Multi-micro-cutting-edge diamond-iron-based spherical composite magnetic grinding material and preparation method and application thereof
By preparing multi-microedge diamond-iron-based spherical composite magnetic abrasives, the problem of separation of magnetic particles and abrasive particles in the magnetorheological polishing fluid is solved, the processing of difficult-to-polishing materials is achieved efficiently, and the stability and stability of magnetorheological processing are improved. Accuracy.
Patent Information
- Application Number
- CN202410800284.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
Magnetic particles and abrasive particles in existing magnetorheological polishing fluids are easily separated during the processing process, resulting in a decrease in control accuracy and timeliness, and typical wide-bandgap semiconductor materials such as diamond are difficult to polish efficiently.
Multi-microedge diamond-iron-based spherical composite magnetic abrasive is used. The abrasive is composed of magnetic iron matrix and diamond particles. It is prepared through processes such as ball milling, calcination, reduction and spray granulation to form a spherical structure and micro-edge structure to ensure the magnetic iron matrix. It has high holding power on diamond particles and has good magnetic saturation strength and catalytic activity.
In magnetorheological processing, the stability and response time of magnetic abrasives are improved, the grinding and polishing efficiency and accuracy are improved, and they have good corrosion resistance, which is suitable for efficient polishing of difficult-to-machine materials.
Smart Images

Figure CN118725824A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive and a preparation method and application thereof. Background Art
[0002] Magnetorheological finishing (MRF) technology was first proposed by Kordonski in the 1990s. Different from traditional surface processing methods, magnetorheological finishing is an ultra-precision processing method that uses an external magnetic field to control the rheology of magnetic polishing fluid to form a flexible "small grinding head" with viscoelastic behavior, driving non-magnetic abrasive particles to shear on the workpiece surface, thereby polishing the workpiece surface material. This feature enables magnetorheological finishing to achieve high material removal rate and high surface quality.
[0003] As an intelligent fluid, magnetorheological fluid exhibits the characteristics of Newtonian fluid with low viscosity and high fluidity when there is no external magnetic field, and exhibits the characteristics of Bingham fluid with high viscosity and low fluidity when an external magnetic field is applied. This transient reversibility from liquid to semi-solid is called magnetorheological effect. The magnetorheological effect is closely related to control accuracy and timeliness. In order to obtain good magnetorheological polishing efficiency and quality, it is necessary to improve the magnetorheological effect of magnetorheological fluid. At present, magnetorheological fluid is mainly composed of a mixture of three parts: base liquid (including water, organic solvent, mineral oil, stabilizer, etc.), magnetic particles (such as carbonyl iron powder CIPs, Fe3O4, etc.) and abrasive particles (such as diamond powder, SiO2, CeO2, Al2O3, ZrO2, etc.). The control of abrasive particles by the magnetic field is indirectly controlled by magnetic particles, and there are deficiencies in the regulation of control force and accuracy.
[0004] In addition, typical wide bandgap semiconductor materials such as diamond, GaN and SiC have the characteristics of high hardness, high brittleness and chemical inertness, and are typical difficult-to-process materials. Softening the surface by oxidants is the main method to improve the polishing efficiency and quality of the above materials. The oxidation potentials of commonly used oxidants H2O2, KMnO4 and NaClO are 1.77V, 1.69V and 1.21V respectively, while the oxidation potential of free radical ·OH is as high as 2.8V. Studies have shown that ·OH can promote the reaction of the surface layer and achieve a good softening effect, and is widely used in chemical mechanical polishing (CMP). Photocatalytic reactions can produce free radicals ·OH, which have achieved good results in chemical mechanical polishing (CMP) of semiconductor materials such as diamond, GaN and SiC. TiO2 is a typical photocatalytic material. Some researchers directly added TiO2 particles to magnetorheological fluids in an attempt to improve the oxidation activity of magnetorheological fluids. However, due to the large difference in size and density between iron-based magnetic particles and TiO2 particles, separation and aggregation between the two are easily caused during use, and the actual effect is relatively limited.
[0005] The use of composite technology to combine magnetic particles, hard abrasive particles and particles with photocatalytic properties into an integral abrasive will hopefully improve the efficiency of magnetorheological polishing.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The purpose of the present invention is to provide a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive and a preparation method and application thereof to solve the above technical problems.
[0008] The present invention is achieved in that:
[0009] In the first aspect, an embodiment of the present invention provides a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, which includes a magnetic iron matrix, and the interior and surface of the magnetic iron matrix contain diamond particles; wherein the external diamond particles and the surface of the magnetic iron matrix form a micro-blade structure; the composite magnetic abrasive is a spherical structure; the material of the magnetic iron matrix is Fe and Fe2TiO4, wherein the mass ratio of Fe element to Ti element is (3-16):1; the saturation magnetization intensity of the composite magnetic abrasive is 30-170emu / g.
[0010] In a second aspect, an embodiment of the present invention provides a method for preparing the composite magnetic abrasive as described above, the preparation method comprising the following steps:
[0011] The iron-containing compound and the titanium-containing compound are mixed and ball-milled to obtain a precursor powder;
[0012] The precursor powder is subjected to high temperature calcination treatment to obtain a calcined iron-based powder;
[0013] The calcined iron-based powder is subjected to high-temperature reduction treatment to obtain a reduced iron-based powder;
[0014] The reduced iron-based powder is mixed with diamond particles, and the diamond-iron-based spherical composite powder is prepared by spray granulation.
[0015] The diamond-iron-based spherical composite powder is subjected to secondary high-temperature reduction treatment to obtain a spherical composite magnetic abrasive.
[0016] In a third aspect, an embodiment of the present invention provides a magnetorheological magnetic abrasive, which includes the composite magnetic abrasive as described above or the composite magnetic abrasive prepared by the preparation method as described above.
[0017] The present invention has the following beneficial effects:
[0018] The multi-micro-blade diamond-iron-based spherical composite magnetic abrasive provided by the embodiment of the present invention has a high holding force of the magnetic iron matrix on the diamond particles, does not separate during the magnetorheological processing, has high stability, and has a short response time. In addition, a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive with high sphericity is prepared through processes such as ball milling, calcination, reduction, and spray granulation. This preparation method is not only simple in process and low in cost, but also can better control its sphericity. The prepared multi-micro-blade diamond-iron-based spherical composite magnetic abrasive has good magnetic saturation strength, catalytic activity, and corrosion resistance, can be used as a magnetorheological magnetic abrasive, and has the characteristics of high grinding and polishing efficiency and high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 This is the SEM test image of 1-D400 prepared in Example 1;
[0021] Figure 2 This is the EDS test image of 1-D400 prepared in Example 1;
[0022] Figure 3 TEM test image of 1-D400 prepared in Example 1;
[0023] Figure 4 Schematic diagram of the particle size distribution test of 1-D400 prepared in Example 1;
[0024] Figure 5 Schematic diagram of the degradation process of methyl orange by 1-D400 prepared in Example 1, 2-D400 prepared in Example 8, and 3-D400 prepared in Example 15;
[0025] Figure 6 This is the appearance test picture of the powder after ball milling. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0027] With the development of science and technology and society, the requirements for the service performance of magnetorheological machining, especially the machining efficiency, are getting higher and higher. For example, the reasonable compounding of diamond particles in the magnetic particle matrix increases the grinding and polishing efficiency and improves the chip holding space, which gives full play to the grinding function of diamond abrasives and has become an important means to improve the service performance of magnetorheological machining. However, as the porosity increases, the chip holding and cooling effects increase, and the mechanical properties of the tool decrease accordingly. When the diamond abrasive content increases to a certain extent, the magnetic saturation performance of the spherical multi-micro-blade diamond-iron-based spherical composite magnetic abrasive is reduced in turn. Therefore, it is necessary to minimize the damage to the magnetic saturation performance of the tool while ensuring high grinding and polishing efficiency.
[0028] At present, some scholars have studied the use of CIP@FeNi to partially replace CIP to improve transient magnetorheological response characteristics. Other scholars have deposited magnetic Fe3O4 on carbon nanotubes (CNTs) to prepare soft magnetic composite particles, which makes the magnetorheological fluid have good sedimentation stability and magnetorheological properties.
[0029] The inventors found that the existing magnetorheological fluid particles contain magnetic particles (carbonyl iron powder, CIPs and Fe3O4, etc.) and abrasive particles (diamond particles, SiO2, CeO2, Al2O3 and ZrO2, etc.), which are independent and separated from each other in the working state. On the one hand, the abrasive cannot respond synchronously with the magnetic particles during magnetorheological processing, and the long abrasive response time will lead to a decrease in control accuracy and timeliness; on the other hand, the movement of magnetic particles will hinder the direct contact between the abrasive and the surface of the object being processed. Therefore, it is urgent to provide a magnetic composite magnetic abrasive with high dimensional consistency, high sphericity and good magnetorheological processing effect to solve the above technical problems.
[0030] In the first aspect, an embodiment of the present invention provides a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, which includes a magnetic iron matrix, and the interior and surface of the magnetic iron matrix contain diamond particles; wherein the external diamond particles and the surface of the magnetic iron matrix form a micro-blade structure; the composite magnetic abrasive is a spherical structure; the magnetic iron matrix is composed of Fe and Fe2TiO4, wherein the mass ratio of Fe element to Ti element is (3-16):1; the saturation magnetization intensity of the composite magnetic abrasive is 30-170emu / g.
[0031] It should be noted that the diamond particles of the present invention are evenly distributed inside and on the surface of the magnetic iron matrix, and the magnetic iron matrix has a high holding force on the diamond particles and is not easy to fall off; that is, the mechanical bite force and chemical action force of the magnetic particles and the abrasive particles are strong. During the magnetorheological processing, the two move synchronously without separation, with high stability and short response time. In addition, the micro-blade structure on the surface of the composite magnetic abrasive can effectively improve its grinding and polishing accuracy, and the grinding and polishing efficiency is high. The composite magnetic abrasive with a spherical structure has certain advantages in service life and polishing quality.
[0032] The mass ratio of Fe element to Ti element in the magnetic iron matrix is (3-16):1, which is calculated based on the product of the mass of the raw material and the proportion of the element in the material.
[0033] In an optional embodiment, the particle size of the composite magnetic abrasive is ≤13 μm.
[0034] It should be noted that controlling the particle size of the composite magnetic abrasive with a spherical structure is beneficial to controlling the grinding and polishing efficiency and processing quality of the composite magnetic abrasive as a magnetic abrasive in a magnetorheological fluid.
[0035] In a second aspect, an embodiment of the present invention provides a method for preparing the composite magnetic abrasive as described above, the preparation method comprising the following steps:
[0036] The iron-containing compound and the titanium-containing compound are mixed and ball-milled to obtain a precursor powder;
[0037] The precursor powder is subjected to high temperature calcination treatment to obtain a calcined iron-based powder;
[0038] The calcined iron-based powder is subjected to high-temperature reduction treatment to obtain a reduced iron-based powder;
[0039] The reduced iron-based powder is mixed with diamond particles, and the diamond-iron-based spherical composite powder is prepared by spray granulation.
[0040] The diamond-iron-based spherical composite powder is subjected to secondary high-temperature reduction treatment to obtain a spherical composite magnetic abrasive.
[0041] In an optional embodiment, the iron-containing compound is selected from any one of iron oxide (Fe2O3) and iron(III) oxide (Fe3O4); the titanium-containing compound includes titanium hydride (TiH2); further, the iron-containing compound is Fe2O3.
[0042] Furthermore, the amount of the titanium-containing compound is 4.0%-20.0% of the precursor powder by mass.
[0043] Furthermore, the amount of the titanium-containing compound is 4.4%-15.5% of the precursor powder by mass fraction; and the amount of Fe2O3 is 84.5%-95.6% of the precursor powder.
[0044] It should be noted that the content of TiH2 affects the saturation magnetization of the final product; the higher the content of TiH2, the lower the saturation magnetization of the final product. In addition, the present invention adds a substance containing the Ti element to the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, the main purpose of which is to increase the catalytic properties of the composite magnetic abrasive. The improvement of the catalytic activity can soften the processed surface, thereby improving the polishing efficiency and quality.
[0045] In an optional embodiment, the iron-containing compound and the titanium-containing compound are mixed and ball-milled for 10-20 hours at a rotation speed of 280-320 r / min, and the particle size of the precursor powder is controlled to be ≤1 μm.
[0046] Furthermore, the ball milling treatment time is 10-12 hours.
[0047] It should be noted that the smaller particle size distribution of the precursor powder gives it a larger specific surface area, which is conducive to the full reaction of the subsequent high-temperature calcination and high-temperature reduction processes.
[0048] In an optional embodiment, the high temperature calcination treatment is performed at a temperature of 400-1000°C for a time of 110-130 minutes. Specifically, the high temperature calcination temperature is selected from any one of 400°C, 500°C, 600°C, 700°C, 800°C, 900°C and 1000°C, and other temperature values between 400-1000°C can also be set according to actual needs.
[0049] It should be noted that the particle size uniformity of the composite powder obtained at a suitable calcination temperature is relatively high, while calcination at a higher temperature will cause severe sintering of the material.
[0050] Furthermore, the temperature of the high temperature calcination treatment is 400-700°C.
[0051] It should be noted that the time control of high-temperature calcination can make the precursor powder react more fully. If the time is too short, it will lead to incomplete reaction, and if the time is too long, it will lead to excessive sintering and waste of resources.
[0052] In order to avoid the influence of the external environment on the calcination process, such as oxygen in the air, in an optional embodiment, the high-temperature calcination process is carried out in a vacuum environment; further, the vacuum degree of the vacuum furnace is controlled to be less than 1×10 -1Pa; in other embodiments of the present invention, high-temperature calcination can also be carried out in an inert atmosphere according to actual needs, wherein the inert atmosphere is argon with a purity of 99.99%; or the reaction can be carried out in a vacuum environment or an inert atmosphere according to actual needs.
[0053] Furthermore, the gas flow rate of the inert gas is 1.8-2.2 L / min.
[0054] It should be noted that if the inert gas filling flow rate is too low, the reaction time will be prolonged, the reaction will be incomplete, and other impurities will be mixed in the reaction products; if the filling flow rate exceeds the set range, it will lead to waste of resources.
[0055] During the high-temperature calcination process, TiH2 preferentially decomposes to produce metallic Ti, which reacts with Fe2O3 powder to produce Fe2TiO4, while part of Fe2O3 is transformed into Fe3O4. As the calcination temperature increases, the powder particles grow and sinter and melt to form larger particles, so that the high-temperature calcined powder becomes a denser block as the calcination temperature increases, and a calcined iron-based powder is obtained.
[0056] It should be noted that the dense block formed by high temperature calcination needs to be crushed, specifically crushing the dense block into a powder state to obtain the calcined iron-based powder. The present invention does not specifically limit the tool for the crushing process, and a suitable tool or device can be selected according to actual needs.
[0057] Further, the calcined iron-based powder includes Fe3O4 / Fe2TiO4.
[0058] In an optional embodiment, the calcined iron-based powder is subjected to a high-temperature reduction treatment, the temperature of the high-temperature reduction treatment is 690-710°C, and the time is 110-130 minutes; further, the high-temperature reduction reaction can be carried out in a vacuum furnace, after the calcined iron-based powder is sent into the vacuum furnace, the vacuum is evacuated to 1×10 -1 The reducing gas for high temperature reduction treatment is hydrogen, the purity of hydrogen is 99.99%, and the gas flow rate of hydrogen is 1.8-2.2L / min.
[0059] It should be noted that during the high-temperature reduction process, Fe3O4 is reduced to Fe, and Fe2TiO4 remains unchanged. For samples with the same original composition, as the reduction temperature of the mixture increases, the iron particles melt into the larger particles enriched with titanium, resulting in a decrease in the content of iron particles, which is manifested as a gradual decrease in the magnetic saturation intensity value of the reduced powder.
[0060] The material after high temperature reduction needs to be crushed, specifically crushed into powder state, to obtain reduced iron-based powder. Here, the tool for crushing is not particularly limited, and a suitable tool or device can be selected according to actual needs.
[0061] Furthermore, the reduced iron-based powder obtained after high-temperature reduction treatment includes Fe / Fe2TiO4.
[0062] In an optional embodiment, the reduced iron-based powder is mixed with diamond particles and subjected to a spray granulation process to obtain a diamond-iron-based spherical composite powder.
[0063] Specifically, the spray granulation process is to mix water, alcohol solvent, defoamer and dispersant evenly, then add the second composite powder to obtain a suspension; then, add diamond particles to the suspension, mix evenly, and obtain spherical composite magnetic abrasives through a spray granulator. Among them, the role of the alcohol solvent is to dissolve organic matter; the role of the defoamer is to prevent the suspension from generating excessive foam during the mixing process; the role of the dispersant is to evenly disperse the powder in the liquid to prevent precipitation or aggregation and improve the stability of the preparation.
[0064] Furthermore, the water used in the embodiment of the present invention is deionized water. In other embodiments of the present invention, distilled water, purified water or high-purity water can be selected according to actual needs.
[0065] It should be noted that the alcohol solvent is selected from any one of ethylene glycol, propylene glycol and butylene glycol; the dispersant is selected from any one of 4190 dispersant, 4290 dispersant and 4032 dispersant. Further, in a preferred embodiment of the present invention, ethylene glycol is used as the alcohol solvent and 4290 dispersant is used as the dispersant. In other embodiments of the present invention, the specifications of the alcohol solvent and the dispersant can be reasonably adjusted according to actual needs.
[0066] Further, the amount of deionized water is 500-550 mL, the amount of ethylene glycol is 2.5-3.0 g, the amount of defoaming agent is 1-1.2 g, the amount of defoaming agent is 1-1.2 g, the amount of dispersant is 10-12 g and the amount of reduced iron-based powder is 150-170 g.
[0067] It should be noted that diamond particles are added after the suspension is wet-milled, wherein the wet-milling time is 10-12 hours and the wet-milling speed is 290-310 r / min. Wet-milling the suspension can promote full mixing of the components and reduce the particle size of the powder in the solution, thereby improving the stability of the suspension.
[0068] Furthermore, the amount of diamond particles added is 1.5%-2.0% of the amount of reduced iron-based powder by mass fraction; and the particle size of the diamond particles is 1.0-1.5 μm.
[0069] Specifically, deionized water, ethylene glycol, defoaming agent, and 4290 dispersant are first fully mixed by magnetic stirring, and then the reduced iron-based powder obtained by high-temperature reduction is added to the mixed solution. After being fully stirred, the mixture is fully ball-milled using a ball mill to obtain a stable suspension. Diamond particles are added to the suspension, and mechanical stirring is used to fully mix. Then, a spray granulator is used to spray granulate the mixed solution to obtain a diamond-iron-based spherical composite powder.
[0070] It should be noted that the diamond particles are mainly used as abrasive particles. In other embodiments of the present invention, the added abrasive particles can be selected from other materials according to actual conditions, such as SiO2, CeO2, Al2O3 and ZrO2. In order to make the composite magnetic abrasive with a spherical structure as the working particle of the magnetorheological fluid, the amount of diamond abrasive particles added is reasonably controlled. Properly increasing the amount of diamond abrasive particles added will significantly improve the grinding and polishing efficiency of the magnetorheological fluid. However, too high a content of diamond abrasive particles will lead to a decrease in the metal base content, thereby reducing the magnetic saturation intensity of the spherical composite magnetic abrasive, which prolongs the response time of the magnetic abrasive. At the same time, too much diamond abrasive particles will cause the diamond particles to fall off during the grinding and polishing process.
[0071] In an optional embodiment, the diamond-iron-based spherical composite powder is subjected to a secondary high-temperature reduction treatment to prepare a multi-micro-edged diamond-iron-based spherical composite magnetic abrasive.
[0072] Furthermore, the temperature of the secondary high-temperature reduction treatment is 890-910°C, and the time is 110-130 minutes; further, the reducing gas of the second high-temperature reduction treatment is hydrogen, the purity of the hydrogen is 99.99%, and the gas flow rate of the hydrogen is 1.8-2.2L / min. The high-temperature reduction reaction can be carried out in a vacuum furnace. After the spherical composite magnetic abrasive is fed into the vacuum furnace, the vacuum is evacuated to 1×10 -1 Pa, and finally a multi-micro-edged diamond-iron-based spherical composite magnetic abrasive was obtained.
[0073] It should be noted that the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive prepared in the embodiment of the present invention has a spherical structure, has high sphericity, small particle size and high particle size concentration, and can give the magnetorheological polishing fluid higher magnetorheological properties.
[0074] Furthermore, the saturation magnetization intensity of the prepared multi-micro-edged diamond-iron-based spherical composite magnetic abrasive is 80-166emu / g.
[0075] In a third aspect, an embodiment of the present invention provides a magnetorheological magnetic abrasive, which includes the composite magnetic abrasive as described above or the composite magnetic abrasive prepared by the preparation method as described above.
[0076] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0077] Examples 1-7
[0078] This embodiment 1-7 provides a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, and the preparation method thereof comprises the following steps:
[0079] S1. According to the mass fraction, 5% TiH2 and 95% Fe2O3 are weighed, wherein the mass of TiH2 is 5g and the mass of Fe2O3 is 95g; the two substances are put into a mixer and mixed thoroughly to obtain a mixed material;
[0080] The mixed material was added into the ball mill at a ratio of 10:1 for ball milling. The mass of the mixed material was 100g. The ball milling was carried out in air atmosphere for 10 hours at a speed of 300r / min. During the ball milling process, the ball mill worked for 2 minutes and rested for 1 minute to reduce overheating of the ball mill and affect the smooth progress of the experiment. The particle size of the precursor powder obtained after ball milling was 100-200nm. Figure 6 .
[0081] S2. Add the precursor powder in step S1 into a vacuum furnace and evacuate to 1×10 -1 Pa or less, and then perform high temperature calcination treatment; the high temperature calcination temperature is 400°C, 500°C, 600°C, 700°C, 800°C, 900°C or 1000°C, and the high temperature calcination time is 120min;
[0082] After high-temperature calcination, the material is fully crushed to obtain calcined iron-based powder Fe3O4 / Fe2TiO4.
[0083] S3. Add the calcined iron-based powder into a vacuum furnace and evacuate to 1×10 -1 Pa, introduce 99.99% pure hydrogen at a gas flow rate of 2 L / min, and perform high-temperature reduction treatment at a temperature of 700°C for 120 min;
[0084] After high-temperature reduction, the material is fully crushed to obtain reduced iron-based powder Fe / Fe2TiO4.
[0085] S4. 500 ml of deionized water, 2.5 g of ethylene glycol, 1 g of defoamer, and 10 g of 4290 dispersant were mixed by magnetic stirring to obtain a mixed solution; 150 g of reduced iron-based powder was weighed and added to the mixed solution and stirred thoroughly; and then the stirred material was added to a ball mill and ball-milled in an air atmosphere for 10 h at a speed of 300 r / min to obtain a wet-milled solution;
[0086] Add 2.5 g of diamond particles with a particle size of 1.5 μm to the wet grinding solution, stir mechanically to mix evenly, and a stable suspension containing diamond particles can be obtained; then use a spray granulator to spray granulate the stable suspension containing diamond particles, with a feed rate of 400 ml / h, an inlet temperature of 150°C, and an outlet temperature of 105°C. Feed the material while mechanically stirring to obtain a diamond-iron-based spherical composite powder.
[0087] S5. Add diamond-iron-based spherical composite powder into a vacuum furnace and evacuate to 1×10 -1 Pa, introduce 99.99% pure hydrogen at a gas flow rate of 2L / min, and carry out secondary high-temperature reduction treatment at a temperature of 900°C for 120min to obtain multi-micro-edged diamond-iron-based spherical composite magnetic abrasive.
[0088] The products obtained in Examples 1-7 are respectively denoted as 1-D400 to 1000, specifically 1-D400, 1-D500, 1-D600, 1-D700, 1-D800, 1-D900, and 1-D1000.
[0089] Embodiment 8-14
[0090] The present embodiments 8-14 provide a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, which differs from the embodiments 1-7 only in that:
[0091] S1. According to mass fraction, weigh 10% TiH2 and 90% Fe2O3, where the mass of TiH2 is 10g and the mass of Fe2O3 is 90g.
[0092] The products obtained in Examples 8-14 are respectively recorded as 2-D400 to 1000, specifically 2-D400, 2-D500, 2-D600, 2-D700, 2-D800, 2-D900, and 2-D1000.
[0093] Examples 15-21
[0094] The present embodiment 15-21 provides a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, which differs from the embodiment 1-7 only in that:
[0095] S1. According to mass fraction, weigh 15% TiH2 and 85% Fe2O3, where the mass of TiH2 is 15g and the mass of Fe2O3 is 85g.
[0096] The products obtained in Examples 15 to 21 are respectively recorded as 3-D400 to 1000, specifically 3-D400, 3-D500, 3-D600, 3-D700, 3-D800, 3-D900, and 3-D1000.
[0097] Test Example 1
[0098] In this test example, the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive prepared in Examples 1-21 was respectively subjected to saturation magnetization measurement, and the measuring instrument was a vibrating sample magnetometer (VSM, Dongfang Chenjing), and the specific parameter setting was that the probe magnetic field was set in the range of -18KOe to 18KOe, and the rate was 0.5A / s. The results of the measured saturation magnetization are summarized in Table 1:
[0099] Table 1
[0100]
[0101] As can be seen from Table 1, with the increase of TiH2 content and the decrease of Fe2O3 content in the raw material, the saturation magnetization of the finally obtained multi-micro-blade diamond-iron-based spherical composite magnetic abrasive decreases. The different Fe2O3 contents in the raw material components also have different temperatures of the highest saturation magnetization. Among them, the highest saturation magnetization in Examples 1-7 is 1-D400 obtained at a calcination temperature of 400°C, and the highest saturation magnetization is 165.2emu / g, the highest saturation magnetization of 2-D600 obtained at 600°C in Examples 8-14 is 132.3emu / g, and the highest saturation magnetization of 3-D600 obtained at 600°C in Examples 15-21 is 104.6emu / g. For raw materials of the same component, their saturation magnetization shows an overall downward trend as the high-temperature calcination temperature increases.
[0102] Test Example 2
[0103] In this test example, the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive 1-D400 prepared in Example 1 was subjected to SEM testing. The testing instrument was a scanning electron microscope (SEM, Zeiss Gemini SEM 300). The test results are shown in Figure 1 ,from Figure 1 It can be seen that the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive has a spherical structure and a high sphericity; diamond particles are evenly distributed on the surface of the matrix.
[0104] Test Example 3
[0105] In this test example, the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive 1-D400 prepared in Example 1 was subjected to EDS testing. The testing instrument was a scanning electron microscope (SEM, Zeiss Gemini SEM 300) equipped with EDS. The test results are shown in Figure 2 ,from Figure 2 It can be seen that the Fe, Ti and O elements are evenly distributed in the matrix, and the diamond is well bonded to the matrix.
[0106] Test Example 4
[0107] In this test example, the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive 1-D400 prepared in Example 1 was subjected to TEM testing. The testing instrument was a transmission electron microscope (TEM, FEI Talos F200x). The test results are shown in Figure 3 ,from Figure 3 It can be seen from the electron diffraction pattern that the composite magnetic abrasive contains Fe2TiO4; the three elements Fe, Ti and O are evenly distributed in the particles, which further proves the existence of Fe2TiO4.
[0108] Test Example 5
[0109] In this test example, the particle size distribution of the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive 1-D400 prepared in Example 1 was tested using a laser particle size analyzer (Mastersizer). The test results are shown in Figure 4 ,from Figure 4 It can be seen that the composite magnetic abrasive particle size is normally distributed, with an average particle size of 6.2 μm.
[0110] Test Example 6
[0111] In this test example, the multi-micro-blade diamond-iron-based spherical composite magnetic abrasives 1-D400, 2-D400 and 3-D400 prepared in Example 1 were subjected to a photocatalytic degradation experiment of methyl orange to characterize the relative concentration of ·OH produced by the composite magnetic abrasives. The sample content was 1 g / L, the methyl orange concentration was 20 mg / L, the pH was 3, and the UV intensity was 100 m W / cm 2 The faster the color degradation of methyl orange solution, the higher the relative concentration of ·OH produced, which in turn indicates that the catalytic activity of the composite magnetic abrasive is higher and the softening effect on the processed surface is better. The results show that 3-D400 has the highest catalytic activity, indicating that the catalytic activity of the abrasive can be improved with the increase of Ti content.
[0112] In summary, the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive provided by the present invention has dual characteristics of grinding and polishing and magnetism; at the same time, the composite magnetic abrasive with a spherical structure moves synchronously during the magnetorheological processing process, has high stability, and has high grinding and polishing accuracy. In addition, a multi-micro-blade diamond-iron-based spherical composite magnetic abrasive with high sphericity is prepared by ball milling, high-temperature calcination and high-temperature reduction, spray granulation, secondary high-temperature reduction and other operations; this preparation method is not only simple in process and low in cost, but also can better control its sphericity and particle size uniformity. The composite magnetic abrasive provided by the present invention has good magnetic saturation strength and can be used as a magnetorheological magnetic abrasive.
[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A multi-micro-blade diamond-iron-based spherical composite magnetic abrasive, characterized in that: The composite magnetic abrasive comprises a magnetic iron matrix, and the interior and surface of the magnetic iron matrix contain diamond abrasive grains; wherein the diamond abrasive grains on the surface form a micro-blade structure on the surface of the magnetic iron matrix; The composite magnetic abrasive is a spherical structure; The magnetic iron matrix is composed of Fe and Fe2TiO4, wherein the mass ratio of Fe element to Ti element is (3-16):1; The saturation magnetization intensity of the composite magnetic abrasive is 30-170emu / g.
2. The composite magnetic abrasive according to claim 1, characterized in that: The particle size of the composite magnetic abrasive is ≤13 μm.
3. A method for preparing a composite magnetic abrasive according to any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: The iron-containing compound and the titanium-containing compound are mixed and ball-milled to obtain a precursor powder; The precursor powder is subjected to high temperature calcination treatment to obtain a calcined iron-based powder; The calcined iron-based powder is subjected to high-temperature reduction treatment to obtain reduced iron-based powder; The reduced iron-based powder is mixed with diamond abrasive grains, and the diamond-iron-based spherical composite powder is prepared by spray granulation; The diamond-iron-based spherical composite powder is subjected to a secondary high-temperature reduction treatment to obtain the multi-micro-blade diamond-iron-based spherical composite magnetic abrasive.
4. The preparation method according to claim 3, characterized in that: The iron-containing compound includes iron oxide; the titanium-containing compound includes titanium hydride; Preferably, the amount of the titanium-containing compound is 4.0%-20.0% of the precursor powder by mass fraction; More preferably, the amount of the titanium-containing compound is 4.4%-15.5% of the precursor powder by mass.
5. The preparation method according to claim 3, characterized in that: The ball milling time is 10-20 hours, and the speed of the ball milling is 250-350 r / min; Preferably, the particle size of the precursor powder is less than 1 μm.
6. The preparation method according to claim 3, characterized in that: The high temperature calcination treatment is performed at a temperature of 400-1000°C and a time of 110-130 minutes; Preferably, the high temperature calcination treatment is carried out at a temperature of 400-700°C and a time of 110-130 minutes; Preferably, the high temperature calcination treatment is carried out in a vacuum environment, and the vacuum degree of the vacuum environment is less than 1×10 -1 Pa; Preferably, the high-temperature calcination treatment is carried out in an inert atmosphere, and the gas flow rate of the inert gas is 1.5-2.5 L / min; Preferably, the main phase of the calcined iron-based powder includes Fe3O4 / Fe2TiO4.
7. The preparation method according to claim 3, characterized in that: The high temperature reduction treatment is performed at a temperature of 690-710°C and a time of 110-130 minutes; Preferably, the reducing gas for the high-temperature reduction treatment is hydrogen, and the gas flow rate of the hydrogen is 1.5-2.5 L / min; Preferably, the main phase of the reduced iron-based powder includes Fe / Fe2TiO4.
8. The preparation method according to claim 3, characterized in that: The spray granulation treatment is to mix water, alcohol solvent, defoamer and dispersant evenly, then add the reduced iron-based powder to prepare a suspension; add the diamond abrasive grains to the suspension, mix evenly, and obtain the diamond-iron-based spherical composite powder through a spray granulator; Preferably, the amount of water is 500-550 mL, the amount of the alcohol solvent is 2.5-3.0 g, the amount of the defoamer is 1-1.2 g, the amount of the dispersant is 10-12 g, and the amount of the reduced iron-based powder is 150-170 g; Preferably, the diamond abrasive particles are added after the suspension is subjected to wet grinding; the wet grinding time is 10-20 hours, and the wet grinding speed is 290-310 r / min; Preferably, the alcohol solvent is selected from any one of ethylene glycol, propylene glycol and butylene glycol; Preferably, the dispersant is selected from any one of 4190 dispersant, 4290 dispersant and 4032 dispersant; Preferably, the added amount of the diamond abrasive grains is 1.5%-2.0% of the reduced iron-based powder in terms of mass fraction; and the particle size of the diamond abrasive grains is 1.0-1.5 μm.
9. The preparation method according to claim 3, characterized in that: The temperature of the secondary high temperature reduction treatment is 890-910°C and the time is 110-130min; Preferably, the reducing gas for the secondary high-temperature reduction treatment is hydrogen, and the gas flow rate of the hydrogen is 1.8-2.2 L / min; Preferably, the saturation magnetization intensity of the composite magnetic abrasive is 80-100emu / g.
10. A magnetorheological magnetic abrasive, characterized in that: The invention comprises the composite magnetic abrasive material as claimed in any one of claims 1 to 2 or the composite magnetic abrasive material prepared by the preparation method as claimed in any one of claims 3 to 9.
Citation Information
Cited By
Diamond-iron-based magnetic composite abrasive and preparation method thereof
CN120637077A
Diamond-iron-based magnetic composite abrasive and preparation method thereof
CN120637077B