IZO ceramic target material and preparation method thereof
By using a mixed slurry of indium oxide, zinc oxide and tin oxide powder for cold sintering and low-temperature heat treatment in the preparation of IZO targets, the problems of high sintering temperature and long time are solved, and high density, fine particle size and low temperature are obtained. The resistivity of the IZO ceramic target ensures composition uniformity and mechanical properties.
Patent Information
- Application Number
- CN202410774928.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing IZO target preparation methods require high sintering temperatures and long times, which can easily lead to oxygen loss during oxide sintering, uneven component distribution, poor density, and easy cracking.
The mixed slurry of indium oxide, zinc oxide and trace tin oxide powder is ground and spray granulated to form IZO composite powder, which is then mixed with an acetic acid solution for cold sintering, and finally is subjected to low-temperature heat treatment in a pressureless oxygen atmosphere to simplify the process and reduce the cost. sintering temperature and time.
It is possible to obtain IZO ceramic targets with high density, fine particle size, and low resistivity at lower temperatures and times, solving the problem of oxygen loss during oxide sintering and ensuring composition uniformity and mechanical properties.
Smart Images

Figure CN118754608A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of target materials, and in particular relates to an IZO ceramic target material and a preparation method thereof. Background Art
[0002] Among the vast TCO series, IZO thin films have attracted widespread attention due to their low resistivity, high visible light transmittance, and the ability to be prepared using simple conventional sputtering methods. Since IZO amorphous films lack a crystalline structure, they have a smooth surface, low internal stress, and good micro-etching properties. In addition, IZO thin films can be deposited at lower temperatures, so they can be used in flexible devices such as solar cells and flat panel displays. During the sintering process of IZO targets, Zn k In2O k+3 The formation of phases such as Z can help improve the density of the target material, refine the grains, and greatly increase the sputtering rate during sputtering. nk In2O k+3 (k=3, 4, 5) ternary compound films have good chemical stability, high conductivity and optical transparency. Therefore, the research on IZO sputtering targets can effectively meet the rapid development of the domestic flat panel display industry, meet the demand for high-performance oxide ceramic sputtering targets, and break the barriers of foreign target preparation technology.
[0003] However, the existing preparation method has high sintering temperature and long sintering time. The oxides are prone to sintering oxygen loss during the sintering process. The resulting IZO target material has uneven composition distribution, poor density, and is prone to cracking. Summary of the invention
[0004] In view of this, some embodiments disclose a method for preparing an IZO ceramic target, comprising:
[0005] The indium oxide powder, the zinc oxide powder and the tin oxide powder are uniformly mixed in deionized water according to a set mass ratio to obtain a mixed slurry with a solid content of 30 to 60%;
[0006] Adding a dispersant to the mixed slurry, stirring and grinding, and then adding a binder, spray granulation to form an IZO composite powder;
[0007] Taking a set amount of IZO composite powder and mixing it with acetic acid solution to obtain IZO composite slurry;
[0008] Cold sintering the IZO composite slurry to obtain an IZO green body;
[0009] The IZO blank is subjected to low temperature heat treatment in a pressureless oxygen atmosphere to obtain an IZO ceramic target.
[0010] In the preparation method of the IZO ceramic target disclosed in some embodiments, the mass ratio of indium oxide powder, zinc oxide powder and tin oxide powder is 89.3:10.7:0.01-1.
[0011] In the preparation method of the IZO ceramic target disclosed in some embodiments, in the mixed slurry:
[0012] The mass content of the dispersant is 2-6%; the dispersant is citric acid, sodium hexametaphosphate, ammonium polyacrylate or sodium polyacrylate;
[0013] The mass content of the binder is 1-5%; the binder is polyvinyl alcohol or polyethylene glycol.
[0014] In some embodiments of the IZO ceramic target preparation method disclosed, the grinding speed is 1600-2000 r / min and the time is 20-60 min.
[0015] Some embodiments disclose a method for preparing an IZO ceramic target, in which spray granulation is carried out in a granulator, the inlet air temperature of the granulator is 180-300°C, the exhaust air temperature is 80-120°C, the feed rate is 400mL / h, the frequency is 30-50Hz, and the drying speed is 13000-27000rpm.
[0016] In the preparation method of the IZO ceramic target disclosed in some embodiments, the concentration of the acetic acid solution is 1-3M.
[0017] In the preparation method of the IZO ceramic target disclosed in some embodiments, the cold sintering temperature is 100-450° C., the pressure is 100-500 MPa, and the time is 10-200 min.
[0018] In the preparation method of the IZO ceramic target disclosed in some embodiments, the temperature of the low-temperature heat treatment is 500 to 1100° C. and the time is 0.5 to 8 hours.
[0019] Some embodiments disclose an IZO ceramic target obtained by the above-mentioned method for preparing the IZO ceramic target.
[0020] The IZO ceramic target disclosed in some embodiments has a density of 98-99.8%, a grain size of 2-10 μm, and a resistivity of 3-20 mΩ·cm.
[0021] The preparation method of the IZO ceramic target disclosed in the embodiment of the present invention uses indium oxide and zinc oxide as raw materials, adds a trace amount of tin oxide, grinds and sprays to form an IZO composite powder, then mixes the IZO composite powder with acetic acid to form an IZO composite slurry, directly cold-sinters the IZO composite slurry to obtain an IZO blank, and then performs low-temperature heat treatment on the IZO blank in a pressureless oxygen atmosphere to obtain an IZO ceramic target. The preparation method of the IZO ceramic target disclosed in the embodiment of the present invention simplifies the preparation process, can obtain an IZO ceramic target with high density, fine particle size and low resistivity at a lower sintering temperature and a lower sintering time, solves the problem of oxygen loss during oxide sintering, and the obtained IZO ceramic target has uniform composition, is not easy to crack, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 SEM image of IZO ceramic target in Example 1. DETAILED DESCRIPTION
[0023] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0024] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0025] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0026] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0027] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0028] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be arbitrarily combined, and the obtained technical solutions belong to the contents disclosed in the embodiments of the present application. It should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like mentioned in the present application indicate the orientation or position relationship based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the technical features and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, unless it conflicts with the context. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance, unless it conflicts with the context.
[0029] In some embodiments, the method for preparing an IZO ceramic target comprises:
[0030] The indium oxide powder, the zinc oxide powder and the tin oxide powder are uniformly mixed in deionized water according to a set mass ratio to obtain a mixed slurry with a solid content of 30 to 60%; preferably, the solid content in the mixed slurry is 50%; the amount of the solid content is directly related to the dispersion effect of the mixed powder and the uniformity of granulation in the subsequent granulation process;
[0031] Add dispersant to the mixed slurry, stir and grind. Generally, the mixed slurry is ground by high-energy ball milling, and then a binder is added and spray granulated to form IZO composite powder. Spray granulation uses the van der Waals force between particles to connect the powders to form soft agglomerates, increase the powder particle size, enhance fluidity, and make it easy to mix evenly, which is conducive to subsequent cold sintering and forming; forming a high-density IZO ceramic target;
[0032] A set amount of IZO composite powder is mixed with an acetic acid solution to obtain an IZO composite slurry; the IZO composite powder is moistened by a small amount of acetic acid solution to form a supersaturated solution, and the IZO composite powder generates a liquid phase between the interfaces of the particles to accelerate the dissolution and movement of the particles;
[0033] The IZO composite slurry is cold sintered to obtain an IZO blank; during the cold sintering process, the IZO composite powder particles are densified by dissolution-precipitation, and the supersaturated solution from the epitaxial growth on the particle surface is precipitated; under a specific temperature and pressure, the IZO composite powder particles will undergo particle rearrangement with the help of an acetic acid solution, and then the atoms or ion clusters will separate from the particle contact points and accelerate diffusion, so as to minimize the surface free energy of the particles; therefore, in some embodiments, the cold sintering temperature is 100-450°C, the pressure is 100-500Mpa, and the time is 10-200min; directly cold sintering the IZO composite slurry at this temperature and pressure can shorten the sintering time, reduce the sintering temperature, save energy consumption, and inhibit the abnormal growth of grains during the ceramic sintering process, so as to obtain a ceramic IZO blank with uniform and fine grain size; in addition, the cold sintering process can also effectively reduce the volatilization of indium oxide and zinc oxide during high-temperature sintering, thereby avoiding the problem of uncontrollable grain boundary defects;
[0034] The IZO blank is subjected to low-temperature heat treatment in a pressureless oxygen atmosphere to obtain an IZO ceramic target. According to the Oswald rule, a supersaturated solution will nucleate an amorphous phase in an unstable state. When the nucleation rate of the amorphous phase is greater than that of the stable phase, the free energy of the system will be reduced, and the generated metastable phase will reduce the driving force for crystallization. Therefore, the IZO blank needs to be subjected to low-temperature heat treatment to assist crystallization.
[0035] Low-temperature heat treatment under pressureless conditions can transfer heat more evenly, avoid uneven sintering caused by excessive local temperature, and effectively control the stable forming of the IZO blank into an IZO ceramic target. Secondly, the introduction of oxygen during the low-temperature heat treatment process can reduce the fluctuation of the number of oxygen ions in the grain boundaries and lattices, effectively inhibit the generation of oxygen vacancies, and effectively reduce the volatilization of indium oxide and zinc oxide.
[0036] In some embodiments, the temperature of the low-temperature heat treatment is 500-1100°C, and the time is 0.5-8h; when the low-temperature heat treatment is carried out at this temperature, the subgrain boundaries in the IZO blank disappear, the number of grain boundaries decreases, the defects and stresses in the crystal system are significantly eliminated, and the scattering effect is significantly weakened. The composition of the obtained IZO ceramic target is more uniform, the carrier mobility is significantly improved, the resistivity is significantly reduced, the grain size is increased, the purity is high, the grain density is increased, the relative density is high, and it is not easy to crack.
[0037] Preferably, the cold sintering temperature is 300-400° C., the pressure is 350-450 MPa, and the time is 30-120 min.
[0038] Preferably, the temperature of the low temperature heat treatment is 500-1000° C., and the time is 2-4 hours.
[0039] In some embodiments, the flow rate of the oxygen atmosphere is 6 L / min.
[0040] In some embodiments, the mass ratio of indium oxide powder, zinc oxide powder and tin oxide powder is 89.3:10.7:0.01-1.
[0041] In some embodiments, in the mixed slurry:
[0042] The mass content of the dispersant is 2-6%; the dispersant is citric acid, sodium hexametaphosphate, ammonium polyacrylate or sodium polyacrylate; generally, adding a dispersant to the mixed slurry can prevent the IZO particles from agglomerating and make the IZO particles more uniform; preferably, the dispersant is citric acid;
[0043] The mass content of the binder is 1-5%; the binder is polyvinyl alcohol or polyethylene glycol; preferably, the binder is polyvinyl alcohol.
[0044] In some embodiments, a defoaming agent may be added to the mixed slurry to prevent the uneven IZO particles caused by a large amount of foam during the stirring and dispersing process; the defoaming agent is selected from DF-8868A, DF-879 or DF-805.
[0045] In some embodiments, the grinding speed is 1600-2000 r / min, and the grinding time is 20-60 min.
[0046] Preferably, the grinding speed is 1800 r / min and the grinding time is 30 min.
[0047] Preferably, zirconium oxide sand grinding beads with a diameter of 0.6 mm are selected as ball milling media to grind the mixed slurry, the number ratio of zirconium oxide sand grinding beads to the mixed slurry is 2:1, the grinding speed is 1800 r / min, and the time is 50 min.
[0048] In some embodiments, spray granulation is carried out in a granulator with an inlet air temperature of 180-300°C, an exhaust air temperature of 80-120°C, a feed rate of 400 mL / h, a frequency of 30-50 Hz, and a drying speed of 13000-27000 rpm.
[0049] In some embodiments, the concentration of the acetic acid solution is 1-3M.
[0050] Preferably, the concentration of the acetic acid solution is 1.5-2.5M.
[0051] In some embodiments, the IZO ceramic target is obtained by the above-mentioned method for preparing the IZO ceramic target.
[0052] In some embodiments, the density of the IZO ceramic target is 98-99.8%, the grain size is 2-10 μm, and the resistivity is 3-20 mΩ·cm.
[0053] The technical details are further illustrated below in conjunction with embodiments.
[0054] Example 1
[0055] Figure 1 This is the SEM image of the IZO ceramic target disclosed in Example 1.
[0056] This embodiment 1 discloses a method for preparing an IZO ceramic target, comprising:
[0057] 8.97 kg of indium oxide powder, 1.03 kg of zinc oxide powder and 0.01 kg of tin oxide powder were mixed uniformly in deionized water to obtain a mixed slurry with a solid content of 60%;
[0058] Add 5 wt% citric acid to the mixed slurry and stir for 30 minutes;
[0059] Zirconia sand grinding beads with a diameter of 0.6 mm were used as ball milling media to grind the mixed slurry. The ratio of the number of zirconia sand grinding beads to the mixed slurry was 2:1, the grinding speed was 1800 r / min, and the time was 50 min.
[0060] 3 wt % polyvinyl alcohol was added to the mixed slurry and stirred for 30 min; the mixed slurry was then sprayed and granulated by a granulator to form an IZO composite powder; the inlet air temperature of the granulator was 200° C., the exhaust air temperature was 100° C., the feed rate was 400 mL / h, the frequency was 40 Hz, and the drying speed was 20000 rpm;
[0061] 3 g of IZO composite powder was mixed with 1 mL of 2 M acetic acid solution in a mortar for 6 min to obtain an IZO composite slurry;
[0062] The IZO composite slurry was placed in a mold with a diameter of 12 mm for cold sintering. The cold sintering pressure was 200 MPa, the temperature was 200 °C, the heating rate was 5 °C / min, and the temperature was kept for 1 h.
[0063] After sintering is completed, the mold is removed by cooling to obtain an IZO green body;
[0064] The IZO blank was subjected to low temperature heat treatment in an oxygen atmosphere with a flow rate of 6 L / min, the heat treatment temperature was 500°C, the heating rate was 5°C / min, and the temperature was kept for 4 hours to obtain an IZO ceramic target. Figure 1 As shown, the surface of the IZO ceramic target has only a small amount of pores and high density. The light-colored part in the figure is In2O3 and the dark-colored part is In2O3(ZnO)3.
[0065] Example 2
[0066] The preparation method of the IZO ceramic target disclosed in this embodiment 2 refers to that in embodiment 1, wherein in this embodiment 2: the pressure of cold sintering is 250 MPa, the temperature is 250°C, the heating rate is 10°C / min, and the heat preservation is 1 hour; the temperature of low-temperature heat treatment is 600°C, the heating rate is 5°C / min, and the heat preservation is 4 hours.
[0067] Example 3
[0068] The preparation method of the IZO ceramic target disclosed in this embodiment 3 refers to that in embodiment 1, wherein in this embodiment 3: the pressure of cold sintering is 350 MPa, the temperature is 300°C, the heating rate is 10°C / min, and the heat preservation is 1 hour; the temperature of low-temperature heat treatment is 600°C, the heating rate is 5°C / min, and the heat preservation is 4 hours.
[0069] Example 4
[0070] The preparation method of the IZO ceramic target disclosed in this embodiment 4 refers to that in embodiment 1, wherein, in this embodiment 4: the pressure of cold sintering is 400 MPa, the temperature is 300°C, the heating rate is 10°C / min, and the heat preservation is 1 hour; the temperature of low-temperature heat treatment is 700°C, the heating rate is 5°C / min, and the heat preservation is 4 hours.
[0071] Example 5
[0072] The preparation method of the IZO ceramic target disclosed in this embodiment 5 refers to that in embodiment 1, wherein, in this embodiment 5: the pressure of cold sintering is 400 MPa, the temperature is 300°C, the heating rate is 10°C / min, and the heat preservation is 1 hour; the temperature of low-temperature heat treatment is 600°C, the heating rate is 5°C / min, and the heat preservation is 4 hours.
[0073] Example 6
[0074] The preparation method of the IZO ceramic target disclosed in this embodiment 6 refers to that in embodiment 1, wherein, in this embodiment 6: the pressure of cold sintering is 400 MPa, the temperature is 350°C, the heating rate is 10°C / min, and the heat preservation is 1 hour; the temperature of low-temperature heat treatment is 700°C, the heating rate is 5°C / min, and the heat preservation is 4 hours.
[0075] Comparative Example 1
[0076] The preparation method of the IZO ceramic target disclosed in this comparative example 1 refers to Example 1, wherein, in this comparative example 1: the pressure of cold sintering is 100 MPa, the temperature is 100°C, the heating rate is 10°C / min, and the heat preservation is 1 hour; the temperature of low-temperature heat treatment is 500°C, the heating rate is 5°C / min, and the heat preservation is 4 hours.
[0077] Comparative Example 2
[0078] The preparation method of the IZO ceramic target disclosed in this comparative example 2 refers to Example 1, wherein, in this comparative example 2: the pressure of cold sintering is 400MPa, the temperature is 350°C, the heating rate is 10°C / min, and the heat preservation is 1h; the temperature of low-temperature heat treatment is 1000°C, the heating rate is 5°C / min, and the heat preservation is 4h.
[0079] In summary, the grain size, relative density and resistivity of the IZO ceramic targets prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested using a scanning electron microscope, Archimedes drainage method and a probe tester. The results are shown in Table 1 below:
[0080] Table 1 Performance test results of Examples 1 to 6 and Comparative Examples 1 to 2
[0081]
[0082] It can be seen from Table 1 that the IZO ceramic target materials prepared in Examples 1 to 6 have uniform grain size and small average grain size, and grains below 10 μm can be obtained. The density is high, and the relative density can reach 99.8%; the cold sintering temperature and pressure of Comparative Example 1 are lower than those of Examples 1 to 6, and the IZO ceramic target material prepared in Comparative Example 1 has poor density; the low-temperature heat treatment temperature of Comparative Example 2 is higher than that of Examples 1 to 6, and the grain size of the IZO ceramic target material prepared in Comparative Example 2 is too large.
[0083] The preparation method of the IZO ceramic target disclosed in the embodiment of the present invention uses indium oxide and zinc oxide as raw materials, adds a trace amount of tin oxide, grinds and sprays to form an IZO composite powder, then mixes the IZO composite powder with acetic acid to form an IZO composite slurry, directly cold-sinters the IZO composite slurry to obtain an IZO blank, and then performs low-temperature heat treatment on the IZO blank in a pressureless oxygen atmosphere to obtain an IZO ceramic target. The preparation method of the IZO ceramic target disclosed in the embodiment of the present invention simplifies the preparation process, can obtain an IZO ceramic target with high density, fine particle size and low resistivity at a lower sintering temperature and a lower sintering time, solves the problem of oxygen loss during oxide sintering, and the obtained IZO ceramic target has uniform composition, is not easy to crack, and has good industrial application prospects.
[0084] The technical solutions disclosed in the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the present invention. Any conventional changes, substitutions or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. Preparation method of IZO ceramic target, It is characterized in that include: The indium oxide powder, the zinc oxide powder and the tin oxide powder are uniformly mixed in deionized water according to a set mass ratio to obtain a mixed slurry with a solid content of 30 to 60%; Adding a dispersant to the mixed slurry, stirring and grinding, and then adding a binder, spray granulation to form an IZO composite powder; Taking a set amount of IZO composite powder and mixing it with acetic acid solution to obtain IZO composite slurry; The IZO composite slurry is cold sintered to obtain an IZO green body; The IZO blank is subjected to low temperature heat treatment in a pressureless oxygen atmosphere to obtain an IZO ceramic target.
2. The method for preparing an IZO ceramic target according to claim 1, It is characterized in that The mass ratio of the indium oxide powder, the zinc oxide powder and the tin oxide powder is 89.3:10.7:0.01-1.
3. The method for preparing the IZO ceramic target according to claim 1, It is characterized in that In the mixed slurry: The mass content of the dispersant is 2-6%; the dispersant is citric acid, sodium hexametaphosphate, ammonium polyacrylate or sodium polyacrylate; The mass content of the binder is 1-5%; the binder is polyvinyl alcohol or polyethylene glycol.
4. The method for preparing an IZO ceramic target according to claim 1, It is characterized in that The grinding speed is 1600-2000 r / min, and the grinding time is 20-60 min.
5. The method for preparing the IZO ceramic target according to claim 1, It is characterized in that The spray granulation is carried out in a granulator, the air inlet temperature of the granulator is 180-300°C, the exhaust temperature is 80-120°C, the feed rate is 400mL / h, the frequency is 30-50Hz, and the drying speed is 13000-27000rpm.
6. The method for preparing an IZO ceramic target according to claim 1, It is characterized in that The concentration of the acetic acid solution is 1-3M.
7. The method for preparing an IZO ceramic target according to claim 1, It is characterized in that The cold sintering is performed at a temperature of 100 to 450° C., a pressure of 100 to 500 MPa, and a time of 10 to 200 minutes.
8. The method for preparing an IZO ceramic target according to claim 1, It is characterized in that The temperature of the low temperature heat treatment is 500-1100° C., and the time is 0.5-8 hours. 9.IZO ceramic target, It is characterized in that The IZO ceramic target is obtained by the preparation method of any one of claims 1 to 8.
10. The IZO ceramic target according to claim 9, It is characterized in that The IZO ceramic target has a density of 98-99.8%, a grain size of 2-10 μm, and a resistivity of 3-20 mΩ·cm.
Citation Information
Patent Citations
Ultralow-temperature cold sintering method of ZnO-based ceramic
CN109133911A
Cerium oxide doped IZO powder, target material and preparation methods of cerium oxide doped IZO powder and target material
CN113716953A
Indium tin zinc oxide target material and preparation method thereof
CN116253556A
Lanthanide rare earth doped indium zinc oxide sputtering target material and preparation method thereof
CN116751049A
IZO target material and preparation method thereof
CN117263653A
Cited By
Preparation method of ErBCO superconducting target material
CN119320271A
A method for preparing an erbcO superconducting target
CN119320271B