method for preparing a diluent is as described in Example 3, except that isopentanol polyoxyethylene ether is not added; other steps and conditions are the same as in Example 3.
[0076] The details are as follows:
[0077] 1) Add 48 mg of hydrogen peroxide (3%) and 50 g of deionized water into a three-bottom round-mouth flask and stir to obtain a mixed solution;
[0078] 2) The three-bottom round-mouth flask was stirred and reacted at room temperature for 4 hours under nitrogen protection;
[0079] 3) Dissolve 6.3g of sodium methyl propylene sulfonate in 7.2g of acrylic acid and 3.5g of N-vinyl pyrrolidone, and add dropwise to one side of a three-necked round-bottom flask using a constant pressure separatory funnel at room temperature under nitrogen protection and stirring for 2 hours;
[0080] 4) Mix 48 mg of ascorbic acid and 50 g of deionized water, and add dropwise to the other side of the three-necked round-bottom flask using a constant pressure separatory funnel at room temperature under nitrogen protection and stirring for 2 hours;
[0081] 5) Stir the reaction at room temperature under nitrogen protection for 4 hours;
[0082] 6) After the reaction is completed, the pH value is adjusted to 7 using a 20% sodium hydroxide aqueous solution, and the resulting product is the diluent.
[0083] Comparative Example 7
[0084] A method for preparing a diluent is as described in Example 3, except that N-vinyl pyrrolidone is not added; the other steps and conditions are the same as those in Example 3.
[0085] Comparative Example 8
[0086] A method for preparing a diluent is as described in Example 3, except that sodium methyl methacrylate sulfonate is not added; the other steps and conditions are the same as those in Example 3.
[0087] Comparative Example 9
[0088] A method for preparing a diluent is as described in Example 3, except that isopentanol polyoxyethylene ether is replaced by allyl alcohol polyoxyethylene ether; other steps and conditions are the same as in Example 3.
[0089] Test Example 1
[0090] The diluents prepared in the examples and comparative examples were subjected to rheological tests.
[0091] (1) Sample preparation:
[0092] The drilling fluid composition is as follows: 400 mL of 4% drilling fluid base slurry (520 g of bentonite and 18.2 g of sodium carbonate are added to 1300 mL of water), 0.6 g of carboxymethyl cellulose sodium salt, 0.6 g of polyanionic cellulose, 20 g of sulfonated phenolic resin, 20 g of lignite resin, 580 g of barite (the drilling fluid density is adjusted to 1.8 kg / m³), 16 g of sodium carbonate, 16 g of sodium bicarbonate and 8 g of the diluent in the embodiment or comparative example are added to the drilling fluid base slurry, and the mixture is stirred on a high-speed stirrer for 30 min to obtain a sample. The sample is aged at 180° C. for 16 h and then cooled, and then the rheological properties and filtration loss properties of the sample before and after aging are tested at room temperature. The drilling fluid without diluent is used as the control sample.
[0093] (2) Test method:
[0094] Take a certain amount of prepared sample and pour it into the test slurry cup. Use an electronic six-speed viscometer to record θ 600 ,θ 300 ,θ 200 ,θ 100 ,θ 6 ,θ 3 , G 1 , G 2 (initial cut, final cut) readings.
[0095] The API filtration loss of the samples was measured at 100 MPa using a medium-pressure filtration instrument (ZNSJ-5A, Qingdao Tongchun Petroleum Instrument Co., Ltd., China), and the filtrate volume was recorded after seven and a half minutes. Twice of this volume was the API filtration loss.
[0096] Rheological properties were determined and the test results are shown in Table 1-2.
[0097] Table 1 Performance test of drilling fluid diluent before aging
[0098]
[0099] Table 2 Performance test of drilling fluid diluent after aging at 180℃
[0100]
[0101] It can be seen from the data in Table 1-2 that the drilling fluid diluent prepared by the present invention exhibits good viscosity reduction performance after aging at room temperature and 180°C, and the viscosity reduction effect is significant. At the same time, it also has a large dynamic plasticity ratio, which makes the drilling fluid have good shear thinning properties and has a low filtration loss.
[0102] In summary, the polycarboxylate diluent for drilling fluid resistant to carbonate / bicarbonate pollution of the present invention can meet the needs of drilling fluid carbonate / bicarbonate pollution.
[0103] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0104] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0105] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A polycarboxylate diluent for water-based drilling fluids resistant to carbonate / bicarbonate pollution, characterized in that: The method comprises the following raw materials in parts by weight: 5-10 parts of acrylic acid, 1-5 parts of N-vinyl pyrrolidone, 5-10 parts of sodium methyl propylene sulfonate, 40-50 parts of isopentanol polyoxyethylene ether, 0.02-0.6 parts of oxidant, 45-55 parts of reducing agent, and 40-60 parts of water; The oxidant is hydrogen peroxide with a mass concentration of 3%; the reducing agent is ascorbic acid.
2. The polycarboxylate diluent for anti-carbonate / bicarbonate contamination water-based drilling fluid according to claim 1, characterized in that: The polycarboxylate diluent for carbonate / bicarbonate pollution-resistant water-based drilling fluid is prepared by including the following raw materials in parts by weight: 7-8 parts of acrylic acid, 2.5-3.5 parts of N-vinyl pyrrolidone, 6.3-8.3 parts of sodium methyl propylene sulfonate, 45-50 parts of isopentanol polyoxyethylene ether, 0.048-0.168 parts of oxidant, 50-51 parts of reducing agent and 45-50 parts of water.
3. The polycarboxylate diluent for anti-carbonate / bicarbonate contamination water-based drilling fluid according to claim 2, characterized in that: The polycarboxylate diluent for carbonate / bicarbonate pollution-resistant water-based drilling fluid is prepared by including the following raw materials in parts by weight: 7.2 parts of acrylic acid, 3.5 parts of N-vinyl pyrrolidone, 6.3 parts of sodium methyl propylene sulfonate, 48 parts of isopentanol polyoxyethylene ether, 0.168 parts of oxidant, 50.048 parts of reducing agent, and 50 parts of water.
4. The polycarboxylate diluent for anti-carbonate / bicarbonate contamination water-based drilling fluid according to claim 1, characterized in that: The prenol polyoxyethylene ether is TPEG-2400 or TPEG-3000.
5. The method for preparing the polycarboxylate diluent for carbonate / bicarbonate pollution resistant water-based drilling fluid according to any one of claims 1 to 4, characterized in that: Includes steps: The isopentanol polyoxyethylene ether and the oxidant are fully dispersed in water, and a mixed solution is obtained through reaction; a mixed solution of acrylic acid, N-vinyl pyrrolidone and sodium methyl propylene sulfonate is added dropwise, and then a reducing agent aqueous solution is added dropwise, and the pH is adjusted through reaction to obtain a polycarboxylate diluent for water-based drilling fluid resistant to carbonate / bicarbonate pollution.
6. The method for preparing the polycarboxylate diluent for anti-carbonate / bicarbonate contamination water-based drilling fluid according to claim 5, characterized in that: Includes one or more of the following conditions: i. After fully dispersing the isopentanol polyoxyethylene ether and the oxidant in water, the reaction temperature is room temperature, the reaction time is 3-5 hours, and the reaction is carried out under the protection of protective gas and stirring; the protective gas is nitrogen or argon; ii. The dropping rate of the mixed solution of acrylic acid, N-vinyl pyrrolidone and sodium methacrylate sulfonate is 5-10 g / h; the dropping is carried out at room temperature, under protective gas protection and stirring; the protective gas is nitrogen or argon; iii. The mass concentration of the reducing agent aqueous solution is 0.05%-0.1%; the dropping rate of the reducing agent aqueous solution is 10-30g / h; the dropping of the reducing agent aqueous solution is carried out at room temperature, under protective gas protection and stirring conditions; the protective gas is nitrogen or argon; iv. The reaction temperature after adding the reducing agent aqueous solution is room temperature, the reaction time is 2-6 hours, and the reaction is carried out under the protection of protective gas and stirring; the protective gas is nitrogen or argon; v. Use a 10%-30% sodium hydroxide aqueous solution to adjust the pH to 7-11.
7. The method for preparing the polycarboxylate diluent for water-based drilling fluid resistant to carbonate / bicarbonate pollution according to claim 5, characterized in that: Use a 10%-30% sodium hydroxide aqueous solution to adjust the pH to 7-8.
8. The use of a polycarboxylate diluent for carbonate / bicarbonate contamination resistant water-based drilling fluid according to any one of claims 1 to 4, characterized in that: Used as a diluent in carbonate / bicarbonate contaminated water-based drilling fluids to reduce viscosity, shear stress and fluid loss.