A multi-digital three-dimensional fire-imitation surface tile and its preparation method

By designing most digital three-dimensional imitation fire-burning surface structures on ceramic tiles, optimizing the composition and composition ratio, the problems of high gloss and poor effects of imitation fire-burning surface tiles in the existing technology are solved, and a more realistic imitation fire-burning surface effect and significant Improve anti-slip performance.

CN118637943BActive Publication Date: 2024-11-01FOSHAN JINDUO CERAMICS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411117047.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-01
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The ceramic tiles prepared in the prior art have problems such as high gloss, poor imitation fire effect and poor anti-slip effect, which cannot meet the consumer's requirements for the use of the product.

Method used

The ceramic tile design adopts most digital three-dimensional imitation fire-fired surfaces, including ceramic body, digital base glaze layer, digital surface glaze layer, pattern layer, dry particle layer and protective glaze layer. By optimizing the composition and composition ratio, combining different temperatures and colors Dry grains for more realistic texture and color effects, and improve the roughness of the tiles to improve anti-slip performance.

Benefits of technology

The prepared ceramic tile has rich appearance and regular grayscale changes in the pattern layer, forming a unique imitation fire texture effect, improving visual effect and anti-slip performance, and reducing the consumption and use cost of natural stone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637943B_ABST
    Figure CN118637943B_ABST
Patent Text Reader

Abstract

The present invention discloses a multi-digital three-dimensional imitation fire-burned surface tile and a preparation method thereof, and belongs to the field of architectural ceramics. The tile of the present invention comprises a ceramic body, a digital base glaze layer covering the surface of the ceramic body, a digital surface glaze layer covering the surface of the digital base glaze layer, a pattern layer covering the surface of the digital surface glaze layer, a dry particle layer covering the surface of the pattern layer, and a protective glaze layer covering the surface of the dry particle layer. The present invention optimizes the composition, composition ratio and particle grading, so that the appearance of the prepared tile is rich in color and has an excellent layering effect. The texture change of the tile surface after the firing treatment presents a flaky cleavage texture, which not only forms a unique imitation fire-burned texture effect, but also reduces the consumption of natural stone, reduces the use cost and maintenance components, and significantly improves the roughness of the tile surface, thereby improving the anti-slip performance of the tile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building ceramic preparation, in particular to a multi-digital three-dimensional fire-imitation surface tile and a preparation method thereof. Background Art

[0002] To a certain extent, ceramic tiles are designed to imitate the texture, color, light and touch of natural stone. However, due to the limitations of process technology and equipment, there is a large gap between the prepared ceramic tiles and natural stone. For example, the glossiness of the tile surface is too high, and the comfort experience is poor; the surface quality of the ceramic tiles does not reach the natural effect, that is, it is not realistic enough. As people like natural stone, the ceramic tile industry is required to be more innovative in process technology, including the development of ceramic tiles with more realistic imitation of fire-burned surface effects.

[0003] The fire-burned surface of ceramic tiles is to heat the ceramic tiles at high temperature until the crystals burst. Due to the high temperature, some impurities and low-melting-point components on the surface of the ceramic tiles are burned off, thereby forming a rough finish on the surface, which will feel rough to the touch. Since the ceramic tiles with fire-burned surfaces are rough and natural and do not reflect light, they are widely used in places such as subways, airports, squares, exterior wall hangings, sidewalks, parks, and parking lots. However, in the prior art, the surface of the processed ceramic tiles is controlled by methods such as dry printing, embossing, screen printing, and roller printing, so that the processed ceramic tiles have the texture effect pattern of natural stone, and then are heated at high temperature to have the effect of imitating the fire-burned surface, but the texture effect pattern is limited to a small part of the thickness of the surface layer, resulting in the problem of poor imitating the fire-burned surface effect. In addition, the ceramic tiles with imitating the fire-burned surface prepared in the prior art basically have the characteristics of being porous. In order to increase the usability of the ceramic tiles, a penetrating sealant is generally required, which also leads to the problem of poor anti-slip performance of the ceramic tiles with imitating the fire-burned surface.

[0004] In summary, the tiles with imitation fire-burned surfaces prepared in the prior art have the problems of high gloss, poor imitation fire-burned effect and poor anti-slip effect, and cannot meet the consumer's requirements for the product. Summary of the invention

[0005] Based on this, in order to solve the problem that the existing technology of preparing imitation fire-burned surface tiles has high gloss, poor imitation fire effect and poor anti-slip effect, the present invention provides a multi-digital three-dimensional imitation fire-burned surface tile and a preparation method thereof, and the specific technical scheme is as follows:

[0006] A multi-digital three-dimensional imitation fire-burned surface tile, the tile comprises a ceramic body, a digital base glaze layer covering the surface of the ceramic body, a digital surface glaze layer covering the surface of the digital base glaze layer, a pattern layer covering the surface of the digital surface glaze layer, a dry particle layer covering the surface of the pattern layer, and a protective glaze layer covering the surface of the dry particle layer, and the height difference of the surface of the tile is 0.05mm~0.35mm;

[0007] The gray value difference of the pattern layer is 40% to 100%, and the gray value difference of the connecting position is 15% to 35%;

[0008] The raw materials for preparing the dry particle layer include digital glue dry particles, yellow dry particles, red dry particles and green dry particles, and the digital glue dry particles are obtained by mixing high-temperature dry particles A and low-temperature dry particles, the temperature difference between the high-temperature dry particles A and the low-temperature dry particles is 40° C. to 60° C., and the mass ratio of the high-temperature dry particles A to the low-temperature dry particles is (3-5): (5-7);

[0009] The protective glaze used in the protective glaze layer is prepared by mixing high-temperature dry particles B, low-temperature glaze and glue, and the weight ratio of the high-temperature dry particles B, the low-temperature glaze and the glue is (25-45): (10-25): (80-100).

[0010] Furthermore, the specific gravity of the digital base glaze used in the digital base glaze layer is 1.75 g / cm 3 ~1.85 g / cm 3 , glaze application amount is 200 g / m 2 ~500g / m 2 ;

[0011] The digital base glaze includes the following chemical components in weight percentage:

[0012] SiO2: 65~75%, Al2O3: 8~13%, Fe2O3: 0~1%, TiO2: 0~1%, Na2O: 1~5%, CaO: 0~1%, MgO: 0~2%, K2O: 1~5%, ZnO: 1~3%, ZrO2: 5~10% and loss on ignition: 1~3%.

[0013] Furthermore, the specific gravity of the digital glaze used in the digital glaze layer is 1.1 g / cm 3 ~1.2 g / cm 3 , glaze application amount is 100 g / m 2 ~200g / m 2 ;

[0014] The digital glaze comprises the following chemical components in weight percentage:

[0015] SiO2: 55~65%, Al2O3: 5~10%, Fe2O3: 0~1%, TiO2: 0~0.5%, CaO: 8~12%, MgO: 0.5~2%, K2O: 2~5%, Na2O: 0.5~2%, ZnO: 5~8%, ZrO: 3~6% and loss on ignition: 5~8%.

[0016] Furthermore, the application amount of the digital glue dry particles, the yellow dry particles, the red dry particles and the green dry particles are all 400 g / m 2 ~500 g / m 2 .

[0017] Furthermore, the initial melting temperature of the high-temperature dry particles A is 1160-1250°C;

[0018] The high temperature dry particles A include the following chemical components in weight percentage: SiO2: 50-60%, Al2O3: 15-25%, K2O: 3-7%, Na2O: 1-4%, CaO: 5-10%, MgO: 1-5%, ZnO: 2-6%, SrO: 3-8%, BaO: 3-7% and loss on ignition: 1-5%;

[0019] The particle grading of the high-temperature dry particles A is: above 60 mesh: none, 60 mesh to 80 mesh: 5-15%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 20-35%, 150 mesh to 200 mesh: 15-25%, 200 mesh to 250 mesh: 10-20%, and below 250 mesh: 5-15%.

[0020] Furthermore, the initial melting temperature of the low-temperature dry particles is 1100-1170°C;

[0021] The low-temperature dry particles include the following chemical components in weight percentage: SiO2: 55-65%, Al2O3: 15-25%, K2O: 3-7%, Na2O: 5-10%, CaO: 5-10%, ZnO: 2-5% and loss on ignition: 1-5%;

[0022] The particle grading of the low-temperature dry particles is: above 60 mesh: none, 60 mesh to 80 mesh: 7 to 15%, 80 mesh to 100 mesh: 15 to 25%, 100 mesh to 120 mesh: 15 to 25%, 120 mesh to 150 mesh: 5 to 15%, 150 mesh to 200 mesh: 5 to 15%, 200 mesh to 250 mesh: 5 to 15%, and below 250 mesh: 5 to 15%.

[0023] Furthermore, the particle grading of the yellow dry particles, the red dry particles and the green dry particles are all as follows: above 60 mesh: none, 60 mesh to 80 mesh: 5 to 10%, 80 mesh to 100 mesh: 10 to 20%, 100 mesh to 120 mesh: 15 to 25%, 120 mesh to 150 mesh: 25 to 35%, 150 mesh to 200 mesh: 12 to 23%, 200 mesh to 250 mesh: 7 to 15%, and below 250 mesh: 5 to 10%.

[0024] Further, the high temperature dry particles B include the following chemical components in weight percentage: SiO2: 55-65%, Al2O3: 5-10%, Fe2O3: 0-1%, TiO2: 0-0.5%, CaO: 5-8%, MgO: 6-10%, K2O: 2-5%, Na2O: 0.5-2%, BaO: 2-5% and loss on ignition: 5-8%;

[0025] The particle grading of the high-temperature dry particles B is: above 60 mesh: none, 60 mesh to 80 mesh: 5-15%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 20-35%, 150 mesh to 200 mesh: 15-25%, 200 mesh to 250 mesh: 10-20%, and below 250 mesh: 5-15%.

[0026] Furthermore, the low-temperature glaze includes the following chemical components in weight percentage: SiO2: 35~45%, Al2O3: 8~18%, Fe2O3: 0~1%, TiO2: 0~1%, CaO: 1~3%, MgO: 2~5%, K2O: 2~5%, Na2O: 1~3%, ZnO: 5~8%, BaO: 20~26% and loss on ignition: 5~8%.

[0027] In addition, the present invention also provides a method for preparing a multi-digital three-dimensional imitation fire-burned surface tile, the preparation method comprising the following steps:

[0028] After the ceramic green body powder is pressed, it is dried at 190° C. for 35 minutes to obtain a ceramic green body with a moisture content of 0.5% to 0.7%.

[0029] Spraying a prefabricated digital base glaze on the surface of the ceramic body to form a digital base glaze layer with a pattern texture;

[0030] Spraying digital top glaze on the digital base glaze layer to form a digital top glaze layer;

[0031] Inkjet printing a preset pattern on the digital glaze layer, and then spraying a digital glue pattern to form a pattern layer;

[0032] Applying dry particles on the pattern layer, wherein the dry particles include digital glue dry particles, yellow dry particles, red dry particles and green dry particles, and recovering the dry particles that are not attached to the pattern layer through an absorption system, and repeating this process several times to perform a drying process to form a dry particle layer;

[0033] A protective glaze is sprayed on the dry particle layer, and after drying in a drying kiln, a protective glaze layer is formed, and then the ceramic tile is fired in a roller kiln. The surface of the ceramic tile is lightly swept and edged to obtain a plurality of digital three-dimensional imitation fire-burned ceramic tiles.

[0034] The above scheme optimizes the ingredients and the ratio of ingredients, so that the appearance of the prepared tiles is rich in color and has excellent layering effect. The grayscale of the pattern layer changes regularly in a gradient manner, and the places where the dry particles are accumulated also change regularly in a gradient increasing or decreasing manner. The texture change of the tile surface after firing treatment presents a flaky cleavage texture, forming a unique imitation fire-burned texture effect; the tiles prepared by the present invention not only improve the visual effect, but also the multi-layered digital glaze and digital glue dry particle glaze layer cooperate synergistically to achieve excellent texture and color effects through dry particles of different temperatures, different glosses and different colors, making the pattern and texture more realistic; after optimizing the ingredients and the ratio of ingredients of the tiles, the present invention can not only obtain tiles with a burned surface, reduce the consumption of natural stone, reduce the use cost and maintenance components, but also significantly improve the roughness of the tile surface, thereby improving the anti-slip performance of the tile. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a schematic diagram of a process flow for preparing a multi-digital three-dimensional fire-imitation surface tile according to Example 1 of the present invention;

[0036] Figure 2 A schematic diagram of a product of a plurality of digital three-dimensional imitation fire-burned surface tiles prepared in Example 1 of the present invention;

[0037] Figure 3 This is a schematic structural diagram of a plurality of digital three-dimensional imitation fire-burned surface tiles prepared in Example 1 of the present invention.

[0038] Description of Reference Numerals

[0039] 1. Ceramic body, 2. Digital base glaze layer, 3. Digital top glaze layer, 4. Pattern layer, 5. Dry particle layer, 6. Protective glaze layer. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0042] In one embodiment of the present invention, a multi-digital three-dimensional imitation fire-burned surface tile comprises a ceramic body, a digital base glaze layer covering the surface of the ceramic body, a digital surface glaze layer covering the surface of the digital base glaze layer, a pattern layer covering the surface of the digital surface glaze layer, a dry particle layer covering the surface of the pattern layer, and a protective glaze layer covering the surface of the dry particle layer, and the height difference of the surface of the tile is 0.05 mm to 0.35 mm;

[0043] The gray value difference of the pattern layer is 40% to 100%, and the gray value difference of the connecting position is 15% to 35%. If the gray value difference is too small, the surface drop of the tile obtained after the firing treatment is too small, and the layering is poor. If the gray value difference is too large, the surface drop of the tile obtained after the firing treatment is too large, the transition is unnatural, and the tile with better visual effect cannot be formed.

[0044] The raw materials for preparing the dry particle layer include digital glue dry particles, yellow dry particles, red dry particles and green dry particles, and the digital glue dry particles are obtained by mixing high-temperature dry particles A and low-temperature dry particles, the temperature difference between the high-temperature dry particles A and the low-temperature dry particles is 40°C~60°C, and the mass ratio of the high-temperature dry particles A to the low-temperature dry particles is (3~5):(5~7); if the temperature difference is too small, it is not conducive to temperature adjustment, which indirectly affects the firing effect. If the temperature difference is too large, it is easy to cause serious crystallization problems, which will also affect the apparent quality of the tile.

[0045] The protective glaze used in the protective glaze layer is prepared by mixing high-temperature dry particles B, low-temperature glaze and glue, and the weight ratio of the high-temperature dry particles B, the low-temperature glaze and the glue is (25-45): (10-25): (80-100).

[0046] In one embodiment, the specific gravity of the digital base glaze is 1.75 g / cm 3 ~1.85 g / cm 3 , glaze application amount is 200 g / m 2 ~500g / m 2 ;

[0047] The digital base glaze used in the digital base glaze layer includes the following chemical components in weight percentage:

[0048] SiO2: 65~75%, Al2O3: 8~13%, Fe2O3: 0~1%, TiO2: 0~1%, Na2O: 1~5%, CaO: 0~1%, MgO: 0~2%, K2O: 1~5%, ZnO: 1~3%, ZrO2: 5~10% and loss on ignition: 1~3%.

[0049] In one embodiment, the digital glaze layer has a specific gravity of 1.1 g / cm3 ~1.2g / cm 3 , glaze application amount is 100 g / m 2 ~200g / m 2 ;

[0050] The digital glaze comprises the following chemical components in weight percentage:

[0051] SiO2: 55~65%, Al2O3: 5~10%, Fe2O3: 0~1%, TiO2: 0~0.5%, CaO: 8~12%, MgO: 0.5~2%, K2O: 2~5%, Na2O: 0.5~2%, ZnO: 5~8%, ZrO: 3~6% and loss on ignition: 5~8%.

[0052] In one embodiment, the amount of glue applied in the pattern layer is 35 g / m 2 ~ 45g / m 2 .

[0053] In one embodiment, the application amount of the digital glue dry particles, the yellow dry particles, the red dry particles and the green dry particles is 400 g / m 2 ~500 g / m 2 .

[0054] In one embodiment, the initial melting temperature of the high temperature dry particles A is 1160-1250°C;

[0055] The high temperature dry particles A include the following chemical components in weight percentage: SiO2: 50-60%, Al2O3: 15-25%, K2O: 3-7%, Na2O: 1-4%, CaO: 5-10%, MgO: 1-5%, ZnO: 2-6%, SrO: 3-8%, BaO: 3-7% and loss on ignition: 1-5%;

[0056] The particle grading of the high-temperature dry particles A is: above 60 mesh: none, 60 mesh to 80 mesh: 5-15%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 20-35%, 150 mesh to 200 mesh: 15-25%, 200 mesh to 250 mesh: 10-20%, and below 250 mesh: 5-15%.

[0057] In one embodiment, the initial melting temperature of the low-temperature dry particles is 1100-1170°C;

[0058] The low-temperature dry particles include the following chemical components in weight percentage: SiO2: 55-65%, Al2O3: 15-25%, K2O: 3-7%, Na2O: 5-10%, CaO: 5-10%, ZnO: 2-5% and loss on ignition: 1-5%;

[0059] The particle grading of the low-temperature dry particles is: above 60 mesh: none, 60 mesh to 80 mesh: 7 to 15%, 80 mesh to 100 mesh: 15 to 25%, 100 mesh to 120 mesh: 15 to 25%, 120 mesh to 150 mesh: 5 to 15%, 150 mesh to 200 mesh: 5 to 15%, 200 mesh to 250 mesh: 5 to 15%, and below 250 mesh: 5 to 15%.

[0060] In one embodiment, the particle grading of the yellow dry particles, the red dry particles and the green dry particles are: above 60 mesh: none, 60 mesh to 80 mesh: 5-10%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 25-35%, 150 mesh to 200 mesh: 12-23%, 200 mesh to 250 mesh: 7-15%, and below 250 mesh: 5-10%.

[0061] In one embodiment, the yellow dry particles include the following chemical components in weight percentage: Al2O3: 10-20%, SiO2: 55-65%, CaO: 5-10%, MgO: 2-7%, K2O: 1-3%, Na2O: 3-6%, ZnO: 2-4%, BaO: 4.5%, CoO: 1-3%, PrO: 5-10% and loss on ignition: 0.5-2%.

[0062] In one embodiment, the red dry particles include the following chemical components in weight percentage: Al2O3: 10-15%, SiO2: 45-55%, CaO: 3-7%, MgO: 1-5%, K2O: 3-7%, Na2O: 3-8%, ZnO: 2-6%, BaO: 3-8%, CuO: 8-12% and loss on ignition: 1-4%.

[0063] In one embodiment, the green dry particles include the following chemical components in weight percentage: Al2O3: 10-15%, SiO2: 45-55%, CaO: 3-7%, MgO: 1-5%, K2O: 3-7%, Na2O: 3-8%, ZnO: 2-6%, BaO: 3-8%, Cr2O3: 5-10% and loss on ignition: 1-5%.

[0064] In one embodiment, the specific gravity of the protective glaze is 1.35 g / cm 3 ~1.50g / cm 3, glaze amount 200 g / m 2 ~500g / m 2 .

[0065] In one embodiment, the high temperature dry particles B include the following chemical components in weight percentage: SiO2: 55-65%, Al2O3: 5-10%, Fe2O3: 0-1%, TiO2: 0-0.5%, CaO: 5-8%, MgO: 6-10%, K2O: 2-5%, Na2O: 0.5-2%, BaO: 2-5% and loss on ignition: 5-8%;

[0066] The particle grading of the high-temperature dry particles B is: above 60 mesh: none, 60 mesh to 80 mesh: 5-15%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 20-35%, 150 mesh to 200 mesh: 15-25%, 200 mesh to 250 mesh: 10-20%, and below 250 mesh: 5-15%.

[0067] In one embodiment, the low-temperature glaze includes the following chemical components in weight percentage: SiO2: 35~45%, Al2O3: 8~18%, Fe2O3: 0~1%, TiO2: 0~1%, CaO: 1~3%, MgO: 2~5%, K2O: 2~5%, Na2O: 1~3%, ZnO: 5~8%, BaO: 20~26% and loss on ignition: 5~8%.

[0068] In addition, the present invention also provides a method for preparing a multi-digital three-dimensional imitation fire-burned surface tile, the preparation method comprising the following steps:

[0069] After the ceramic green body powder is pressed, it is dried at 190° C. for 35 minutes to obtain a ceramic green body with a moisture content of 0.5% to 0.7%.

[0070] Spraying a prefabricated digital base glaze on the surface of the ceramic body to form a digital base glaze layer with a pattern texture;

[0071] Spraying digital top glaze on the digital base glaze layer to form a digital top glaze layer;

[0072] Inkjet printing a preset pattern on the digital glaze layer, and then spraying a digital glue pattern to form a pattern layer;

[0073] Applying dry particles on the pattern layer, wherein the dry particles include digital glue dry particles, yellow dry particles, red dry particles and green dry particles, and recovering the dry particles that are not attached to the pattern layer through an absorption system, and repeating this process several times to perform a drying process to form a dry particle layer;

[0074] A protective glaze is sprayed on the dry particle layer, and after drying in a drying kiln, a protective glaze layer is formed, and then the ceramic tile is fired in a roller kiln. The surface of the ceramic tile is lightly swept and edged to obtain a plurality of digital three-dimensional imitation fire-burned ceramic tiles.

[0075] In one embodiment, the drying temperature is 100°C to 200°C.

[0076] In one embodiment, the sintering treatment temperature is 1150°C to 1200°C, and the holding time is 10min to 15min.

[0077] In the above scheme, by optimizing the components and the ratio of the components, a ceramic tile with a fire-burned effect can be obtained, and the surface roughness of the ceramic tile can be significantly improved, thereby improving the anti-slip performance.

[0078] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0079] Embodiment 1:

[0080] A multi-digital three-dimensional imitation fire-burned surface tile includes a ceramic body, a digital base glaze layer covering the surface of the ceramic body, a digital surface glaze layer covering the surface of the digital base glaze layer, a pattern layer covering the surface of the digital surface glaze layer, a dry particle layer covering the surface of the pattern layer, and a protective glaze layer covering the surface of the dry particle layer; wherein various parameters of the digital base glaze layer, the digital surface glaze layer, the dry particle layer and the protective glaze layer are shown in Table 1.

[0081] A method for preparing a multi-digital three-dimensional fire-imitation surface tile, the preparation method comprising the following steps:

[0082] After the ceramic green body powder is pressed, it is dried at 190° C. for 35 minutes to obtain a ceramic green body with a moisture content of 0.7%.

[0083] A prefabricated digital base glaze is sprayed on the surface of the ceramic body, and the specific gravity of the digital base glaze is 1.75 g / cm 3 , glaze application amount is 250g / m 2 , forming a digital base glaze layer with pattern texture;

[0084] The digital top glaze is sprayed on the digital base glaze layer, and the specific gravity of the digital top glaze is 1.1 g / cm 3 , glaze application amount is 200g / m 2 , forming a digital glaze layer;

[0085] A preset pattern is inkjet printed on the digital glaze layer, and then a digital glue pattern is sprayed. The digital glue pattern is processed according to the color change. The grayscale of the digital glue pattern changes regularly in a gradient manner. The place where the dry particles are accumulated also changes with a regular gradient increase or decrease. The grayscale value difference of the digital glue pattern is 40%-100%, and the grayscale value difference of the connection position is 15%-35%. The amount of glue applied is 40g / m 2 , forming a pattern layer;

[0086] Dry particles are applied on the pattern layer, and the dry particles include digital glue dry particles (the mass ratio of high temperature dry particles A to low temperature dry particles is 4:6, the initial melting temperature of high temperature dry particles A is 1205°C, the initial melting temperature of low temperature dry particles is 1163°C, and the temperature difference between high temperature dry particles A and low temperature dry particles is 42°C), yellow dry particles, red dry particles and green dry particles, and the application amount of digital glue dry particles, yellow dry particles, red dry particles and green dry particles is 450g / m 2 , recovering the dry particles not adhering to the pattern layer through an absorption system, repeating this process three times, and performing a drying process to form a dry particle layer;

[0087] Spray protective glaze (prepared from high-temperature dry particles B: low-temperature glaze: glue in a weight ratio of 35:15:100) on the dry particle layer, and the specific gravity of the protective glaze is 1.43 g / cm 3 , glaze application amount is 285g / m 2 , after being dried in a drying kiln and the drying temperature is controlled at 150°C to form a protective glaze layer, it is then fired in a roller kiln at a temperature of 1190°C and a holding time of 10 minutes. Five groups of 1000-mesh fiber modules are used to lightly sweep and edge grind the surface of the tile to obtain mostly digital three-dimensional imitation fire-burned tiles.

[0088] Table 1:

[0089]

[0090] Embodiment 2:

[0091] The difference between Example 2 and Example 1 is that the temperature difference between the high-temperature dry particles A and the low-temperature dry particles in Example 2 is 60° C., and the other preparation methods and particle grading are the same as those in Example 1.

[0092] Embodiment 3:

[0093] The difference between Example 3 and Example 1 is that in Example 3, the mass ratio of high-temperature dry particles A to low-temperature dry particles is 3:7, and other preparation methods and particle grading are the same as those in Example 1.

[0094] Embodiment 4:

[0095] The difference between Example 4 and Example 1 is that the weight ratio of high-temperature dry particles B, low-temperature glaze and glue in Example 4 is 30:20:100, and the rest is the same as Example 1.

[0096] The surfaces of the tile samples 1-4 prepared in the above-mentioned embodiments 1-4 respectively show excellent imitation fire-burned surface effects and realistic textures; the height differences of the surfaces of the tile samples 1-4 prepared in embodiments 1-4 are all in the range of 0.05mm-0.35mm, which not only have significant anti-slip properties, but also have excellent anti-fouling and wear-resistant properties.

[0097] Comparative Example 1:

[0098] The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, no yellow dry particles, red dry particles and green dry particles are administered, and the rest is the same as Example 1.

[0099] The tile comparison sample 1 prepared in comparative example 1 has a pear skin roughness on the surface, but lacks the color effect of the burnt surface, has a poor visual layering effect, and cannot meet the market demand.

[0100] Comparative Example 2:

[0101] The difference between Comparative Example 2 and Example 1 is that the mass ratio of the high-temperature dry particles A to the low-temperature dry particles in Comparative Example 2 is 6:4, and the rest is the same as Example 1.

[0102] The ceramic tile comparison sample 2 prepared in comparative example 2 has a burnt surface effect, but its surface roughness is too large and has a noticeable prickly feel, which affects the overall comfort of the ceramic tile. Its performance fails to meet the market demand.

[0103] Comparative Example 3:

[0104] The difference between Comparative Example 3 and Example 1 is that the mass ratio of the high-temperature dry particles A to the low-temperature dry particles in Comparative Example 3 is 1:10, and the rest is the same as Example 1.

[0105] The tile comparison sample 3 prepared in comparative example 3 contains more low-temperature dry particles and has a low initial melting temperature. The surface dry particles are in a molten state, resulting in a poor three-dimensional effect on the surface of the tile comparison sample 3 and excessive glossiness, with a glossiness of 20°. At the same time, defects such as pinholes and prickly heat also appear on the surface of the tile, which cannot meet market usage requirements.

[0106] Comparative Example 4:

[0107] The particle size distribution of the high temperature dry particles A and the low temperature dry particles in Comparative Example 4 is controlled at 150 mesh to 250 mesh, and the others are the same as those in Example 1.

[0108] The tile comparison sample 4 prepared in Comparative Example 4 is prone to clogging during the preparation process and is prone to uneven application of dry particles. Since the overall particle size of the dry particles is relatively small, the surface area of ​​the dry particles increases, the friction between the particles increases, the angle of repose increases, and the fluidity also changes, resulting in the prepared tile comparison sample 4 having a poor apparent quality and cannot meet the market's usage needs.

[0109] Comparative Example 5:

[0110] The difference between Comparative Example 5 and Example 1 is that the gray value difference of the connecting position in Comparative Example 5 is 0%-10%, and the others are the same as Example 1.

[0111] The tile comparative sample 5 prepared in comparative example 5 has a low range of grayscale value difference at the connection position, the pattern connection on the tile surface is smooth, and the transition height is small, which leads to a poor three-dimensional sense of the tile surface and a poor overall appearance, which cannot meet the market usage needs.

[0112] Comparative Example 6:

[0113] The difference between Comparative Example 6 and Example 1 is that the temperature difference between the high-temperature dry particles A and the low-temperature dry particles in Comparative Example 6 is 10° C., and the rest is the same as Example 1.

[0114] The tile comparison sample 6 prepared in Comparative Example 6 has problems such as unstable surface quality, uneven surface color, and uneven particle distribution during the firing process due to the small temperature difference, and cannot meet the market demand.

[0115] Comparative Example 7:

[0116] The difference between Comparative Example 7 and Example 1 is that the digital base glaze and the digital top glaze in Comparative Example 7 are sprayed in a conventional manner, and the rest is the same as Example 1.

[0117] The surface of the tile comparison sample 7 obtained in comparative example 7 is too smooth and does not meet the roughness requirement. The overall texture of the surface has a poor three-dimensional sense and poor anti-slip performance, which cannot meet the market demand.

[0118] The performance tests were performed on the tile samples 1-4 prepared in Examples 1-4 and the tile comparison samples 1-7 prepared in Comparative Examples 1-7. The results are shown in Table 2 below.

[0119] Table 2: Test results

[0120]

[0121] It can be seen from Table 2 that the ceramic tiles prepared in the present application have suitable glossiness, and also have anti-fouling, anti-slip and wear-resistant properties.

[0122] in addition, Figure 2 The product schematic diagram of the multi-digital three-dimensional imitation fire-burned surface tile prepared in Example 1 of the present invention, combined with Figure 2 It can be clearly seen that the surface pattern and texture of the ceramic tile prepared in this application are realistic, the gloss and color can achieve the effect of imitating the fire-burned surface, and the colors and layers are relatively rich, and it has a certain surface roughness to achieve an anti-slip effect, which can meet the market's use needs. The ceramic tile samples prepared in Examples 2 to 4 have the same effect, which will not be repeated here.

[0123] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0124] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A multi-digital three-dimensional imitation fire-burned surface tile, characterized in that: The ceramic tile comprises a ceramic body, a digital base glaze layer covering the surface of the ceramic body, a digital surface glaze layer covering the surface of the digital base glaze layer, a pattern layer covering the surface of the digital surface glaze layer, a dry particle layer covering the surface of the pattern layer, and a protective glaze layer covering the surface of the dry particle layer. The height difference of the surface of the ceramic tile is 0.05 mm to 0.35 mm, and the digital base glaze layer with pattern texture is formed by spraying the digital base glaze, and the digital surface glaze layer is formed by spraying the digital surface glaze. The gray value difference of the pattern layer is 40% to 100%, and the gray value difference of the connecting position is 15% to 35%; The raw materials for preparing the dry particle layer include digital glue dry particles, yellow dry particles, red dry particles and green dry particles, and the digital glue dry particles are obtained by mixing high-temperature dry particles A and low-temperature dry particles, the temperature difference between the high-temperature dry particles A and the low-temperature dry particles is 40° C. to 60° C., and the mass ratio of the high-temperature dry particles A to the low-temperature dry particles is (3-5): (5-7); The particle grading of the yellow dry granules, the red dry granules and the green dry granules are all as follows: above 60 mesh: none, 60 mesh to 80 mesh: 5-10%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 25-35%, 150 mesh to 200 mesh: 12-23%, 200 mesh to 250 mesh: 7-15%, below 250 mesh: 5-10%; The high temperature dry particles A include the following chemical components in weight percentage: SiO2: 50-60%, Al2O3: 15-25%, K2O: 3-7%, Na2O: 1-4%, CaO: 5-10%, MgO: 1-5%, ZnO: 2-6%, SrO: 3-8%, BaO: 3-7% and loss on ignition: 1-5%; The particle gradation of the high temperature dry particles A is: above 60 mesh: none, 60 mesh to 80 mesh: 5-15%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 20-35%, 150 mesh to 200 mesh: 15-25%, 200 mesh to 250 mesh: 10-20%, below 250 mesh: 5-15%; The low-temperature dry particles include the following chemical components in weight percentage: SiO2: 55-65%, Al2O3: 15-25%, K2O: 3-7%, Na2O: 5-10%, CaO: 5-10%, ZnO: 2-5% and loss on ignition: 1-5%; The particle grading of the low-temperature dry particles is: above 60 mesh: none, 60 mesh to 80 mesh: 7 to 15%, 80 mesh to 100 mesh: 15 to 25%, 100 mesh to 120 mesh: 15 to 25%, 120 mesh to 150 mesh: 5 to 15%, 150 mesh to 200 mesh: 5 to 15%, 200 mesh to 250 mesh: 5 to 15%, below 250 mesh: 5 to 15%; The protective glaze used in the protective glaze layer is prepared by mixing high-temperature dry particles B, low-temperature glaze and glue, and the weight ratio of the high-temperature dry particles B, the low-temperature glaze and the glue is (25-45): (10-25): (80-100); The high temperature dry particles B include the following chemical components in weight percentage: SiO2: 55-65%, Al2O3: 5-10%, Fe2O3: 0-1%, TiO2: 0-0.5%, CaO: 5-8%, MgO: 6-10%, K2O: 2-5%, Na2O: 0.5-2%, BaO: 2-5% and loss on ignition: 5-8%; The particle gradation of the high temperature dry particles B is: above 60 mesh: none, 60 mesh to 80 mesh: 5-15%, 80 mesh to 100 mesh: 10-20%, 100 mesh to 120 mesh: 15-25%, 120 mesh to 150 mesh: 20-35%, 150 mesh to 200 mesh: 15-25%, 200 mesh to 250 mesh: 10-20%, below 250 mesh: 5-15%; The low-temperature glaze includes the following chemical components in weight percentage: SiO2: 35~45%, Al2O3: 8~18%, Fe2O3: 0~1%, TiO2: 0~1%, CaO: 1~3%, MgO: 2~5%, K2O: 2~5%, Na2O: 1~3%, ZnO: 5~8%, BaO: 20~26% and loss on ignition: 5~8%.

2. The multi-digital three-dimensional imitation fire-burned surface tile according to claim 1, characterized in that: The specific gravity of the digital base glaze used in the digital base glaze layer is 1.75g / cm 3 ~1.85 g / cm 3 , glaze application amount is 200 g / m 2 ~500g / m 2 ; The digital base glaze includes the following chemical components in weight percentage: SiO2: 65~75%, Al2O3: 8~13%, Fe2O3: 0~1%, TiO2: 0~1%, Na2O: 1~5%, CaO: 0~1%, MgO: 0~2%, K2O: 1~5%, ZnO: 1~3%, ZrO2: 5~10% and loss on ignition: 1~3%.

3. The multi-digital three-dimensional imitation fire-burned surface tile according to claim 1, characterized in that: The specific gravity of the digital glaze used in the digital glaze layer is 1.1 g / cm 3 ~1.2 g / cm 3 , glaze application amount is 100 g / m 2 ~200g / m 2 ; The digital glaze comprises the following chemical components in weight percentage: SiO2: 55~65%, Al2O3: 5~10%, Fe2O3: 0~1%, TiO2: 0~0.5%, CaO: 8~12%, MgO: 0.5~2%, K2O: 2~5%, Na2O: 0.5~2%, ZnO: 5~8%, ZrO: 3~6% and loss on ignition: 5~8%.

4. The multi-digital three-dimensional imitation fire-burned surface tile according to claim 1, characterized in that: The application amount of the digital glue dry particles, the yellow dry particles, the red dry particles and the green dry particles is 400 g / m 2 ~500 g / m 2 .

5. The digital three-dimensional imitation fire-burned surface tile according to claim 1, characterized in that: The initial melting temperature of the high-temperature dry particles A is 1160-1250°C.

6. The multi-digital three-dimensional imitation fire-burned surface tile according to claim 5, characterized in that: The initial melting temperature of the low-temperature dry particles is 1100-1170°C.

7. A method for preparing a multi-digital three-dimensional fire-imitation surface tile, characterized in that: The preparation method is used to prepare the multi-digital three-dimensional imitation fire-burned surface ceramic tile as claimed in any one of claims 1 to 6, and the preparation method comprises the following steps: After the ceramic green body powder is pressed, it is dried at 190° C. for 35 minutes to obtain a ceramic green body with a moisture content of 0.5% to 0.7%. Spraying a prefabricated digital base glaze on the surface of the ceramic body to form a digital base glaze layer with a pattern texture; Spraying digital top glaze on the digital base glaze layer to form a digital top glaze layer; Inkjet printing a preset pattern on the digital glaze layer, and then spraying a digital glue pattern to form a pattern layer; Applying dry particles on the pattern layer, wherein the dry particles include digital glue dry particles, yellow dry particles, red dry particles and green dry particles, and recovering the dry particles that are not attached to the pattern layer through an absorption system, and repeating this process several times to perform a drying process to form a dry particle layer; A protective glaze is sprayed on the dry particle layer, and after drying in a drying kiln, a protective glaze layer is formed, and then the ceramic tile is fired in a roller kiln. The surface of the ceramic tile is lightly swept and edged to obtain a plurality of digital three-dimensional imitation fire-burned ceramic tiles.