Preparation method of LLZTO ceramic tube with large length-diameter ratio
By adjusting the slurry and granulation parameters, combined with the compounding of plasticizers and binders, high-strength, flexible, large-aspect-ratio LLZTO ceramic tubes were prepared, which solved the problems of material brittleness and uneven density in the existing technology. problem, meeting the application needs of lithium-ion solid-state batteries.
Patent Information
- Application Number
- CN202410978040.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-22
AI Technical Summary
It is difficult to prepare LLZTO ceramic tubes with large aspect ratios that meet the performance requirements using existing technology, which limits their application in lithium-ion solid-state batteries. In particular, structural failure occurs due to the brittleness and uneven density of the material.
By adjusting the solid content of the slurry, spray granulation parameters, and the composition and method of the aging material, a defect-free green body is obtained, and a large aspect ratio LLZTO ceramic tube with high strength and flexibility is obtained through a two-stage sintering process, saving The binder is removed to improve density, and a combination of plasticizer and binder is used to ensure uniformity.
The prepared ceramic tube has good flexibility and high strength, is suitable for composite with collective materials, can withstand certain impacts, meets the needs of large-scale energy storage equipment, and improves the safety and application performance of solid-state lithium-ion batteries.
Smart Images

Figure CN118754661A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic metallurgy engineering and lithium battery electrolyte manufacturing, and particularly relates to a preparation method of a large aspect ratio LLZTO ceramic tube. Background Art
[0002] At present, the energy system of mankind is mainly composed of nuclear energy, fossil fuels and renewable energy. Nuclear energy has a very low gas emission rate and is relatively clean energy, but its waste is not easy to handle, and once a safety accident occurs during the operation of a nuclear power plant, it will cause irreversible impact. Fossil fuels are currently the most widely used energy source, but the large-scale use of fossil fuels also brings great problems: on the one hand, it takes tens of millions of years for them to form in the earth's crust, but their reserves are consumed very quickly; on the other hand, the use of fossil fuels will inevitably bring about environmental pollution and greenhouse effect. At present, electric energy is one of the most environmentally friendly forms of energy, and its sources are rich and diverse, especially renewable resources such as solar energy, wind energy, geothermal energy and tidal energy, which are inexhaustible and can be collected and converted into electric energy without destroying the earth's environment on which humans depend. However, how to safely store and transport electric energy has become the top issue restricting the further development of electric energy.
[0003] Lithium-ion batteries have the characteristics of high energy density, long cycle life, and wide operating temperature range, and are widely used in electric vehicles and various electronic products. The liquid organic electrolytes used in traditional lithium-ion secondary batteries are prone to explosion in the event of collision or combustion, which can cause more serious accidents. This safety hazard has caused people to worry about the safety of digital products or electric vehicles. The use of solid electrolytes is one of the important means to solve safety problems. Using solid electrolytes to replace organic liquid electrolytes will simplify the structure of lithium-ion batteries, and all-solid-state batteries will greatly improve the safety of batteries. All-solid-state electrolytes have better thermal and chemical stability than liquid electrolytes and polymer electrolytes, and can operate at higher temperatures and voltages.
[0004] Lithium lanthanum zirconium tantalum oxide solid electrolyte (LLTZO) has attracted the attention of a large number of researchers due to its advantages such as high ionic conductivity, wide electrochemical window and good compatibility with negative electrode lithium. Traditional LLZTO ceramic materials are mostly block or sheet structures, with the following disadvantages: 1. Large volume, not easy to integrate with collective structure, not suitable for large-area use; 2. Large brittleness, cannot withstand large impact, and cannot be applied to curved planes. Therefore, in order to adapt to the development of modern engineering application technology and meet different application needs, LLZTO ceramic materials are developing towards complex composition and diversified structure, and large aspect ratio ceramic tubes have emerged. Due to the different gravity in different parts of the length direction, the density of the ceramic body after phase inversion is different, which introduces problems such as density and local deformation. As the aspect ratio increases, the gravity per unit area in the vertical direction will become larger and larger, which will lead to uneven density and local deformation during the sintering process. Local deformation and uneven density may cause structural failure due to uneven stress during actual use of the product, thereby affecting the production and subsequent application of such products.
[0005] CN115799615A discloses a modified lithium lanthanum zirconium tantalum oxide solid electrolyte and its preparation method, the preparation method comprises: pre-sintering potassium source, tantalum pentoxide and excess strontium source to obtain strontium-doped K2SrTa2O7 precursor; doping and sintering the mixture of lithium source, lanthanum source, zirconium source, tantalum pentoxide and the strontium-doped K2SrTa2O7 precursor in sequence to obtain the strontium-doped K2SrTa2O7 coated modified lithium lanthanum zirconium tantalum oxide solid electrolyte. CN113363564A discloses a lithium lanthanum zirconium tantalum oxide solid electrolyte and its preparation method and application, the preparation method comprises the following steps: mixing lithium source, zirconium source, lanthanum source, tantalum source, sintering aid and first solvent, drying and sintering, mixing the obtained sintered product with second solvent and washing ceramic membrane to obtain the lithium lanthanum zirconium tantalum oxide solid electrolyte.
[0006] However, the above patents cannot successfully produce rod-shaped LLZTO ceramic tubes with a large aspect ratio, and cannot meet the current demand for lithium battery packs in large-scale energy storage equipment, limiting the application of such materials in lithium-ion solid-state batteries. Summary of the invention
[0007] In order to solve the problem that it is difficult to prepare a large aspect ratio LLZTO ceramic tube with satisfactory performance in the prior art, the present invention proposes a method for preparing a large aspect ratio LLZTO ceramic tube. The present invention adjusts the solid content of the slurry, the spray granulation parameters, the composition of the aged material and the aging method, so that the aged material obtained can be pressed into a defect-free green body. The ceramic tube after sintering the green body has 1. good flexibility, and the geometric shape meets the integration requirements, which is convenient for compounding with collective materials; 2. high strength and can withstand certain impacts. Therefore, the technical solution of the present invention will contribute to the development and application of solid-state lithium-ion batteries.
[0008] In order to solve the above technical problems, the present invention provides a method for preparing a large aspect ratio LLZTO ceramic tube, comprising the following steps:
[0009] (S1) Lithium source, lanthanum source, zirconium source and tantalum source are prepared according to the chemical formula Li 7-x LqCy 2-x Ta x O 12 The material mixture is obtained by feeding materials at a molar ratio, wherein 0.4≤x≤0.8, Li is fed in excess, and pre-calcined to obtain LLZTO pre-calcined powder;
[0010] (S2) adding water to the LLZTO pre-calcined powder to prepare a slurry, and wet grinding the slurry to obtain a submicron particle size;
[0011] (S3) spray granulating the sand-milled slurry to obtain LLZTO granulated powder;
[0012] (S4) granulating powder, plasticizer, binder and water are uniformly mixed, sealed and aged to obtain aged material;
[0013] (S5) loading the aged material into a rod-shaped mold, vibrating and pressing the material by cold isostatic pressing to obtain a green body;
[0014] (S6) Adding LLZTO mother powder as buried powder at the bottom of the sintering container, placing the green body on the buried powder, sintering, and cooling to obtain a large aspect ratio LLZTO ceramic tube.
[0015] The present invention omits the binder in the spray granulation stage. Because the inventors found that the binder was added to the slurry before spray granulation, it is difficult to remove it completely during the sintering process, which will affect the compactness of the sintered product. However, after omitting the binder, the shape, density and uniformity of the granulated powder are difficult to control. The inventors need to adjust the solid content and inlet and outlet temperatures of the slurry to ensure the sphericity, loose density and uniformity of the granulated powder. Otherwise, the sphericity of the granulated powder is poor, the fluidity is poor, or the interior is hollow, which will lead to problems such as many internal pores and easy cracking in the later pressed and sintered products. In addition, the present invention uses a compound of plasticizer and binder in the sealing and aging stage. Although the binder can increase the viscosity of the material, if used alone, it will hinder the uniform distribution of water during the aging process, resulting in uneven materials; in addition, if only a plasticizer is used without a binder, the sintered product has a loose structure, is easy to crack, and has a low yield.
[0016] The high aspect ratio LLZTO ceramic tube prepared by the present invention has an aspect ratio of ≥8, a length of 200-400mm, an inner diameter of 20-30mm, an outer diameter of 30-50mm, and the outer diameter is greater than the inner diameter by more than 5mm. The aspect ratio is the ratio of the length to the outer diameter of the rod-shaped ceramic tube.
[0017] Furthermore, in step (S1), the lithium source is selected from at least one of lithium carbonate and lithium sulfate, and the lanthanum source, zirconium source, and tantalum source are selected from at least one of their oxides and hydroxides; the lithium source is in excess of 10-20% to compensate for the loss of lithium volatilization; and the pre-sintering process is sintering at 800-1000°C for 10-15h to make the material present in phase.
[0018] Furthermore, in step (S2), the solid content of the slurry is 30-50%, and the submicron size is 0.1-1 μm.
[0019] Furthermore, in step (S3), the spray granulation process is performed at an air inlet temperature of 160-190°C and an air outlet temperature of 80-110°C, thereby obtaining granulated powder with good fluidity and high bulk density. Furthermore, the granulated powder has a particle size of 20-50 μm and a bulk density of 1.2-1.4 g / cm 3 .
[0020] Furthermore, in step (S4), the uniform mixing is performed by using a mixer for mixing for 0.5-1 h and the sealed aging time is 20-30 h.
[0021] Furthermore, in step (S4), the mass ratio of granulating powder, plasticizer, adhesive and water is 100:1-3:1-3:1-5. The plasticizer is at least one of glycerol, pentaerythritol, polyethylene glycol and polypropylene glycol.
[0022] Furthermore, the adhesive is at least one of polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyacrylamide (PAM), and vinyl pyrrolidone copolymer, preferably a vinyl pyrrolidone copolymer, wherein the vinyl pyrrolidone copolymer is obtained by copolymerizing vinyl pyrrolidone, a side chain hydroxyl-containing vinyl compound, and (meth) alkyl acrylate in a molar ratio of 30-50:10-15:20-30, and the weight average molecular weight of the vinyl pyrrolidone copolymer is 15,000 to 30,000.
[0023] Furthermore, the side chain hydroxyl-containing vinyl compound is selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, N-hydroxymethyl acrylamide, and 4-hydroxyphenyl acrylamide; the alkyl (meth)acrylate is selected from at least one of propyl (meth)acrylate, butyl (meth)acrylate, and cyclohexyl (meth)acrylate.
[0024] Furthermore, the vinylpyrrolidone copolymer is prepared by a preparation method comprising the following steps:
[0025] Vinyl pyrrolidone, side chain hydroxyl vinyl compound and (meth) alkyl acrylate are added to an organic solvent, heated to 100-120°C under a nitrogen atmosphere, and an initiator solution is added dropwise. The addition is completed within 2-4 hours, and the reaction is continued by heat preservation for 4-8 hours. The temperature is lowered, water is added to precipitate, the precipitate is washed and dried to obtain a vinyl pyrrolidone copolymer.
[0026] Furthermore, the initiator is benzoyl peroxide, and the amount of the initiator is 1-2wt% of the total mass of the monomers; the organic solvent is selected from at least one of ethyl acetate and ethylene glycol dimethyl ether.
[0027] Furthermore, in step (S5), the cold isostatic pressing process condition is to maintain the pressure at a pressure of 120-200 MPa for 10-30 seconds.
[0028] Further, in step (S6), the mass of the buried powder is 30-40wt% of the mass of the green body; the sintering is a two-stage sintering, first at 400-600°C for 1-3h, then heated to 1000-1200°C, and kept for 6-10h. The heating rate is not particularly limited, such as 1-20°C / min. The purpose of the low-temperature sintering at 400-600°C is to burn off the binder and perform debinding. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the XRD pattern of the LLZTO ceramic tube prepared in Example 1.
[0030] Figure 2 This is a SEM image of the LLZTO ceramic tube obtained in Example 1.
[0031] Figure 3 This is a physical picture of the LLZTO ceramic tube obtained in Example 1.
[0032] Figure 4 This is the SEM image of the LLZTO ceramic tube prepared in Comparative Example 1.
[0033] Figure 5 This is the SEM image of the LLZTO ceramic tube prepared in Comparative Example 2. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further explained in detail below by way of specific embodiments.
[0035] Preparation Example 1
[0036] Vinyl pyrrolidone, hydroxyethyl acrylate and butyl methacrylate are added to ethylene glycol dimethyl ether in a molar ratio of 30:10:25, and the temperature is raised to 110°C under a nitrogen atmosphere. A 5wt% BPO initiator solution in ethylene glycol dimethyl ether is added dropwise. The amount of the initiator solution added is such that BPO is 1wt% of the total mass of the monomers (the sum of vinyl pyrrolidone, hydroxyethyl acrylate and butyl methacrylate). The initiator solution is added dropwise within 2 hours, and the reaction is continued by keeping warm for 8 hours. The temperature is lowered, and deionized water is added for precipitation. The precipitate is washed with ethanol to remove unreacted monomers, and dried in vacuo at 60°C to obtain a vinyl pyrrolidone copolymer with a weight average molecular weight of about 15,000.
[0037] Preparation Example 2
[0038] The other conditions were the same as those in Preparation Example 1, except that the monomers were a mixture of vinyl pyrrolidone, hydroxyethyl acrylate, and butyl methacrylate in a molar ratio of 50:15:25. The weight average molecular weight of the obtained copolymer was about 17,000.
[0039] Example 1
[0040] (S1) In order to compensate for the volatilization of Li element at high temperature, 20% excess Li source is used according to the chemical calculation ratio of n(Li2CO3)=3.84, n(La2O3)=1.5, n(ZrO2)=1.4, n(Ta2O5)=0.3 to obtain a material mixture, and water is added for wet sand grinding. The sanding speed is 2000rpm and the sanding time is 3h. Then the material is dried. The dried material is pre-sintered at 900℃ for 8h to form a phase and ground into powder.
[0041] (S2) Add water to the above-mentioned pre-burnt powder to prepare a slurry with a solid content of 30%, and perform wet sand grinding at a grinding speed of 2000 rpm and a grinding time of 3 hours to make the material particle size submicron level.
[0042] (S3) The sand-milled slurry is subjected to spray granulation, the air inlet temperature of the spray granulation is 160° C., and the air outlet temperature is 100° C., to obtain granulated powder, the particle size of the granulated powder is about 50 μm, and the bulk density is 1.32 g / cm 3 .
[0043] (S4) Prepare materials according to the mass ratio of granulating powder, plasticizer propylene glycol, binder PVA (number average molecular weight of about 20,000) and water of 100:1:1:5. First, add 50% of water, granulating powder, plasticizer and binder into a mixer. After mixing for 1 hour, take out the materials and seal and age them for 12 hours to obtain a first aged material. Then, add the remaining water and the first aged material into the mixer. After mixing for 0.5 hour, take out the materials and seal and age them for 12 hours to obtain a second aged material.
[0044] (S5) loading the second aged material into a rod-shaped polyurethane mold, vibrating it on a vibrator until it is flush with the top of the mold, and cold isostatically pressing it at 120 MPa for 15 seconds to obtain a green body, the green body having an outer diameter of 35.5 mm, an inner diameter of 25.5 mm, and a length of 297 mm;
[0045] (S6) LLZTO mother powder is added to the bottom of the sintering container as buried powder, and the tubular green body obtained in step (S3) is placed on the buried powder, and the temperature is increased to 600° C. at 1° C. / min and kept for 2 h for debinding, and the temperature is further increased to 1200° C. and kept for 12 h, and cooled to obtain a large aspect ratio LLZTO ceramic tube with dimensions of an outer diameter of 31.2 mm, an inner diameter of 21.7 mm, and a length of 265 mm.
[0046] Figure 1 This is the XRD diagram of the LLZTO ceramic tube obtained in Example 1. It can be seen that the main phase is cubic LLZTO.
[0047] Figure 2 This is a SEM image of the LLZTO ceramic tube obtained in Example 1. It can be seen that the obtained product has fewer pores and a uniform particle size distribution.
[0048] Figure 3 This is a physical picture of the LLZTO ceramic tube obtained in Example 1.
[0049] Example 2
[0050] The other conditions are the same as those in Example 1, except that in step (S2), the solid content is 50%.
[0051] Example 3
[0052] The other conditions are the same as those in Example 1, except that in step (S2), the air inlet temperature is 190°C and the air outlet temperature is 80°C.
[0053] Example 4
[0054] The other conditions are the same as those in Example 1, except that in step (S2), the mass ratio of granulating powder, plasticizer (propylene glycol), binder (PAA, number average molecular weight of about 15,000), and water is 100:3:1:3.
[0055] Example 5
[0056] The other conditions are the same as those in Example 1, except that in step (S2), the mass ratio of granulating powder, plasticizer, binder and water is 100:3:1:5.
[0057] Example 6
[0058] The other conditions are the same as those in Example 1, except that in step (S4), the materials are prepared according to the mass ratio of granulation powder, plasticizer (propylene glycol), binder (PVA) and water of 100:1:1:5, all the water, granulation powder, plasticizer and binder are first added into a mixer, and after mixing for 1 hour, the materials are taken out and sealed and aged for 24 hours to obtain aged materials.
[0059] Example 7
[0060] The other conditions are the same as those in Example 1, except that in step (S4), the binder is the vinylpyrrolidone copolymer prepared in Preparation Example 1.
[0061] Example 8
[0062] The other conditions are the same as those in Example 1, except that in step (S4), the binder is the vinyl pyrrolidone copolymer prepared in Preparation Example 2.
[0063] Comparative Example 1
[0064] The other conditions are the same as those in Example 1, except that in step (S4), no plasticizer is added.
[0065] Figure 4 This is a SEM image of the LLZTO ceramic tube obtained in Example 1. It can be seen that compared with the product in Example 1, the material is unevenly dispersed, resulting in poor uniformity of the sintered product and many pores, suggesting that the product obtained by the method of Comparative Example 1 may not have the same mechanical properties and yield as Example 1.
[0066] Comparative Example 2
[0067] The other conditions are the same as those in Example 1, except that in step (S4), no adhesive is added.
[0068] Figure 5 This is a SEM image of the LLZTO ceramic tube obtained in Example 2. It can be seen that compared with the product in Example 1, not adding an adhesive will lead to a loose structure and easy cracking, thereby affecting the mechanical properties and yield rate of the product.
[0069] The LLZTO ceramic tubes prepared in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1 below.
[0070] The bending strength was tested using a three-point bending test method on a pressure testing machine DR-509Z. The test environment temperature was 23°C and the bending test distance was 100mm.
[0071] The yield rate is the percentage of qualified products among all 20 products.
[0072] Table 1 LLZTO ceramic tube performance test results
[0073]
[0074]
Claims
1. A method for preparing a large aspect ratio LLZTO ceramic tube, characterized in that: The following steps are involved: (S1) Lithium source, lanthanum source, zirconium source and tantalum source are prepared according to the chemical formula Li 7-x Ln3Z 2-x Ta x O 12 The material mixture is obtained by feeding materials at a molar ratio, wherein 0.4≤x≤0.8, Li is fed in excess, and pre-calcined to obtain LLZTO pre-calcined powder; (S2) adding water to the LLZTO pre-calcined powder to prepare a slurry, and wet grinding the slurry to obtain a submicron particle size; (S3) spray granulating the sand-milled slurry to obtain LLZTO granulated powder; (S4) granulating powder, plasticizer, binder and water are uniformly mixed, sealed and aged to obtain aged material; (S5) loading the aged material into a rod-shaped mold, vibrating and pressing the material by cold isostatic pressing to obtain a green body; (S6) Adding LLZTO mother powder as buried powder at the bottom of the sintering container, placing the green body on the buried powder, sintering, and cooling to obtain a large aspect ratio LLZTO ceramic tube.
2. The preparation method according to claim 1, characterized in that: The large aspect ratio LLZTO ceramic tube has an aspect ratio of ≥8, a length of 200-400 mm, an inner diameter of 20-30 mm, an outer diameter of 30-50 mm, and the outer diameter is more than 5 mm larger than the inner diameter.
3. The preparation method according to claim 1, characterized in that: In step (S1), the lithium source is selected from at least one of lithium carbonate and lithium sulfate, and the lanthanum source, zirconium source and tantalum source are selected from at least one of their oxides and hydroxides; the lithium source is in excess of 10-20% to compensate for the loss of lithium volatilization; The pre-sintering process is to sinter at 800-1000℃ for 10-15h in order to make the material phase.
4. The preparation method according to claim 1, characterized in that: In step (S2), the solid content of the slurry is 30-50%, and the submicron size is 0.1-1 μm.
5. The preparation method according to claim 1, characterized in that: In step (S3), the spray granulation process is performed at an air inlet temperature of 160-190°C and an air outlet temperature of 80-110°C, thereby obtaining granulated powder with good fluidity and high bulk density. Furthermore, the granulated powder has a particle size of 20-50 μm and a bulk density of 1.2-1.4 g / cm 3 .
6. The preparation method according to claim 1, characterized in that: In step (S4), the mixing is uniformly performed by using a mixer for 0.5-1h and the sealing and aging time is 20-30h; Furthermore, in step (S4), the mass ratio of granulating powder, plasticizer, adhesive and water is 100:1-3:1-3:1-5; the plasticizer is at least one of glycerol, pentaerythritol, polyethylene glycol and polypropylene glycol; the adhesive is at least one of polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyacrylamide (PAM) and vinyl pyrrolidone copolymer, and the vinyl pyrrolidone copolymer is obtained by copolymerization of vinyl pyrrolidone, side chain hydroxyl-containing vinyl compound and (meth) alkyl acrylate.
7. The preparation method according to claim 6, characterized in that: The molar ratio of vinyl pyrrolidone, side chain hydroxyl-containing vinyl compound and (meth) alkyl acrylate is 30-50:10-15:20-30, and the weight average molecular weight of the vinyl pyrrolidone copolymer is 15000 to 30000; Furthermore, the side chain hydroxyl-containing vinyl compound is selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, N-hydroxymethyl acrylamide, and 4-hydroxyphenyl acrylamide; the alkyl (meth)acrylate is selected from at least one of propyl (meth)acrylate, butyl (meth)acrylate, and cyclohexyl (meth)acrylate.
8. The preparation method according to claim 6, characterized in that: The vinylpyrrolidone copolymer is prepared by a preparation method comprising the following steps: Vinyl pyrrolidone, a side chain hydroxyl vinyl compound, and an alkyl (meth)acrylate are added to an organic solvent, the temperature is raised to 100-120° C. under a nitrogen atmosphere, an initiator solution is added dropwise, the addition is completed within 2-4 hours, the reaction is continued at the temperature for 4-8 hours, the temperature is lowered, water is added to precipitate, the precipitate is washed, and dried to obtain a vinyl pyrrolidone copolymer; Furthermore, the initiator is benzoyl peroxide, and the amount of the initiator is 1-2wt% of the total mass of the monomers; the organic solvent is selected from at least one of ethyl acetate and ethylene glycol dimethyl ether.
9. The preparation method according to claim 1, characterized in that: In step (S5), the cold isostatic pressing process condition is to maintain the pressure at a pressure of 120-200 MPa for 10-30 seconds.
10. The preparation method according to claim 1, characterized in that: In step (S6), the mass of the buried powder is 30-40wt% of the mass of the green body; The sintering is a two-stage sintering, first keeping the temperature at 400-600℃ for 1-3h, then raising the temperature to 1000-1200℃ and keeping it for 6-10h.
Citation Information
Patent Citations
Preparation method of piezoelectric tubes with high length-diameter ratio
CN106007711A
Polymethylacrylic acid-2-hydroxyethyl ester / N-vinyl pyrrolidone binary copolymer hydrogel and preparation method thereof
CN111978567A
Lithium lanthanum zirconium tantalum oxide solid electrolyte and preparation method and application thereof
CN113363564A
Preparation method of additive-free high-purity yttrium oxide spherical particles for thermal spraying
CN114195517A
Method for producing a polycrystalline transparent ceramic
EP2067754A2
Cited By
Lithium lanthanum zirconium oxide solid electrolyte and preparation and application thereof
CN122705294A
Lithium-based ceramic material and preparation method therefor
WO2026107857A1