Baking method for batteries without electrolyte injection

Through gradient heating and circulating vacuum/gas operation baking methods, the problem of excessive drying time of lithium-ion batteries is solved, rapid drying is achieved, and production efficiency is improved.

CN118687345BActive Publication Date: 2024-11-01JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162423.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The drying time of lithium-ion batteries is long, which affects the production cycle and supply speed, and it is difficult for the existing technology to effectively shorten.

Method used

The baking method of gradient heating is adopted. By heating multiple adjacent time periods in the oven, combined with vacuum and inert gas circulation, the internal temperature of the battery can be quickly reached to the set temperature and shortened the drying time.

Benefits of technology

On the basis of ensuring the integrity of the internal structure of the battery, the total drying time of lithium-ion batteries is significantly shortened, production efficiency is improved, and manufacturing cycle is shortened.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118687345B_ABST
    Figure CN118687345B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery manufacturing technology, and specifically provides a method for baking a battery without electrolyte injection, aiming to solve the problem of how to shorten the drying time of lithium-ion batteries. To this end, the method for baking a battery without electrolyte injection of the present invention comprises: step S1, placing the battery in an oven; step S2, vacuuming the oven and filling it with inert gas; step S3, heating the oven in sequence in multiple adjacent time periods to preheat the battery, wherein the heating temperature of the oven in the latter time period is lower than the heating temperature in the previous time period; step S4, vacuuming the oven; step S5, heating the oven for a first preset time; step S6, filling the oven with inert gas and stabilizing the pressure to a preset pressure for a second preset time; step S7, cyclically performing steps S4 to S6 until the water content of the battery's pole piece and / or diaphragm is reduced to below the target content; step S8, leaving the battery still in an inert gas atmosphere to cool the battery. This shortens the total drying time of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery manufacturing, and in particular provides a method for baking a battery without electrolyte injection. Background Art

[0002] In recent years, the demand for lithium-ion batteries in electric vehicles, energy storage, 3C and other fields has increased year by year, and the demand for lithium-ion batteries has entered a stage of rapid growth.

[0003] In the production process of lithium-ion batteries, there are strict requirements for moisture control. Abnormal moisture content will lead to increased internal resistance, reduced capacity, and poor cycle performance of lithium-ion batteries, which will directly affect the performance of lithium-ion batteries. After the assembly of large-capacity metal-shell lithium-ion batteries is completed and before the liquid is injected, the lithium-ion batteries need to be baked to remove the moisture contained in the pole pieces and diaphragms in the lithium-ion batteries.

[0004] Generally, the method for baking a lithium-ion battery includes: step 1, placing the battery without electrolyte injection into an oven; step 2, introducing nitrogen after vacuuming; step 3, heating the oven to preheat the battery; step 4, vacuuming; step 5, heating; step 6, filling with nitrogen; step 7, repeating steps 4 to 6 for a certain number of times (such as 8 times); step 8, cooling. Since the drying time of lithium-ion batteries accounts for a large proportion of the entire manufacturing cycle of lithium-ion batteries, it has a great impact on the production cycle of lithium-ion batteries. At present, the market has put forward higher requirements for the delivery speed of lithium-ion batteries. It has become a general consensus in the industry to significantly shorten the manufacturing cycle of lithium-ion batteries. Shortening the drying time of lithium-ion batteries is the main means to shorten the manufacturing cycle of lithium-ion batteries. How to shorten the drying time of lithium-ion batteries has become the focus of research in the industry.

[0005] Therefore, this field needs a new technical solution to solve the above problems. Summary of the invention

[0006] The present invention aims to solve the above technical problem, that is, to solve the problem of how to shorten the drying time of lithium-ion batteries.

[0007] The present invention provides a method for baking a battery without electrolyte injection, and the baking method comprises the following steps: step S1, placing the battery in an oven; step S2, evacuating the oven and filling it with an inert gas; step S3, heating the oven in sequence in multiple adjacent time periods to preheat the battery, wherein the heating temperature of the oven in a later time period is lower than the heating temperature in a previous time period; step S4, evacuating the oven; step S5, heating the oven for a first preset time period; step S6, filling the oven with an inert gas and stabilizing the pressure to a preset pressure for a second preset time period; step S7, looping steps S4 to S6 until the water content of the electrode and / or diaphragm of the battery is reduced to below a target content; step S8, leaving the battery still in an inert gas atmosphere to cool the battery.

[0008] In a preferred technical solution of the above baking method, heating elements are arranged on six sides of the oven. In the baking method, the heating operation of the oven is achieved by generating heat by the heating elements on the six sides of the oven.

[0009] In the preferred technical solution of the above baking method, the step of "evacuating the oven" specifically includes: evacuating the oven to an absolute pressure below 10 Pa; step S6 specifically includes: filling the oven with inert gas to a positive pressure and stabilizing the pressure for a second preset time.

[0010] In the preferred technical solution of the above baking method, step S6 specifically includes: filling the oven with inert gas to 170 kPa-180 kPa and stabilizing the pressure for a second preset time.

[0011] In the preferred technical solution of the above baking method, the second preset time length is 20s to 80s.

[0012] In the preferred technical solution of the above baking method, step S8 specifically includes: leaving the battery at rest in an inert gas atmosphere at normal temperature or below normal pressure to cool the battery.

[0013] In the preferred technical solution of the above baking method, the temperature of the inert gas filled into the oven in step S2 and step S6 is 90°C to 110°C.

[0014] In a preferred technical solution of the above baking method, in step S2 and / or step S6, while the oven is heated, the inert gas in the oven is caused to flow.

[0015] In the preferred technical scheme of the above baking method, the heating temperature of the oven in the first time period in step S3 is 110°C to 120°C, and the heating temperature of the oven in the last time period is 95°C to 105°C; and / or the heating temperature of the oven in step S5 is 95°C to 105°C.

[0016] In a preferred technical solution of the above baking method, the inert gas is nitrogen.

[0017] In the case of adopting the above technical solution, the baking method of the battery without electrolyte injection includes the following steps: step S1, placing the battery in an oven; step S2, vacuuming the oven and filling it with inert gas; step S3, heating the oven in a plurality of adjacent time periods in sequence to preheat the battery, wherein the heating temperature of the oven in the latter time period is lower than the heating temperature in the previous time period; step S4, vacuuming the oven; step S5, heating the oven for a first preset time; step S6, filling the oven with inert gas and stabilizing the pressure to a preset pressure for a second preset time; step S7, looping steps S4 to S6 until the water content of the battery's pole piece and diaphragm is reduced to below the target content; step S8, leaving the battery still in an inert gas atmosphere to cool the battery. It should be noted that "vacuuming" in this application refers to evacuating the oven so that the oven reaches a negative pressure state or even an absolute vacuum state.

[0018] Compared with the existing battery baking method, the battery baking method of the present invention adopts a gradient heating method in the preheating stage, which can ensure that the temperature inside the battery quickly reaches the set temperature without damaging the internal structure of the battery, thereby shortening the total drying time of the battery, which is beneficial to shortening the battery production cycle and improving the battery production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The preferred embodiments of the present invention are described below with reference to the accompanying drawings, in which:

[0020] Figure 1 It is a schematic diagram of the main steps of the baking method of the battery without electrolyte injection of the present invention. DETAILED DESCRIPTION

[0021] First, it should be understood by those skilled in the art that the embodiments described below are only used to explain the technical principles of the present invention and are not intended to limit the scope of protection of the present invention. It should be noted that in the description of the invention, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0022] Based on the problem of how to shorten the drying time of lithium-ion batteries mentioned in the background art, the present invention provides a method for baking batteries without electrolyte injection. Figure 1As shown, the baking method of the battery without electrolyte injection of the present invention comprises the following steps:

[0023] Step S1, placing the battery in an oven;

[0024] Step S2, evacuating the oven and filling it with inert gas;

[0025] Step S3, heating the oven in sequence in a plurality of adjacent time periods to preheat the battery; wherein the heating temperature of the oven in a later time period is lower than the heating temperature in a previous time period;

[0026] Step S4, evacuating the oven;

[0027] Step S5, heating the oven for a first preset time;

[0028] Step S6, filling the oven with inert gas and stabilizing the pressure to a preset pressure for a second preset time;

[0029] Step S7, looping steps S4 to S6 until the water content of the battery electrode and / or separator drops below the target content;

[0030] Step S8: leaving the battery to stand in an inert gas atmosphere to cool the battery.

[0031] Compared with the existing battery baking method, the battery baking method of the present invention adopts a gradient heating method in the preheating stage, which can ensure that the temperature inside the battery quickly reaches the set temperature without damaging the internal structure of the battery, thereby shortening the total drying time of the battery, which is beneficial to shortening the battery production cycle and improving the battery production efficiency.

[0032] Preferably, heating elements are arranged on the six sides of the oven. In the baking method, the heating operation of the oven is realized by generating heat by the heating elements on the six sides of the oven. With such an arrangement, the temperature of the battery in the oven can reach the required preheating and baking temperature more quickly, and the total drying time of the battery can be shortened.

[0033] Preferably, the step of "evacuating the oven" specifically includes: evacuating the oven to an absolute pressure below 10 Pa; step S6 specifically includes: filling the oven with an inert gas to a positive pressure and stabilizing the pressure for a second preset time.

[0034] Preferably, step S6 specifically includes: filling the oven with inert gas to a pressure of 170 kPa to 180 kPa and stabilizing the pressure for a second preset time.

[0035] Preferably, the second preset time length is 20s~80s.

[0036] Preferably, step S8 specifically includes: placing the battery in an inert gas atmosphere at normal temperature or below normal pressure to cool the battery. This arrangement can speed up the cooling of the battery, shorten the cooling time of the battery, and thus shorten the total drying time of the battery.

[0037] Preferably, the temperature of the inert gas filled into the oven in step S2 and step S6 is 90° C. to 110° C. With such a setting, the preheating time of the oven for the battery can be shortened, and the situation that the temperature of the battery after vacuum baking is greatly reduced after the inert gas is filled, which is not conducive to the precipitation of moisture on the battery pole piece and diaphragm, is avoided, the precipitation speed of moisture on the battery pole piece and diaphragm is increased, and the total drying time of the battery is further shortened.

[0038] Preferably, while the oven is heated in step S3 and / or step S6, the inert gas in the oven is made to flow. With such an arrangement, the flowing inert gas can achieve faster and more uniform heat transfer between the heating element of the oven and the battery, shortening the heating time of the battery, thereby further shortening the total drying time of the battery.

[0039] The following takes a 314Ah lithium-ion battery as an example, and describes the baking method and effect of the battery without electrolyte injection of the present invention in combination with the following embodiments and comparative examples.

[0040] Comparative Example

[0041] The method for baking a battery without electrolyte injection comprises the following steps:

[0042] Step S1, placing the battery in an oven with heated bottom surface;

[0043] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0044] Step S3, preheating the oven at 105°C until the battery pole piece and diaphragm reach 100°C;

[0045] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is between 50 Pa and 100 Pa;

[0046] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0047] Step S6, filling with nitrogen at room temperature to normal pressure and stabilizing the pressure for 20 seconds;

[0048] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0049] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0050] It should be noted that the bottom-heated oven refers to an oven with a heating element only on the bottom, and the heating element may be a heating rod, a heating wire or a heating plate.

[0051] Example 1

[0052] The method for baking a battery without electrolyte injection comprises the following steps:

[0053] Step S1, placing the battery in an oven with heated bottom surface;

[0054] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0055] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0056] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is between 50 Pa and 100 Pa;

[0057] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0058] Step S6, filling with nitrogen at room temperature to normal pressure and stabilizing the pressure for 20 seconds;

[0059] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0060] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0061] Example 2

[0062] The method for baking a battery without electrolyte injection comprises the following steps:

[0063] Step S1, placing the battery in a six-sided heated oven;

[0064] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0065] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0066] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is between 50 Pa and 100 Pa;

[0067] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0068] Step S6, filling with nitrogen at room temperature to normal pressure and stabilizing the pressure for 20 seconds;

[0069] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0070] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0071] It should be noted that the six-sided heating oven refers to an oven with heating elements arranged on all six sides.

[0072] Example 3

[0073] The method for baking a battery without electrolyte injection comprises the following steps:

[0074] Step S1, placing the battery in an oven with heated bottom surface;

[0075] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0076] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0077] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0078] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0079] Step S6, filling with nitrogen at room temperature to make the absolute pressure in the oven reach 120000Pa and stabilizing the pressure for 20s;

[0080] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0081] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0082] Example 4

[0083] The method for baking a battery without electrolyte injection comprises the following steps:

[0084] Step S1, placing the battery in an oven with heated bottom surface;

[0085] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0086] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0087] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0088] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0089] Step S6, filling with nitrogen at room temperature to make the absolute pressure in the oven reach 170000Pa and stabilizing the pressure for 20s;

[0090] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0091] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0092] Example 5

[0093] The method for baking a battery without electrolyte injection comprises the following steps:

[0094] Step S1, placing the battery in an oven with heated bottom surface;

[0095] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0096] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0097] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0098] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0099] Step S6, filling with nitrogen at room temperature to make the absolute pressure in the oven reach 180000Pa and stabilizing the pressure for 20s;

[0100] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0101] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0102] Example 6

[0103] The method for baking a battery without electrolyte injection comprises the following steps:

[0104] Step S1, placing the battery in an oven with heated bottom surface;

[0105] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0106] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0107] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0108] Step S5, the heating temperature of the oven is 105°C, and the heating time is 550s;

[0109] Step S6, filling with nitrogen at room temperature to make the absolute pressure in the oven reach 190000Pa and stabilizing the pressure for 20s;

[0110] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0111] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0112] Example 7

[0113] The method for baking a battery without electrolyte injection comprises the following steps:

[0114] Step S1, placing the battery in an oven with heated bottom surface;

[0115] Step S2, evacuating the oven and then filling it with hot nitrogen to make the oven reach normal pressure;

[0116] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0117] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0118] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0119] Step S6, filling with hot nitrogen to normal pressure and maintaining the pressure for 20 seconds;

[0120] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0121] Step S8, leaving the battery at rest in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature;

[0122] The temperature of the hot nitrogen is 90°C.

[0123] Example 8

[0124] The method for baking a battery without electrolyte injection comprises the following steps:

[0125] Step S1, placing the battery in a six-sided heated oven;

[0126] Step S2, evacuating the oven and then filling it with hot nitrogen to make the oven reach normal pressure;

[0127] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0128] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0129] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0130] Step S6, filling with hot nitrogen to normal pressure and maintaining the pressure for 20 seconds;

[0131] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0132] Step S8, leaving the battery at rest in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature;

[0133] The temperature of the hot nitrogen is 100°C.

[0134] Example 9

[0135] The method for baking a battery without electrolyte injection comprises the following steps:

[0136] Step S1, placing the battery in an oven with heated bottom surface;

[0137] Step S2, evacuating the oven and then filling it with hot nitrogen to make the oven reach normal pressure;

[0138] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0139] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0140] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0141] Step S6, filling hot nitrogen to make the absolute pressure in the oven reach 120000 Pa and stabilizing the pressure for 20 seconds;

[0142] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0143] Step S8, leaving the battery at rest in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature;

[0144] The temperature of the hot nitrogen is 90°C.

[0145] Example 10

[0146] The method for baking a battery without electrolyte injection comprises the following steps:

[0147] Step S1, placing the battery in an oven with heated bottom surface;

[0148] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0149] Step S3, heating to 115° C. within 0 min-30 min, heating to 108° C. within 30 min-60 min, heating to 100° C. within 60 min-90 min, and flowing nitrogen during the heating process;

[0150] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0151] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0152] Step S6, filling with nitrogen at room temperature to normal pressure and stabilizing the pressure for 20 seconds;

[0153] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0154] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0155] It should be noted that a fan may be provided in the oven, and the rotation of the fan allows the nitrogen to flow in the oven. An inlet and an outlet may also be provided on the oven, and the inlet and the outlet are respectively connected to a circulating fan through pipes, so that the nitrogen can continuously flow into and out of the oven through the circulating fan.

[0156] Embodiment 11

[0157] The method for baking a battery without electrolyte injection comprises the following steps:

[0158] Step S1, placing the battery in an oven with heated bottom surface;

[0159] Step S2, evacuating the oven and then filling it with nitrogen at room temperature to make the oven reach normal pressure;

[0160] Step S3, heating to 115°C within 0min-30min, heating to 108°C within 30min-60min, and heating to 100°C within 60min-90min;

[0161] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0162] Step S5, the heating temperature of the oven is 105°C, and the heating time is 60 minutes;

[0163] Step S6, filling with nitrogen at room temperature to normal pressure and stabilizing the pressure for 20 seconds, and allowing the nitrogen to flow during the pressure stabilization process;

[0164] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0165] Step S8, leaving the battery to stand in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature.

[0166] Example 12

[0167] The method for baking a battery without electrolyte injection comprises the following steps:

[0168] Step S1, placing the battery in a six-sided heated oven;

[0169] Step S2, evacuating the oven and then filling it with hot nitrogen to make the oven reach normal pressure;

[0170] Step S3, heating to 115° C. within 0 min-30 min, heating to 108° C. within 30 min-60 min, heating to 100° C. within 60 min-90 min, and flowing nitrogen during the heating process;

[0171] Step S4, evacuate the oven to a vacuum level so that the absolute pressure inside the oven is 10 Pa;

[0172] Step S5, the heating temperature of the oven is 105°C, and the heating time is 550s;

[0173] Step S6, filling with hot nitrogen to normal pressure and stabilizing the pressure for 20 seconds, and allowing the nitrogen to flow during the stabilization process;

[0174] Step S7, looping steps S4 to S6 until the water content of the battery electrode and the separator is reduced to below the target content;

[0175] Step S8, leaving the battery at rest in a nitrogen atmosphere at room temperature and pressure to cool the battery to room temperature;

[0176] The temperature of the hot nitrogen is 100°C.

[0177] The 314Ah lithium-ion battery was baked according to the baking method of the above comparative example and embodiment. Three groups of experiments were conducted on the comparative example and each embodiment, and the experimental results were obtained as shown in the following table:

[0178]

[0179] By comparing the experimental results of Example 1 with the experimental results of the comparative example, it can be seen that the battery baking method of the present invention adopts a gradient heating method in the preheating stage. On the basis of ensuring that the internal structure of the battery is not damaged, the temperature inside the battery quickly reaches the set temperature, which greatly shortens the total drying time of the battery. Compared with the existing baking method, the total drying time of Example 1 which adopts the gradient heating method in the preheating stage is shortened by about 17%.

[0180] By comparing the experimental results of Example 2 with the experimental results of Example 1, it can be seen that when a six-sided heated oven is used for heating in the baking method of the present invention, the total drying time is greatly shortened. Compared with Example 1, the total drying time of Example 2 using a six-sided heated oven for heating is shortened by approximately 76%.

[0181] By comparing the experimental results of Examples 3, 4, 5, and 6 with the experimental results of Example 1 and comparing the experimental results of Example 9 with the experimental results of Example 7, it can be seen that during the breathing cycle operation of "vacuuming-heating-filling with nitrogen" after preheating, vacuuming to an absolute pressure of 10Pa and filling with nitrogen to a positive pressure state (that is, the absolute pressure is greater than atmospheric pressure) is beneficial to the precipitation of moisture on the battery's pole pieces and diaphragms, and to a certain extent shortens the total drying time of the battery. Compared with Example 1, the total drying time is shortened by approximately 8% to 19%, respectively, and the greater the absolute pressure when filling with nitrogen to a positive pressure state, the greater the degree of shortening of the total drying time.

[0182] By comparing the experimental results of Example 7 with the experimental results of Example 1, comparing the experimental results of Example 8 with the experimental results of Example 2, and comparing the experimental results of Example 9 with the experimental results of Example 3, it can be seen that in the baking method of the present invention, the introduction of hot nitrogen during preheating and heating can shorten the total drying time to a certain extent, and the total drying time is shortened by about 12% to 24%, and as the temperature of the hot nitrogen increases, the greater the degree of shortening of the total drying time.

[0183] By comparing the experimental results of Example 10 with the experimental results of Example 1, it can be seen that in the baking method of the present invention, nitrogen is allowed to flow during the preheating stage, and the total drying time is shortened to a certain extent. Compared with Example 1, the total drying time is shortened by about 7% to 14%.

[0184] By comparing the experimental results of Example 11 with the experimental results of Example 1, it can be seen that in the baking method of the present invention, nitrogen is allowed to flow during the stage of nitrogen pressure stabilization after heating, and the total drying time is shortened to a certain extent. Compared with Example 1, the total drying time is shortened by about 10% to 14%.

[0185] By comparing the experimental results of Example 12 with those of Example 8, it can be seen that in the baking method of the present invention, during the breathing cycle operation of "vacuuming-heating-filling with nitrogen" after preheating, vacuuming to an absolute pressure of 10Pa, filling with nitrogen to a positive pressure state (i.e., the absolute pressure is greater than the atmospheric pressure), and nitrogen is allowed to flow during the preheating stage and the stage of filling with nitrogen for stabilizing the pressure after heating, which can greatly shorten the total drying time. Compared with Example 8, the total drying time of Example 12 is shortened by approximately 28% to 38%. Compared with the comparative example, the total drying time of Example 12 is shortened by approximately 89%.

[0186] By comparing the above experimental results, it can be known that the baking method of the present application can effectively shorten the total drying time of the battery.

[0187] It should be noted that in the above-mentioned embodiments 1 to 12, in step S3, the oven is heated sequentially in three adjacent time periods to preheat the battery. This is only a specific setting method, which can be adjusted in actual applications. For example, in step S3, the oven can be heated sequentially in two adjacent time periods to heat the battery, can be heated sequentially in four adjacent time periods to heat the battery, and can also be heated sequentially in more adjacent time periods to heat the battery, as long as the heating temperature of the oven in the latter time period is lower than the heating temperature in the previous time period. Preferably, the heating temperature of the oven in the first time period is 110°C to 120°C, and the heating temperature of the oven in the last time period is 95°C to 105°C. In addition, the heating temperature of the oven in step S5 is 105°C, which is also a specific setting method, which can be adjusted in actual applications, such as the heating temperature of the oven in step S5 is 95°C, 97°C, 100°C, 103°C, etc. In addition, in step S5, the oven is heated for 60 min or 550 s, which is also a specific setting mode, and it can be adjusted in practical applications, such as heating the oven for 50 min, 40 min, 25 min, 500 s, 530 s, 560 s, 600 s, etc. in step S5. In step S4, the oven is evacuated to an absolute pressure below 10 Pa, and nitrogen is filled to 170 kPa~180 kPa in step S6. In step S5, the oven heating time is preferably 500 s to 600 s, so as to ensure that the electrode and the diaphragm have a higher average water separation rate in this process, avoid the heating time being too long to reduce the average water separation rate, and thus shorten the total drying time.

[0188] It should also be noted that the voltage is stabilized for 20 seconds in step S6, which is also a more preferred setting mode, and it can be adjusted in actual applications, such as stabilizing the voltage for 30 seconds, 35 seconds, 40 seconds, 52 seconds, 60 seconds, 73 seconds, 80 seconds, etc. in step S6. In addition, the nitrogen in the above embodiments can be replaced by helium, neon, argon or other feasible inert gases. In addition, according to actual needs, the step S7 in the above embodiments "until the water content of the battery pole piece and the diaphragm is reduced to below the target content" can be set to "until the water content of the battery pole piece is reduced to below the target content" or "until the water content of the battery diaphragm is reduced to below the target content".

[0189] Based on any one of the above embodiments 1 to 12, preferably, step S8 is to place the battery at rest in a low-temperature nitrogen atmosphere at normal pressure to cool the battery to normal temperature. For example, place the battery at rest in a nitrogen atmosphere at normal pressure of -2°C to 10°C to cool the battery to normal temperature. By such a setting, the total drying time can be further shortened.

[0190] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A method for baking a battery without electrolyte injection, characterized in that: The baking method comprises the following steps: Step S1, placing the battery in an oven; Step S2, evacuating the oven and then filling it with an inert gas; Step S3, heating the oven in sequence in a plurality of adjacent time periods to preheat the battery, wherein the heating temperature of the oven in a later time period is lower than the heating temperature in a previous time period; Step S4, evacuating the oven; Step S5, heating the oven for a first preset time; Step S6, filling the oven with inert gas and stabilizing the pressure to a preset pressure for a second preset time; Step S7, looping steps S4 to S6 until the water content of the electrode sheet and / or the separator of the battery drops below the target content; Step S8: leaving the battery to stand in an inert gas atmosphere to cool the battery.

2. The baking method according to claim 1, characterized in that: The oven is provided with heating elements on six sides. In the baking method, the heating operation of the oven is achieved by generating heat from the heating elements on the six sides of the oven.

3. The baking method according to claim 1, characterized in that: The step of "evacuating the oven" specifically includes: evacuating the oven to an absolute pressure of less than 10Pa; Step S6 specifically includes: filling the oven with inert gas to a positive pressure and stabilizing the pressure for a second preset time.

4. The baking method according to claim 3, characterized in that: Step S6 specifically includes: The oven is filled with inert gas to a pressure of 170 kPa to 180 kPa and the pressure is stabilized for a second preset time.

5. The baking method according to claim 4, characterized in that: The second preset time length is 20s~80s.

6. The baking method according to claim 1, characterized in that: Step S8 specifically includes: The battery is left to stand in an inert gas atmosphere at normal temperature or lower than normal temperature and normal pressure to cool the battery.

7. The baking method according to any one of claims 1 to 6, characterized in that The temperature of the inert gas filled into the oven in step S2 and step S6 is 90°C to 110°C.

8. The baking method according to any one of claims 1 to 6, characterized in that: In step S3 and / or step S6, while the oven is heated, an inert gas in the oven is caused to flow.

9. The baking method according to any one of claims 1 to 6, characterized in that: In step S3, the heating temperature of the oven in the first time period is 110° C. to 120° C., and the heating temperature of the oven in the last time period is 95° C. to 105° C.; and / or The heating temperature of the oven in step S5 is 95°C to 105°C.