Modified resorcinol resin as well as preparation method and application thereof
Resorcinol resin is modified by composite modification of N-(hydroxymethyl)acrylamide and styrene, and carbon-carbon double bond active sites are introduced to solve the problems of fuming and insufficient adhesive performance of resorcinol resin, and improve the The tensile strength and adhesion of rubber improve the aging resistance of tires.
Patent Information
- Application Number
- CN202310317080.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
Existing resorcinol resins in the field of automobile tires contain high levels of free resorcinol and are prone to smoke, which affects the workshop environment. At the same time, styrene modification leads to a reduction in the degree of cross-linking, affecting the adhesive performance.
Using N-(hydroxymethyl)acrylamide or its derivatives and styrene or its derivatives to composite modified resorcin resin, by introducing carbon-carbon double bond active sites, the cross-linked network of the resin and rubber is enhanced, reducing the Free resorcinol content and improved adhesive properties.
It effectively reduces the free resorcinol content, improves the tensile strength and heat-generating properties of the rubber, enhances the adhesion between the rubber and the skeleton material, and improves the aging resistance and bonding strength of the tire.
Smart Images

Figure BDA0004150797400000021 
Figure BDA0004150797400000031 
Figure BDA0004150797400000032
Abstract
Description
Technical Field
[0001] The invention belongs to the field of resorcinol resins, and relates to a composite modified resorcinol resin of N-(hydroxymethyl)acrylamide or its derivatives and styrene or its derivatives, and a preparation method and application thereof. Background Art
[0002] Resorcinol resin is a polymer formed by the condensation of resorcinol and formaldehyde. In the field of automobile tires, resorcinol resin is a commonly used adhesive between rubber and steel wire or polyester cord.
[0003] Pure resorcinol resin contains a high content of free resorcinol, which is easy to smoke when used, affecting the health of workshop workers. At present, in order to solve the smoke problem, the main modification method of resorcinol resin adhesive is styrene modification. However, due to the access of some reactive active sites to styrene molecules, the cross-linking degree of the product is reduced, which ultimately has an adverse effect on the bonding performance. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a resorcinol resin modified by a composite of N-(hydroxymethyl)acrylamide or its derivatives and styrene or its derivatives, and a preparation method and application thereof. The present invention uses part of N-(hydroxymethyl)acrylamide or its derivatives to replace styrene or its derivatives to modify the resorcinol resin. On the one hand, it can also reduce free resorcinol and solve the smoke problem; on the other hand, it introduces carbon-carbon double bond active sites in the side chain of the resorcinol resin, which can participate in the vulcanization of rubber during the vulcanization process to form a cross-linked network between the resin and the rubber, thereby enhancing the adhesion to the rubber and the skeleton material. The modified resorcinol resin of the present invention can also improve the tensile strength and heat generation performance of the rubber.
[0005] Specifically, one aspect of the present invention provides a modified resorcinol resin, wherein the modified resorcinol resin comprises a structural unit represented by formula I, a structural unit represented by formula II, and a structural unit represented by formula III:
[0006] 226098 1CNCN
[0007]
[0008] wherein p is an integer selected from 0 to 5, and each R1 is independently selected from C1-C6 alkyl and C1-C6 alkoxy;
[0009] R2 is selected from C2-C10 straight chain alkenyl, C3-C10 branched alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond.
[0010] In one or more embodiments, in the structural unit represented by formula I, p is 0.
[0011] In one or more embodiments, in the structural unit represented by formula II, R2 is vinyl.
[0012] In one or more embodiments, in the modified resorcinol resin, the number of the structural units represented by formula I accounts for 20% to 95%, preferably 30% to 70%, more preferably 40% to 65%, for example 50% to 60% of the total number of the structural units represented by formula I, the structural units represented by formula II and the structural units represented by formula III.
[0013] In one or more embodiments, in the modified resorcinol resin, the amount of the structural unit represented by formula II accounts for 5% to 70%, preferably 5% to 65%, more preferably 10% to 40%, for example 10% to 30%, of the total amount of the structural unit represented by formula I, the structural unit represented by formula II, and the structural unit represented by formula III.
[0014] In one or more embodiments, in the modified resorcinol resin, the total amount of the structural units represented by formula I and the structural units represented by formula II accounts for 50% to 90%, preferably 55% to 85%, for example 60% to 80% of the total amount of the structural units represented by formula I, the structural units represented by formula II and the structural units represented by formula III.
[0015] In one or more embodiments, in the monomers of the modified resorcinol resin, the molar ratio of resorcinol to aldehyde compound is 1:(0.5-0.7), preferably 1:(0.55-0.65), for example 1:(0.55-0.6).
[0016] In one or more embodiments, the softening point of the modified resorcinol resin is 90°C to 115°C, such as 95°C to 112°C.
[0017] In one or more embodiments, the free phenol content of the modified resorcinol resin is ≤ 1.5 wt %, preferably ≤ 1.2 wt %, and more preferably ≤ 1 wt %.
[0018] Another aspect of the present invention provides a method for preparing the modified resorcinol resin described in any embodiment herein, the method comprising the following steps:
[0019] (1) providing a mixture of molten resorcinol and an acid catalyst;
[0020] (2) adding a compound of formula A to the mixture of step (1) and reacting at 110-130° C., wherein p is an integer selected from 0 to 5, and each R1 is independently selected from C1-C6 alkyl and C1-C6 alkoxy;
[0021]
[0022] (3) cooling the reaction system obtained in step (2) to 90-110° C., adding an aldehyde compound, and reacting, and distilling off water after the reaction is completed;
[0023] (4) adding a compound of formula B to the reaction system obtained in step (3) and reacting at 100-150° C., wherein R2 in formula B is selected from the group consisting of C2-C10 straight-chain alkenyl, C2-C10 branched alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond;
[0024]
[0025] (5) Post-treating the reaction product obtained in step (4) to obtain the modified resorcinol resin.
[0026] In one or more embodiments, the compound of formula A is styrene.
[0027] In one or more embodiments, the compound of formula B is N-(hydroxymethyl)acrylamide.
[0028] In one or more embodiments, the ratio of the amount of resorcinol added in the method to the amount of compound of formula A is 1:(0.2-0.95), preferably 1:(0.3-0.7), more preferably 1:(0.4-0.65), for example 1:(0.5-0.6).
[0029] In one or more embodiments, the ratio of the amount of resorcinol added in the method to the amount of the compound of formula B is 1:(0.05-0.7), preferably 1:(0.05-0.65), more preferably 1:(0.1-0.4), for example 1:(0.1-0.3).
[0030] In one or more embodiments, the ratio of the amount of resorcinol added in the method to the total amount of the compound of formula A and the compound of formula B is 1:(0.5-0.9), preferably 1:(0.55-0.85), more preferably 1:(0.6-0.8).
[0031] In one or more embodiments, the molar ratio of resorcinol to aldehyde compound added in the method is 1:(0.5-0.7), preferably 1:(0.55-0.65), for example 1:(0.55-0.6).
[0032] In one or more embodiments, in step (1), the acid catalyst is selected from one or more of p-toluenesulfonic acid, methanesulfonic acid, benzenesulfonic acid, benzene disulfonic acid, dodecylbenzenesulfonic acid, hydrochloric acid, sulfuric acid and phosphoric acid, preferably p-toluenesulfonic acid.
[0033] In one or more embodiments, the mass of the acid catalyst added in step (1) is 0.2% to 1%, preferably 0.3% to 0.5%, of the mass of resorcinol.
[0034] In one or more embodiments, the reaction time in step (2) is 15 to 60 minutes.
[0035] In one or more embodiments, after the aldehyde compound is added in step (3), the reaction is continued at 90 to 110° C. for 10 to 30 minutes.
[0036] In one or more embodiments, the reaction time in step (4) is 15 to 60 minutes.
[0037] In one or more embodiments, the post-treatment in step (5) comprises: neutralizing the p-toluenesulfonic acid in the reaction product obtained in step (4), and then distilling out impurities; preferably, the terminator used for neutralization is selected from one or more of triethanolamine, diethanolamine, N-methyldiethanolamine, alkylamine, dialkylamine, trialkylamine and NaOH, preferably triethanolamine.
[0038] Another aspect of the present invention provides a rubber composition, wherein the rubber composition includes the modified resorcinol resin according to any one of the embodiments herein.
[0039] In one or more embodiments, the rubber composition further includes a diene elastomer.
[0040] In one or more embodiments, based on 100 parts by weight of the diene elastomer, the content of the modified resorcinol resin in the rubber composition is 1 to 5 parts by weight.
[0041] Another aspect of the present invention provides a tire, wherein the adhesive layer rubber material of the tire is the rubber composition described in any embodiment of the present invention.
[0042] The present invention also provides use of the modified resorcinol resin described in any embodiment herein for improving the tensile strength, adhesive strength, aging resistance and / or heat generation performance of rubber.
[0043] In one or more embodiments, the bond strength is the bond strength between rubber and a cord, such as a steel cord. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1This is the infrared spectrum of the resorcinol resin modified by N-(hydroxymethyl)acrylamide and styrene in Example 1.
[0045] Figure 2 This is the infrared spectrum of the styrene-modified resorcinol resin of Comparative Example 3.
[0046] Figure 3 This is a comparison of the infrared spectra of resorcinol resin before and after modification with N-(hydroxymethyl)acrylamide. Figure 3 In the figure, "before modification" refers to the styrene-modified resorcinol resin of Comparative Example 3, and "after modification" refers to the resorcinol resin composite-modified with N-(hydroxymethyl)acrylamide and styrene of Example 1. DETAILED DESCRIPTION
[0047] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0048] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0049] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0050] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions).
[0051] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0052] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0053] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0054] In the present invention, alkyl refers to a linear or branched monovalent saturated hydrocarbon group. Examples of alkyl include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, etc. In the present invention, alkoxy refers to alkyl-O-.
[0055] In the present invention, a straight-chain alkenyl group refers to a straight-chain monovalent unsaturated hydrocarbon group containing a carbon-carbon double bond; a branched alkenyl group refers to a branched monovalent unsaturated hydrocarbon group containing a carbon-carbon double bond; an alicyclic alkenyl group refers to a monovalent unsaturated hydrocarbon group having a carbon-carbon double bond and an alicyclic structure; an aromatic alkenyl group refers to a monovalent unsaturated hydrocarbon group having a carbon-carbon double bond and an aromatic ring structure; a heterocyclic alkenyl group refers to a monovalent unsaturated group having a carbon-carbon double bond and a heterocyclic structure; and a heteroaromatic alkenyl group refers to a monovalent unsaturated group having a carbon-carbon double bond and a heteroaromatic ring structure.
[0056] The modified resorcinol resin of the present invention is a resorcinol resin modified by a compound of formula A and a compound of formula B:
[0057] 226098 1CNCN
[0058]
[0059] In formula A, p can be an integer selected from 0 to 5, and each R1 is independently selected from C1-C6 alkyl and C1-C6 alkoxy; in formula B, R2 can be selected from C2-C10 straight chain alkenyl, C2-C10 branched alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond.
[0060] In some embodiments, in Formula A, p is 0, that is, R1 does not exist, and the compound of Formula A is styrene. In some embodiments, in Formula A, p is an integer of 1 to 4, and the compound of Formula A is a styrene derivative described herein.
[0061] In some embodiments, in Formula B, R2 is vinyl, and the compound of Formula B is N-(hydroxymethyl)acrylamide. In some embodiments, in Formula B, R2 is a group other than vinyl selected from C2-C10 straight-chain alkenyl, C2-C10 branched alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond, and the compound of Formula B is the N-(hydroxymethyl)acrylamide derivative described herein.
[0062] The modified resorcinol resin of the present invention comprises a structural unit represented by formula I, a structural unit represented by formula II and a structural unit represented by formula III:
[0063]
[0064] In Formula I, p can be an integer selected from 0 to 5, and each R1 is independently selected from C1-C6 alkyl and C1-C6 alkoxy. In some embodiments, in the structural unit shown in Formula I, p is 0, that is, R1 does not exist.
[0065] In Formula II, R2 can be selected from C2-C10 straight chain alkenyl, C3-C10 branched chain alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond. In some embodiments, in the structural unit shown in Formula II, R2 is vinyl.
[0066] In the modified resorcinol resin of the present invention, the amount of the structural unit represented by formula I accounts for 20% to 95%, preferably 30% to 70%, more preferably 40% to 65%, for example 45%, 50%, 55%, 60% of the total amount of the structural unit represented by formula I, the structural unit represented by formula II and the structural unit represented by formula III. Controlling the content of the structural unit represented by formula I within the aforementioned range is conducive to reducing the free resorcinol content of the modified resorcinol resin.
[0067] In the modified resorcinol resin of the present invention, the amount of the structural unit represented by formula II accounts for 5% to 70%, preferably 5% to 65%, more preferably 10% to 40%, for example 10%, 15%, 25%, 30%, 35% of the total amount of the structural unit represented by formula I, the structural unit represented by formula II and the structural unit represented by formula III. Controlling the content of the structural unit represented by formula II within the aforementioned range is beneficial to improving the anti-aging, viscosity-increasing, tensile strength-enhancing and heat-generating properties of the modified resorcinol resin.
[0068] In the modified resorcinol resin of the present invention, the total amount of the structural units represented by formula I and the structural units represented by formula II accounts for 50% to 90%, preferably 55% to 85%, for example 60%, 65%, 70%, 75%, 80% of the total amount of the structural units represented by formula I, the structural units represented by formula II and the structural units represented by formula III. Controlling the content of the structural units represented by formula I and the structural units represented by formula II within the aforementioned range is conducive to reducing the free resorcinol content of the modified resorcinol resin.
[0069] The monomers of the resorcinol resin of the present invention include resorcinol and aldehyde compounds. The molar ratio of resorcinol to aldehyde compounds is 1:(0.5-0.7), preferably 1:(0.55-0.65), for example 1:0.55, 1:0.6. Controlling the molar ratio of resorcinol to aldehyde compounds within the above range is conducive to obtaining a suitable resin softening point.
[0070] The aldehyde compound suitable for use as the monomer of the resorcinol resin may be one or more selected from formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, valeraldehyde, hexanal, benzaldehyde and furfural, preferably formaldehyde.
[0071] The softening point of the modified resorcinol resin of the present invention is 90° C. to 115° C., such as 95° C., 98° C., 110° C., 112° C. The free phenol content of the modified resorcinol resin of the present invention is preferably ≤1.5wt%, more preferably ≤1.2wt%, more preferably ≤1wt%.
[0072] The resorcinol resin of the present invention can be prepared by a method comprising the following steps:
[0073] (1) providing a mixture of molten resorcinol and an acid catalyst;
[0074] (2) adding the compound of formula A to the mixture of step (1) and reacting at 110-130° C.;
[0075]
[0076] (3) cooling the reaction system obtained in step (2) to 90-110° C., adding an aldehyde compound, and reacting, and distilling off water after the reaction is completed;
[0077] (4) adding the compound of formula B to the reaction system obtained in step (3) and reacting at 100-150° C.;
[0078]
[0079] (5) Post-treating the reaction product obtained in step (4) to obtain the modified resorcinol resin.
[0080] In the present invention, the compound of formula A is added to react in step (2), and the compound of formula B is added to react in step (4), which is conducive to obtaining a suitable softening point of the resin.
[0081] In the method of the present invention, the ratio of the amount of the added resorcinol to the amount of the compound of formula A can be 1: (0.2-0.95), preferably 1: (0.3-0.7), more preferably 1: (0.4-0.65), for example 1: 0.45, 1: 0.5, 1: 0.55, 1: 0.6. The ratio of the amount of the added resorcinol to the amount of the compound of formula B can be 1: (0.05-0.7), preferably 1: (0.05-0.65), more preferably 1: (0.1-0.4), for example 1: 0.1, 1: 0.15, 1: 0.2, 1: 0.25, 1: 0.3, 1: 0.35. The ratio of the amount of the added resorcinol to the total amount of the compound of formula A and the compound of formula B can be 1:(0.5-0.9), preferably 1:(0.55-0.85), for example 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8. The ratio of the amount of the added resorcinol to the amount of the aldehyde compound can be 1:(0.5-0.7), preferably 1:(0.55-0.65), for example 1:0.55, 1:0.6.
[0082] In step (1), the acid catalysts include p-toluenesulfonic acid, methanesulfonic acid, benzenesulfonic acid, benzene disulfonic acid, dodecylbenzenesulfonic acid, hydrochloric acid, sulfuric acid, phosphoric acid, etc., preferably p-toluenesulfonic acid. The mass of the acid catalyst added in step (1) is preferably 0.2% to 1%, preferably 0.3% to 0.5% of the mass of resorcinol.
[0083] In step (1), resorcinol and p-toluenesulfonic acid can be heated at 120°C to 130°C, for example, 125°C to melt them. In step (2), the compound of formula A is preferably added dropwise. After the addition is completed, the reaction is carried out at 110°C to 130°C, for example, 125°C for 15 to 60 minutes, for example, 30 minutes. In step (2), the carbon-carbon double bonds of the compound of formula A are preferably reacted completely. In step (3), after the reaction system is cooled to 90°C to 110°C, for example, 95°C or 100°C, an aldehyde compound is added for reaction. The aldehyde compound can be provided in the form of an aldehyde compound solution. The aldehyde compound is preferably added dropwise. After the aldehyde compound is added, the reaction temperature can be 90°C to 110°C, for example, 90°C to 100°C, the reaction time can be 10 to 30 minutes, for example, 20 minutes, and water is distilled off after the reaction is completed. In step (3), the aldehyde compound is preferably reacted completely. The distillation in step (3) may be performed by first distilling at 130°C to 140°C, for example, 135°C and normal pressure for 0.5 to 1.5 hours, for example, 1 hour, and then continuing to distill at -95KPa to -100KPa, for example, -95KPa for 0.5 to 1.5 hours, for example, 1 hour. After adding the compound of formula B in step (4), the reaction is continued at 100 to 150°C, for example, 130°C, for 15 to 60 minutes, for example, 30 minutes. In step (4), the hydroxyl group of the compound of formula B is preferably reacted completely. In step (5), the post-treatment method may be to neutralize the p-toluenesulfonic acid in the reaction product obtained in step (4), and then distill out impurities such as small organic molecules and water. The terminator used for neutralization may be selected from triethanolamine, diethanolamine, N-methyldiethanolamine, alkylamine, dialkylamine, trialkylamine, NaOH, etc., preferably triethanolamine. The distillation in step (5) can be carried out at 170°C to 190°C, for example, 180°C. The distillation time can be 0.5 to 2 hours, for example, 1 hour. The vacuum degree during distillation can be -95KPa to -100KPa.
[0084] Resorcinol resin of the present invention can be used as adhesive resin in rubber, and can improve the anti-aging performance, tensile strength, bonding strength and heat generation performance of rubber. Therefore, the present invention also includes a rubber composition, which includes resorcinol resin of the present invention. The rubber composition is preferably a rubber composition used as a tire adhesive layer rubber material.
[0085] The raw materials of the rubber composition generally include diene elastomer, reinforcing filler, antioxidant and crosslinking agent. The rubber composition used as the tire adhesive layer rubber material also includes an adhesive resin and a methylene donor. The raw materials of the rubber composition of the present invention include the resorcinol resin of the present invention as an adhesive resin. Herein, the rubber composition includes unvulcanized rubber and vulcanized rubber. The unvulcanized rubber can be vulcanized rubber by vulcanization (curing).
[0086] In the raw materials of the rubber composition of the present invention, based on 100 parts by weight of the diene elastomer, the content of the reinforcing filler may be 30-70 parts by weight, the content of the antioxidant may be 0.1-8 parts by weight, the content of the crosslinking agent may be 0.5-10 parts by weight, and the content of the adhesive resin may be 1-5 parts by weight, for example, 2±0.5 parts by weight. Herein, parts by weight are calculated relative to 100 parts by weight of the diene elastomer contained in the raw materials of the rubber composition, unless otherwise specified.
[0087] Herein, diene elastomer refers to an elastomer whose monomers contain dienes (such as butadiene, isoprene). Suitable diene elastomers for the present invention can be various diene elastomers known in the art, including but not limited to one or more selected from natural rubber (NR), butadiene rubber (BR), isoprene rubber, styrene-butadiene rubber (SBR), chloroprene rubber (CR), nitrile rubber (NBR), isoprene / butadiene copolymer, isoprene / styrene copolymer and isoprene / butadiene / styrene copolymer. In some embodiments, in the raw materials of the rubber composition of the present invention, the diene elastomer is natural rubber.
[0088] The raw materials of the rubber composition of the present invention generally include 0.1-8 parts by weight, preferably 1-5 parts by weight, more preferably 2±0.5 parts by weight of an antioxidant. The antioxidant suitable for the present invention can be various antioxidants commonly used in rubber compositions, such as antioxidant 6PPD.
[0089] The reinforcing filler suitable for the present invention can be a reinforcing filler conventionally used for rubber compositions, including but not limited to one or more selected from carbon black, white carbon black, titanium oxide, magnesium oxide, calcium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, clay and talc. The raw material of the rubber composition generally comprises 30-70 parts by weight, preferably 40-60 parts by weight, more preferably 45-55 parts by weight of reinforcing filler. In some embodiments, in the rubber composition of the present invention, the reinforcing filler is carbon black and white carbon black, and the mass ratio of carbon black and white carbon black can be 4: 1 to 5: 1.
[0090] The crosslinking agent may be sulfur. The raw materials of the rubber composition generally contain 0.5-10 parts by weight, preferably 4-6 parts by weight of the crosslinking agent. In some embodiments, in the rubber composition of the present invention, the crosslinking agent is insoluble sulfur.
[0091] The methylene donor suitable for the present invention may be a methylene donor commonly used in tire adhesive layer rubber, such as hexamethoxymethyl melamine (HMMM). The raw materials of the rubber composition may contain 1-10 parts by weight, such as 1-5 parts by weight of the methylene donor.
[0092] The raw materials of the rubber composition of the present invention may also include other ingredients commonly used in rubber compositions, including but not limited to one or more of an activator, an accelerator and a cobalt salt. The amounts of the activator, the accelerator and the cobalt salt may be conventional amounts in the art.
[0093] The activator can accelerate the vulcanization speed, improve the thermal conductivity, wear resistance, tear resistance of the rubber, etc. The activator can be zinc oxide. In some embodiments, the raw materials of the rubber composition of the present invention include an activator, such as zinc oxide. The raw materials of the rubber composition of the present invention can include 0-10 parts by weight, preferably 5-10 parts by weight, for example 8±1 parts by weight of an activator, such as zinc oxide.
[0094] The accelerator is generally a vulcanization accelerator, and may be selected from sulfonamide vulcanization accelerators, thiazole vulcanization accelerators, thiuram vulcanization accelerators, thiourea vulcanization accelerators, guanidine vulcanization accelerators, dithiocarbamate vulcanization accelerators, aldehyde amine vulcanization accelerators, aldehyde ammonia vulcanization accelerators, imidazoline vulcanization accelerators and xanthate vulcanization accelerators One or more. For example, the accelerator may be accelerator DZ (N, N- dicyclohexyl -2- benzothiazole sulfonamide). In some embodiments, the raw material of the rubber composition of the present invention includes an accelerator, such as accelerator DZ. The raw material of the rubber composition of the present invention may include an accelerator of 0-2 parts by weight, preferably 1-2 parts by weight, such as 1.4 ± 0.1 parts by weight, such as accelerator DZ.
[0095] The cobalt salt may be cobalt boroacylate. The raw materials of the rubber composition of the present invention may include 0.5-2 parts by weight, such as 1±0.2 parts by weight or 1±0.1 parts by weight of a cobalt salt, such as cobalt boroacylate.
[0096] The unvulcanized rubber of the present invention can be prepared by a conventional rubber mixing method, for example, by a two-stage mixing method: one stage of mixing in an internal mixer, mixing the diene elastomer, reinforcing filler, activator, antioxidant, cobalt salt and adhesive resin to obtain a masterbatch, and the mixing temperature can be 150±10°C; and the second stage of mixing in an open mixer, mixing the masterbatch obtained in the first stage, the crosslinking agent, the accelerator and the methylene donor to obtain the unvulcanized rubber, and the mixing temperature can be 90-100°C.
[0097] The unvulcanized rubber of the present invention can be vulcanized by conventional vulcanization methods to obtain vulcanized rubber. The vulcanization temperature is usually 130°C-200°C, such as 150±2°C, 160±2°C. The vulcanization time depends on the vulcanization temperature, the vulcanization system and the vulcanization kinetics, and is usually 15-60 minutes, such as 25-35 minutes. Before vulcanization, the kneaded unvulcanized rubber can be conventionally sheeted.
[0098] The present invention also provides a rubber product, part or all of which is the rubber composition described in any embodiment of the present invention, or is prepared from the rubber composition described in any embodiment of the present invention. The rubber product can be a tire, a rubber shoe, a sealing strip, a sound insulation board, a shock-absorbing pad, etc. In certain embodiments, the rubber product is a tire, and the adhesive layer rubber material of the tire is the rubber composition described in any embodiment of the present invention.
[0099] The present invention achieves the following beneficial technical effects: the resorcinol resin modified by the composite of N-(hydroxymethyl)acrylamide and styrene of the present invention can significantly reduce the compression heat generation of the rubber composition, improve the rubber attachment rate, and significantly improve the tensile properties and steel cord adhesion properties of the rubber composition before and after thermal oxidation aging and salt water aging; at the same time, the resorcinol resin modified by the composite of N-(hydroxymethyl)acrylamide and styrene of the present invention has a low free phenol content and a suitable softening point, and has good environmental protection and processability.
[0100] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0101] In the present invention, the free resorcinol content of the resin is determined by high performance liquid chromatography.
[0102] In the present invention, the softening point of the prepared resin is determined by the ring and ball method:
[0103] Principle: Place a steel ball of specified weight on a metal ring filled with the sample, heat the assembly at a constant heating rate, and when the sample softens and falls to a specified distance under the action of the steel ball's gravity, the temperature is taken as the softening point.
[0104] Instruments: softening point tester, thermometer (division value is 0.1℃, length is about 300mm), electric furnace and voltage regulator, porcelain plate or glass plate, evaporator with handle (50ml), flat knife, heat transfer liquid (glycerol).
[0105] Sample preparation:
[0106] 1. Place the ring on a porcelain or glass plate coated with a small amount of glycerin;
[0107] 2. Take about 5g of the sample, place it in a 50ml handle evaporator, heat and melt it on an electric stove and stir it continuously to prevent local overheating. The heating temperature must not be higher than the estimated softening point of the sample by 40℃. Inject the sample into the copper ring until it is slightly above the ring surface;
[0108] 3. After the sample has cooled for about 30 minutes at ambient temperature, use a hot knife to scrape off the portion of the sample that protrudes above the ring surface to make it flush with the ring surface.
[0109] Determination steps:
[0110] 1. Place the heater bath containing glycerin on an electric furnace and heat it to a temperature 50°C lower than the estimated softening point of the sample, and keep the temperature constant for 10 to 15 minutes;
[0111] 2. Place the copper ring containing the sample horizontally in the round hole of the ring stand, put on the steel ball positioner, place the steel ball on the sample, and then put the sample stand into the heating bath. The glycerin bath surface should be slightly lower than the depth mark on the connecting rod, and there should be no bubbles in any part of the ring stand;
[0112] 3. Insert the thermometer vertically through the center hole of the upper bearing plate so that the bottom of the mercury ball and the bottom of the ring are at the same level;
[0113] 4. Heat the oil bath so that the glycerol temperature rises by 3±0.5℃ per minute after 3 minutes. If the heating rate exceeds this range, the test should be repeated;
[0114] 5. The sample is softened by heat. Under the action of the gravity of the steel ball, the temperature at which the sample and the steel ball fall together and contact the bottom plate surface is the softening point of the sample. The arithmetic mean of the results of two repeated measurements is taken as the measurement result.
[0115] Example 1
[0116] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottom reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, and the mixture was heated to 125° C. to melt. Then, 52 g (0.5 mol) of styrene was added dropwise over 1.2 hours. After the addition was completed, the temperature was maintained at 125° C. for 30 minutes. After the temperature was lowered to 95° C., 44.64 g (0.55 mol) of a 37% formaldehyde solution was added dropwise over a period of 1 hour. After the addition was completed, the reaction was continued at 90-100° C. for 20 minutes to complete the reaction. After the reaction was completed, the temperature was raised to 130° C., water was distilled at normal pressure for 1 hour, and distillation was continued at -95 KPa for 1 hour. Then, 0.2 mol of N-(Hydroxymethyl)acrylamide was reacted at 130°C for 30 minutes, and the acid catalyst was neutralized with 0.52g of triethanolamine, and then the temperature was raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa), to obtain 183.7g of resorcinol resin modified by N-(hydroxymethyl)acrylamide and styrene. The obtained resin had a softening point of 97.5°C and a free resorcinol content of 1.04%.
[0117] Example 2
[0118] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottom reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, and the mixture was heated to 125° C. to melt. Then, 52 g (0.5 mol) of styrene was added dropwise over 1.2 hours. After the addition was completed, the temperature was kept at 125° C. for 30 minutes. After the temperature was lowered to 95° C., 48.7 g (0.60 mol) of a 37% formaldehyde solution was added dropwise over a period of 1 hour. After the addition was completed, the reaction was continued at 90-100° C. for 20 minutes to complete the reaction. After the reaction was completed, the temperature was raised to 130° C., water was distilled at normal pressure for 1 hour, and distillation was continued at -95 KPa for 1 hour. Then, 0.2 mol of N-(Hydroxymethyl)acrylamide was reacted at 130°C for 30 minutes, and the acid catalyst was neutralized with 0.52g of triethanolamine, and then the temperature was raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa) to obtain 184.3g of resorcinol resin modified by N-(hydroxymethyl)acrylamide and styrene. The obtained resin had a softening point of 105.4°C and a free resorcinol content of 0.73%.
[0119] Example 3
[0120] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottom reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, and the mixture was heated to 125° C. to melt. Then, 62.4 g (0.6 mol) of styrene was added dropwise over 1.2 hours. After the addition was completed, the temperature was maintained at 125° C. for 30 minutes. After the temperature was lowered to 95° C., 44.64 g (0.55 mol) of a 37% formaldehyde solution was added dropwise over a period of 1 hour. After the addition was completed, the reaction was continued at 90-100° C. for 20 minutes to complete the reaction. After the reaction was completed, the temperature was raised to 130° C., water was distilled at normal pressure for 1 hour, and distillation was continued at -95 KPa for 1 hour. Then, 0.1 mol of N-(Hydroxymethyl)acrylamide was reacted at 130°C for 30 minutes, and the acid catalyst was neutralized with 0.52g of triethanolamine, and then the temperature was raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa), to obtain 186g of resorcinol resin modified by N-(hydroxymethyl)acrylamide and styrene. The obtained resin had a softening point of 95.0°C and a free resorcinol content of 0.84%.
[0121] Example 4
[0122] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottomed reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, and the mixture was heated to 125° C. to melt. Then, 62.4 g (0.6 mol) of styrene was added dropwise over 1.2 hours. After the addition was completed, the temperature was maintained at 125° C. for 30 minutes. After the temperature was lowered to 95° C., 48.7 g (0.6 mol) of a 37% formaldehyde solution was added dropwise over a period of 1 hour. After the addition was completed, the reaction was continued at 90-100° C. for 20 minutes to complete the reaction. After the reaction was completed, the temperature was raised to 130° C., water was distilled at normal pressure for 1 hour, and distillation was continued at -95 KPa for 1 hour. Then, 0.2 mol of N-(Hydroxymethyl)acrylamide was reacted for 30 minutes at 130°C, and the acid catalyst was neutralized with 0.52g of triethanolamine, and then the temperature was raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa), to obtain 194.9g of resorcinol resin modified by N-(Hydroxymethyl)acrylamide and styrene. The obtained resin had a softening point of 107.3°C and a free resorcinol content of 0.53%.
[0123] Example 5
[0124] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottom reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, and the mixture was heated to 125° C. to melt. Then, 52 g (0.5 mol) of styrene was added dropwise over 1.2 hours. After the addition was completed, the temperature was kept at 125° C. for 30 minutes. After the temperature was lowered to 95° C., 52.76 g (0.65 mol) of a 37% formaldehyde solution was added dropwise over a period of 1 hour. After the addition was completed, the reaction was continued at 90-100° C. for 20 minutes to complete the reaction. After the reaction was completed, the temperature was raised to 130° C., water was distilled at normal pressure for 1 hour, and distillation was continued at -95 KPa for 1 hour. Then, 0.1 mol of N-(Hydroxymethyl)acrylamide was reacted for 30 minutes at 130°C, and the acid catalyst was neutralized with 0.52g of triethanolamine, and then the temperature was raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa), to obtain 176.1g of resorcinol resin modified by N-(Hydroxymethyl)acrylamide and styrene. The obtained resin had a softening point of 112.0°C and a free resorcinol content of 0.88%.
[0125] Example 6
[0126] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottom reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, and the mixture was heated to 125° C. to melt. Then, 41.6 g (0.4 mol) of styrene was added dropwise within 1 hour. After the addition was completed, the temperature was kept at 125° C. for 30 minutes. After the temperature was lowered to 95° C., 48.7 g (0.6 mol) of a 37% formaldehyde solution was added dropwise. The addition time was 1 hour. After the addition was completed, the reaction was continued at 90-100° C. for 20 minutes to complete the reaction. After the reaction was completed, the temperature was raised to 130° C., and water was distilled at normal pressure for 1 hour. After the distillation was continued at -95 KPa for 1 hour, 0.3 mol of the mixture was added. N-(Hydroxymethyl)acrylamide was reacted for 30 minutes at 130°C, and the acid catalyst was neutralized with 0.52g triethanolamine, and then the temperature was raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa), to obtain 181.9g of resorcinol resin modified by N-(hydroxymethyl)acrylamide and styrene. The obtained resin had a softening point of 109.6°C and a free resorcinol content of 1.12%.
[0127] Comparative Example 1
[0128] 110 g (1.0 mol) of resorcinol and 0.6 g (3.5 mmol) of p-toluenesulfonic acid were added to a 500 mL four-necked round-bottom reaction flask equipped with a stirrer, a reflux condenser and a dropping funnel, heated to 125°C to melt, and then 52 g (0.5 mol) of styrene was added dropwise over 1.2 hours. After the addition was completed, the temperature was kept at 125°C for 30 minutes, and then 0.2 mol of N-(hydroxymethyl) acrylamide was reacted for 1 hour, and after cooling to 95°C, 44.64g (0.55mol) of 37% formaldehyde solution was added dropwise for 1 hour. After the addition was completed, the reaction was continued at 90-100°C for 20 minutes to complete the reaction. After neutralizing the acid catalyst with 0.52g triethanolamine, the temperature was raised to 160°C and distilled under normal pressure for 1 hour, and then the temperature was continued to be raised to 180°C and distilled under reduced pressure for 1 hour (vacuum degree -95KPa) to obtain a resorcinol resin compositely modified by N-(hydroxymethyl) acrylamide and styrene. The obtained resin had a softening point of 133.1°C and a free resorcinol content of 0.73%.
[0129] Comparative Example 2
[0130] In a 500mL four-mouth round-bottomed reaction flask equipped with agitator, reflux condenser and dropping funnel, 110g (1.0mol) of resorcinol and 0.6g (3.5mmol) of p-toluenesulfonic acid were added, and after being heated to 125°C and melted, 48.7g (0.6mol) of 37% formaldehyde solution was dropwise added, and the dropping time was 1 hour. After the dropwise addition was completed, the mixture was kept warm for 15-20 minutes. After the reaction was completed, the mixture was warmed up to 130°C, and water was distilled under normal pressure for 1 hour. Under -95KPa, distillation was continued for 1 hour. Then 0.7mol of N-(hydroxymethyl) acrylamide was added and the reaction was continued for 2 hours. After neutralizing the acidic catalyst with 0.52g of triethanolamine, the mixture was warmed up to 160°C of normal pressure distilled water for 1 hour. The mixture was continued to be warmed up to 180°C of reduced pressure distillation for 1 hour (vacuum degree -95KPa) to obtain N-(hydroxymethyl) acrylamide-modified resorcinol resin. The obtained resin had a softening point of 118.5°C and a free resorcinol content of 1.36%.
[0131] Comparative Example 3
[0132] 110g (1.0mol) of resorcinol and 0.6g (3.5mmol) of p-toluenesulfonic acid were added to a 500mL four-mouth round-bottomed reaction flask equipped with an agitator, a reflux condenser and a dropping funnel, heated to 125°C for melting, then 72.8g (0.7mol) of styrene was added dropwise within 1 hour, kept at 125°C for 30 minutes after the addition was completed, 48.7g (0.6mol) of a 37% formaldehyde solution was added dropwise after the temperature was lowered to 95°C, and the addition time was 1 hour. After the addition was completed, the reaction was continued at 90-100°C for 20 minutes, and the acid catalyst was neutralized with 0.52g of triethanolamine, and then the temperature was raised to 160°C for atmospheric distillation for 1 hour, and the temperature was further raised to 180°C for reduced pressure distillation for 1 hour (vacuum degree -95KPa), to obtain a styrene-modified resorcinol resin. The resulting resin had a softening point of 102.9°C and a free resorcinol content of 0.91%.
[0133] Test Example 1
[0134] The N-(hydroxymethyl)acrylamide and styrene composite modified resorcinol resin of Example 1 and the styrene modified resorcinol resin of Comparative Example 3 were tested by infrared spectroscopy. The results are as follows: Figures 1 to 3 shown.
[0135] After N-(hydroxymethyl) acrylamide undergoes a dehydration reaction with the resin, the nitrogen methyl group is connected to the aromatic ring of the resin. Figure 3 The infrared test results of the resin before and after modification with N-(hydroxymethyl)acrylamide show that there are two obvious absorption signal peaks after modification, among which 1654.94 cm -1The absorption peak at 1739.14cm is the characteristic absorption peak of the carbonyl group in the amide structure. Because the carbonyl group and double bond of the amide in the acrylamide structure introduced by the resin side chain are conjugated, the π electron delocalization increases, the performance of the carbon-oxygen double bond decreases, and the vibration frequency decreases, so the absorption peak moves to a lower wave number; and the carbon-carbon double bond increases the vibration frequency due to the effect of the carbonyl group, and the absorption peak moves to a higher wave number, so 1739.14cm -1 The characteristic absorption of the terminal double bond is at 3100~3400cm; and compared with the simple styrene-modified resin, the N-(hydroxymethyl) acrylamide-modified -1 The absorption signal at (characteristic absorption peak under the phenolic hydroxyl group association state) is significantly enhanced, which is due to the superposition of the stretching vibration of the amide NH bond in this range. In summary, it can be seen that N-(hydroxymethyl)acrylamide is successfully introduced into the resin side end through dehydration.
[0136] Application Examples
[0137] According to the formulation shown in Table 1, rubber compositions 1-8 were prepared using the resorcinol resins of Examples 1-6 and Comparative Examples 2-3, respectively:
[0138] The rubber material adopts a two-stage mixing process. The first stage of mixing is carried out in a Banbury internal mixer, and natural rubber, carbon black, zinc oxide, white carbon black, cobalt salt, antioxidant 6PPD are added, and the resorcinol resin prepared in Examples 1-6 and Comparative Examples 2-3 are respectively added as adhesive resins, and the mixing (draining) temperature is 150°C; the second stage of mixing is carried out on an X(S)K-160 open mill, and the masterbatch obtained in the first stage, insoluble sulfur, accelerator DZ and methylene donor HMMM (containing 65wt% of HMMM and 35wt% of SiO2) are added, and the mixing temperature is 90-100°C; finally, the prepared rubber composition is molded on a flat vulcanizer to test the physical properties, mechanical properties and steel wire bonding properties, and the vulcanization conditions are 160°C×30min.
[0139] Table 1: Rubber composition formula (unit: mass parts)
[0140]
[0141]
[0142] Test Example 2
[0143] The properties of rubber compositions 1-8 were tested according to the following performance test method, and the results are shown in Table 2:
[0144] The vulcanization characteristics are determined with reference to GB / T 16584-1996 and GB / T 1233-2008; in an oscillating disc rheometer, the rubber sample is subjected to an oscillating shear force of constant amplitude, and the torque of the oscillating mesh disc embedded in the rubber sample at the vulcanization temperature is measured.
[0145] The mechanical properties are tested according to the standard of GB / T 528-2009; the larger the mechanical property value, the greater the degree of cross-linking of the rubber and the better the mechanical properties.
[0146] The tear strength is tested according to the method of GB / T 529-2008; a tensile testing machine is used to continuously stretch a sample with or without a cut at a specified speed until the maximum force required to tear the sample is reached. The larger the value, the better the tear resistance of the rubber.
[0147] The Shore hardness of the vulcanized rubber is measured according to standard GB / T 531.1-2008; the greater the hardness value, the higher the rigidity of the rubber composition.
[0148] The thermal oxidation aging test was carried out according to GB / T 3512-2014, and the aging conditions are shown in Table 2.
[0149] The salt water aging experiment was carried out according to GB / T 35858-2018, and the aging conditions are shown in Table 2.
[0150] The wire pull-out force is measured according to standard ASTM D 2229-2002; it tests the force of pulling a single steel cord out of the embedded rubber in the axial direction. The larger the value, the higher the bonding strength.
[0151] The compression heat generation is measured with reference to the test standard ISO4666-4-2007. The test conditions are constant temperature of 55°C, preheating time of 30 minutes, test time of 25 minutes, static load of 100N, dynamic load of 700N, and frequency of 10HZ.
[0152] Table 2: Rubber composition performance test results
[0153]
[0154]
[0155] According to Table 2, compared with other rubber compositions, the rubber composition 7 using only resorcinol resin modified with N-(hydroxymethyl) acrylamide (Comparative Example 2) as the adhesive resin has a larger Mooney viscosity and a shorter vulcanization scorch time, but the mechanical properties of the rubber and the steel wire bonding performance before and after aging are relatively excellent.
[0156] Compared with the rubber composition 8 using the resorcinol formaldehyde adhesive resin modified only with styrene (Comparative Example 3), the compression heat generation of the rubber composition 1-6 using the resorcinol resin modified by N-(hydroxymethyl)acrylamide and styrene composite prepared in Examples 1-6 is significantly reduced, and the adhesive rate is improved, indicating that the double bonds introduced after the dehydration of N-(hydroxymethyl)acrylamide and the resin can participate in the vulcanization of the rubber, so that the resin and rubber form an interpenetrating and bonded cross-linked network, which effectively limits the movement and friction between rubber molecules, thereby reducing the heat generation performance, so it shows lower compression heat generation and higher adhesive rate.
[0157] Compared with the rubber composition 8 using the resorcinol formaldehyde adhesive resin modified only with styrene (Comparative Example 3), the tensile properties, steel cord adhesion and anti-aging properties of the rubber composition 1-6 using the resorcinol resin modified by N-(hydroxymethyl) acrylamide and styrene prepared in Example 1-6 are effectively improved. This may be mainly because compared with the resorcinol resin modified by styrene, the composite modified resin prepared in Example 1-6 introduces an amide group, which increases the polarity of the resin, so the migration rate in the rubber compound will be faster, so it can be more enriched on the surface where the rubber and the steel cord contact before vulcanization. During the vulcanization process, the cross-linking density of the resin layer generated at the bonding interface layer formed by the rubber and the steel cord is larger, and the vulcanization bonding action of the double bond also makes the entanglement degree of the resin network and the rubber network higher. Therefore, compared with Comparative Example 3, the composite modified resin of Example 1-6 shows higher adhesion, better tensile strength and better aging resistance.
Claims
1. A modified resorcinol resin, It is characterized in that The modified resorcinol resin includes a structural unit shown in formula I, a structural unit shown in formula II, and a structural unit shown in formula III: Wherein, p is an integer selected from 0 to 5, each R 1 Independently selected from C1-C6 alkyl and C1-C6 alkoxy; R 2 The group consisting of C2-C10 straight chain alkenyl, C3-C10 branched chain alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond.
2. The modified resorcinol resin according to claim 1, It is characterized in that In the structural unit represented by formula I, p is 0; and / or in the structural unit represented by formula II, R 2 For vinyl.
3. The modified resorcinol resin according to claim 1, It is characterized in that The modified resorcinol resin has one or more of the following characteristics: In the modified resorcinol resin, the amount of the structural unit represented by formula I accounts for 20% to 95%, preferably 30% to 70%, more preferably 40% to 65%, for example 50% to 60%, of the total amount of the structural unit represented by formula I, the structural unit represented by formula II and the structural unit represented by formula III; In the modified resorcinol resin, the amount of the structural unit represented by formula II accounts for 5% to 70% of the total amount of the structural unit represented by formula I, the structural unit represented by formula II and the structural unit represented by formula III, preferably 5% to 65%, more preferably 10% to 40%, for example 10% to 30%; In the modified resorcinol resin, the total amount of the structural units represented by formula I and the structural units represented by formula II accounts for 50% to 90%, preferably 55% to 85%, for example 60% to 80% of the total amount of the structural units represented by formula I, the structural units represented by formula II and the structural units represented by formula III; In the monomers of the modified resorcinol resin, the molar ratio of resorcinol to aldehyde compound is 1:(0.5-0.7), preferably 1:(0.55-0.65), for example 1:(0.55-0.6).
4. The modified resorcinol resin according to claim 1, It is characterized in that The softening point of the modified resorcinol resin is 90° C. to 115° C., for example, 95° C. to 112° C.; and / or The free phenol content of the modified resorcinol resin is ≤1.5 wt %, preferably ≤1.2 wt %, more preferably ≤1 wt %.
5. A method for preparing the modified resorcinol resin according to any one of claims 1 to 4, It is characterized in that The method comprises the following steps: (1) providing a mixture of molten resorcinol and an acid catalyst; (2) Adding the compound of formula A to the mixture of step (1) and reacting at 110-130° C., wherein p is an integer selected from 0 to 5, and each R 1 Independently selected from C1-C6 alkyl and C1-C6 alkoxy; (3) cooling the reaction system obtained in step (2) to 90-110° C., adding an aldehyde compound, and reacting, and distilling off water after the reaction is completed; (4) Add the compound of formula B to the reaction system obtained in step (3) and react at 100-150° C., wherein R 2 is selected from C2-C10 straight-chain alkenyl, C2-C10 branched alkenyl, C5-C10 alicyclic alkenyl, C6-C10 aromatic alkenyl, C5-C10 heterocyclic alkenyl and C5-C10 heteroaromatic cyclic alkenyl containing a carbon-carbon double bond; (5) Post-treating the reaction product obtained in step (4) to obtain the modified resorcinol resin.
6. The method according to claim 5, It is characterized in that The method has one or more of the following features: The compound of formula A is styrene; The aldehyde compound is selected from one or more of formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, valeraldehyde, hexanal, benzaldehyde and furfural, preferably formaldehyde; The compound of formula B is N-(hydroxymethyl)acrylamide; The ratio of the amount of resorcinol added in the method to the amount of the compound of formula A is 1:(0.2-0.95), preferably 1:(0.3-0.7), more preferably 1:(0.4-0.65), for example 1:(0.5-0.6); The ratio of the amount of resorcinol added in the method to the amount of the compound of formula B is 1:(0.05-0.7), preferably 1:(0.05-0.65), more preferably 1:(0.1-0.4), for example 1:(0.1-0.3); The ratio of the amount of resorcinol added in the method to the total amount of the compound of formula A and the compound of formula B is 1:(0.5-0.9), preferably 1:(0.55-0.85), more preferably 1:(0.6-0.8); The molar ratio of resorcinol to aldehyde compound added in the method is 1:(0.5-0.7), preferably 1:(0.55-0.65), for example 1:(0.55-0.6).
7. The method according to claim 5, It is characterized in that In step (1), the acid catalyst is selected from one or more of p-toluenesulfonic acid, methanesulfonic acid, benzenesulfonic acid, benzene disulfonic acid, dodecylbenzenesulfonic acid, hydrochloric acid, sulfuric acid and phosphoric acid, preferably p-toluenesulfonic acid; The mass of the acid catalyst added in step (1) is 0.2% to 1% of the mass of resorcinol, preferably 0.3% to 0.5%; The reaction time in step (2) is 15 to 60 minutes; In step (3), after adding the aldehyde compound, the reaction is continued at 90 to 110° C. for 10 to 30 minutes; The reaction time in step (4) is 15 to 60 minutes; The post-treatment in step (5) comprises: neutralizing the p-toluenesulfonic acid in the reaction product obtained in step (4), and then distilling out impurities; preferably, the terminator used for neutralization is selected from one or more of triethanolamine, diethanolamine, N-methyldiethanolamine, alkylamine, dialkylamine, trialkylamine and NaOH, preferably triethanolamine.
8. A rubber composition, It is characterized in that The rubber composition comprises the modified resorcinol resin according to any one of claims 1 to 4; Preferably, the rubber composition further comprises a diene elastomer; preferably, based on 100 parts by weight of the diene elastomer, the content of the modified resorcinol resin in the rubber composition is 1 to 5 parts by weight.
9. A tire, It is characterized in that The adhesive layer rubber material of the tire is the rubber composition according to claim 8.
10. Use of the modified resorcinol resin according to any one of claims 1 to 4 for improving the tensile strength, adhesive strength, aging resistance and / or heat generation performance of rubber.