A high-service performance low-rare earth magnesium alloy with element segregation and preparation method and application thereof

By introducing intra-crystal element agglomeration and grain boundary element partial agglomeration in magnesium alloys, the problems of complex processes and high energy consumption of existing magnesium alloys have been solved, significantly improving its service performance and broadening its industrial application prospects.

CN118653112BActive Publication Date: 2024-11-26HUNAN JINGE NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072472.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-26
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

When increasing strength, existing magnesium alloys have complex processes and high energy consumption, which affects service performance and are not suitable for industrial production.

Method used

By introducing intra-crystal element agglomeration and grain boundary element agglomeration, 650-730℃ melting and inert gas protection, A and B elements are added, homogenized annealing, low-temperature extrusion and low-speed thermal deformation are carried out to control grain refinement and The elements are partially aggregated to form an ultrafine crystal magnesium alloy.

Benefits of technology

It significantly improves the service performance of magnesium alloys, significantly improves fatigue life and creep life, simplified process and low cost, and is suitable for aerospace and rail transit fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118653112B_ABST
    Figure CN118653112B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of alloy materials, and specifically discloses a low-rare earth magnesium alloy with high service performance and element segregation, and its preparation method and application, including the following steps. The low-rare earth magnesium alloy contains 0.2‑1wt% of element A, 0.2‑1wt% of element B, and the remainder is magnesium and other inevitable impurities; the element A is one of manganese and calcium; the element B is one of neodymium, cerium, and yttrium; the preparation method is: smelting, casting, cutting and peeling, homogenizing annealing, low-temperature extrusion and then low-temperature, low-speed unidirectional thermal deformation. The extrusion temperature is controlled to be 150‑250°C, the extrusion ratio is 20:1‑30:1, and the extrusion speed is 50‑200mm / min. The unidirectional thermal deformation temperature is controlled to be 200‑350°C, and the strain rate is less than 1×10 ‑3 s ‑1 , the deformation is 5%-50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of alloy materials, and specifically discloses a high-service performance low-rare earth magnesium alloy with element segregation, a preparation method and application thereof. Background Art

[0002] Due to its advantages such as low density, high specific strength / specific stiffness, good damping and abundant resources, magnesium alloy has an increasingly broad application prospect in the fields of transportation, aerospace and aviation, and has become an ideal material to replace aluminum alloy. At present, magnesium alloy extrusions are an important bulk product form for the production of deformed magnesium alloy structural parts. They can not only be used in the fields of people's livelihood such as bicycles, automobiles, sports equipment, but also in high-speed rail, aerospace and military fields on a large scale.

[0003] At present, the main way to improve the strength of magnesium alloys is to prepare them through severe plastic deformation such as equal channel angular extrusion, high pressure torsion and repeated bending. Although it can effectively improve the strength, it has a great impact on the service performance of magnesium alloys, is complex in process, requires complex equipment, and has high energy consumption, making it unsuitable for industrial production. Therefore, it is of great significance to explore new magnesium alloys with higher service performance. Summary of the invention

[0004] In order to solve the above problems, the present invention discloses a high service performance, low rare earth magnesium alloy with element segregation, and a preparation method and application thereof, which promotes grain boundary sliding and non-basal sliding by introducing intracrystalline element agglomeration and grain boundary element segregation, effectively refines the grains, and thus significantly improves the service performance.

[0005] The present invention includes the following technical solutions:

[0006] A method for preparing a low-rare earth magnesium alloy with high service performance and element segregation, wherein the low-rare earth magnesium alloy contains 0.2-1wt% of element A, 0.2-1wt% of element B, and the remainder is magnesium and other inevitable impurities;

[0007] The element A is one of manganese and calcium;

[0008] The B element is one of neodymium, cerium and yttrium;

[0009] The preparation method of the low rare earth magnesium alloy comprises the following steps:

[0010] (1) Smelting magnesium ingots in the range of 650-730°C, using inert gas protection during the smelting process, raising the temperature to 750-800°C after complete melting, adding element A and element B in sequence, refining for 20-40 min under inert gas protection conditions, allowing the molten metal to stand, slag removal and cooling to 680-710°C, and casting into ingots;

[0011] (2) The magnesium alloy obtained in step (1) is subjected to homogenization annealing treatment at a temperature range of 350-500°C for a time of 20-40 h;

[0012] (3) The homogenized annealed magnesium alloy obtained in step (2) is subjected to low temperature extrusion to obtain an ultrafine-grained magnesium alloy, the extrusion temperature is controlled to be 100~300°C, the extrusion ratio is 10:1~30:1, and the extrusion speed is 50~200 mm / min;

[0013] (4) subjecting the ultrafine-grained magnesium alloy obtained in step (3) to unidirectional low-temperature and low-speed thermal deformation, controlling the unidirectional thermal deformation temperature to be 200-350°C and the strain rate to be less than 1×10 -3 s -1 , the deformation amount is 5%~50%, and the high service performance low rare earth magnesium alloy with element segregation is obtained.

[0014] Furthermore, the above-mentioned method for preparing a high-service performance, low-rare earth magnesium alloy with element segregation eliminates organizational defects and homogenizes the organization by using dislocations and thermal deformation generated by extrusion, and causes the elements to segregate near the grain boundaries, and causes the element grain boundaries to segregate at the grain boundaries to form a thin-skinned GP zone by low-temperature extrusion, and then increases the grain boundary element segregation and generates element clusters inside the grains by low-temperature, low-speed unidirectional thermal deformation; wherein the size of the element clusters within the crystal is 5~20 nm, and the concentration of A and B elements at the grain boundaries is 1.2~3 times that of the crystal.

[0015] Furthermore, in the above-mentioned method for preparing a high service performance low rare earth magnesium alloy with element segregation, the homogenization annealing treatment temperature range in step (2) is 400-500°C and the time is 30-40 h.

[0016] Furthermore, in the above-mentioned method for preparing a high service performance low rare earth magnesium alloy with element segregation, the extrusion temperature in step (3) is 150-250° C., the extrusion ratio is 20:1-30:1, and the extrusion speed is 50-200 mm / min.

[0017] Furthermore, in the above-mentioned method for preparing a high-service performance low-rare earth magnesium alloy with element segregation, the unidirectional low-temperature and low-speed thermal deformation in step (4) comprises one of unidirectional tensile deformation and unidirectional compression deformation, the unidirectional thermal deformation temperature is 200-300°C, and the strain rate is less than 1×10 -3 s -1 The deformation amount is 5%~30%, and the deformation time is more than 2 h.

[0018] Furthermore, the above-mentioned method for preparing a low-rare earth magnesium alloy with high service performance and element segregation, wherein the service performance refers to fatigue life in the range of room temperature to 200°C and creep life in the range of 200-300°C.

[0019] On the other hand, the present invention discloses a high service performance low rare earth magnesium alloy with element segregation, which is prepared by any of the methods described above.

[0020] Furthermore, the above-mentioned high service performance low rare earth magnesium alloy with element segregation has the characteristics of intracrystalline element agglomeration and grain boundary element segregation.

[0021] Furthermore, in the above-mentioned high service performance low rare earth magnesium alloy with element segregation, the A element is manganese; the B element is neodymium; preferably, the contents of the A element and the B element are both 0.5wt%.

[0022] On the other hand, the present invention discloses the application of the above-mentioned high service performance low rare earth magnesium alloy with element segregation in aerospace or rail transportation.

[0023] Compared with the prior art, the present invention has the following outstanding beneficial effects:

[0024] (1) Homogenization annealing can eliminate casting defects and improve the dynamic recrystallization degree, dynamic precipitation and element segregation of extrusion.

[0025] (2) Extrusion deformation can produce high strain rates, induce a large number of dislocations to start, and accumulate dislocations at the grain boundaries, creating channels for the diffusion of elements A and B. At low temperatures, the solid solubility of elements A and B decreases with temperature. At this time, the solid solubility is in a supersaturated state. The amount of dynamic precipitation increases during extrusion, which not only provides more dynamic recrystallization nucleation points and increases the degree of recrystallization, but also diffuses to the grain boundaries and hinders the growth of grains. The deformation temperature determines the diffusion rate of elements in magnesium alloys. If the temperature is too high, elements A and B exist in the grains as solid solutions, making it difficult to precipitate. Once precipitated, the diffusion rate is too fast, resulting in element-enriched phases at the grain boundaries, reducing impact resistance. If the temperature is too low, it is difficult to deform, and the forward migration rate is too slow, making it difficult to form element intracrystalline clusters and grain boundary segregation.

[0026] (3) Through low-temperature, low-speed unidirectional thermal deformation, more intracrystalline element clusters are introduced without damaging the element grain boundary segregation phenomenon. Intracrystalline element clusters and grain boundary element segregation promote grain boundary sliding and non-basal sliding, thereby significantly improving the service performance. A large number of experimental explorations have shown that only by controlling the process temperature can the effective segregation of elements at the grain boundary and the formation of intracrystalline clusters be achieved without producing blocky phases.

[0027] (4) The fatigue life of the magnesium alloy rod or tube treated by the present invention can be increased by more than 20 times, and the creep life can be increased by more than 2 times.

[0028] (5) The present invention does not require special equipment. It can effectively prepare ultrafine-grained magnesium alloys by improving deformation temperature and deformation degree, and greatly improve the service life of magnesium alloys. The process design is reasonable, the process is short, the operation is convenient, the cost is low, and the efficiency is high. It can prepare long and large magnesium alloys, broaden the industrial application of magnesium alloys, and make magnesium alloys have good application prospects in aerospace and rail transportation. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Diagram of element clusters inside Mg-0.5Mn-0.5Nd grains and element segregation at grain boundaries. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0031] A low rare earth magnesium alloy with high service performance contains 0.5% Mn and 0.5% Nd by mass, and the balance is Mg and unavoidable impurities.

[0032] The high service performance low rare earth magnesium alloy of this embodiment has Mn and Nd elements segregated near the grain boundaries, a large number of intracrystalline clusters in the crystals, the size of the intracrystalline element clusters is 5-15 nm, and the concentration of A and B elements at the grain boundaries is twice that in the crystals.

[0033] The preparation method of the rare earth magnesium alloy comprises the following steps: casting a magnesium alloy ingot according to the raw material Mg-0.5Mn-0.5Nd, homogenizing the magnesium alloy at 450°C for 30 hours, pressurizing the magnesium alloy at an extrusion temperature of 200°C, an extrusion ratio of 20:1, and an extrusion speed of 50 mm / min, and then performing a pressure deformation at 200°C and a strain rate of 1×10 -4 s -1 , the deformation is 5%.

[0034] The element clusters inside the grains and the element segregation at the grain boundaries of the obtained Mg-0.5Mn-0.5Nd alloy are shown in Figure 2. Figure 1 shown. Comparative Example 1

[0035] A magnesium alloy comprising, by mass percentage, 0.5% Mn, and the balance being Mg and inevitable impurities.

[0036] The only difference between the preparation method of the magnesium alloy and that of Example 1 is that the raw material composition is Mg-0.5Mn.

[0037] The obtained Mg-0.5Mn alloy only has element clusters within the grain, but no element segregation at the grain boundaries. Comparative Example 2

[0038] A magnesium alloy containing, by mass percentage, 0.5% Nd, and the balance being Mg and inevitable impurities.

[0039] The only difference between the preparation method of the magnesium alloy and that of Example 1 is that the raw material composition is Mg-0.5Nd.

[0040] The obtained Mg-0.5Nd alloy only shows element segregation at the grain boundaries, but no element clusters within the grains. Comparative Example 3

[0041] AZ31 alloy (commercially available).

[0042] Test Example 1

[0043] The above three magnesium alloys were subjected to uniaxial tension at room temperature to obtain room temperature mechanical properties; the magnesium alloys were subjected to tension-compression fatigue tests at 100°C, with the frequency of the fatigue cycle being 0.5 Hz and the ratio of the minimum stress to the maximum stress being -1, to obtain the fatigue limit; the magnesium alloys were subjected to compression creep tests at 160°C and 100 MPa to obtain the creep life, and the results are shown in Table 1.

[0044] Table 1 Magnesium alloy performance test 1

[0045]

[0046] From the data in Table 1, it can be seen that Example 1 contains 0.5% Mn and 0.5% Nd. The dislocation and thermal deformation generated by extrusion are used to eliminate organizational defects, homogenize the organization, and make the elements segregate near the grain boundaries. The elements are segregated at the grain boundaries to form a thin skin-like GP zone through low-temperature extrusion, and then the grain boundary element segregation is increased through low-temperature, low-speed unidirectional thermal deformation, and element clusters are generated inside the grains. The fatigue limit of the magnesium alloy rod or tube treated by the present invention is increased by more than 3 times, and the creep life is increased by more than 2 times. Comparative Example 1 containing only Mn and Comparative Example 2 containing only Nd cannot achieve the above performance. Compared with the commercially available AZ31 magnesium alloy, Example 1 of the present invention has obvious improvements in fatigue limit and creep life.

[0047] Test Example 2

[0048] The contents of elements A and B were adjusted and performance tests were performed. The test method was the same as that of Test Example 1. The results are shown in Table 2.

[0049] Table 2 Magnesium alloy performance test 2

[0050]

[0051] It can be seen that in the present invention, by adjusting the elements A and B between 0.2% and 1%, better fatigue limit and creep life can be obtained.

[0052] Test Example 3

[0053] The element types of A and B are adjusted and performance tests are performed. The test method is the same as that of Test Example 1. The results are shown in Table 3.

[0054] Table 3 Magnesium alloy performance test three

[0055]

[0056] It can be seen from Table 3 that in the present invention, when the A element is one of manganese and calcium; the B element is one of neodymium, cerium and yttrium, the purpose of the present invention can be achieved to obtain a low rare earth magnesium alloy with good fatigue limit and creep life.

[0057] It can be seen from the above embodiments that the present invention discloses a method for preparing a low-rare earth magnesium alloy with high service performance and element segregation, which promotes grain boundary sliding and non-basal sliding by introducing intracrystalline element agglomeration and grain boundary element segregation, effectively refines the grains, and thus significantly improves the service performance.

[0058] The above are only a few preferred embodiments of the present invention, which are described in a more specific and detailed manner, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a low rare earth magnesium alloy with high service performance and element segregation, characterized in that: The low rare earth magnesium alloy contains 0.5wt% of element A, 0.5wt% of element B, and the remainder is magnesium and other inevitable impurities; The element A is calcium; The B element is yttrium; The preparation method of the low rare earth magnesium alloy comprises the following steps: (1) Smelting magnesium ingots in the range of 650-730°C, using inert gas protection during the smelting process, raising the temperature to 750-800°C after complete melting, adding element A and element B in sequence, refining for 20-40 min under inert gas protection conditions, allowing the molten metal to stand, slag removal and cooling to 680-710°C, and casting into ingots; (2) The magnesium alloy obtained in step (1) is subjected to homogenization annealing treatment at a temperature range of 400-500°C for 30-40 h; (3) The homogenized annealed magnesium alloy obtained in step (2) is subjected to low temperature extrusion to obtain an ultrafine-grained magnesium alloy, the extrusion temperature is controlled to be 150-250°C, the extrusion ratio is 20:1-30:1, and the extrusion speed is 50-200 mm / min; (4) subjecting the ultrafine-grained magnesium alloy obtained in step (3) to unidirectional low-temperature and low-speed thermal deformation, controlling the unidirectional thermal deformation temperature to be 200-300°C and the strain rate to be less than 1×10 -3 s -1 , the deformation amount is 5%-30%, the deformation time is more than 2 h, and the high service performance low rare earth magnesium alloy with element segregation is obtained; The service performance refers to the fatigue life in the range of room temperature to 200°C and the creep life in the range of 200-300°C.

2. A high service performance low rare earth magnesium alloy with element segregation, characterized in that: Prepared by the method described in claim 1.

3. A high service performance low rare earth magnesium alloy with element segregation according to claim 2, characterized in that: The low rare earth magnesium alloy has the characteristics of intracrystalline element agglomeration and grain boundary element segregation.

4. Application of the high service performance low rare earth magnesium alloy with element segregation as claimed in claim 2 in aerospace or rail transportation.