A polylactic acid material and its preparation method and application

By combining levopolylactic acid and dextropolylactic acid co-crystalline with fiber assembly, an orderly layered structure is formed, which solves the problem of low efficiency of polylactic acid materials in tooth whitening applications, and achieves efficient catalytic pigment degradation and safe teeth Whitening effect.

CN118725532BActive Publication Date: 2024-12-06SICHUAN UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411170418.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing polylactic acid materials are too low in efficiency in teeth whitening applications, and have problems such as high tissue irritation and uncontrolled release of active substances, making it difficult to meet the needs of safe and efficient teeth whitening.

Method used

By co-crystallizing levopolylactic acid and dextropolylactic acid to form a stereocomplex sheet crystal and combining it with the fiber assembly to form an ordered layered structure. The porous structure is constructed with a porous agent to improve stress sensitivity and piezoelectric catalytic efficiency .

Benefits of technology

It achieves efficient catalytic pigment degradation, avoids tooth sensitivity and structural damage, and provides a safe and efficient tooth whitening material with significant teeth whitening effects and excellent piezoelectric catalytic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725532B_ABST
    Figure CN118725532B_ABST
Patent Text Reader

Abstract

The present invention discloses a polylactic acid material and a preparation method and application thereof, which belongs to the technical field of polylactic acid materials and solves the problem of low efficiency of polylactic acid materials in the prior art for whitening teeth. In the polylactic acid material provided by the present invention, polylactic acid lamellae are vertically stacked on the surface of a fiber assembly to form an ordered layered structure, and there is a cavity between two adjacent lamellae on the ordered layered structure; and the polylactic acid lamellae contain left-handed polylactic acid lamellae and right-handed polylactic acid lamellae. The polylactic acid material provided by the present invention can not only effectively capture low-frequency mechanical energy such as daily brushing and thus promote the generation of piezoelectric charges, but also enhance the separation and transmission of piezoelectric charges, so that it exhibits high piezoelectric catalytic activity and has the ability to efficiently catalyze the degradation of pigments under the action of brushing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polylactic acid materials, and more specifically to a polylactic acid material and a preparation method and application thereof. Background Art

[0002] In daily life, strong tea, coffee, beverages, red wine, soy sauce and other foods can absorb pigments on the surface of teeth, leading to pigment deposition; in addition, tobacco, drugs (such as antibiotics), tooth development defects, dental plaque, caries and other factors can also cause tooth discoloration (even the inside of the teeth is penetrated by discolored substances). Ordinary cleaning and care methods such as brushing and washing teeth can only remove pigments and plaque with weak adhesion on the surface of teeth, but cannot remove pigments inside the teeth. For most tooth discoloration problems, professional teeth whitening materials are needed to achieve the effect of whitening teeth.

[0003] The main components of existing teeth whitening materials are hydrogen peroxide or carbamide peroxide. The whitening principle is to release active oxygen and other free radicals that can penetrate into the teeth to achieve oxidative degradation of pigment molecules, making the teeth whiter. However, hydrogen peroxide whitening has problems such as high tissue irritation and poor controllability of active substance release (such as violent release at high concentrations), which can easily cause side effects such as gum damage and atrophy, tooth sensitivity, and enamel damage. Therefore, it is urgent to develop a safer, controllable, and efficient new method for teeth whitening.

[0004] Polylactic acid (PLA) is a biodegradable piezoelectric polymer material with a large number of carbonyl (C=O) electroactive groups on the main chain. It has excellent properties such as good biocompatibility, absorbability, and non-toxicity. It has been widely used in biomedical fields such as tissue repair, vascular stents, and drug sustained release. However, due to the 10 3 The helical conformation causes the C=O bond moments to cancel each other out and the electrical activity is low, resulting in too low piezoelectric catalytic activity; at the same time, the high elastic modulus makes its stress sensitivity weak, and high-frequency and high-energy external forces are required to induce catalysis, which is difficult to meet the practical application needs of tooth whitening. The prior art discloses a method of reducing the offset of dipole moments and improving electrical activity through stereocomplex crystallization, using porogens to construct a porous structure to improve stress sensitivity, and then obtaining a porous polylactic acid material that can activate the piezoelectric catalytic effect under low-frequency and low-energy external forces. However, although the polylactic acid material using this method can achieve tooth whitening, due to disordered crystallization (the lamellae are randomly arranged), it is not conducive to efficiently capturing stress and generating abundant piezoelectric active charges. At the same time, the separation and migration rate of the charges are slow, which ultimately makes the piezoelectric catalytic efficiency low. Therefore, the efficiency of tooth whitening is still relatively low, and it is urgent to develop a new green and safe PLA piezoelectric catalytic material that can achieve efficient tooth whitening. Summary of the invention

[0005] The present invention provides a polylactic acid material and a preparation method and application thereof, so as to solve the problem that the efficiency of the polylactic acid material in the prior art for whitening teeth is too low.

[0006] In the first aspect, the present invention provides a polylactic acid material, including polylactic acid flakes and a fiber assembly; the polylactic acid flakes are vertically stacked on the surface of the fiber assembly to form an ordered layered structure, and there is a cavity between two adjacent layers on the ordered layered structure; the polylactic acid flakes are stereocomposite flakes formed by co-crystallization of left-handed polylactic acid and right-handed polylactic acid.

[0007] As a possible implementation, the mass ratio of the polylactic acid platelets to the fiber assembly is 100:0.1 to 0.7; the mass ratio of the left-handed polylactic acid to the right-handed polylactic acid is 40 to 60:40 to 60. The fiber assembly is an organic compound that can be dissolved in the polylactic acid melt, self-assembled to form an assembly during the melt cooling process, and induce the left-handed polylactic acid / right-handed polylactic acid (PLLA / PDLA) molecular chains to crystallize and co-crystallize on its surface; in addition to the nucleation function, the fiber assembly also has the function of regulating the orderly arrangement of crystals and promoting charge separation.

[0008] As a possible implementation method, the piezoelectric constant (d 33 ) is 30 ~ 44 pC / N.

[0009] As a possible implementation method, the fiber assembly is one or a combination of 1,3,2,4-dibenzylidene sorbitol, di(3,4-dimethyldibenzylidene) sorbitol, N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide, adipic acid dibenzohydrazide, sebacic acid dibenzohydrazide, and aromatic diformamide.

[0010] In a second aspect, the present invention provides a method for preparing the polylactic acid material described in any possible implementation of the first aspect, comprising the following steps: uniformly mixing the left-handed polylactic acid, the right-handed polylactic acid, the fiber assembly and the porogen at room temperature, and then melt-blending them at 180 to 230° C. to obtain a blend; and removing the porogen from the blend to obtain the polylactic acid material.

[0011] Exemplarily, the method for removing the porogen in the blend is: soaking the blend in deionized water, washing with deionized water, and then performing a vacuum drying operation.

[0012] As a possible implementation, the porogen is one or a combination of polyethylene glycol (PEG), polyvinyl acetate (PVAc) or polyvinyl pyrrolidone (PVP); and / or, the mass ratio of the porogen to the fiber assembly is 30-50:0.1-0.7. The porogen is a water-soluble polymer that has good compatibility with both PLLA and PDLA. The porogen is basically compatible when PLLA / PDLA is in a molten state, but phase separation occurs when PLLA / PDLA crystallizes, thereby forming a narrow and long pore structure between the lamellae, so that the lamellae form a regular layered structure.

[0013] As a possible implementation method, the weight average molecular weight of the L-polylactic acid is 5×10 4 ~ 3×10 5 g / mol, optical purity ≥92%; and / or the weight average molecular weight of the dextrorotatory polylactic acid is 5×10 4 ~ 3×10 5 g / mol, optical purity ≥92%; and / or, the purity of the fiber assembly ≥99%.

[0014] In a third aspect, the present invention provides an application of the polylactic acid material described in any possible implementation of the first aspect or the preparation method described in any possible implementation of the second aspect in teeth cleaning.

[0015] As a possible implementation method, the polylactic acid material is used to catalyze the degradation of pigments.

[0016] As a possible implementation, the polylactic acid material is used to prepare a tooth cleaner. Exemplarily, the tooth cleaner is in the form of a paste, powder, gel, solution or solid dispersion; Exemplarily, the polylactic acid material is used to prepare toothpaste, tooth powder, gel, cleaning solution or glue stick.

[0017] In the polylactic acid material provided by the present invention, the basic microstructure characteristics of the material are: the small molecule fiber assembly induces the polylactic acid lamellae to grow vertically on its surface to form an ordered layered structure, and there is a cavity between two adjacent lamellae on the ordered layered structure. The polylactic acid material can effectively capture low-frequency mechanical energy such as daily brushing to promote the generation of piezoelectric charges, and can also enhance the separation and transmission of piezoelectric charges, so that it exhibits high piezoelectric catalytic activity and has the ability to efficiently catalyze the degradation of pigments under the action of brushing.

[0018] Piezoelectric catalysis is an advanced oxidation technology that uses the polarized charge generated by piezoelectric materials under external stimulation to react with water and oxygen to generate hydroxyl radicals (·OH) and superoxide ions (·O 2- ) and singlet oxygen ( 1O 2 ) and other reactive oxygen species (ROS), achieving efficient oxidative degradation of organic pigment molecules such as methylene blue and tannic acid. At the same time, the concentration of ROS generated by piezoelectric catalysis is controllable (the generation of ROS can be controlled by regulating external force to avoid violent release of high concentration), and it is highly safe. In addition, the ROS generated by piezoelectric catalysis can also eliminate harmful oral bacteria, providing a new option for oral plaque control and other disease prevention and treatment. The polylactic acid material provided by the present invention, whose main components are PLLA and PDLA with good biocompatibility and complete biodegradability, is non-toxic and harmless when used; it is environmentally friendly after use and will not cause pollution; at the same time, the organic small molecules used in the present invention are also non-toxic and harmless, and will not damage the tooth structure; the polylactic acid material provided by the present invention is used for tooth whitening treatment, and there is no risk of heavy metal ion release and no Ba 2+ etc. may be related to Ca 2+ The elements that undergo ion exchange avoid damage to tooth enamel and further avoid the threat to health caused by it; the polylactic acid material provided by the present invention is a safe and efficient tooth whitening material and has great application advantages in the field of tooth whitening.

[0019] The preparation method of the polylactic acid material provided by the present invention uses a fiber assembly to control the orderly stacking of the lamellae, promote charge separation, and act as a nucleating agent; a cavity between two lamellae is obtained by means of a porogen, so that the lamellae form a regular layered structure. The preparation method of the present invention has a simple operation process and is efficient, and is suitable for industrial-scale production and preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 Scanning electron microscope (SEM) images of polylactic acid material IV (a), polylactic acid material I (b), polylactic acid material II (c) and polylactic acid material III (d) provided in embodiments of the present invention.

[0022] Figure 2 The curves of the pigment concentration variation over time of different polylactic acid materials under piezoelectric catalytic pigment degradation conditions provided by the embodiments of the present invention, wherein the unit of time is minute (min).

[0023] Figure 3 The whitening ability of the polylactic acid material I provided in an embodiment of the present invention on stained teeth, wherein the left picture is before whitening, and the right picture is after whitening. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In order to solve the problem of low efficiency of polylactic acid materials in the prior art for whitening teeth, an embodiment of the present invention provides a polylactic acid material and a preparation method and application thereof.

[0026] The embodiment of the present invention provides a preparation experiment of a polylactic acid material and provides a comparative experiment of its microstructure observation. It can be seen that the basic microstructural characteristics of the polylactic acid material prepared by the present invention are: the fiber assembly induces the polylactic acid lamellae to grow perpendicular to its surface to form an ordered layered structure, and there is a cavity between two adjacent layers on the ordered layered structure. It can efficiently capture stress and generate abundant piezoelectric active charges, while the charge separation and migration rates are fast, and the piezoelectric catalytic efficiency is high.

[0027] Furthermore, the embodiments of the present invention provide a verification experiment of the pigment degradation ability of the polylactic acid material. It can be seen that the polylactic acid material provided by the embodiments of the present invention exhibits excellent pigment degradation ability.

[0028] Furthermore, the embodiment of the present invention provides an application effect verification experiment of the polylactic acid material, and it can be known that the polylactic acid material provided by the embodiment of the present invention has a significant teeth whitening effect.

[0029] The technical solution of the present invention will be further described below in conjunction with specific embodiments. Example 1

[0030] This embodiment provides a preparation experiment of a polylactic acid material.

[0031] The weight average molecular weight was 7.0×10 4 g / mol and 7.0×10 4 g / mol PLLA and PDLA were vacuum dried at 60°C; then 50 parts by weight of PLLA, 50 parts by weight of PDLA, 0.2 parts by weight of N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide, and 40 parts by weight of PEG (weight average molecular weight 20000 g / mol) were uniformly mixed and added into a melt mixer, melt blended at 200°C for 6 min, and naturally cooled to obtain an initial blend I; finally, the initial blend I was fully washed with deionized water to remove the PEG phase therein, and dried to obtain polylactic acid material I. Example 2

[0032] This embodiment provides a preparation experiment of a polylactic acid material.

[0033] The weight average molecular weight was 7.0×10 4 g / mol and 7.0×10 4 g / mol PLLA and PDLA were vacuum dried at 60°C; then 50 parts by weight of PLLA, 50 parts by weight of PDLA, 0.5 parts by weight of N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide, and 40 parts by weight of PEG (weight average molecular weight 20000 g / mol) were uniformly mixed and added into a melt mixer, melt blended at 200°C for 6 min, and naturally cooled to obtain an initial blend II; finally, the initial blend II was fully washed with deionized water to remove the PEG phase therein, and dried to obtain polylactic acid material II. Example 3

[0034] This embodiment provides a preparation experiment of a polylactic acid material.

[0035] The weight average molecular weight was 7.0×10 4 g / mol and 7.0×10 4 g / mol PLLA and PDLA were vacuum dried at 60°C; then 50 parts by weight of PLLA, 50 parts by weight of PDLA, 0.7 parts by weight of N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide, and 40 parts by weight of PEG (weight average molecular weight 20000 g / mol) were uniformly mixed and added into a melt mixer, melt blended at 200°C for 6 min, and naturally cooled to obtain an initial blend III; finally, the initial blend III was fully washed with deionized water to remove the PEG phase therein, and dried to obtain polylactic acid material III. Comparative Example 1

[0036] This comparative example provides an experiment for preparing a polylactic acid material.

[0037] The weight average molecular weight was 7.0×10 4 g / mol and 7.0×10 4 g / mol PLLA and PDLA were vacuum dried at 60°C; then 50 parts by weight of PLLA, 50 parts by weight of PDLA and 40 parts by weight of PEG (weight average molecular weight 20,000 g / mol) were uniformly mixed and added to a melt mixer, melt-blended at 200°C for 6 min, and naturally cooled to obtain an initial blend IV; finally, the initial blend IV was fully washed with deionized water to remove the PEG phase therein, and dried to obtain a polylactic acid material IV. Comparative Example 2

[0038] This comparative example provides an experiment for preparing a common polylactic acid material.

[0039] The weight average molecular weight was 7.0×10 4 g / mol and 7.0×10 4 g / mol PLLA and PDLA are vacuum dried at 60°C; then 50 parts by weight of PLLA, 50 parts by weight of PDLA, 0.07 parts by weight of N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide, and 40 parts by weight of PEG (weight average molecular weight 20000 g / mol) are uniformly mixed and added into a melt mixer, melt blended at 200°C for 6 min, and naturally cooled to obtain an initial blend V; finally, the initial blend V is fully washed with deionized water to remove the PEG phase therein, and dried to obtain polylactic acid material V. Comparative Example 3

[0040] This comparative example provides an experiment for preparing a common polylactic acid material.

[0041] The weight average molecular weight was 7.0×10 4 g / mol and 7.0×10 4 g / mol PLLA and PDLA were vacuum dried at 60°C; then 50 parts by weight of PLLA, 50 parts by weight of PDLA, 1.0 part by weight of N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide, and 40 parts by weight of PEG (weight average molecular weight 20000 g / mol) were uniformly mixed and added into a melt mixer, melt blended at 200°C for 6 min, and naturally cooled to obtain an initial blend VI; finally, the initial blend VI was fully washed with deionized water to remove the PEG phase therein, and dried to obtain a polylactic acid material VI.

[0042] Experimental Example 1

[0043] This experimental example provides a microstructure observation experiment of polylactic acid material.

[0044] The polylactic acid materials I to VI prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were observed by scanning electron microscope, respectively, and the following results were obtained: Figure 1 The SEM images are shown. The ZJ-3 piezoelectric tester was used to test the d 33 The coefficients are recorded in Table 1.

[0045] Depend on Figure 1 As shown in (a), the stacking of the polylactic acid platelets in the polylactic acid material IV is disordered. At the same time, it may be due to the incomplete phase separation and low porosity, so the structure has insufficient utilization of low-frequency mechanical energy. 33 The coefficient is low and the piezoelectric catalytic degradation efficiency is not high. Figure 1 As shown in (b), the orderliness of the stacking of the PLA sheet crystals in the PLA material I is significantly improved, the benzene tricarboxamide molecules form a fiber assembly and induce the PLA crystallization to form a typical "kebab-like" crystal structure, and the porosity is also improved, which ultimately makes the d 33 The coefficient is increased to 44 pC / N, and the piezoelectric catalytic degradation efficiency is effectively improved. Figure 1 As can be seen from (b), (c) and (d) in Figure 2, when the content of the fiber assembly increases, the length of the fiber assembly formed by the benzene tricarboxamide molecules decreases, the size of the "mutton skewers" crystals decreases, and the long-range order decreases, which ultimately leads to the decrease of the d 33 The coefficient and piezoelectric catalytic degradation efficiency are both reduced, but its electrocatalytic degradation efficiency is still higher than that of polylactic acid material IV.

[0046] Experimental Example 2

[0047] This experimental example provides a verification experiment of the pigment degradation ability of polylactic acid material.

[0048] 0.2 g of the material to be tested was added into 100 mL of an aqueous solution of indigo carmine pigment with a concentration of 5 mg / L to obtain a suspension to be tested. The suspension was subjected to ultrasonic vibration at 50 W and 35 kHz for 25 min. The pigment concentration in the aqueous solution was monitored by an ultraviolet spectrophotometer, and its changes during the ultrasonic treatment (measured every 2 min) were monitored, and the corresponding pigment degradation capacity was calculated.

[0049] In this experiment, the polylactic acid materials I, II, and IV prepared in Example 1, Example 2, and Comparative Example 1 were used as test materials to test their pigment degradation abilities. Figure 2 The concentration of pigment in the aqueous solution containing different polylactic acid materials changes with time. The polylactic acid materials I to VI prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used as test materials to test their respective pigment degradation abilities, and the results of the ability of different polylactic acid materials to degrade pigments were obtained as shown in Table 1.

[0050] Table 1 Results of pigment degradation ability of polylactic acid material

[0051]

[0052] Depend on Figure 2 It can be seen that with the increase of ultrasonic vibration time, the pigment concentration gradually decreases, and the degradation effect of polylactic acid material I is the best, which is basically completely degraded at 25 min (degradation rate reaches 99%), showing excellent piezoelectric catalytic degradation ability.

[0053] As shown in Table 1, as the d 33 The increase in coefficient (d33 The higher the coefficient, the better the piezoelectric performance). The stronger the piezoelectric catalytic degradation ability of the polylactic acid material on the pigment and the faster the pigment degradation rate. In particular, when d 33 The coefficient reaches 44 pC / N, and the degradation rate of pigment can reach 98% after 20 minutes of ultrasonic vibration. Moreover, the degradation efficiency of polylactic acid materials I to III is significantly better than that of polylactic acid materials IV to VI.

[0054] Experimental Example 3

[0055] This experimental example provides an experiment to verify the application effect of polylactic acid material.

[0056] The material to be tested was prepared into a 0.01 g / mL aqueous suspension as a tooth whitening material; normal teeth were stained with a mixture of coffee, tea and cola for one week to obtain stained teeth; the tooth whitening material was applied to the surface of the stained teeth, and the teeth were cleaned with a toothbrush (vibration frequency of about 30,000 Hz), brushing for 10 minutes and staying for 10 minutes, and the tooth surface was cleaned with deionized water each time, and the total cleaning time was 10 hours. The whitening degree of teeth was evaluated with a VITA Easyshade V colorimeter to assess the application effect of the test material on whitening teeth.

[0057] In this experimental example, the polylactic acid materials I to VI prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used as the test materials, respectively, and the results shown in Table 2 were obtained. The polylactic acid material I prepared in Example 1 was used as the test material for the tooth condition before and after the cleaning operation. Figure 3 shown.

[0058] Table 2 Results of teeth whitening using polylactic acid material

[0059]

[0060] As can be seen from Table 2, the polylactic acid materials I to III prepared in Examples 1 to 3 have significantly better teeth whitening effects than the polylactic acid materials IV to VI prepared in Comparative Examples 1 to 3.

[0061] Depend on Figure 3 It can be seen that the polylactic acid material I prepared in Example 1 has a significant teeth whitening effect.

[0062] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0063] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A polylactic acid material, characterized in that: It includes polylactic acid sheet crystals and fiber assemblies; The polylactic acid lamellae are vertically stacked on the surface of the fiber assembly to form an ordered layered structure, and there is a cavity between two adjacent lamellae on the ordered layered structure; The polylactic acid lamellae are stereocomposite lamellae formed by co-crystallization of left-handed polylactic acid and right-handed polylactic acid; The mass ratio of the polylactic acid platelets to the fiber assembly is 100:0.2 to 0.7; The mass ratio of the left-handed polylactic acid to the right-handed polylactic acid is 40-60:40-60; The fiber assembly is N,N',N''-tricyclohexyl-1,3,5-benzenetricarboxamide; The preparation method of the polylactic acid material comprises the following steps: uniformly mixing the left-handed polylactic acid, the right-handed polylactic acid, the fiber assembly and the porogen at room temperature, and then melt-blending at 180-230° C. to obtain a blend; removing the porogen in the blend to obtain the polylactic acid material; Wherein, the porogen is polyethylene glycol; the mass ratio of the porogen to the fiber assembly is 30 ~ 50:0.2 ~ 0.

7.

2. The polylactic acid material according to claim 1, characterized in that: Its piezoelectric constant is 30 ~ 44 pC / N.

3. The polylactic acid material according to claim 1, characterized in that: The weight average molecular weight of the L-polylactic acid is 5×10 4 ~ 3×10 5 g / mol, optical purity ≥92%; The weight average molecular weight of the dextrorotatory polylactic acid is 5×10 4 ~ 3×10 5 g / mol, optical purity ≥92%; The purity of the fiber assembly is ≥99%.

4. Use of the polylactic acid material according to any one of claims 1 to 3 in the preparation of a tooth cleaning preparation.

5. The use according to claim 4, characterized in that: The polylactic acid material is used for catalyzing the degradation of pigments.

Citation Information

Patent Citations

  • High heat-resistant and high-strength polylactic acid fiber and preparation method thereof

    CN105200552A

  • Piezoelectric polylactic acid material as well as preparation method and application thereof

    CN114058165A