Method for repairing and regenerating graphite in waste lithium ion battery
Through a process that combines ultrasonic hot water immersion and high-temperature and high-pressure hydrothermal reaction, combined with ball milling, airflow classification and cyclone separation, the efficiency and cost problems of graphite recycling from waste lithium-ion batteries are solved, and efficient, low-cost graphite repair and regeneration is achieved.
Patent Information
- Application Number
- CN202410723139.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-05
AI Technical Summary
It is difficult to effectively recycle and repair graphite materials in used lithium-ion batteries with existing technology, leading to resource waste and environmental pollution. Moreover, traditional methods consume high energy, are low in efficiency, and have high costs.
A process combining ultrasonic hot water immersion and high-temperature and high-pressure hydrothermal reaction is used to remove the copper foil and binder from the graphite, and then the purity and performance of the graphite are improved through steps such as ball milling, airflow classification and cyclone separation.
It achieves efficient recovery and repair of graphite, with a copper recovery rate of more than 95%, reducing energy consumption and processing time, improving the purity and application performance of graphite, and reducing costs.
Smart Images

Figure CN118723989A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of waste lithium battery recycling, and in particular to a method for repairing and regenerating graphite in waste lithium ion batteries. Background Art
[0002] As the electric vehicle market continues to expand, the application of lithium batteries is becoming more and more widespread. Lithium-ion batteries (LIBs) have gradually become the main power source for electric vehicles (EVs) and hybrid electric vehicles (HEVs) due to their obvious advantages such as high energy, high power density, small memory effect and slow self-discharge. However, with the extensive use of lithium batteries, a large number of waste batteries have also been generated, including a large amount of graphite negative electrode materials. Graphite has the advantages of high crystallinity and high conductivity, a low potential platform close to the potential of lithium metal, high lithium insertion capacity, good layered structure and abundant reserves, making it one of the most widely used negative electrode materials in the lithium-ion battery market. Therefore, the recycling of graphite negative electrode of lithium-ion batteries is particularly important.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The objects of the present invention include, for example, providing a method for repairing and regenerating graphite in waste lithium-ion batteries and a method for recycling waste lithium-ion batteries, which can stably ensure the product quality of the recycled graphite, and the present invention is simple and efficient, has low energy consumption, and short processing time, thereby achieving a dual improvement in production capacity and efficiency.
[0005] The embodiments of the present invention can be implemented as follows:
[0006] In a first aspect, the present invention provides a method for repairing and regenerating graphite in waste lithium-ion batteries, comprising:
[0007] The graphite negative electrode sheet is soaked in ultrasonic hot water to separate the graphite slurry and the copper foil;
[0008] The graphite slurry and the oxidant are subjected to a high temperature and high pressure hydrothermal reaction, and the reaction liquid is subjected to solid-liquid separation and water washing;
[0009] Drying and sintering the washed solid graphite to obtain pyrolytic graphite;
[0010] ball milling the pyrolytic graphite to separate graphite and a binder to obtain graphite powder;
[0011] The graphite powder is subjected to airflow classification and cyclone separation to remove amorphous carbon, and coarse graphite powder is collected as a finished graphite product.
[0012] In an optional embodiment, in the step of ultrasonic hot water soaking and separation, the soaking temperature is 70°C to 90°C, the soaking time is 30-60 minutes, and the ultrasonic power is 1000w to 1500w.
[0013] In an optional embodiment, the ultrasonic hot water soaking and separation step is performed in a recovery device, the recovery device includes a rotating cylinder, a circulating water tank and an ultrasonic generator, the side wall of the rotating cylinder is provided with a mesh and a spiral guide plate, the top of the rotating cylinder is provided with a spray pipe, the spray pipe is connected to the circulating water tank through a circulating pump, a heater is provided in the circulating water tank, the circulating water tank is provided below the rotating cylinder, the lower part of the rotating cylinder extends below the liquid level of the circulating water tank, and the ultrasonic generator is provided at the outer bottom of the circulating water tank;
[0014] Preferably, the feed inlet of the rotary cylinder is provided with a feed guide plate, and the discharge outlet is provided with a discharge guide plate;
[0015] Preferably, the graphite slurry and the copper foil are separated through the mesh on the rotating cylinder, the graphite slurry enters the circulating water tank, and the copper foil is discharged through the discharge drainage plate.
[0016] In an optional embodiment, the temperature of the high temperature and high pressure hydrothermal reaction is 110° C. to 180° C., the reaction pressure is 104 kPa to 123 kPa, and the reaction time is 10 min to 60 min;
[0017] And / or, the high temperature and high pressure hydrothermal reaction is carried out under stirring, and the stirring speed is 200 rpm to 500 rpm;
[0018] and / or, the oxidant comprises at least one of sodium persulfate, potassium persulfate and ammonium persulfate;
[0019] and / or, the solid-to-liquid ratio of the graphite slurry to the oxidant is 5 g / L to 20 g / L;
[0020] And / or, before the high-temperature and high-pressure hydrothermal reaction, the graphite slurry is screened with 100-150 meshes to remove large-particle copper impurities.
[0021] In an optional embodiment, the drying comprises drying at 80°C to 200°C for 10h to 30h;
[0022] Preferably, the sintering comprises sintering at 450° C. to 750° C. for 2 h to 4 h under a protective atmosphere;
[0023] Preferably, the protective atmosphere comprises at least one of nitrogen, helium and argon.
[0024] In an optional embodiment, the rotation speed of the ball mill is 200 rpm to 700 rpm, preferably 400 rpm to 600 rpm;
[0025] And / or, the mass ratio of the pyrolytic graphite to the ball mill used in the ball milling is 1:2 to 1:6, preferably 1:3 to 1:5;
[0026] And / or, the ball milling time is 5 min to 30 min, preferably 5 min to 20 min.
[0027] In an optional embodiment, the feed rate of the airflow classification is 3kg / min to 5kg / min, the pulsation frequency is 30Hz to 50Hz, and the airflow speed is 10cm / s to 12cm / s;
[0028] And / or, the wind pressure of the cyclone separation is 5000Pa-7500Pa, and the wind volume is 250m 3 / min~400m 3 / min.
[0029] In an optional embodiment, the method for preparing the sheet-shaped graphite negative electrode sheet comprises shredding the graphite negative electrode sheet on a double-shaft shredder to obtain sheets with a size of 2 cm to 7 cm;
[0030] Preferably, the graphite negative electrode sheet is a graphite negative electrode sheet that has not been recycled, and the graphite negative electrode sheet includes at least one of scraps that have not been assembled into batteries, defective products and waste materials.
[0031] In an optional embodiment, the Cu content in the finished graphite is 5ppm-9ppm, and the specific surface area is 1.28m 2 / g-1.36m 2 / g, tap density is 1.09g / cm 3 -1.12g / cm 3 .
[0032] In a second aspect, the present invention provides a method for recycling waste lithium-ion batteries, which includes the method for repairing and regenerating graphite in waste lithium-ion batteries as described in any one of the aforementioned embodiments.
[0033] The beneficial effects of the embodiments of the present invention include, for example:
[0034] The method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention adopts a process flow combining ultrasonic hot water immersion and high-temperature and high-pressure hydrothermal reaction, so that the copper foil stripping process is both rapid and efficient, and the copper recovery rate and stripping degree are both as high as 95% or more, which significantly improves the production efficiency. Subsequently, a process flow combining ball milling, airflow classification and cyclone separation is introduced to effectively remove the non-graphite carbon (for graphite, it is an impurity phase) generated during the sample carbonization process, thereby improving the purity of graphite and laying a solid foundation for the production of high-quality products. The process of the present invention is not only simple and efficient, but also can stably ensure product quality. Compared with traditional chemical additive purification and modification methods, the energy consumption of the present invention is significantly reduced, and the processing time is greatly reduced, thereby achieving a dual improvement in production capacity and efficiency. Compared with other coating carbonization processes, the roasting process of the present invention does not need to add asphalt or the like for coating carbonization treatment, and high-performance negative electrode graphite can be achieved, which reduces costs. The method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention combines multiple process steps to obtain regenerated graphite that exhibits excellent performance. It can not only efficiently remove fine powder and amorphous carbon impurities, reduce the specific surface area BET, thereby increasing the discharge capacity and first discharge efficiency of the negative electrode graphite, but also the particle size D50 can reach 15μm, while increasing the tap density and compaction density of the graphite (which is beneficial to the increase in gram capacity); the surface structure repair effect of the graphite sample is significant, further improving the application performance of the graphite. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 A process flow chart of the method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention;
[0037] Figure 2 A front view of a recovery device used in the method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention;
[0038] Figure 3 A side view of a recovery device used in the method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention;
[0039] Figure 4 This is a SEM image of the graphite product provided in Example 1 of the present invention.
[0040] Icons: 100-recovery device; 110-rotating cylinder; 111-mesh; 112-spiral guide plate; 113-spray pipe; 114-feed guide plate; 115-discharge guide plate; 116-conveyor belt; 117-motor; 120-circulating water tank; 121-heater; 122-circulating pump; 123-filter plate; 130-ultrasonic generator. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0042] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0044] In the description of the present invention, it should be noted that if the terms "upper", "lower", "inside", "outside", etc. appear to indicate an orientation or position relationship, they are based on the orientation or position relationship shown in the accompanying drawings, or are the orientation or position relationship in which the product of the invention is usually placed when used. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0045] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention may be combined with each other.
[0046] The present invention provides a method for repairing and regenerating graphite in waste lithium-ion batteries. Figure 1 , which comprises the following steps:
[0047] S1. Separate the graphite slurry and copper foil from the graphite negative electrode sheet by soaking it in ultrasonic hot water.
[0048] The present invention uses a graphite negative electrode sheet that has not been recycled as the graphite negative electrode sheet of the present invention, and the graphite negative electrode sheet includes but is not limited to at least one of the scraps, defective products and waste materials that have not been assembled into batteries. Specifically, the graphite negative electrode sheet in the present invention refers to the scraps, defective products and waste materials of the electrode sheet that have undergone the coating process in the electrode sheet manufacturing process. The main impurity in the graphite of the uncirculated negative electrode sheet and the graphite after the electrode sheet is separated in the present invention is Cu. The graphite negative electrode sheet is shredded on a double-axis shredder to obtain a sheet of 2cm to 7cm in size, that is, a sheet-like graphite negative electrode sheet is obtained. Since the recycled waste batteries will inevitably contain positive electrode impurities, only this recycling process cannot reduce the positive electrode impurities to the battery-grade graphite standard. The process of the present invention is not suitable for used waste batteries. The recycling of recycled waste batteries requires additional impurity removal and purification to meet the battery-grade graphite requirements.
[0049] In the step of separation after ultrasonic hot water soaking, the soaking temperature is 70° C. to 90° C., the soaking time is 30-60 minutes, and the ultrasonic power is 1000w to 1500w.
[0050] For details, please refer to Figure 2 and Figure 3 The step of ultrasonic hot water immersion and separation is carried out in the recovery device 100. The recovery device 100 includes a rotating cylinder 110, a circulating water tank 120 and an ultrasonic generator 130. The side wall of the rotating cylinder 110 is provided with a mesh 111 and a spiral guide plate 112. The top of the rotating cylinder 110 is provided with a spray pipe 113. The spray pipe 113 is connected with the circulating water tank 120 through a circulating pump 122. A heater 121 is provided in the circulating water tank 120. The circulating water tank 120 is arranged below the rotating cylinder 110. The lower part of the rotating cylinder 110 extends below the liquid level of the circulating water tank 120. The ultrasonic generator 130 is arranged at the outer bottom of the circulating water tank 120.
[0051] Among them, the immersion temperature is controlled by the heater 121, the ultrasonic power is controlled by the ultrasonic generator 130, and the output energy of the ultrasonic wave can be adjusted by the ultrasonic controller; the feed port of the rotating cylinder 110 is provided with a feed guide plate 114, and the discharge port is provided with a discharge guide plate 115; the sheet-like graphite negative electrode sheet can be conveyed to the feed guide plate 114 via the conveyor belt 116 and enter the rotating cylinder 110. The rotating cylinder 110 is provided with a motor 117 for driving it to rotate. By adjusting the rotation frequency of the motor 117, the transmission speed of the rotating cylinder 110 can be controlled, thereby controlling the transmission rate of the electrode sheet in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode sheet.
[0052] The flaky graphite negative electrode sheet is stripped and washed under the simultaneous action of ultrasound and water spraying. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the rotating cylinder 110, and the stripped and washed copper foil enters the discharge drainage plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120. The aperture of the mesh 111 in the present invention is 0.5-1 cm. By setting the size of the mesh 111, it can be ensured that the graphite slurry and the copper foil are effectively separated during the ultrasonic hot water immersion process. The graphite slurry enters the circulating water tank 120, and the copper foil is discharged through the discharge drainage plate 115.
[0053] In order to prevent graphite slurry from entering the circulation pump 122, a filter plate 123 is also provided in the circulation water tank 120 in the present invention. The part of the rotating cylinder 110 located in the circulation water tank 120 is located on one side of the filter plate 123, and the circulation pump 122 is located on the other side of the filter plate 123. The filter plate 123 can filter the material in the water body to prevent large particles from entering the spray pipe 113.
[0054] S2, subjecting the graphite slurry and the oxidant to a high temperature and high pressure hydrothermal reaction, and subjecting the reaction liquid to solid-liquid separation and water washing.
[0055] Before the graphite slurry is subjected to the high-temperature and high-pressure hydrothermal reaction, the graphite slurry is screened with 100-150 meshes to remove large copper impurities. The solid-liquid ratio of the graphite slurry and the oxidant is 5g / L-20g / L. The oxidant includes at least one of sodium persulfate, potassium persulfate and ammonium persulfate; the temperature of the high-temperature and high-pressure hydrothermal reaction is 110°C-180°C, the reaction pressure is 104kPa-123kPa, and the reaction time is 10min-60min; the high-temperature and high-pressure hydrothermal reaction is carried out under stirring, and the stirring speed is 200rpm-500rpm; there are many ways to separate the solid and liquid after the reaction, including but not limited to filtration, filter pressing, centrifugation, etc., and the solid is obtained by solid-liquid separation, and the solid graphite is repeatedly washed with water 2-3 times.
[0056] In the hydrothermal reaction process of repairing regenerated graphite, the present invention selects persulfate compounds as oxidative impurity removal media, which is low in cost and pollution-free in the reaction process, and perfectly fits the concept of green production. Compared with traditional acid leaching impurity removal, it eliminates the problem of acid corrosiveness and is more environmentally friendly. At the same time, it uses high-pressure and high-temperature reaction to remove Cu, which has a short reaction time and greatly reduces costs.
[0057] The copper in the graphite slurry is effectively removed by hydrothermal reaction with the oxidant, which significantly reduces the copper content in the graphite, can quickly remove copper and effectively improve the purity of the graphite. In addition, the high temperature and high pressure hydrothermal reaction can also crack the binder in the graphite into amorphous carbon, which is conducive to the subsequent ball milling-airflow classification-cyclone separation and other steps to remove amorphous carbon, and further improve the purity of the finished graphite. The stirring paddle equipped with the high-pressure reactor can break the amorphous carbon produced by the cracking of the binder into fine fragments, which is conducive to the subsequent removal of amorphous carbon.
[0058] Specifically, the binder in graphite is cracked into amorphous carbon through high temperature and high pressure hydrothermal reaction. The basic principle can be divided into the following aspects:
[0059] ①The effect of high temperature and high pressure: Under high temperature and high pressure conditions, the chemical bonds between graphite and the binder are strongly thermally disturbed, making the originally stable structure unstable. This instability causes the organic components in the binder to begin to decompose and cracking reactions to occur.
[0060] ②Influence of hydrothermal reaction: Hydrothermal reaction is a thermochemical reaction carried out in the presence of water. Water not only acts as a reaction medium under high temperature and pressure, but may also directly participate in the reaction. Water molecules may react with certain functional groups in the binder to accelerate the cracking process. At the same time, water can also transfer heat and pressure, making the reaction more uniform and efficient.
[0061] ③ Pyrolysis reaction generates amorphous carbon: The organic components in the binder are gradually pyrolyzed under high temperature and high pressure hydrothermal reaction to generate a series of small molecular compounds, such as gas, liquid and solid residue. Among them, the carbon elements in the solid residue will rearrange and combine under specific reaction conditions to form amorphous carbon. Amorphous carbon is different from the crystal structure of graphite. It does not have a clear crystal structure, but presents a disordered state.
[0062] ④ Reaction kinetics and thermodynamics: This process is also affected by reaction kinetics and thermodynamics. Reaction kinetics describes the relationship between reaction rate and factors such as temperature, pressure, and concentration, while thermodynamics reveals whether the reaction can proceed spontaneously and the direction and limit of the reaction. Under high temperature and high pressure conditions, the reaction rate is accelerated, making the cracking reaction easier to proceed.
[0063] Therefore, the binder in the graphite can quickly remove Cu under high temperature and high pressure hydrothermal reaction conditions. The high pressure environment can change the physical and chemical properties of the reactants, accelerate the reaction speed and improve the reaction efficiency, and trigger chemical reactions that cannot be carried out under normal pressure conditions. The binder in the graphite is cracked into amorphous carbon. Under high temperature and high pressure environment, the binder in the graphite can easily reach the cracking temperature, and under the action of high pressure, the cracking temperature of the binder will be reduced, which will make it easier for it to crack and carbonize, and in this process, with the aid of stirring, it can further cause the cracking process to be "torn" and the cracking products to be extremely small fragments. There is a great difference between the fragments and the graphite particles in terms of particle size and specific gravity. The process of high temperature and high pressure hydrothermal reaction cracking into amorphous carbon of the present invention is a complex physical and chemical process, involving multiple aspects such as the breaking and formation of chemical bonds, phase changes of substances, and the transfer and conversion of energy, thereby changing the structure and properties of graphite and the binder.
[0064] S3. Drying and sintering the washed solid graphite to obtain pyrolytic graphite.
[0065] Drying includes drying at 80°C to 200°C for 10 hours to 30 hours; sintering includes sintering at 450°C to 750°C for 2 hours to 4 hours under a protective atmosphere; the protective atmosphere includes but is not limited to at least one of nitrogen, helium and argon.
[0066] The main purpose of the calcination is to completely crack and carbonize the part of the binder that is not completely cracked in the hydrothermal reaction, so that the subsequent ball milling treatment is easier to dissociate (graphite is dissociated from the completely cracked binder carbon).
[0067] S4. Ball milling the pyrolytic graphite to separate graphite and the binder to obtain graphite powder.
[0068] The ball milling speed is 200 rpm to 700 rpm, preferably 400 rpm to 600 rpm; and / or, the mass ratio of pyrolytic graphite to the ball mill used in the ball milling is 1:2 to 1:6, preferably 1:3 to 1:5; and / or, the ball milling time is 5 min to 30 min, preferably 5 min to 20 min. When the ball milling time is less than 5 min, the graphite powder cannot be well dispersed; when the ball milling time is more than 30 min, the graphite powder is too finely pulverized during ball milling, which will cause a rapid increase in BET.
[0069] The ball milling in the present invention is completely different from the conventional ball milling. The main purpose of the ball milling in the present invention is to break up the graphite and ensure that the graphite and the binder in the sample are effectively separated, thereby promoting the dispersion of amorphous carbon. The purpose of conventional ball milling is to change the particle size and achieve a specific particle size requirement by adjusting the particle size distribution.
[0070] Based on the above different purposes, the ball milling in the present invention does not require high discharge particle size, and does not need to be finely adjusted to a smaller particle size distribution, because too small particle size will be accompanied by a sharp increase in the BET value, which is not conducive to obtaining a graphite product with a smooth surface structure. At the same time, the ball milling time in the present invention is relatively short. Too short or too long ball milling time will have an adverse effect on the dispersion effect of the graphite powder. Too short will result in poor dispersion, and too long will result in excessive pulverization and a rapid increase in the BET value. Conventional ball milling not only requires the particle size to be adjusted to a smaller range in order to further broaden the particle size distribution, but also requires a longer ball milling time.
[0071] S5. Performing airflow classification and cyclone separation on the graphite powder to remove amorphous carbon, and collecting coarse powdered graphite as finished graphite product.
[0072] The feed rate of airflow classification is 3kg / min~5kg / min, the pulsation frequency is 30Hz~50Hz, the airflow speed is 10cm / s~12cm / s; and / or, the wind pressure of cyclone separation is 5000Pa~7500Pa, the air volume is 250m 3 / min~400m 3 / min.
[0073] The Cu content in the finished graphite is 5ppm-9ppm, and the specific surface area is 1.28m 2 / g-1.36m 2 / g, tap density is 1.09g / cm 3 -1.12g / cm 3 .
[0074] In a second aspect, the present invention provides a method for recycling waste lithium-ion batteries, which includes a method for repairing and regenerating graphite in waste lithium-ion batteries according to any one of the aforementioned embodiments.
[0075] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0076] The negative electrode sheets of the following examples and comparative examples are all made of Figure 2 and Figure 3 The recovery device 100 is used to separate the copper foil and the graphite slurry.
[0077] Example 1
[0078] This embodiment provides a method for repairing and regenerating graphite in waste lithium-ion batteries, comprising the following specific steps:
[0079] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0080] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0081] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0082] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0083] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor for a high-temperature and high-pressure hydrothermal reaction, and sodium persulfate was added. The solid-liquid ratio was 6 g / L, the reaction temperature was 150° C., the reaction pressure was 115 kPa, the reaction time was 30 min, and the stirring speed was 300 rpm.
[0084] (6) The reaction liquid after the high temperature and high pressure hydrothermal reaction is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 150° C. for 12 h to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder to obtain pyrolytic graphite.
[0085] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0086] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain high-performance negative electrode graphite products. Figure 4 ,from Figure 4 It can be seen that the graphite surface is smooth and the particles are uniform.
[0087] Example 2
[0088] This embodiment provides a method for repairing and regenerating graphite in waste lithium-ion batteries, comprising the following specific steps:
[0089] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0090] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0091] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0092] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0093] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 130° C., a reaction pressure of 110 kPa, a reaction time of 40 min, and a stirring speed of 300 rpm.
[0094] (6) The reaction liquid after the high temperature and high pressure hydrothermal reaction is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 150° C. for 12 hours to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 hours in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder to obtain pyrolytic graphite.
[0095] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0096] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain a high-performance negative electrode graphite product.
[0097] Example 3
[0098] This embodiment provides a method for repairing and regenerating graphite in waste lithium-ion batteries, comprising the following specific steps:
[0099] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0100] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0101] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0102] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0103] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 100° C., a reaction pressure of 101 kPa, a reaction time of 30 min, and a stirring speed of 300 rpm.
[0104] (6) The reaction liquid after the high temperature and high pressure hydrothermal reaction is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 150° C. for 12 hours to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 hours in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder to obtain pyrolytic graphite.
[0105] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0106] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 6000 Pa, and the air volume is 300m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain a high-performance negative electrode graphite product.
[0107] Example 4
[0108] This embodiment provides a method for repairing and regenerating graphite in waste lithium-ion batteries, comprising the following specific steps:
[0109] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0110] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0111] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 70°C; after the temperature rises to 70°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (through the filter plate 123 to filter the material in the water body to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1500w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 30min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0112] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved with 100 mesh to remove large particles of copper impurities.
[0113] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor for a high-temperature and high-pressure hydrothermal reaction, and potassium persulfate was added. The solid-liquid ratio was 10 g / L, the reaction temperature was 110° C., the reaction pressure was 123 kPa, the reaction time was 20 min, and the stirring speed was 500 rpm.
[0114] (6) separating the reaction liquid after the high-temperature and high-pressure hydrothermal reaction into solid and liquid, and repeatedly washing with water for 2 to 3 times; drying the washed solid graphite at 80° C. for 30 h to obtain dry graphite slag, and sintering the dry slag at 450° C. for 4 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder, thereby obtaining pyrolytic graphite.
[0115] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 200 rpm, the mass ratio of the graphite sample to the ball mill was 1:2, the ball milling time was 30 min, and the graphite powder was obtained by ball milling.
[0116] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 3 kg / min, the pulsation frequency is 30 Hz, and the airflow speed is 11 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 5000 Pa and the air volume is 250m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain a high-performance negative electrode graphite product.
[0117] Example 5
[0118] This embodiment provides a method for repairing and regenerating graphite in waste lithium-ion batteries, comprising the following specific steps:
[0119] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0120] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0121] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 90°C; after the temperature rises to 90°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (through the filter plate 123 to filter the material in the water body to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1000w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117 to control the transmission rate of the electrode in the rotating cylinder 110, and finally the ultrasonic and washing time of the negative electrode electrode is controlled. The final processing time is about 60min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. The negative electrode electrode is stripped and washed under the simultaneous action of ultrasonic wave and water spray. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0122] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 150 meshes to remove large copper impurities.
[0123] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor for a high-temperature and high-pressure hydrothermal reaction, and ammonium persulfate was added at a solid-liquid ratio of 20 g / L, a reaction temperature of 180° C., a reaction pressure of 104 kPa, a reaction time of 60 min, and a stirring speed of 200 rpm.
[0124] (6) The reaction liquid after the high-temperature and high-pressure hydrothermal reaction is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 200° C. for 10 h to obtain dry graphite slag, and the dry slag is sintered at 750° C. for 2 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder, thereby obtaining pyrolytic graphite.
[0125] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 700 rpm, the mass ratio of the graphite sample to the ball mill was 1:6, the ball milling time was 10 min, and the graphite powder was obtained by ball milling.
[0126] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 50 Hz, and the airflow speed is 12 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7500 Pa, and the air volume is 400m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain a high-performance negative electrode graphite product.
[0127] Comparative Example 1
[0128] This comparative example is basically the same as Example 1, except that in this comparative example, the ultrasonic output energy of ultrasonic hot water immersion is different and the final treatment time is different. This comparative example specifically includes the following steps:
[0129] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0130] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0131] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 100% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 2.5h) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0132] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0133] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 150° C., a reaction pressure of 115 kPa, a reaction time of 30 min, and a stirring speed of 300 rpm.
[0134] (6) separating the reaction liquid after the high-temperature and high-pressure hydrothermal reaction from solid to liquid, and repeatedly washing with water for 2 to 3 times; drying the washed solid graphite at 150° C. for 12 h to obtain dry graphite slag, and sintering the dry slag at 650° C. for 3 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder, thereby obtaining pyrolytic graphite;
[0135] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0136] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain the finished negative electrode graphite product.
[0137] Comparative Example 2
[0138] This comparative example is basically the same as Example 1, except that in this comparative example, the ultrasonic output energy of ultrasonic hot water immersion is different, the final treatment time is different, and the high temperature and high pressure hydrothermal reaction conditions are different. This comparative example specifically includes the following steps:
[0139] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0140] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0141] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 100% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 2.5h) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0142] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0143] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 100° C., a reaction pressure of 101 kPa, a reaction time of 30 min, and a stirring speed of 300 rpm.
[0144] (6) The reaction liquid after the high temperature and high pressure hydrothermal reaction is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 150° C. for 12 h to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder to obtain pyrolytic graphite.
[0145] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0146] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain the finished negative electrode graphite product.
[0147] Comparative Example 3
[0148] This comparative example is basically the same as Example 1, except that the sintering step in step (6) and the ball milling step in step (7) are omitted in this comparative example. This comparative example specifically includes the following steps:
[0149] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0150] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0151] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0152] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0153] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 150° C., a reaction pressure of 115 kPa, a reaction time of 30 min, and a stirring speed of 300 rpm.
[0154] (6) separating the reaction liquid after the high temperature and high pressure hydrothermal reaction into solid and liquid, and repeatedly washing with water for 2 to 3 times; drying the washed solid graphite at 150° C. for 12 hours to obtain graphite dry residue, and obtaining dried graphite powder.
[0155] (7) The dried graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain the finished negative electrode graphite product.
[0156] Comparative Example 4
[0157] This comparative example is basically the same as Example 1, except that the airflow classification and cyclone separation process in step (8) are omitted in this comparative example. This comparative example specifically includes the following steps:
[0158] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0159] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0160] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0161] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0162] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 150° C., a reaction pressure of 115 kPa, a reaction time of 30 min, and a stirring speed of 300 rpm.
[0163] (6) The reaction liquid after the high temperature and high pressure hydrothermal reaction is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 150° C. for 12 h to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder to obtain pyrolytic graphite.
[0164] (7) The pyrolytic graphite was ball-milled at a speed of 500 rpm, a mass ratio of graphite sample to ball mill of 1:4, and a ball-milling time of 15 min to obtain negative electrode graphite powder.
[0165] Comparative Example 5
[0166] This comparative example is basically the same as Example 1, except that the high temperature and high pressure hydrothermal reaction of step (5) is omitted in this comparative example. This comparative example specifically comprises the following steps:
[0167] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0168] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0169] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0170] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0171] (5) The graphite slurry from which the large copper impurities have been screened out is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 80 to 200° C. for 10 to 30 hours to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 hours in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder, thereby obtaining pyrolytic graphite.
[0172] (6) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0173] (7) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is used to obtain the negative electrode graphite product.
[0174] Comparative Example 6
[0175] This comparative example is basically the same as Example 1, except that in this comparative example, the temperature and pressure of the high-temperature and high-pressure hydrothermal reaction in step (5) are different. This comparative example specifically comprises the following steps:
[0176] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0177] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0178] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0179] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0180] (5) The graphite slurry from which the large copper particles were screened out was transferred to a reactor, and sodium persulfate was added at a solid-liquid ratio of 6 g / L, a reaction temperature of 25° C., a reaction pressure of 101 kPa, a reaction time of 30 min, and a stirring speed of 300 rpm.
[0181] (6) The reaction liquid after the reaction at room temperature and pressure is subjected to solid-liquid separation, and is repeatedly washed with water for 2 to 3 times; the washed solid graphite is dried at 150° C. for 12 h to obtain dry graphite slag, and the dry slag is sintered at 650° C. for 3 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder to obtain pyrolytic graphite.
[0182] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 15 min, and the graphite powder was obtained by ball milling.
[0183] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain the finished negative electrode graphite product.
[0184] Comparative Example 7
[0185] This comparative example is substantially the same as Example 1, except that the ball milling time in step (7) is different in this comparative example. This comparative example specifically comprises the following steps:
[0186] (1) Collect unrecycled graphite negative electrode sheets as raw materials for repair and regeneration.
[0187] (2) The negative electrode sheet is shredded on a double-shaft shredder to obtain sheets of about 2 cm to 7 cm in size.
[0188] (3) The sheet-like negative electrode is processed through the following recovery device 100: first, the heater 121 is turned on to heat the water temperature to 80°C; after the temperature rises to 80°C, the belt conveyor conveys the electrode material, and a feed guide plate 114 is arranged at the top of the belt conveyor. The material enters the rotating cylinder 110 through the feed guide plate 114. The side wall of the rotating cylinder 110 is provided with a mesh 111 of 0.5 to 1 cm and a spiral guide plate 112. A spray pipe 113 is arranged in the middle of the rotating cylinder 110. The circulating pump 122 uses the water in the circulating water tank 120 (the material in the water is filtered through the filter plate 123 to prevent large particles from entering the spray pipe 113) to spray and wash the electrode material. At the same time, the electrode material in the rotating cylinder 110 and the ultrasonic generator 130 ( The ultrasonic power is 1200w, and the output energy of the ultrasonic wave is adjusted to 70% through the ultrasonic controller. The transmission speed of the rotating cylinder 110 can be controlled by adjusting the frequency of the transmission motor 117, thereby controlling the transmission rate of the electrode in the rotating cylinder 110, and finally controlling the ultrasonic and washing time of the negative electrode electrode. The final processing time is about 40min) and the negative electrode electrode is in contact with the water in the circulating water tank 120. Under the simultaneous action of ultrasonic wave and water spray, the negative electrode electrode is stripped and washed. The stripped and washed graphite powder enters the circulating water tank 120 through the mesh 111 of the cylinder, and the stripped and washed copper foil enters the discharge guide plate 115 through the spiral guide plate 112 of the rotating cylinder 110. The copper foil with the graphite powder stripped off is collected in the recovery tank, and the graphite slurry is collected in the circulating water tank 120.
[0189] (4) The graphite slurry collected in the circulating water tank 120 after ultrasonic immersion and hot water spray washing is sieved through 120 meshes to remove large copper impurities.
[0190] (5) The graphite slurry from which the large copper particles were screened out was transferred to a high-pressure reactor for a high-temperature and high-pressure hydrothermal reaction, and sodium persulfate was added. The solid-liquid ratio was 6 g / L, the reaction temperature was 150° C., the reaction pressure was 115 kPa, the reaction time was 30 min, and the stirring speed was 300 rpm.
[0191] (6) separating the reaction liquid after the high-temperature and high-pressure hydrothermal reaction from solid to liquid, and repeatedly washing with water for 2 to 3 times; drying the washed solid graphite at 150° C. for 12 h to obtain dry graphite slag, and sintering the dry slag at 650° C. for 3 h in a nitrogen atmosphere to remove the organic binder remaining in the graphite slag and to crack and carbonize the binder, thereby obtaining pyrolytic graphite;
[0192] (7) The pyrolytic graphite was subjected to ball milling treatment, the ball milling speed was 500 rpm, the mass ratio of the graphite sample to the ball mill was 1:4, the ball milling time was 60 min, and the graphite powder was obtained by ball milling.
[0193] (8) The graphite powder is treated by airflow classification and cyclone separation. The feed rate of airflow classification is 4 kg / min, the pulsation frequency is 45 Hz, and the airflow speed is 10 cm / s. After classification, the graphite powder is treated by cyclone separation and cyclone separation into fine powder and coarse powder. The wind pressure of cyclone separation is 7000 Pa and the air volume is 350m 3 / min. The coarse powder obtained by cyclone separation is collected to obtain the finished negative electrode graphite product.
[0194] Experimental Example 1: Physical and Chemical Properties
[0195] The finished graphite products prepared in the above Examples 1-5 and Comparative Examples 1-7 were tested for copper content, specific surface area and tap density, wherein the copper content was tested by inductively coupled plasma atomic emission spectrometry and ICP method; the specific surface area was tested by gas adsorption BET method GB / T19587-2017; and the tap density was tested by tap density test method for graphite negative electrode materials for lithium ion batteries GB / T 24533-2009. Please refer to Table 1 for the test results.
[0196] Table 1. Statistical table of copper content, specific surface area and tap density test data of graphite samples
[0197]
[0198]
[0199] As can be seen from the above table, Examples 1-5, Comparative Examples 1-4 and 7 are all treated with high temperature and high pressure hydrothermal reaction, and the copper content is significantly reduced. Among them, when the ultrasonic output energy of Comparative Examples 1-2 is not within the scope of the present application and the treatment time is not within the scope of the present application, the copper removal effect is significantly lower than that of Example 1, while Comparative Example 5 omits the high temperature and high pressure hydrothermal reaction, and Comparative Example 6 reacts at room temperature and pressure. It can be seen that the copper removal effect of Comparative Examples 5 and 6 is not obvious, and the copper content in the final product is significantly higher than that of other embodiments and comparative examples. After subsequent treatment steps such as ball milling, airflow classification and cyclone separation, the specific surface area of graphite has decreased significantly, while TD has been significantly improved. Comparative Example 3 omits the steps of sintering and ball milling. At this time, the binder is not completely carbonized, which is not conducive to subsequent separation. Comparative Example 4 omits airflow classification and cyclone separation, and Comparative Example 7 prolongs the ball milling time. It can be seen that its specific surface area is significantly higher than that of other embodiments and comparative examples, while TD is significantly lower than that of other embodiments and comparative examples.
[0200] Experimental Example 2: Electrochemical Performance
[0201] The finished graphite products prepared in the above-mentioned Examples 1-5 and Comparative Examples 1-7 were tested for the first discharge specific capacity and coulombic efficiency, wherein the first discharge specific capacity and coulombic efficiency testing methods include the first discharge specific capacity and first charge and discharge efficiency testing methods of lithium ion battery negative electrode materials. Please refer to Table 2 for the test results.
[0202] Table 2. Statistical table of first discharge specific capacity and coulombic efficiency test data of graphite samples
[0203]
[0204]
[0205] As can be seen from Table 2, after a series of processing steps such as high pressure reaction, pyrolysis, ball milling, airflow classification and cyclone separation, we found that the discharge specific capacity and first discharge efficiency of the samples were significantly improved, and the discharge specific capacity and coulomb efficiency of Examples 1-5 were very high. Although the discharge capacity and coulomb efficiency of Comparative Examples 1 and 2 were high, the Cu content was high; Comparative Example 3 was directly subjected to classification and cyclone separation without pyrolysis. Although the Cu content was low, it was not subjected to pyrolysis, and the classification and cyclone separation effects were not good, the specific surface area was large, and the coulomb efficiency was low; Comparative Example 4 was not subjected to classification and cyclone separation, the specific surface area was high, and the first coulomb efficiency was low; and although the discharge capacity and coulomb efficiency of Comparative Examples 5 and 6 were high, the Cu content was very high, which would bring safety and performance risks to lithium-ion batteries; Comparative Example 7 was subjected to long-term ball milling, the graphite powder was over-finely milled, the specific surface area was high, and the first coulomb efficiency was low.
[0206] In summary, the method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention adopts a process flow combining ultrasonic hot water immersion and high-temperature and high-pressure hydrothermal reaction, so that the copper foil stripping process is both rapid and efficient, and the copper recovery rate and stripping degree are both as high as 95% or more, which significantly improves the production efficiency. Subsequently, a process flow combining ball milling, airflow classification and cyclone separation is introduced to effectively remove the non-graphite carbon (for graphite, it is an impurity phase) produced during the carbonization of the sample, thereby improving the purity of the graphite and laying a solid foundation for the production of high-quality products. The process of the present invention is not only simple and efficient, but also can stably ensure the quality of the product. Compared with the traditional chemical additive purification and modification method, the energy consumption of the present invention is significantly reduced, and the processing time is greatly reduced, thereby achieving a dual improvement in production capacity and efficiency. Compared with other coating carbonization processes, the roasting process of the present invention does not need to add asphalt or the like for coating carbonization treatment, and high-performance negative electrode graphite can be achieved, which reduces costs. The method for repairing and regenerating graphite in waste lithium-ion batteries provided by the present invention combines multiple process steps to obtain regenerated graphite that exhibits excellent performance. It can not only efficiently remove fine powder and amorphous carbon impurities, reduce the specific surface area BET, thereby increasing the discharge capacity and first discharge efficiency of the negative electrode graphite, but also the particle size D50 can reach 15μm, while increasing the tap density and compaction density of the graphite (which is beneficial to the increase in gram capacity); the surface structure repair effect of the graphite sample is significant, further improving the application performance of the graphite.
[0207] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for repairing and regenerating graphite in waste lithium-ion batteries, characterized in that: include: The graphite negative electrode sheet is soaked in ultrasonic hot water to separate the graphite slurry and the copper foil; The graphite slurry and the oxidant are subjected to a high temperature and high pressure hydrothermal reaction, and the reaction liquid is subjected to solid-liquid separation and water washing; Drying and sintering the washed solid graphite to obtain pyrolytic graphite; ball milling the pyrolytic graphite to separate graphite and a binder to obtain graphite powder; The graphite powder is subjected to airflow classification and cyclone separation to remove amorphous carbon, and coarse graphite powder is collected as a finished graphite product.
2. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 1, characterized in that: In the step of ultrasonic hot water soaking and separation, the soaking temperature is 70° C. to 90° C., the soaking time is 30-60 minutes, and the ultrasonic power is 1000w to 1500w.
3. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 2, characterized in that: The ultrasonic hot water soaking and separation step is performed in a recovery device (100). The recovery device (100) comprises a rotating cylinder (110), a circulating water tank (120) and an ultrasonic generator (130). The side wall of the rotating cylinder (110) is provided with mesh holes (111) and a spiral guide plate (112). The top of the rotating cylinder (110) is provided with a spray pipe (113). The spray pipe (113) is connected to the circulating water tank (120) through a circulating pump (122). A heater (121) is provided in the circulating water tank (120). The circulating water tank (120) is provided below the rotating cylinder (110). The lower part of the rotating cylinder (110) extends below the liquid level of the circulating water tank (120). The ultrasonic generator (130) is provided at the outer bottom of the circulating water tank (120). Preferably, the feed port of the rotating cylinder (110) is provided with a feed guide plate (114), and the discharge port of the rotating cylinder (110) is provided with a discharge guide plate (115); Preferably, the graphite slurry and the copper foil are separated through the mesh (111) on the rotating cylinder (110), the graphite slurry enters the circulating water tank (120), and the copper foil is discharged through the discharge guide plate (115).
4. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 1, characterized in that: The temperature of the high temperature and high pressure hydrothermal reaction is 110°C to 180°C, the reaction pressure is 104kPa to 123kPa, and the reaction time is 10min to 60min; And / or, the high temperature and high pressure hydrothermal reaction is carried out under stirring, and the stirring speed is 200 rpm to 500 rpm; and / or, the oxidant comprises at least one of sodium persulfate, potassium persulfate and ammonium persulfate; and / or, the solid-to-liquid ratio of the graphite slurry to the oxidant is 5 g / L to 20 g / L; And / or, before the high-temperature and high-pressure hydrothermal reaction, the graphite slurry is screened with 100-150 meshes to remove large-particle copper impurities.
5. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 1, characterized in that: The drying comprises drying at 80°C to 200°C for 10h to 30h; Preferably, the sintering comprises sintering at 450° C. to 750° C. for 2 h to 4 h under a protective atmosphere; Preferably, the protective atmosphere comprises at least one of nitrogen, helium and argon.
6. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 1, characterized in that: The ball mill has a rotation speed of 200 rpm to 700 rpm, preferably 400 rpm to 600 rpm; And / or, the mass ratio of the pyrolytic graphite to the ball mill used in the ball milling is 1:2 to 1:6, preferably 1:3 to 1:5; And / or, the ball milling time is 5 min to 30 min, preferably 5 min to 20 min.
7. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 1, characterized in that: The feed rate of the airflow classification is 3kg / min to 5kg / min, the pulsation frequency is 30Hz to 50Hz, and the airflow speed is 10cm / s to 12cm / s; And / or, the wind pressure of the cyclone separation is 5000Pa-7500Pa, and the wind volume is 250m 3 / min~400m 3 / min.
8. The method for repairing and regenerating graphite in waste lithium-ion batteries according to claim 1, characterized in that: The method for preparing the sheet-shaped graphite negative electrode sheet comprises shredding the graphite negative electrode sheet on a double-shaft shredder to obtain sheets with a size of 2 cm to 7 cm; Preferably, the graphite negative electrode sheet is a graphite negative electrode sheet that has not been recycled, and the graphite negative electrode sheet includes at least one of scraps that have not been assembled into batteries, defective products and waste materials.
9. The method for repairing and regenerating graphite in waste lithium-ion batteries according to any one of claims 1 to 8, characterized in that: The Cu content in the finished graphite product is 5ppm-9ppm, and the specific surface area is 1.28m 2 / g-1.36m 2 / g, tap density is 1.09g / cm 3 -1.12g / cm 3 .
10. A method for recycling waste lithium-ion batteries, characterized in that: The invention comprises a method for repairing and regenerating graphite in waste lithium-ion batteries as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method for purifying, repairing and regenerating graphite in retired power battery
CN111204757A
Lithium manganese iron phosphate positive electrode material, preparation method thereof and lithium ion battery
CN115763809A
Recycling method and application of graphite negative electrode material of waste lithium ion battery
CN117477083A
Cited By
Regeneration and recovery method and recovery device of copper-containing battery negative electrode material
CN119542596A
Repairing and regenerating method of lithium battery negative electrode graphite material and regenerated graphite material
CN121688212A