A modified epoxy resin toughening agent and preparation method thereof

By using a modified toughening agent prepared under the protection of nitrogen in epoxy resin, combined with halogen-free flame retardant elements and quaternary ammonium salt structure, the problems of insufficient toughness, flame retardancy and antibacterial properties of epoxy resin are solved, and the problem of insufficient toughness, flame retardancy and antibacterial properties of epoxy resin is achieved. Enhanced mechanical properties and long-lasting and stable antibacterial effects.

CN118599082BActive Publication Date: 2024-11-15SHANGHAI ZHEYINGHONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074357.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-15
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Existing epoxy resins have poor toughness and are prone to cracking after curing, and are insufficient in the fields of construction, adhesives, coatings, etc., making it difficult to meet the multiple performance needs of materials.

Method used

The modified epoxy resin toughening agent prepared under nitrogen protection is formed by reacting diisocyanate with a catalyst and an auxiliary agent containing halogen-free flame retardant elements nitrogen, phosphorus and silicon to form an interpenetrating network structure to enhance toughness and flame retardant properties. And achieve antibacterial effects through the quaternary ammonium salt structure.

Benefits of technology

It significantly improves the toughness, flame retardancy and antibacterial properties of epoxy resin, forms an efficient and safe toughening agent, and achieves the multiple performance improvement of epoxy resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a modified epoxy resin toughener and a preparation method thereof, and belongs to the technical field of epoxy resin. Under nitrogen protection, diisocyanate and a catalyst are added to a reaction bottle equipped with a reaction solvent, stirred, an auxiliary agent is slowly added, the temperature is raised to 40-60°C for reaction for 2-4h, and vacuum distillation is performed to obtain a modified epoxy resin toughener. An auxiliary agent having high-density halogen-free flame retardant elements of nitrogen, phosphorus, silicon, and multiple long carbon chains and quaternary ammonium salt structures reacts chemically with diisocyanate under the action of a catalyst to obtain a toughener having a longer polyurethane segment, and the toughener forms an interpenetrating network structure with an epoxy cured product, thereby achieving toughening and strengthening of epoxy resin, and the toughener enables epoxy resin to have excellent and stable antibacterial effect and efficient and safe flame retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resins, and in particular relates to a modified epoxy resin toughening agent and a preparation method thereof. Background Art

[0002] Epoxy resin refers to a low molecular weight polymer containing two or more epoxy groups in its molecular structure. It can undergo a cross-linking reaction with a curing agent to form a three-dimensional structure, exhibiting advantages such as good bonding properties, mechanical properties, electrical insulation properties, wear resistance and heat resistance. Therefore, it can be used as an adhesive, coating, sealant, potting material, and resin matrix for composite materials, and is widely used in machinery, construction, electronic devices, adhesives, coatings and other fields.

[0003] However, the cured epoxy resin also exhibits defects such as poor toughness and easy cracking due to its high cross-linking density, which limits its application in more fields. In addition, the fields of construction, adhesives, coatings, etc. usually have high requirements for the antibacterial properties of materials. Directly adding small molecule organic antibacterial agents or inorganic antibacterial agents to the materials by physical mixing can easily lead to the migration and release of the antibacterial agents, which in turn causes the materials to gradually lose their antibacterial effects. At present, there are few studies on adding antibacterial components to epoxy resin toughening agents to give the materials a long-lasting and stable antibacterial effect. At the same time, epoxy resin is a flammable substance. With the widespread use of epoxy resin in different fields, the potential for fire is also increasing. Therefore, improving its flame retardancy has become a top priority in epoxy resin research. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a modified epoxy resin toughening agent and a preparation method thereof.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing a modified epoxy resin toughening agent comprises the following steps:

[0007] Under nitrogen protection, add diisocyanate and catalyst into a reaction bottle containing reaction solvent, stir thoroughly until mixed evenly, then slowly add auxiliary agent under stirring, raise the temperature to 40-60°C after adding, keep warm for 2-4h, and after the reaction is completed, perform reduced pressure distillation to obtain modified epoxy resin toughening agent.

[0008] Furthermore, the diisocyanate is one or more of diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and toluene diisocyanate.

[0009] Furthermore, the catalyst is one of the organotin compounds.

[0010] Furthermore, the mass of the catalyst is 0.08-0.12% of the total mass of the reaction raw materials.

[0011] Furthermore, the reaction solvent is one or more of chloroform, toluene, xylene, 1,4-dioxane, tetrahydrofuran, dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide.

[0012] Furthermore, the molar ratio of the diisocyanate to the auxiliary agent is 1:(0.8-1.2).

[0013] Furthermore, the auxiliary agent is prepared by the following steps:

[0014] S1. Add (2-aminoethyl) diethyl phosphonate, pyridine and diethyl ether to a dry three-necked flask at room temperature, stir until a uniform solution is formed, dilute tetradecane chloride with diethyl ether and slowly add it to the above three-necked flask through a constant pressure dropping funnel, stir and heat to 60°C, keep the temperature for reaction for 2h, cool to room temperature after the reaction is completed, and distill under reduced pressure to obtain intermediate 1; the amount ratio of (2-aminoethyl) diethyl phosphonate, tetradecane chloride, pyridine and diethyl ether is 0.08mol:0.085mol:9.7mL:150mL;

[0015] Pyridine is used as an acid-binding agent. Under heating conditions, -NH2 of diethyl (2-aminoethyl)phosphonate and -Cl of tetradecyl chloride undergo a nucleophilic substitution reaction. The reaction process is as follows:

[0016]

[0017] S2. Replace the air in a dry three-necked flask with nitrogen at room temperature, then add intermediate 1, triethylamine and DMSO (dimethyl sulfoxide), stir and dissolve, slowly add a mixed solution of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and DMSO, stir and heat to 75°C, keep warm for 2 hours, cool to room temperature after the reaction, and distill under reduced pressure. The whole process is carried out under nitrogen protection to obtain intermediate 2; the amount ratio of intermediate 1, 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane, triethylamine and DMSO is 0.074 mol:0.035 mol:15.4 mL:200 mL;

[0018] Under heating and the presence of triethylamine, -NH- of intermediate 1 and -Cl of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane undergo nucleophilic substitution reaction. The reaction process is shown below:

[0019]

[0020] S3, nitrogen was blown into a dry brown three-necked flask for 30 min to drive away the air in the flask, and then intermediate 2, triethylamine and DMSO were added, and the mixture was fully stirred until uniformly mixed. 3-chloro-1-propanol was diluted with DMSO and slowly added to the above brown three-necked flask through a constant pressure dropping funnel, and the mixture was heated to 80° C. and kept for 3 h. After the reaction was completed, the mixture was cooled to room temperature and distilled under reduced pressure to obtain intermediate 3; the amount ratio of intermediate 2, 3-chloro-1-propanol, triethylamine and DMSO was 0.035 mol: 0.036 mol: 7.3 mL: 200 mL;

[0021] Triethylamine is used as an acid-binding agent. Under heating conditions, the tertiary amine group of intermediate 2 and the -Cl of 3-chloro-1-propanol undergo a nucleophilic substitution reaction. The reaction process is as follows:

[0022]

[0023] S4. Replace the air in the four-necked reaction bottle with nitrogen at room temperature, add intermediate 3 and DMF (N,N-dimethylformamide), stir to dissolve, and then slowly add octadecyltrichlorosilane. The system temperature is not higher than 20°C during the addition process. After the addition is completed, stir and react at 30°C for 6 hours. When no HCl gas is released, cool to below 20°C, filter, rinse the filter cake with DMF, and vacuum dry to obtain intermediate 4; the amount ratio of octadecyltrichlorosilane, intermediate 3 and DMF is 0.015mol:0.03mol:180mL;

[0024] At 30°C, intermediate 3 and octadecyltrichlorosilane undergo esterification reaction, and the reaction process is as follows:

[0025]

[0026] S5, nitrogen blowing dry three-necked flask for 30min to expel the air in the flask, then add intermediate 4 and DMF, stir to dissolve, dilute glycerol with DMF and slowly add it to the above three-necked flask through a constant pressure dropping funnel, the system temperature is not higher than 20°C during the addition process, after the drop is complete, stir and react at 40°C for 6h, wait until no HCl gas is released, cool to below 20°C, filter, rinse the filter cake with DMF, and vacuum dry to obtain an auxiliary agent. The amount ratio of intermediate 4, glycerol and DMF is 0.01mol:0.011mol:180mL.

[0027] Under heating conditions, intermediate 4 and propylene glycol undergo esterification reaction, and the reaction process is as follows:

[0028]

[0029] The auxiliary agent of the present invention contains halogen-free flame retardant elements of nitrogen, phosphorus and silicon, and the three flame retardant elements act synergistically to give the toughening agent an efficient and safe flame retardant effect.

[0030] The auxiliary agent contains a quaternary ammonium salt structure containing a long carbon chain (14 carbon atoms). The quaternary ammonium salt structure is adsorbed onto the surface of the bacteria, and the hydrophobic group is inserted into the lipid layer, which changes the permeability of the cell membrane, destroys the membrane structure, causes leakage of intracellular substances, denatures enzymes or proteins, inhibits the activity of enzymes or proteins, affects the cell metabolism process, and finally causes the death of the bacteria. In addition, when the carbon number of the alkyl chain of the quaternary ammonium salt structure is 10-16, the antibacterial effect is better, and when the carbon number is 14, the antibacterial effect is the best. Therefore, the auxiliary agent of the present invention imparts excellent antibacterial effect to the toughening agent.

[0031] The additive contains two terminal hydroxyl groups, which can react chemically with diisocyanate under the action of a catalyst to prepare a toughening agent with a longer polyurethane chain segment. The toughening agent forms an interpenetrating network structure with the epoxy cured product, thereby achieving toughening and strengthening of the epoxy resin. In addition, the additive contains multiple long carbon chains, and the methylene groups that can be freely stretched and rotated can further enhance the mechanical properties of the epoxy resin, such as toughness and tensile strength.

[0032] The invention also discloses a modified epoxy resin toughening agent, which is prepared according to the preparation method of the modified epoxy resin toughening agent.

[0033] The beneficial effects of the present invention are as follows: an auxiliary agent having high-density halogen-free flame-retardant elements of nitrogen, phosphorus, silicon, and multiple long carbon chains and quaternary ammonium salt structures reacts chemically with diisocyanate under the action of a catalyst to prepare a toughening agent having a relatively long polyurethane chain segment; the toughening agent forms an interpenetrating network structure with an epoxy cured product, thereby achieving toughening and strengthening of the epoxy resin; and at the same time, the toughening agent enables the epoxy resin to have an excellent and stable antibacterial effect and an efficient and safe flame-retardant effect. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] All chemicals used in the examples and comparative examples come from the following sources:

[0036] (2-Aminoethyl)phosphonic acid diethyl ester: Shanghai Haohong Biopharmaceutical Technology Co., Ltd., purity 98%, CAS number: 41468-36-4, product number: 1505419;

[0037] Chlorotetradecane: Shanghai Haohong Biopharmaceutical Technology Co., Ltd., purity 98%, CAS number: 2425-54-9, product number: 1026959;

[0038] Triethylamine: Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 99.5% (GC), CAS No.: 121-44-8, product No.: T103290;

[0039] 1,3-Bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane: Shanghai Myrel Biochemical Technology Co., Ltd., purity 97%, CAS number: 2362-10-9, product number: GEL-SIB1055.0;

[0040] 3-Chloro-1-propanol: Shanghai MacLean Biochemical Technology Co., Ltd., purity 98%, CAS number: 627-30-5, product number: C805065;

[0041] Octadecyltrichlorosilane: Shanghai MacLean Biochemical Technology Co., Ltd., purity 95%, CAS number: 112-04-9, product number: T821379;

[0042] Glycerol: Shanghai Aladdin Biochemical Technology Co., Ltd., purity > 99.7% (GC), CAS No.: 56-81-5, product No.: G116202;

[0043] Pyridine: Shanghai Aladdin Biochemical Technology Co., Ltd., basic grade reagent, CAS No.: 110-86-1, product No.: P431463;

[0044] Ether: CAS No.: 60-29-7;

[0045] DMSO (dimethyl sulfoxide): Shandong Lierbang New Materials Co., Ltd., purity 99.95%, CAS number: 67-68-5;

[0046] DMF (N,N-dimethylformamide): Shanghai Mairui Biochemical Technology Co., Ltd., purity 99.8%, CAS number: 68-12-2, product number: 68-12-2;

[0047] Isophorone diisocyanate: Shanghai MacLean Biochemical Technology Co., Ltd., purity 99%, CAS number: 4098-71-9, product number: I811865;

[0048] Dibutyltin dilaurate: Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 95%, CAS number: 77-58-7, product number: D100274;

[0049] Diphenylmethane diisocyanate: Shanghai Hanhong Technology Co., Ltd., purity 98%, CAS number: 26447-40-5, product number: GN020507;

[0050] N,N-Dimethylacetamide: Shanghai Aladdin Biochemical Technology Co., Ltd., purity> 99.8% (GC), CAS number: 127-19-5, product number: D108095;

[0051] Hexamethylene diisocyanate: Shanghai Aladdin Biochemical Technology Co., Ltd., purity 99%, CAS number: 822-06-0, product number: H106723;

[0052] E51 epoxy resin: Shandong Pinshang New Materials Co., Ltd., epoxy equivalent: 184-194 g / mol, viscosity (25°C): 10000-16000 mPa·s;

[0053] Methyltetrahydrophthalic anhydride: Shanghai MacLean Biochemical Technology Co., Ltd., purity 95%, CAS number: 19438-64-3, product number: M915856;

[0054] 2,4,6-Tris(dimethylaminomethyl)phenol: Shanghai Eon Chemical Technology Co., Ltd., purity 95%, CAS number: 90-72-2, product number: R012758.

[0055] Example 1

[0056] Preparation of auxiliary agent, the specific steps are as follows:

[0057] S1. Add 14.5 g of diethyl (2-aminoethyl)phosphonate, 9.7 mL of pyridine and 130 mL of ether to a 500 mL dry three-necked flask at room temperature, stir until a uniform solution is formed, dilute 23 mL of tetrachlorodecane with 20 mL of ether and slowly add it to the above three-necked flask through a constant pressure dropping funnel, stir and heat to 60° C., keep the temperature for reaction for 2 h, cool to room temperature after the reaction is completed, and distill under reduced pressure to obtain intermediate 1;

[0058] S2. Replace the air in a 500 mL dry three-necked flask with nitrogen at room temperature, then add 27.9 g of intermediate 1, 15.4 mL of triethylamine and 190 mL of DMSO, stir and dissolve, then slowly add a mixed solution of 7.7 mL of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 10 mL of DMSO, stir and heat to 75°C, keep warm for 2 h, cool to room temperature after the reaction, and distill under reduced pressure. The whole process is carried out under nitrogen protection to obtain intermediate 2.

[0059] S3, nitrogen was blown into a 500 mL dry brown three-necked flask for 30 min to drive away the air in the flask, then 32 g of intermediate 2, 7.3 mL of triethylamine and 190 mL of DMSO were added, and the mixture was stirred thoroughly until uniformly mixed, 3 mL of 3-chloro-1-propanol was diluted with 10 mL of DMSO and slowly added into the above brown three-necked flask through a constant pressure dropping funnel, and the mixture was stirred and heated to 80°C, and the mixture was kept warm for 3 h. After the reaction was completed, the mixture was cooled to room temperature and distilled under reduced pressure to obtain intermediate 3;

[0060] S4, replace the air in a 500mL four-necked reaction bottle with nitrogen at room temperature, add 30.2g of intermediate 3 and 180mL of DMF, stir to dissolve, then slowly add 5.9mL of octadecyltrichlorosilane, the system temperature is not higher than 20°C during the addition process, stir and react at 30°C for 6h after the addition is complete, wait until no HCl gas is released, cool to below 20°C, filter, rinse the filter cake with DMF, and vacuum dry to obtain intermediate 4;

[0061] S5. Blow nitrogen gas into a 500 mL dry three-necked flask for 30 min to expel the air in the flask, then add 22.6 g of intermediate 4 and 170 mL of DMF, stir to dissolve, dilute 1 g of propylene glycol with 10 mL of DMF and slowly add it to the above three-necked flask through a constant pressure dropping funnel. During the addition, the system temperature is not higher than 20° C. After the addition is completed, stir and react at 40° C. for 6 h. When no HCl gas is released, cool to below 20° C., filter, rinse the filter cake with DMF, and vacuum dry to obtain an auxiliary agent.

[0062] Example 2

[0063] The modified epoxy resin toughening agent is prepared in the following specific steps:

[0064] Under nitrogen protection, 4.2 mL of isophorone diisocyanate and 0.068 g of dibutyltin dilaurate were added to a reaction bottle containing 160 mL of dimethyl sulfoxide, and the mixture was stirred thoroughly until uniformly mixed. Then, 38.2 g of the auxiliary agent prepared in Example 1 was slowly added under stirring. After the addition was completed, the temperature was raised to 40° C. and the reaction was kept warm for 2 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain a modified epoxy resin toughening agent.

[0065] Example 3

[0066] The modified epoxy resin toughening agent is prepared in the following specific steps:

[0067] Under nitrogen protection, 5 g of diphenylmethane diisocyanate and 0.075 g of dibutyltin dilaurate were added to a reaction bottle containing 200 mL of N, N-dimethylacetamide, and the mixture was stirred thoroughly until uniformly mixed. Then, 57.3 g of the auxiliary agent prepared in Example 1 was slowly added under stirring. After the addition was completed, the temperature was raised to 60° C. and the reaction was kept warm for 4 hours. After the reaction was completed, the mixture was distilled under reduced pressure to obtain a modified epoxy resin toughening agent.

[0068] Example 4

[0069] The modified epoxy resin toughening agent is prepared in the following specific steps:

[0070] Under nitrogen protection, 3.2 mL of hexamethylene diisocyanate and 0.05 g of dibutyltin dilaurate were added to a reaction bottle containing 180 mL of N,N-dimethylformamide, and the mixture was stirred thoroughly until uniformly mixed. Then, 47.7 g of the auxiliary agent prepared in Example 1 was slowly added under stirring. After the addition was completed, the temperature was raised to 50° C. and the reaction was kept warm for 3 hours. After the reaction was completed, the mixture was distilled under reduced pressure to obtain a modified epoxy resin toughening agent.

[0071] Example 5

[0072] Preparation of epoxy resin cured product, the specific steps are as follows:

[0073] Add 40g of E51 epoxy resin and 6g of the modified epoxy resin toughening agent prepared in Example 2 into a beaker, stir in a water bath at a constant temperature of 60°C until the toughening agent is completely dissolved, add 28.8g of methyltetrahydrophthalic anhydride and stir thoroughly in a water bath at a constant temperature of 80°C for 1h, add 0.48g of 2,4,6-tris(dimethylaminomethyl)phenol into the beaker after stirring for 15min, pour into a mold for pre-curing (100°C), and take out after 5h to obtain an epoxy resin cured product.

[0074] Example 6

[0075] Preparation of epoxy resin cured product, the specific steps are as follows:

[0076] The remaining steps remain unchanged, and the toughening agent in Example 5 is replaced by the toughening agent in Example 3, thereby preparing a cured epoxy resin.

[0077] Example 7

[0078] Preparation of epoxy resin cured product, the specific steps are as follows:

[0079] The remaining steps remain unchanged, and the toughening agent in Example 5 is replaced by the toughening agent in Example 4, thereby preparing a cured epoxy resin.

[0080] Comparative Example 1

[0081] Preparation of epoxy resin cured product, the specific steps are as follows:

[0082] The remaining steps remain unchanged, and the toughening agent of Example 7 is removed to prepare the epoxy resin cured product.

[0083] Performance Testing

[0084] The limiting oxygen index (LOI) of the cured resins obtained in Examples 5-7 and Comparative Example 1 was measured according to the ASTM D2863 standard, and the vertical combustion test was performed according to the UL-94 standard. The mechanical properties were measured using a universal mechanical testing machine and a pendulum impact tester. The tensile strength was tested using a universal mechanical testing machine in accordance with GB / T 1040.5-2008, and the impact strength was tested using a pendulum impact tester in accordance with GB / T 1843-2008. The test results are shown in Table 1:

[0085] Table 1

[0086]

[0087] It can be seen from the test results in Table 1 that the epoxy resin cured product prepared by using the toughening agent of Examples 2-4 of the present invention has excellent mechanical properties and excellent flame retardant effect.

[0088] Antibacterial test: Add 20 mL of agar medium (prepare agar solution at a ratio of 3.2 g of nutrient agar per 100 mL of deionized water, shake well and sterilize in an autoclave. When the temperature in the autoclave drops to 60°C, take it out for later use) and 0.1 mL of Escherichia coli suspension (Escherichia coli 35218: from China National Center for Microbiological Culture Collection, 6×10 5 CFU / mL), after oscillation, 70mL of phosphate buffered saline solution was added (8.0g of sodium chloride, 1.44g of disodium hydrogen phosphate and 0.24g of potassium dihydrogen phosphate were weighed and dissolved in 800mL of distilled water, the pH value of the solution was adjusted to 7.4 with hydrochloric acid, and finally distilled water was added to make up to 1L to obtain 0.01mol / L phosphate buffered saline solution), the epoxy cured products of Examples 5-7 and Comparative Example 1 were cut into slices with a diameter of 5mm and added to culture dishes, and each group of culture dishes was placed in a constant temperature and humidity incubator (temperature of 37°C, relative humidity greater than 90%), and cultured at 37°C for 24h and 30 days, and then the antibacterial rate was calculated. The test results are shown in Table 2 below:

[0089] Table 2

[0090]

[0091] It can be seen from the test results in Table 2 that the epoxy resin cured product prepared by using the toughening agent of Examples 2-4 of the present invention has excellent antibacterial effect and the antibacterial effect is long-lasting and stable.

[0092] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0093] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a modified epoxy resin toughening agent, characterized in that: The steps include: Under nitrogen protection, add diisocyanate and catalyst into a reaction bottle containing reaction solvent, stir, slowly add auxiliary agent, heat to 40-60°C and react for 2-4h, and distill under reduced pressure to obtain modified epoxy resin toughening agent; Wherein, the auxiliary agent is prepared by the following steps: S1. Add diethyl (2-aminoethyl)phosphonate, pyridine and diethyl ether to a flask, stir, add tetradecane chloride and diethyl ether, react at 60°C for 2h, cool, and distill under reduced pressure to obtain intermediate 1. ; S2, replace the air in the bottle with nitrogen, add intermediate 1, triethylamine and DMSO, stir, add 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and DMSO, react at 75℃ for 2h, cool, and distill under reduced pressure to obtain intermediate 2 ; S3, nitrogen purged the flask, added intermediate 2, triethylamine and DMSO, stirred, added 3-chloro-1-propanol and DMSO, reacted at 80°C for 3h, cooled, and distilled under reduced pressure to obtain intermediate 3 ; S4, replace the air in the bottle with nitrogen, add intermediate 3 and DMF, stir, add octadecyltrichlorosilane, react at 30°C for 6h, cool, filter, rinse the filter cake, and dry to obtain intermediate 4 ; S5. Blow nitrogen into the flask, add intermediate 4 and DMF, stir, add propylene glycol and DMF, react at 40°C for 6h, cool, filter, wash the filter cake, and dry to obtain the auxiliary agent. 。 2. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The usage ratio of diethyl (2-aminoethyl)phosphonate, tetradecane chloride, pyridine and diethyl ether in step S1 is 0.08 mol: 0.085 mol: 9.7 mL: 150 mL.

3. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The usage ratio of the intermediate 1, 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane, triethylamine and DMSO in step S2 is 0.074 mol:0.035 mol:15.4 mL:200 mL.

4. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The usage ratio of the intermediate 2, 3-chloro-1-propanol, triethylamine and DMSO in step S3 is 0.035 mol: 0.036 mol: 7.3 mL: 200 mL.

5. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The usage ratio of octadecyltrichlorosilane, intermediate 3 and DMF in step S4 is 0.015 mol:0.03 mol:180 mL.

6. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The usage ratio of intermediate 4, propylene glycol and DMF in step S5 is 0.01 mol: 0.011 mol: 180 mL.

7. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The diisocyanate is one or more of diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, and toluene diisocyanate; the molar ratio of the diisocyanate to the auxiliary agent is 1:(0.8-1.2).

8. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The catalyst is one of the organic tin compounds; the mass of the catalyst is 0.08-0.12% of the total mass of the reaction raw materials.

9. The method for preparing a modified epoxy resin toughening agent according to claim 1, characterized in that: The reaction solvent is one or more of chloroform, toluene, xylene, 1,4-dioxane, tetrahydrofuran, dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide.

10. A modified epoxy resin toughening agent, characterized in that: The modified epoxy resin toughening agent is prepared according to the preparation method of any one of claims 1 to 9.