Ferrite for high frequency wireless charging and preparation method thereof

By designing the ratio of the main components of nickel-copper-zinc ferrite and the combination of auxiliary components, and using balanced oxygen partial pressure sintering technology, the problems of power loss and temperature stability of high-frequency wireless charging materials at high frequencies are solved, and the charging efficiency and The ability to resist magnetic disturbance ensures the reliability of the material.

CN118675877BActive Publication Date: 2024-10-22TDG HLDG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411155346.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-22
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Existing wireless charging materials have high power loss at high frequencies and are unstable to temperature and magnetic disturbances, and cannot meet the efficiency and reliability requirements of high-frequency wireless charging.

Method used

Design the main component ratio of nickel-copper-zinc ferrite, and combine it with auxiliary components such as Co2O3, SiO2, Bi2O3, and MoO3 through two additions and sanding treatments, and use balanced oxygen partial pressure sintering to form a uniform grain structure to reduce magnetic permeability. rate imaginary part and improve the ability to withstand magnetic disturbances.

Benefits of technology

It improves the charging efficiency and power of high-frequency wireless charging materials, enhances temperature stability and resistance to magnetic field impact, and ensures the reliability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118675877B_ABST
    Figure CN118675877B_ABST
Patent Text Reader

Abstract

The present invention provides a ferrite for high-frequency wireless charging and a preparation method thereof, which mainly adjusts the content of each element of the main component to obtain a higher real part of the complex magnetic permeability and a lower imaginary part of the complex magnetic permeability, so as to improve the charging efficiency; wherein a small amount of iron oxide in the main component is added together with cobalt tetroxide in a doping manner, and sintered in a balanced oxygen partial pressure manner to form Co 2+ and Fe 2+ Ions can improve high-frequency large signal loss and temperature coefficient, and enhance the charging power and temperature stability of wireless charging; among them, a small amount of copper oxide in the main component is added together with the auxiliary component in the form of doping to improve the microstructure, ensure that it has a higher density and mechanical properties, reduce the material stress anisotropy, and improve its resistance to magnetic field shock and mechanical shock, thereby preparing a ferrite material for high-frequency wireless charging with excellent performance and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnetic materials, and in particular to a ferrite for high-frequency wireless charging and a preparation method thereof. Background Art

[0002] Traditional power transmission generally uses transmission media such as metal wires and cables, which will inevitably cause transmission loss, line aging, and tip discharge during power transmission. Frequent unplugging will cause physical damage to the device, and the charging cable needs to be replaced regularly. There are currently three main wireless charging standards. The first is the QI standard, which uses electromagnetic induction wireless charging, with a charging frequency of about 100-205kHz and a charging power of tens to more than one hundred watts. It is currently mainly used for wireless charging of consumer electronics such as mobile phones; the second is the A4WP standard, which uses electromagnetic resonance technology, with a charging frequency of 6.78MHz and a charging power of several thousand to more than ten kilowatts, suitable for wireless charging of new energy vehicles; the third is the new wireless charging specification WLC, which uses magnetic resonance wireless charging, with a charging frequency of 13.56MHz and a charging power of only a few watts. Due to its high frequency, it has the characteristics of being able to use smaller antennas, and is commonly used in small products such as smart watches, smart bracelets, wireless headphones, and styluses.

[0003] The soft magnetic material in the wireless charging system needs to have a high real part of magnetic permeability to effectively aggregate magnetic flux and a low imaginary part of magnetic permeability to reduce energy loss and thus improve transmission efficiency. The wireless charging system not only requires soft magnetic materials to improve transmission efficiency, but also requires hard magnetic materials for positioning. After the soft magnetic material is magnetized under the magnetic field of the hard magnetic material, its electromagnetic properties will change greatly, so the material needs to have a strong ability to resist magnetic disturbances; in addition, a low specific temperature coefficient is required to ensure that it can be used in different temperature environments; because of its high charging frequency, it can use a smaller antenna, which means that its transmission power will not be too high. Reducing its loss under high-frequency large signals will help improve its transmission power.

[0004] The patent with publication number CN108164260A discloses a nickel-zinc soft ferrite for wireless charging and its preparation method and application, which discloses a wireless charging material suitable for the QI standard (100-205kHz). The patent with publication number CN109320228A discloses a nickel-zinc ferrite material for magnetic resonance wireless charging and its preparation method, which discloses a wireless charging material suitable for the A4WP standard (6.78MHz). The patent with announcement number CN115894005B discloses a nickel-zinc ferrite material and its preparation method and application. It discloses a material suitable for new energy vehicles, wireless charging or Internet of Things technology fields under high frequency. It adopts a main formula correction process. The main formula component deviation problem caused by the existing process is manually corrected by adding appropriate amounts of Fe2O3 and Ni2O3 during doping. The power loss at high frequency at 25°C and 100°C is reduced by combining functional additives. However, it does not consider the impact of this main formula correction process (adding the main component after pre-burning) on ​​other electrical properties, nor does it consider more factors affecting high-frequency charging efficiency and charging power. Summary of the invention

[0005] The present invention provides a ferrite for high-frequency wireless charging and a preparation method thereof. The material preparation method mainly comprises the following steps:

[0006] 1) Design the molar ratio of the main components of nickel-copper-zinc ferrite: Fe2O3: 47-50mol%, ZnO: 15-26mol%, CuO: 2-6mol%, NiO: 18-36mol%. During the preparation of ferrite, the main component is divided into two parts and added twice. The main components of the first part are Fe2O3, CuO, ZnO and NiO, and the main components of the second part are Fe2O3 and CuO, and their contents are not equal to 0;

[0007] 2) Weigh the first part of the main components from the main components in step 1 and mix them by sand grinding, wherein the total molar amount of the main components in step 1 is used as the calculation basis, Fe2O3: 45.5-49.5mol%, CuO: 0.5-5.5mol%, ZnO: 15-26mol%, NiO: 18-36mol%, and the molar amounts of ZnO and NiO are the same as in step 1;

[0008] 3) drying, sieving and pre-calcining the mixed slurry in step 2;

[0009] 4) The pre-sintered powder, the second part of the main components Fe2O3 and CuO, and the auxiliary components are placed in a sand mill for secondary sand grinding. The auxiliary components include Co2O3 and SiO2, and also include one or two of Bi2O3 and MoO3. The total weight of the main components in step 1 is used as the calculation basis, Co2O3: 5000~15000ppm, SiO2: 2000~5000ppm, Bi2O3: 2000~10000ppm, MoO3: 2000~5000ppm;

[0010] 5) Granulate the powder after secondary sand grinding, sieve and press into the required green billet;

[0011] 6) Sintering the pressed green body in a balanced oxygen partial pressure manner.

[0012] Preferably, in step 1, the main component ratio is Fe2O3: 48.0~49.5mol%, ZnO: 17~23mol%, CuO: 3~5mol%, NiO: 22.5~32mol%; in step 2, based on the total molar amount of the main components in step 1, Fe2O3: 46.5~49.0mol%, CuO: 1.5~4.5mol%, ZnO: 17~23mol%, NiO: 22.5~32mol%, and the molar amount of ZnO and NiO is the same as that in step 1.

[0013] Preferably, in step 1, the main component ratio is Fe2O3: 48.5~49.0mol%, ZnO: 18~21mol%, CuO: 3.5~4.5mol%, NiO: 25.5~30mol%; in step 2, based on the total molar amount of the main components in step 1, Fe2O3: 47.0~48.0mol%, CuO: 2~3mol%, ZnO: 18~21mol%, NiO: 25.5~30mol%, and the molar amounts of ZnO and NiO are the same as in step 1.

[0014] Among them, the molar amount of Fe2O3 and CuO in the first part of the main components weighed in step 2 should be lower than the molar amount of the corresponding substances in step 1 to ensure that the main components Fe2O3 and CuO are residual, so as to ensure that the content of the second part of the main components Fe2O3 and CuO in step 4 is not equal to 0.

[0015] In step 2, the main ingredients are wet sand-milled and mixed for 10 to 30 minutes, preferably 15 minutes, 20 minutes or 25 minutes.

[0016] In step 3, the slurry mixed in step 2 is dried at 100-150°C for 12-24h, and the dried powder is passed through a 120-mesh sieve and pre-fired in an air furnace at a pre-fired temperature of 850-1000°C for 2-4h.

[0017] Preferably, in step 3, the pre-firing temperature is 880°C, 900°C, 920°C, 950°C or 980°C.

[0018] In step 4, the sand grinding time is 60 to 120 min, preferably 70 min, 80 min, 90 min, 100 min or 110 min, and the final powder particle size D50 is in the range of 1.0 to 2.0 μm.

[0019] Preferably, in step 4, based on the total weight of the main components in step 1, the following are calculated: Co2O3: 7000~13000ppm, SiO2: 2500~4500ppm, Bi2O3: 3000~8000ppm, MoO3: 3000~4000ppm.

[0020] Preferably, in step 4, based on the total weight of the main components in step 1, the following are calculated: Co2O3: 8000~12000ppm, SiO2: 3000~4000ppm, Bi2O3: 4000~7000ppm, MoO3: 3200~3800ppm.

[0021] Preferably, in step 4, based on the total weight of the main components in step 1, the following are calculated: Co2O3: 9000~11000ppm, SiO2: 3200~3800ppm, Bi2O3: 5000~6000ppm, MoO3: 3300~3500ppm.

[0022] In step 5, the powder after secondary sand grinding is mixed with 12-15wt% of PVA to form granules, and the granules after granulation are passed through 80-mesh and 240-mesh sieves and then pressed into the desired green compacts;

[0023] Preferably, in step 5, the PVA content is 13wt% or 14wt%.

[0024] In step 6, the pressed green body is sintered in a balanced atmosphere to obtain a final product, the sintering temperature is 1000-1150° C., the holding time is 2-4 hours, and the oxygen partial pressure is 4-8%.

[0025] Preferably, in step 6, the sintering temperature is 1050-1100° C., the holding time is 2.5-3 h, and the oxygen partial pressure is 5-7%.

[0026] A ferrite for high-frequency wireless charging is manufactured by adopting the above-mentioned preparation method.

[0027] The present invention is designed in the selection of the main components. By selecting an iron content slightly lower than the positive fraction and a lower zinc content, the final product is controlled to maintain a higher real part of the magnetic permeability while having a lower imaginary part of the magnetic permeability, thereby improving the charging efficiency. Improving the wireless charging power requires increasing the working magnetic flux density of the soft magnetic material, and under a large current signal, the domain wall of the soft magnetic material undergoes irreversible displacement, and the loss will increase significantly. In addition, due to the hysteresis effect, the soft magnetic ferrite in a magnetically neutral state will be magnetized by a strong magnetic field and then the magnetic field will be removed, and the magnetic flux density will remain inside it. At this time, the electrical properties of the soft magnetic ferrite will change compared to before.

[0028] The present invention designs that part of Fe2O3 and CuO in the main components are added after pre-calcination. This is because: due to the lack of Fe in the iron-poor formula system 2+ To compensate K1, the material has a larger positive temperature coefficient. Therefore, part of the Fe2O3 in the main component is added after pre-sintering, and then sintered in an oxygen atmosphere to form part of the Fe 2+ ions, through Fe 2+ and Co 2+ Compensating K1 can reduce the positive specific temperature coefficient of the material; due to the hysteresis effect, the soft ferrite in the magnetic neutral state is magnetized by a strong magnetic field and then the magnetic field is removed, and the magnetic flux density will remain inside it. At this time, the electrical properties of the soft ferrite will change compared with before. In order to reduce the impact of magnetic disturbance, the ferrite grain structure should be as uniform as possible without pores and impurities to reduce the hysteresis effect. Therefore, a part of CuO in the main component is designed to be added after pre-sintering. On the one hand, when CuO is sintered with other material components, a liquid phase can appear at a lower temperature (1026℃). On the other hand, the lattice distortion caused by the entry of Cu ions into the spinel phase will also promote sintering. With the help of fluxes with different melting points such as Bi2O3 or MoO3, a liquid phase can be formed in the multi-temperature stage of sintering, making the grain structure more perfect and improving its ability to resist magnetic disturbance. And because the pre-sintering process only forms the spinel phase initially, the Fe2O3 and CuO added after pre-sintering will still enter the main phase during the grain growth process during the final sintering, completing the initial main component design.

[0029] SiO2 can form a homogeneous glass phase with other oxides at the grain boundaries. On the one hand, the glass phase at the grain boundaries can stabilize the magnetic domain walls, improve the ability to resist thermal disturbances, and further improve the temperature stability. On the other hand, while the flux generates a liquid phase to accelerate the solid-phase reaction, the glass phase can inhibit excessive grain growth, so that samples with uniform and fine grains, obvious grain boundaries and extremely low porosity are generated at low temperatures. This can eliminate stress anisotropy, reduce coercivity, improve its ability to resist magnetic field impact, and improve the mechanical strength of the product.

[0030] The beneficial effects of the present invention are:

[0031] 1. By designing the content of the main component and coordinating the auxiliary components, a higher real part of the magnetic permeability is obtained while a lower imaginary part of the magnetic permeability is obtained, thereby improving the charging efficiency of high-frequency wireless charging materials;

[0032] 2. By designing a small amount of iron oxide in the main component to be added together with cobalt tetroxide in a doping manner and sintering it in the form of balanced oxygen partial pressure, Co 2+ and Fe 2+ Ions can reduce Rs (increase the working magnetic flux density) and specific temperature coefficient under large signals, thereby improving the charging power and temperature stability of high-frequency wireless charging materials;

[0033] 3. By designing a small amount of copper oxide in the main component to be added together with the auxiliary components in the form of doping, the microstructure is improved, ensuring that it has a higher density and mechanical properties, reducing the material stress anisotropy, improving its resistance to magnetic field shock and mechanical shock, and increasing the reliability of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Rs-B curves of the embodiments and comparative examples;

[0035] Figure 2 μ is the μ of the embodiment and the comparative example i -T curve. DETAILED DESCRIPTION

[0036] This embodiment is a preferred implementation manner of the present invention. Based on the embodiment of the present invention, all other embodiments obtained by other technicians without making any creative work belong to the protection scope of the present invention.

[0037] Example 1 is as follows:

[0038] In this embodiment, ferrite for high-frequency wireless charging is prepared according to the following method:

[0039] 1) Design the molar ratio of the main components of nickel-copper-zinc ferrite, i.e., Fe2O3: 49mol%, ZnO: 22mol%, NiO: 25mol%, CuO: 4mol%. During the preparation of ferrite, the main components are divided into two parts and added twice. The main components of the first part are Fe2O3, CuO, ZnO and NiO, and the main components of the second part are Fe2O3 and CuO.

[0040] 2) Weigh the first part of the main components and mix them by wet sand milling for 10-30 minutes. The total molar amount of the main components in step 1 is used as the calculation basis: Fe2O3: 48mol%, ZnO: 22mol%, NiO: 25mol%, CuO: 3mol%;

[0041] 3) Dry the main component slurry after mixed sand grinding in step 2 at 100-150°C for 12-24h, and pre-calculate the dried powder in an air furnace after passing through a 120-mesh sieve at a temperature of 950°C for 2h;

[0042] 4) The pre-sintered powder, the second part main components Fe2O3 and CuO, and the auxiliary components are placed in a sand mill for secondary sand grinding. The sand grinding time is 60-120 min, and the particle size D50 is controlled in the range of 1.0-2.0 μm. The total molar amount of the main components in step 1 is used as the calculation basis. The content of the main components of the second part is: Fe2O3: 1 mol%, CuO: 1 mol%, and the total weight of the main components in step 1 is used as the calculation basis. The auxiliary components are Co2O3: 8000 ppm, SiO2: 3000 ppm, and Bi2O3: 5000 ppm;

[0043] 5) The powder after secondary sand grinding is mixed with 13wt% PVA to form granules, and the granules are passed through 80 and 240 mesh sieves and pressed into the required green billets;

[0044] 6) The pressed green body is sintered in a balanced atmosphere to obtain the final product. The sintering temperature is 1050°C, the holding time is 2h, and the oxygen partial pressure is 6%.

[0045] Comparative Example 1

[0046] This comparative example prepares high-frequency wireless charging ferrite according to the following method:

[0047] 1) The molar ratio of the main components of nickel-copper-zinc ferrite is the same as that of Example 1, except that: during the preparation of the ferrite, the main component is divided into two parts and added twice, the main components of the first part are Fe2O3, CuO, ZnO and NiO, and the main component of the second part is only CuO;

[0048] 2) Weigh the first part of the main components and mix them by wet sand milling for 10-30 minutes. The total molar amount of the main components in step 1 is used as the calculation basis: Fe2O3: 49mol%, ZnO: 22mol%, NiO: 25mol%, CuO: 3mol%;

[0049] 3) Same as Example 1;

[0050] 4) The pre-sintered powder, the second main component CuO, and the auxiliary components are placed in a sand mill for secondary sand grinding. The sand grinding time is 60-120 min, and the particle size D50 is controlled in the range of 1.0-2.0 μm. The total molar amount of the main component in step 1 is used as the calculation basis. The main component content of the second part is CuO: 1 mol%, and the total weight of the main component in step 1 is used as the calculation basis. The auxiliary components are Co2O3: 8000 ppm, SiO2: 3000 ppm, and Bi2O3: 5000 ppm;

[0051] 5) Same as Example 1;

[0052] 6) Same as Example 1.

[0053] Comparative Example 2

[0054] This comparative example prepares high-frequency wireless charging ferrite according to the following method:

[0055] 1) The molar ratio of the main components of nickel-copper-zinc ferrite is the same as that of Example 1, except that: during the preparation of the ferrite, the main component is divided into two parts and added twice, the main components of the first part are Fe2O3, CuO, ZnO and NiO, and the main component of the second part is only Fe2O3;

[0056] 2) Weigh the first part of the main components and mix them evenly by wet sand grinding. The total molar amount of the main components in step 1 is used as the calculation basis: Fe2O3: 48mol%, ZnO: 22mol%, NiO: 25mol%, CuO: 4mol%;

[0057] 3) Same as Example 1;

[0058] 4) Put the pre-sintered powder, the second part main component Fe2O3, and the auxiliary components into a sand mill for secondary sand grinding. The sand grinding time is 60-120 min, and the particle size D50 is controlled in the range of 1.0-2.0 μm. The total molar amount of the main component in step 1 is used as the calculation basis. The main component content of the second part is Fe2O3: 1 mol%, and the total weight of the main component in step 1 is used as the calculation basis. The auxiliary components are Co2O3: 8000 ppm, SiO2: 3000 ppm, and Bi2O3: 5000 ppm;

[0059] 5) Same as Example 1;

[0060] 6) Same as Example 1.

[0061] Comparative Example 3

[0062] This comparative example prepares high-frequency wireless charging ferrite according to the following method:

[0063] 1) Same as Example 1;

[0064] 2) Same as Example 1;

[0065] 3) Same as Example 1;

[0066] 4) Same as Example 1;

[0067] 5) Same as Example 1;

[0068] 6) The pressed green body is sintered in an air furnace to obtain the final product. The sintering temperature is 1050°C and the holding time is 2h.

[0069] Comparative Example 4

[0070] This comparative example prepares high-frequency wireless charging ferrite according to the following method:

[0071] 1) Same as Example 1;

[0072] 2) Same as Example 1;

[0073] 3) Same as Example 1;

[0074] 4) The main process is the same as Example 1, except that the content of the auxiliary components is different. Based on the total weight of the main components in step 1, the auxiliary components are Co2O3: 2000ppm, SiO2: 1000ppm, and Bi2O3: 1500ppm;

[0075] 5) Same as Example 1;

[0076] 6) Same as Example 1.

[0077] Comparative Example 5

[0078] This comparative example prepares high-frequency wireless charging ferrite according to the following method:

[0079] 1) The molar ratio of the main components of nickel-copper-zinc ferrite is the same as that of Example 1, except that all the main components are added at one time;

[0080] 2) Weigh all the main ingredients and mix them evenly by wet sand grinding until there is no remaining main ingredient;

[0081] 3) Same as Example 1;

[0082] 4) The pre-sintered powder and auxiliary components are placed in a sand mill for secondary sand grinding. The sand grinding time is 60-120 min, and the particle size D50 is controlled in the range of 1.0-2.0 μm. The total weight of the main components in step 1 is used as the calculation basis, and the auxiliary components are Co2O3: 8000ppm, SiO2: 3000ppm, and Bi2O3: 5000ppm;

[0083] 5) Same as Example 1;

[0084] 6) The pressed green body is sintered in an air furnace to obtain the final product. The sintering temperature is 1050°C and the holding time is 2h.

[0085] Table 1 shows the differences in experimental conditions between the embodiment and the comparative example. The test frequency of μ' and μ" data is 13.56 MHz, and the complex permeability test equipment is an impedance analyzer. The data in Table 2 are all test results at room temperature, wherein μ'1 and μ''1 are the real and imaginary test data of the complex permeability of the sample in the magnetic neutralization state, μ'2 and μ''2 are the real and imaginary test data of the complex permeability after the sample is magnetized by a strong magnetic field, and Δμ' and Δμ" are the change rates of the real and imaginary parts of the complex permeability before and after magnetization, respectively; Figure 1 Rs-B curve data, the test frequency is 5MHz.

[0086] Table 1 Differences in experimental conditions between the examples and the comparative examples

[0087]

[0088] Table 2 Performance data of examples and comparative examples

[0089]

[0090] The μ', μ" and Q value data examples and the comparative examples in Table 2 show that the technology of the present invention can effectively increase the real part of the complex magnetic permeability, reduce the imaginary part of the complex magnetic permeability, improve the quality factor, and improve the charging efficiency of wireless charging; Figure 1 The Rs-B curve in the figure shows that the technology of the present invention can effectively reduce the loss under large signal; improve the working magnetic flux density of the material and improve the charging power of wireless charging; the Δμ' and Δμ" data examples and comparative examples in Table 2 show that the technology of the present invention can effectively improve the ability to resist magnetic disturbance; Figure 2 Medium i The -T curve indicates that the technology of the present invention can effectively improve the temperature stability.

[0091] The above content is a further explanation of the present invention in combination with specific or preferred implementation methods. It cannot be considered that the implementation of the present invention is limited to the above embodiments. For ordinary practitioners in the field of the present invention, simple modifications or changes made within the conceptual framework of this invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing ferrite for high-frequency wireless charging, characterized in that: The following steps are involved: 1) Design the molar ratio of the main components of nickel-copper-zinc ferrite: Fe2O3: 47-50mol%, ZnO: 15-26mol%, CuO: 2-6mol%, NiO: 18-36mol%. During the preparation of ferrite, the main component is divided into two parts and added twice. The main components of the first part are Fe2O3, CuO, ZnO and NiO, and the main components of the second part are Fe2O3 and CuO, and their contents are not equal to 0; 2) Weigh the first part of the main components from the main components in step 1 and mix them by sand grinding, wherein the total molar amount of the main components in step 1 is used as the calculation basis, Fe2O3: 45.5-49.5mol%, CuO: 0.5-5.5mol%, ZnO: 15-26mol%, NiO: 18-36mol%, and the molar amounts of ZnO and NiO are the same as in step 1; 3) drying, sieving and pre-calcining the mixed slurry in step 2; 4) The pre-sintered powder, the second part of the main components Fe2O3 and CuO, and the auxiliary components are subjected to secondary sand grinding. The auxiliary components include Co2O3 and SiO2, and also include one or two of Bi2O3 and MoO3. The total weight of the main components in step 1 is used as the calculation basis, Co2O3: 5000~15000ppm, SiO2: 2000~5000ppm, Bi2O3: 2000~10000ppm, MoO3: 2000~5000ppm; 5) The powder after secondary sand grinding is granulated, sieved, and pressed into the required green body; 6) Sintering the pressed green body in a balanced oxygen partial pressure manner.

2. The preparation method according to claim 1, characterized in that: In the step 1, the main component ratio is Fe2O3: 48.0~49.5mol%, ZnO: 17~23mol%, CuO: 3~5mol%, NiO: 22.5~32mol%; in the step 2, based on the total molar amount of the main components in step 1, Fe2O3: 46.5~49.0mol%, CuO: 1.5~4.5mol%, ZnO: 17~23mol%, NiO: 22.5~32mol%, and the molar amounts of ZnO and NiO are the same as those in step 1.

3. The preparation method according to claim 1, characterized in that: In the step 1, the main component ratio is Fe2O3: 48.5~49.0mol%, ZnO: 18~21mol%, CuO: 3.5~4.5mol%, NiO: 25.5~30mol%; in the step 2, based on the total molar amount of the main components in step 1, Fe2O3: 47.0~48.0mol%, CuO: 2~3mol%, ZnO: 18~21mol%, NiO: 25.5~30mol%, and the molar amounts of ZnO and NiO are the same as those in step 1.

4. The preparation method according to claim 1, characterized in that: In the step 2, the main components are wet-grinded and mixed for 10 to 30 minutes; in the step 3, the slurry mixed in the step 2 is dried at 100 to 150° C. for 12 to 24 hours, and the dried powder is passed through a 120-mesh sieve and pre-fired in an air furnace at a pre-fired temperature of 850 to 1000° C. for a heat preservation time of 2 to 4 hours.

5. The preparation method according to claim 1, characterized in that: In step 4, the total weight of the main components in step 1 is used as the calculation basis, Co2O3: 7000~13000ppm, SiO2: 2500~4500ppm, Bi2O3: 3000~8000ppm, MoO3: 3000~4000ppm.

6. The preparation method according to claim 5, characterized in that: Based on the total weight of the main components in step 1, the calculation is as follows: Co2O3: 8000~12000ppm, SiO2: 3000~4000ppm, Bi2O3: 4000~7000ppm, MoO3: 3200~3800ppm.

7. The preparation method according to claim 1, characterized in that: In the step 4, the sand grinding time is 60-120 min, and the final powder particle size D50 is in the range of 1.0-2.0 μm; in the step 5, the powder after the secondary sand grinding is mixed with 12-15 wt% of PVA for granulation, and the granulated granules are passed through 80 mesh and 240 mesh sieves and then pressed into the required green body.

8. The preparation method according to claim 1, characterized in that: In the step 6, the pressed green body is sintered in a balanced oxygen partial pressure manner, the sintering temperature is 1000-1150° C., the holding time is 2-4 hours, and the oxygen partial pressure is 4-8%.

9. A ferrite for high-frequency wireless charging, characterized in that: The invention is manufactured by the preparation method described in any one of claims 1 to 8.