Optical laminate and method for manufacturing same

By forming a photocurable adhesive layer on the side of the liquid crystal phase retardation layer and then irradiating it with light, the problem of scratches appearing on the liquid crystal phase retardation layer after peeling off the substrate layer is solved, and the high durability and flatness of the optical laminate are achieved.

CN118732133APending Publication Date: 2024-10-01SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410366985.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When manufacturing optical laminates, scratches can easily occur in the liquid crystal phase retardation layer after the substrate layer is peeled off, which affects product quality.

Method used

A photocurable adhesive composition is used to form an adhesive layer on the side of the liquid crystal phase retardation layer and then irradiate it with light to fully cure it, thereby forming a rigid adhesive layer to protect the liquid crystal phase retardation layer.

Benefits of technology

It effectively suppresses the scratches generated by the liquid crystal phase retardation layer after the substrate layer is peeled off, and improves the durability and flatness of the optical laminate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732133A_ABST
    Figure CN118732133A_ABST
Patent Text Reader

Abstract

The invention provides an optical laminate and a method for manufacturing the same. The optical laminate is capable of suppressing the occurrence of scratches in the liquid crystal phase difference layer. The optical laminate is provided with an adhesive layer and a first liquid crystal phase difference layer with a base material. The adhesive layer is a cured product layer of a photocurable adhesive composition. The first liquid crystal phase difference layer with the base material is provided with a first liquid crystal phase difference layer and a first base material layer in this order from the adhesive layer side. The first liquid crystal phase difference layer has a first polymer layer containing a polymer of a polymerizable liquid crystal compound. The first substrate layer is peelable from the first liquid crystal phase difference layer. The first liquid crystal phase difference layer with the base material has a light transmittance Tx of 20% or more at a wavelength of 317 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical layered body and a method for producing the same. Background Art

[0002] As an optical laminate with anti-reflection performance, a circular polarizing plate comprising a polarizing element and a phase difference element is known. As the phase difference element possessed by the circular polarizing plate, a liquid crystal phase difference layer of a polymer layer having a layer of a polymer as a polymerizable liquid crystal compound is sometimes used. The polymer layer of the liquid crystal phase difference layer can be obtained by applying a composition comprising a polymerizable liquid crystal compound on a substrate layer or on an orientation layer formed on a substrate layer to form a coating layer, irradiating the coating layer with active energy rays and polymerizing the polymerizable liquid crystal compound (e.g., patent document 1). The liquid crystal phase difference layer is attached to an optical film constituting an optical laminate such as a polarizing plate or other liquid crystal phase difference layers in a state supported by the substrate layer, and then the substrate layer is peeled off and removed.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 2020-52365 Summary of the Invention

[0006] Problems to be solved by the invention

[0007] In order to meet the requirements for thinning of optical laminates used in display devices such as organic EL display devices, photocurable adhesives are sometimes used to bond the layers of the optical laminate. For example, when a liquid crystal phase difference layer supported by a substrate layer and an optical film are laminated with the aid of a photocurable adhesive, the photocurable adhesive is sometimes cured by irradiating light from the substrate layer side, and then the substrate layer is peeled off and removed, thereby manufacturing an optical laminate. The optical laminate is usually manufactured by conveying the liquid crystal phase difference layer and the optical film supported by the substrate layer, and the laminate obtained by peeling off the substrate layer is also conveyed and supplied to the product processing. During such product processing, scratches are sometimes generated on the liquid crystal phase difference layer exposed by peeling off the substrate layer.

[0008] An object of the present invention is to provide an optical laminate comprising a pressure-sensitive adhesive layer which is a cured layer of a photocurable pressure-sensitive adhesive composition and a liquid crystal retardation layer, and capable of suppressing scratches on the liquid crystal retardation layer, and a method for producing the same.

[0009] Means for solving problems

[0010] The present invention provides the following optical layered body and a method for producing the same.

[0011] [1] An optical laminate comprising a pressure-sensitive adhesive layer and a first liquid crystal retardation layer with a substrate,

[0012] The adhesive layer is a cured layer of a photocurable adhesive composition.

[0013] The first liquid crystal retardation layer with a substrate includes a first liquid crystal retardation layer and a first substrate layer in this order from the adhesive layer side.

[0014] The first liquid crystal retardation layer includes a first polymer layer containing a polymer of a polymerizable liquid crystal compound.

[0015] The first substrate layer is releasable relative to the first liquid crystal retardation layer.

[0016] The first liquid crystal retardation layer with a substrate has a light transmittance Tx of 20% or more at a wavelength of 317 nm.

[0017] [2] The optical layered body according to [1], wherein the light transmittance Ts of the first substrate layer at a wavelength of 317 nm is 20% or more.

[0018] [3] The optical layered body according to [1] or [2], wherein the first substrate layer is a film substrate.

[0019] The resin constituting the above-mentioned film base material is triacetyl cellulose.

[0020] [4] The optical layered body according to any one of [1] to [3], wherein the thickness of the first substrate layer is 40 μm or less.

[0021] [5] The optical layered body according to any one of [1] to [4], wherein the first liquid crystal retardation layer has positive wavelength dispersion.

[0022] [6] The optical layered body according to any one of [1] to [5], wherein the first liquid crystal retardation layer is the first polymer layer.

[0023] [7] The optical laminate according to any one of [1] to [6], wherein the adhesive composition contains a photopolymerization initiator.

[0024] The remaining amount of the photopolymerization initiator in the tackiness adhesive layer is 0.050% by mass or less.

[0025] [8] The optical layered body according to any one of [1] to [7], wherein the thickness of the adhesive layer is 2 μm or more.

[0026] [9] The optical laminate according to any one of [1] to [8], wherein the adhesive composition contains a photopolymerization initiator.

[0027] The photopolymerization initiator has a maximum absorption wavelength within a wavelength range of 280 nm to 340 nm.

[0028]

[10] The optical layered body according to any one of [1] to [9], further comprising an optical film on the side of the adhesive layer opposite to the first liquid crystal retardation layer.

[0029]

[11] The optical laminate according to

[10] , wherein the optical film comprises at least one of a polarizing plate including a polarizing element and a second liquid crystal retardation layer,

[0030] The second liquid crystal retardation layer includes a second polymer layer containing a polymer of a polymerizable liquid crystal compound.

[0031]

[12] The optical laminate according to

[10] or

[11] , wherein the light transmittance Ty of the optical film is the same as or smaller than the light transmittance Tx of the first liquid crystal retardation layer with a substrate.

[0032]

[13] A method for producing an optical layered body, which is the method for producing an optical layered body according to any one of [1] to

[12] , comprising:

[0033] Step (S1) is to form a coating layer of the above-mentioned adhesive composition on the above-mentioned first liquid crystal phase difference layer side of the above-mentioned first liquid crystal phase difference layer with a substrate; and step (S2) is to irradiate the above-mentioned coating layer formed in the above-mentioned step (S1) with light through the above-mentioned first liquid crystal phase difference layer with a substrate, thereby forming the above-mentioned adhesive layer.

[0034]

[14] The method for producing an optical layered body according to

[13] , wherein the light is ultraviolet light,

[0035] The cumulative amount of light irradiated on the coating layer in the step (S2) is 10 mJ / cm 2 Above and 1000mJ / cm 2 the following.

[0036] Effects of the Invention

[0037] According to the present invention, it is possible to provide an optical layered body capable of suppressing the occurrence of scratches in a liquid crystal retardation layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a cross-sectional view schematically showing an optical layered body according to one embodiment of the present invention.

[0039] Figure 2 This is a cross-sectional view schematically showing an optical layered body according to another embodiment of the present invention.

[0040] Figure 3 This is a cross-sectional view schematically showing an optical layered body according to still another embodiment of the present invention. DETAILED DESCRIPTION

[0041] Hereinafter, preferred embodiments of an optical layered body and a method for producing the optical layered body will be described with reference to the drawings.

[0042] <Optical laminate>

[0043] Figures 1 to 3 : is a cross-sectional view schematically showing an optical laminate according to one embodiment of the present invention. Figures 1 to 3 As shown, the optical laminates 1 to 3 include a first tackiness adhesive layer 31 (tackiness adhesive layer) and a first liquid crystal retardation layer 13 with a substrate. The first tackiness adhesive layer 31 is a cured product layer of a photocurable tackiness adhesive composition.

[0044] The first liquid crystal retardation layer 13 with a substrate includes, in order from the first tackiness adhesive layer 31 side, the first liquid crystal retardation layer 11 and the first substrate layer 16. In the optical laminates 1 to 3, the first tackiness adhesive layer 31 is preferably in direct contact with the first liquid crystal retardation layer 11. In the first liquid crystal retardation layer 13 with a substrate, the first liquid crystal retardation layer 11 is preferably in direct contact with the first substrate layer 16.

[0045] The first liquid crystal retardation layer 11 includes a first polymer layer containing a polymerizable liquid crystal compound. The first liquid crystal retardation layer 11 is a first polymer layer, or a multilayer structure of a first polymer layer and a first orientation layer. The first substrate layer 16 is removable from the first liquid crystal retardation layer 11. When the first liquid crystal retardation layer is a multilayer structure, the first orientation layer is disposed on the first substrate layer 16 side, and the first polymer layer is disposed on the first tackiness adhesive layer 31 side.

[0046] The optical laminates 1 to 3 generally have a layer on the side of the first tackiness adhesive layer 31 opposite to the first liquid crystal retardation layer 11, and this layer may be the optical film 20. When the optical laminates 1 to 3 include the optical film 20, it is preferred that the optical film 20 and the first tackiness adhesive layer 31 are in direct contact.

[0047] In the optical laminates 1 to 3, the first liquid crystal retardation layer 13 with a substrate has a light transmittance Tx of 20% or greater at a wavelength of 317 nm. The light transmittance Tx is preferably 25% or greater, more preferably 30% or greater, 40% or greater, or 50% or greater, and is typically 90% or less. The light transmittance Tx can be measured by the method described in the Examples below.

[0048] As described below, the optical laminates 1 to 3 can be produced by laminating the first liquid crystal retardation layer 11 side of the first liquid crystal retardation layer 13 with a substrate with an optical film 20 and other layers via a coating layer of a photocurable adhesive composition, and curing the adhesive composition by irradiating the first liquid crystal retardation layer 13 with a substrate with light. By setting the transmittance Tx of the first liquid crystal retardation layer 13 with a substrate within the above range, the irradiated light easily passes through the first liquid crystal retardation layer 13 with a substrate, and the irradiated light easily reaches the coating layer of the adhesive composition, which allows the adhesive composition to react sufficiently, and easily produces a hard first adhesive layer 31.

[0049] After the first adhesive layer 31 is formed and the first substrate layer 16 is peeled off, the optical laminates 1 to 3 are further transported and provided for product processing, etc. During such product processing, if a conveying roller or the like comes into contact with the surface of the first liquid crystal phase difference layer 11 exposed by the peeling of the first substrate layer 16, scratches may sometimes be generated. For the optical laminates 1 to 3, as described above, the transmittance Tx of the first liquid crystal phase difference layer 13 with the substrate is within the above range, so that a hard first adhesive layer 31 formed by fully curing the adhesive composition can be obtained. The first liquid crystal phase difference layer 11 on the relatively hard first adhesive layer 31 is less likely to be scratched by contact with a conveying roller or the like than the first liquid crystal phase difference layer on the relatively soft first adhesive layer. Therefore, the optical laminates 1 to 3 can suppress the scratches generated in the first liquid crystal phase difference layer 11.

[0050] Since the light transmittance Tx of the first liquid crystal retardation layer 13 with a substrate is within the above range, when light is irradiated onto the adhesive composition隔着the first liquid crystal retardation layer 13 with a substrate, even if the cumulative light amount of the irradiated light is reduced, the adhesive composition can be sufficiently cured. Thereby, heat generated accompanying light irradiation can be suppressed, and thus generation of heat wrinkles in which the first liquid crystal retardation layer 13 with a substrate is deformed can also be suppressed. Heat wrinkles refer to a phenomenon in which the flatness of layers such as the film forming the optical laminate is impaired due to heat generated by the light source of light irradiation and the influence of curing shrinkage of the adhesive composition caused by light irradiation. For example, it refers to deformation occurring in a corrugated iron sheet shape (Japanese: トタン状) along the conveyance direction (processing direction) during the manufacture of the optical laminate. If deformation occurs, tunneling (Japanese: トンネリング) may occur in layers such as the first substrate layer that can be peeled off during the conveyance of the layers forming the optical laminate. If the deformation is maintained even after the first liquid crystal retardation layer 13 with a substrate is adhered to a polarizing plate or the like, unevenness is observed due to reflected light, or it is observed in a non-uniform form due to transmitted light, which is not preferable. Particularly, when the thickness of the adhesive layer is 1.0 μm or more and the thickness of the first substrate layer on the light irradiation side is 60 μm or less, the first substrate layer is liable to be deformed by heat.

[0051] In contrast, if the light transmittance Tx of the first liquid crystal retardation layer 13 with a substrate is lower than the above range, it is difficult for the irradiated light to pass through the first liquid crystal retardation layer 13 with a substrate, and it is difficult for the light to reach the coating layer of the adhesive composition. Therefore, the reaction of the adhesive composition is difficult to proceed. The reaction of the adhesive composition does not proceed sufficiently, and the first adhesive layer that is not sufficiently cured becomes soft. Scars are liable to occur when the first liquid crystal retardation layer on the soft first adhesive layer comes into contact with a conveyance roller or the like. Further, if the cumulative light amount of the irradiated light is increased in order to make the adhesive composition react sufficiently, the curing shrinkage accompanying the reaction of the adhesive composition increases, and heat wrinkles in which the first liquid crystal retardation layer with a substrate is deformed are liable to occur.

[0052] The optical laminates 1 to 3 can be used for a display device or the like described later. When the optical laminates 1 to 3 include the optical film 20, a laminate with an optical film (described later) obtained by peeling off the first substrate layer 16 can be applied to a display device or the like. The optical laminates 1 to 3 including the optical film 20 and the laminate with an optical film can be a retardation body including the first liquid crystal retardation layer 11 and the second liquid crystal retardation layer 21. The optical laminates 1 to 3 and the laminate with an optical film can include a polarizing element or a polarizing plate 50, and the first liquid crystal retardation layer 11( Figure 1 ), or can include a polarizing element or a polarizing plate 50, the first liquid crystal retardation layer 11, and the second liquid crystal retardation layer 21( Figure 2) Such optical layered bodies 1 to 3 and the layered body with an optical film can have an antireflection function and function as a circular polarizing plate.

[0053] (First Adhesive Layer)

[0054] As described above, the first adhesive layer 31 is a cured product layer of a photocurable adhesive composition. A photocurable adhesive composition generally contains a curable (polymerizable) compound, and preferably contains a photopolymerization initiator (described later).

[0055] The residual amount of the photopolymerization initiator in the first adhesive layer 31 is preferably 0.050% by mass or less, can be 0.030% by mass or less, can also be 0.020% by mass or less, more preferably 0.015% by mass or less, can be 0.010% by mass or less, further preferably 0.005% by mass or less, usually 0% by mass or more, and can be 0.0001% by mass or more. It is believed that by making the residual amount of the photopolymerization initiator in the first adhesive layer 31 within the above range, the reaction of the adhesive composition is fully carried out, forming a hard first adhesive layer 31. Therefore, by having a first adhesive layer 31 with a residual amount of the photopolymerization initiator within the above range, it is possible to further suppress the scratches generated on the surface of the first liquid crystal retardation layer 11.

[0056] The photopolymerization initiator contained in the adhesive composition preferably has a maximum absorption wavelength within a wavelength range of 280 nm to 340 nm. The maximum absorption wavelength of the photopolymerization initiator may be within a wavelength range of 280 nm to 330 nm, or within a wavelength range of 300 nm to 320 nm. By using a photopolymerization initiator having a maximum absorption wavelength within this range, it is easy to react the adhesive composition with light passing through the first liquid crystal retardation layer 13 with a substrate having the above-mentioned transmittance Tx. As a result, optical laminates 1 to 3 can be provided that can further suppress scratches generated on the surface of the first liquid crystal retardation layer 11.

[0057] The photopolymerization initiator preferably includes at least one of a photocationic polymerization initiator and a photoradical polymerization initiator, which will be described later. The amount of the photopolymerization initiator in the adhesive composition may be from 0.1 to 10 parts by mass, or from 1 to 8 parts by mass, relative to 100 parts by mass of the curable compound.

[0058] The thickness of the first adhesive layer 31 is preferably 2.0 μm or greater, more preferably 2.5 μm or greater, and can be 3.0 μm or greater. A thicker first adhesive layer 31 can further suppress scratches on the surface of the first liquid crystal retardation layer 11. A more detailed description of the first adhesive layer and the adhesive composition is provided below.

[0059] (First liquid crystal retardation layer with substrate)

[0060] The first liquid crystal retardation layer with a substrate comprises a first liquid crystal retardation layer 11 on a first substrate layer 16. The first liquid crystal retardation layer with a substrate can be obtained by coating a first liquid crystal retardation layer-forming composition containing a polymerizable liquid crystal compound on the first substrate layer 16 or on a first orientation layer 17 formed on the first substrate layer 16, and polymerizing the polymerizable liquid crystal compound in the coating layer. A detailed description of the method for producing the first liquid crystal retardation layer will be provided later.

[0061] (First liquid crystal phase difference layer)

[0062] The first liquid crystal phase difference layer 11 includes the first polymer layer as described above, and may further include the first orientation layer. The polymer contained in the first polymer layer is generally a polymer formed by polymerizing a polymerizable liquid crystal compound in an oriented state. As described later, the first polymer layer is formed by a composition for forming a first liquid crystal phase difference layer containing a polymerizable liquid crystal compound. The first polymer layer can be a layer that exhibits a phase difference. When the first liquid crystal phase difference layer 11 includes the first orientation layer, the first polymer layer and the first orientation layer are generally in direct contact. The first orientation layer is arranged on the first substrate layer 16 side of the first polymer layer.

[0063] The first liquid crystal retardation layer 11 is preferably a first polymer layer. This can further suppress scratches generated on the surface of the first liquid crystal retardation layer 11 exposed by peeling the first substrate layer 16 from the optical laminates 1 to 3 .

[0064] From the perspective of fully curing the adhesive composition when irradiated with light from the first liquid crystal retardation layer 13 side with a substrate, the first liquid crystal retardation layer 11 preferably has positive wavelength dispersion. This further reduces scratches on the surface of the first liquid crystal retardation layer 11 exposed after peeling the first substrate layer 16 from the optical laminates 1 to 3. Furthermore, the adhesion between the first liquid crystal retardation layer 11 and the optical film 20 can be improved. A more detailed description of the first liquid crystal retardation layer 11 will be provided later.

[0065] (First base material layer)

[0066] The first substrate layer 16 supports the first liquid crystal phase difference layer 11. The first substrate layer 16 can be peeled off relative to the first liquid crystal phase difference layer 11. The transmittance Ts of the first substrate layer 16 at a wavelength of 317 nm is preferably 20% or more, more preferably 25% or more, and can be 30% or more. By making the transmittance Ts of the first substrate layer 16 within the above range, it is easy to adjust the transmittance Tx of the first liquid crystal phase difference layer 13 with a substrate to the above range. It is believed that when the transmittance Ts of the first substrate layer 16 is within the above range, the first substrate layer 16 does not contain an ultraviolet absorber and has excellent transmittance to ultraviolet rays. The transmittance Ts of the first substrate layer 16 can be measured using the same method as the method for measuring the transmittance Tx of the first liquid crystal phase difference layer 13 with a substrate described in the embodiments described later.

[0067] The first substrate layer 16 is preferably a film substrate. The resin constituting the film substrate is preferably triacetylcellulose. This makes it easy to adjust the light transmittance Tx of the first liquid crystal retardation layer 13 with a substrate to the above range.

[0068] The thickness of the first substrate layer 16 is preferably 40 μm or less, can be 35 μm or less, can also be 30 μm or less, and is usually 10 μm or more. The thickness of the first substrate layer 16 is preferably 30 μm or more and 40 μm or less. By making the thickness of the first substrate layer 16 within the above range, the operability of the first liquid crystal phase difference layer 13 with a substrate is well maintained, and the transmittance Tx of the first liquid crystal phase difference layer 13 with a substrate is easily adjusted to the above range. A more detailed description of the first substrate layer 16 is described later.

[0069] (Optical Film)

[0070] Examples of the optical film 20 include a polarizing element, a polarizing plate 50 including a polarizing element, a second liquid crystal phase difference layer 21, or a combination thereof. The optical film 20 preferably includes at least one of the polarizing plate 50 and the second liquid crystal phase difference layer 21 ( Figure 1 and Figure 2 ), and may also include both the polarizing plate 50 and the second liquid crystal phase difference layer 21 ( Figure 3 In the case of including such an optical film 20 , in order to obtain the optical laminates 1 to 3 capable of suppressing scratches on the surface of the first liquid crystal retardation layer 13 , it is preferable to set the light transmittance Tx of the first liquid crystal retardation layer 13 with a substrate to the above range.

[0071] The optical film 20 may be a second liquid crystal phase difference layer 23 with a substrate ( Figure 2). The second liquid crystal retardation layer 23 with a substrate includes a second substrate layer 26 and a second liquid crystal retardation layer 21. In the second liquid crystal retardation layer 23 with a substrate, the second liquid crystal retardation layer 21 is preferably in direct contact with the second substrate layer 26, and the second substrate layer 26 may be peelable relative to the second liquid crystal retardation layer 21. In the case where the optical film 20 is the second liquid crystal retardation layer 23 with a substrate, the optical laminate 2 generally includes the second liquid crystal retardation layer 21 and the second substrate layer 26 in this order from the first tackiness adhesive layer 31 side.

[0072] The second liquid crystal phase difference layer 21 has a second polymer layer of a polymer containing a polymerizable liquid crystal compound. The second liquid crystal phase difference layer 21 is a second polymer layer, or a multilayer body of a second polymer layer and a second orientation layer. The polymer contained in the second polymer layer is usually a polymer formed by polymerizing a polymerizable liquid crystal compound in an oriented state. As described later, the second polymer layer is formed by a composition for forming a second liquid crystal phase difference layer containing a polymerizable liquid crystal compound. The second polymer layer can be a layer that exhibits a phase difference. In the case where the second liquid crystal phase difference layer 21 includes a second orientation layer, the second polymer layer is usually in direct contact with the second orientation layer. As Figure 2 As shown, when the optical film 20 has the second liquid crystal phase difference layer 21 and the second base material layer 26, it is preferred that the second polymer layer be disposed on the first adhesive layer 31 side and the second orientation layer be disposed on the second base material layer 26 side. Figure 2 The optical stack 2 shown is used for the optical stack 3 ( Figure 3 ), from the perspective of fully curing the adhesive composition between the second liquid crystal phase difference layer 21 and the polarizing plate 50 as described later, the second liquid crystal phase difference layer 21 is preferably positive wavelength dispersion.

[0073] like Figure 3 As shown, the optical film 20 may include a second liquid crystal phase difference layer 21 and a polarizing plate 50 in this order from the first adhesive layer 31 side. The second liquid crystal phase difference layer 21 and the polarizing plate 50 may be laminated via the second adhesive layer 32. In this case, it is preferred that the second liquid crystal phase difference layer 21 is in direct contact with the second adhesive layer 32, and it is preferred that the second adhesive layer 32 is in direct contact with the polarizing plate 50. Figure 3In the optical laminate 3 shown, the second liquid crystal phase difference layer 21 can be a positive wavelength dispersion. As described later, when forming the second adhesive layer 32 between the second liquid crystal phase difference layer 21 and the polarizing plate 50, when the adhesive composition between the second liquid crystal phase difference layer 21 and the polarizing plate 50 is irradiated with light via the first liquid crystal phase difference layer 13 side of the tape substrate to cure it, from the viewpoint of fully curing the adhesive composition, the second liquid crystal phase difference layer 21 is preferably a positive wavelength dispersion. As a result, it is possible to further suppress the scratches generated on the surface of the first liquid crystal phase difference layer 11 exposed by peeling off the first substrate layer 16 from the optical laminate 3. In addition, the adhesion between the second liquid crystal phase difference layer 21 and the polarizing plate 50 can also be improved.

[0074] The transmittance Ty of the optical film 20 is preferably equal to or less than the transmittance Tx of the first liquid crystal retardation layer 13 with a substrate. When such an optical film 20 is provided, in order to obtain optical laminates 1 to 3 that can suppress scratches on the surface of the first liquid crystal retardation layer 13, it is preferable to set the transmittance Tx of the first liquid crystal retardation layer 13 with a substrate within the above range. The transmittance Ty of the optical film 20 can be measured by the method described in the Examples below and is the transmittance at a wavelength of 317 nm. A more detailed description of the optical film 20, polarizing plate 50, and second liquid crystal retardation layer 21 will be provided below.

[0075] In the optical laminate 3 ( Figure 3 ), the laminated portion (hereinafter also referred to as "retarder R") in which the first liquid crystal retardation layer 13 with a substrate, the first adhesive layer 31, and the second liquid crystal retardation layer 21 are laminated in this order has a light transmittance at a wavelength of 317 nm of preferably 3% or more, 5% or more, 10% or more, and usually 30% or less. The light transmittance of the retardation body R can be measured by the method described in the transmittances Tx and Ty described in the examples below.

[0076] When the second tackiness adhesive layer 32 of the optical laminate 3 is a cured product of a tackiness adhesive composition containing a photopolymerization initiator, the remaining amount of the photopolymerization initiator in the second tackiness adhesive layer 32 may be, for example, 0.10% by mass or less, 0.080% by mass or less, 0.050% by mass or less, 0.030% by mass or less, 0.010% by mass or less, or 0.005% by mass or less, and is typically 0% by mass or more, or 0.001% by mass or more. The remaining amount of the photopolymerization initiator in the second tackiness adhesive layer 32 may be greater than the remaining amount of the photopolymerization initiator in the first tackiness adhesive layer 31.

[0077] (Laminate with optical film)

[0078] The laminate with an optical film generally comprises an optical film 20, a first tackiness adhesive layer 31, and a first liquid crystal retardation layer 11 in this order. When the optical film 20 includes a polarizing plate 50 or a second liquid crystal retardation layer 21, the laminate with an optical film may comprise the polarizing plate 50, the first tackiness adhesive layer 31, and the first liquid crystal retardation layer 11 in this order, or may comprise the second substrate layer 26, the second liquid crystal retardation layer 21, the first tackiness adhesive layer 31, and the first liquid crystal retardation layer 11 in this order. When the optical film 20 includes a polarizing plate 50 and a second liquid crystal retardation layer 21, the laminate with an optical film may comprise the polarizing plate 50, the second tackiness adhesive layer 32, the second liquid crystal retardation layer 21, the first tackiness adhesive layer 31, and the first liquid crystal retardation layer 11 in this order.

[0079] <Method for producing an optical layered body>

[0080] The method for producing the optical layered bodies 1 to 3 includes:

[0081] Step (S1) of forming a first coating layer (coating layer) of an adhesive composition on the first liquid crystal retardation layer 11 side of the first liquid crystal retardation layer 13 with a substrate;

[0082] In step ( S2 ), the first coating layer formed in step ( S1 ) is irradiated with light via the first liquid crystal retardation layer 13 with a substrate, thereby forming a first tacky adhesive layer 31 .

[0083] As described above, the transmittance Tx of the first liquid crystal retardation layer 13 with a substrate is 20% or greater. Therefore, even when the first coating layer on the first liquid crystal retardation layer 13 with a substrate is irradiated with light through the first liquid crystal retardation layer 13 with a substrate, a first adhesive layer 31 can be obtained in which the adhesive composition is fully cured. When the adhesive composition contains a photopolymerization initiator, the excess amount of the photopolymerization initiator in the first adhesive layer 31 can be reduced.

[0084] The light irradiated in step (S2) is preferably ultraviolet light. Since the ultraviolet transmittance of the first liquid crystal phase difference layer 13 with a substrate is large, the cumulative light intensity of the light irradiated to the first coating layer in step (S2) can be reduced. The cumulative light intensity of the light irradiated to the first coating layer in step (S2) is, for example, 10 mJ / cm 2 Above and 1000mJ / cm 2 Below, it can also be a smaller cumulative light amount in this range, preferably 10mJ / cm 2 Above and 300mJ / cm 2 Below, it can be 30mJ / cm 2 Above and 200mJ / cm 2 Below, more preferably 50mJ / cm 2Above and 125mJ / cm 2 In the manufacturing method of the optical laminates 1 to 3, even if the cumulative amount of irradiated light is small, the adhesive composition can be fully cured. Therefore, the first liquid crystal retardation layer 13 with a substrate can be prevented from being deformed by heat generated by irradiation with ultraviolet light (heat generated by a lamp, etc.) and the curing shrinkage of the adhesive composition due to light irradiation, thereby suppressing the generation of heat wrinkles. In addition, the first liquid crystal retardation layer 13 can be prevented from being scratched during product processing.

[0085] On the side of the first coating layer opposite to the first liquid crystal retardation layer 11, a layer such as an optical film is typically laminated, which is bonded to the first liquid crystal retardation layer 11 using a pressure-sensitive adhesive composition. In the case where this layer is the optical film 20, the first coating layer of the pressure-sensitive adhesive composition may be formed between the optical film 20 and the first liquid crystal retardation layer 11. The first coating layer may be formed on the first liquid crystal retardation layer 13 with a substrate and then laminated with the optical film 20, the first coating layer may be formed on the optical film 20 and then laminated with the first liquid crystal retardation layer 13 with a substrate, or the first coating layer may be formed on both the first liquid crystal retardation layer 13 with a substrate and the optical film 20 and then laminated.

[0086] The 1st liquid crystal phase difference layer with substrate in the past has a small light transmittance, so it is difficult to irradiate light across the 1st liquid crystal phase difference layer with substrate, and obtain the adhesive layer formed by fully solidifying the adhesive composition of active energy ray curing type adhesive composition and light-curing type. Therefore, due to the polymerization initiator etc. remaining in the adhesive layer, when carrying out durability test etc., sometimes the undesirable conditions such as optical characteristics reduction are produced. In contrast, the light transmittance of the 1st liquid crystal phase difference layer with substrate of the present embodiment is large, so light irradiation is carried out across the 1st liquid crystal phase difference layer with substrate, so as to obtain the 1st adhesion adhesive layer fully solidified by the above-mentioned adhesive composition. In addition, when the 1st liquid crystal phase difference layer, the 1st adhesion adhesive layer and the 2nd liquid crystal phase difference layer are formed using the 1st liquid crystal phase difference layer with substrate (phase difference body R), it is also possible to increase the light transmittance of phase difference body R. Therefore, when a photocurable adhesive composition, such as an active energy ray-curable adhesive composition or a photocurable adhesive composition, is used to bond the phase difference body R to the polarizer, a fully cured second adhesive layer can be easily formed. This makes it possible to thin the optical laminate comprising the first liquid crystal phase difference layer, the second liquid crystal phase difference layer, and the polarizer, thereby achieving improved bendability, suppressed curling, and improved durability due to the improved barrier properties brought about by the first and second adhesive layers.

[0087] Figure 3The optical laminate 3 shown can be obtained by laminating the phase difference body R and the polarizing element as described above. In this case, the phase difference body R can be made of Figure 2 The optical laminate 2 shown is a phase difference body obtained by peeling off the second substrate layer. The manufacturing method of the optical laminate 3 may include, for example:

[0088] Step (S11), preparing an optical laminate 2;

[0089] Step ( S12 ) of peeling the second substrate layer 26 from the optical laminate 2 to obtain a retardation body R in which the first liquid crystal retardation layer 13 with a substrate, the first adhesive layer 31 and the second liquid crystal retardation layer 21 are laminated in this order;

[0090] Step (S13), laminating the second liquid crystal retardation layer 21 side of the retardation body R and the polarizing element via the second coating layer of the adhesive composition; and

[0091] In step ( S14 ), the second coating layer formed in step ( 13 ) is irradiated with light via the phase difference body R to form the second tack adhesive layer 32 .

[0092] Step (S11) may be a step of preparing the optical laminate 2 through the above-mentioned steps (S1) and (S2). When the second substrate layer 26 is peeled off in step (S12), only the second substrate layer 26 may be peeled off, or the second orientation layer and the second substrate layer 26 may be peeled off together.

[0093] In process (S13), a second coating layer of the adhesive composition can be formed on the second liquid crystal phase difference layer 21 of the phase difference body R, a second coating layer of the adhesive composition can be formed on the polarizing element, or a second coating layer of the adhesive composition can be formed on both.

[0094] The light irradiated in the process (S14) is preferably ultraviolet light. As described above, since the transmittance of the phase difference body R is large, even when the second coating layer is irradiated with light from the phase difference body R side, the second adhesive layer 32 in which the adhesive composition is fully cured can be obtained. In addition, the cumulative light amount of the light irradiated to the second coating layer in the process (S14) can be reduced. In the case where the adhesive composition contains a photopolymerization initiator, the remaining amount of the photopolymerization initiator in the second adhesive layer 32 can also be reduced. The cumulative light amount of the light irradiated to the second coating layer in the process (S14) can be set to the cumulative light amount described in the above process (S2).

[0095] <Method for producing a laminate with an optical film>

[0096] The method for producing a laminate with an optical film includes peeling the first substrate layer 16 from the optical laminates 1 to 3 including the optical film 20. When peeling the first substrate layer 16, only the first substrate layer 16 may be peeled off, or the first orientation layer and the first substrate layer 16 may be peeled off together.

[0097] <Display device>

[0098] The optical laminates 1 to 3 can be applied to a display device by peeling off the first substrate layer 16. The display device can include a laminate with an optical film and an image display element (such as an organic EL display element). The laminate with an optical film is placed on the visible side of the image display element. The laminate with an optical film can be attached to the image display element using an adhesive layer.

[0099] The display device is not particularly limited, and examples thereof include display devices such as organic electroluminescent (organic EL) display devices, inorganic electroluminescent (inorganic EL) display devices, liquid crystal display devices, and electroluminescent display devices.

[0100] Display devices can be used in mobile devices such as smartphones and tablets, televisions, digital photo frames, electronic signage, measuring instruments, office equipment, medical equipment, and electronic computing equipment.

[0101] Hereinafter, details of each layer constituting the optical layered body and a method for producing each layer will be described.

[0102] <Adhesive Layers (First Adhesive Layer, Second Adhesive Layer)>

[0103] The first tackiness adhesive layer is suitable for use when laminating the optical film to the first liquid crystal retardation layer. The second tackiness adhesive layer is suitable for use when laminating components constituting the optical film (e.g., a polarizing plate and a second liquid crystal retardation layer). The first tackiness adhesive layer for laminating the first liquid crystal retardation layer to the second liquid crystal retardation layer is preferably an adhesive layer described below.

[0104] The adhesive layer (first adhesive layer or second adhesive layer) is an adhesive layer or an adhesive layer, and can be formed of an adhesive composition. The adhesive composition is an adhesive composition or an adhesive composition.

[0105] (Adhesive layer)

[0106] Adhesive layer shows adhesion by attaching itself to adherend, and is called so-called pressure-sensitive adhesive.As the adhesive composition forming adhesive layer, the adhesive composition with excellent optical transparency known in the past can be used without particular restriction, for example, the adhesive composition with base polymers such as acrylic resin, urethane resin, silicone resin, polyvinyl ether resin can be used. In addition, it can also be active energy ray curing type adhesive composition, thermosetting adhesive composition etc. Wherein, the adhesive composition with the acrylic resin excellent in transparency, adhesion, re-peelability, weather resistance, heat resistance etc. as base polymer is suitable.

[0107] The adhesive composition may further include a cross-linking agent, a silane compound, an antistatic agent, and the like.

[0108] The (meth)acrylic resin contained in the adhesive composition is preferably a polymer (hereinafter also referred to as a "(meth)acrylate polymer") having as a main component a structural unit derived from an alkyl (meth)acrylate represented by the following formula (I) (hereinafter also referred to as "structural unit (I)"). For example, the structural unit contains 50 parts by mass or more with respect to 100 parts by mass of the structural unit of the (meth)acrylic resin.

[0109] In addition, in this specification, (meth)acrylic resin means at least one of acrylic resin and methacrylic resin. The same applies to (meth)acrylate and (meth)acryloyl.

[0110] [Chemical Formula 1]

[0111]

[0112] [In formula (I),

[0113] R 10 represents a hydrogen atom or a methyl group, R 20 It represents an alkyl group having 1 to 20 carbon atoms. The alkyl group may have any structure including linear, branched, and cyclic. The hydrogen atoms of the alkyl group may be substituted by an alkoxy group having 1 to 10 carbon atoms.]

[0114] Examples of the (meth)acrylate represented by formula (X) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, stearyl (meth)acrylate, and t-butyl (meth)acrylate. Specific examples of the alkyl acrylate containing an alkoxy group include 2-methoxyethyl (meth)acrylate and ethoxymethyl (meth)acrylate. Among these, it is preferable to contain n-butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate, and it is particularly preferable to contain n-butyl (meth)acrylate.

[0115] The (meth)acrylate polymer may contain structural units derived from other monomers in addition to the structural unit (I). The structural units derived from other monomers may be one type or two or more types. Examples of other monomers that may be contained in the (meth)acrylate polymer include monomers having polar functional groups, monomers having aromatic groups, and acrylamide monomers.

[0116] Examples of monomers having a polar functional group include (meth)acrylates having a polar functional group. Examples of polar functional groups include hydroxyl groups, carboxyl groups, substituted or unsubstituted amino groups substituted with an alkyl group having 1 to 6 carbon atoms, and heterocyclic groups such as epoxy groups.

[0117] The content of the structural unit derived from the monomer having a polar functional group in the (meth)acrylate polymer is preferably 10 parts by mass or less, more preferably 0.5 parts by mass or more and 10 parts by mass or less, further preferably 0.5 parts by mass or more and 5 parts by mass or less, and particularly preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylate polymer.

[0118] Examples of the monomer having an aromatic group include (meth)acrylates having one (meth)acryloyl group and one or more aromatic rings (eg, a benzene ring, a naphthalene ring, etc.) in the molecule, and having a phenyl group, a phenoxyethyl group, or a benzyl group.

[0119] The content of the structural unit derived from the monomer having an aromatic group in the (meth)acrylate polymer is preferably 20 parts by mass or less, more preferably 4 parts by mass or more and 20 parts by mass or less, and even more preferably 4 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylate polymer.

[0120] Examples of acrylamide monomers include N-(methoxymethyl)acrylamide, N-(ethoxymethyl)acrylamide, N-(propyloxymethyl)acrylamide, N-(butoxymethyl)acrylamide, and N-(2-methylpropyloxymethyl)acrylamide. The inclusion of these structural units can suppress the bleeding of additives such as antistatic agents described below.

[0121] Furthermore, structural units derived from monomers other than the structural unit (I) may include structural units derived from styrene-based monomers, structural units derived from vinyl-based monomers, and structural units derived from monomers having multiple (meth)acryloyl groups in the molecule.

[0122] The weight average molecular weight (hereinafter also referred to as "Mw") of the (meth)acrylic resin is preferably 500,000 to 2.5 million. If the weight average molecular weight is 500,000 or more, the durability of the adhesive layer in a high temperature and high humidity environment can be improved. If the weight average molecular weight is 2.5 million or less, the operability when applying the coating liquid containing the adhesive composition becomes good. The molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight (Mw) to the number average molecular weight (hereinafter also referred to as "Mn") is usually 2 to 10. In this specification, the "weight average molecular weight" and the "number average molecular weight" are polystyrene conversion values ​​measured by gel permeation chromatography (GPC).

[0123] When a (meth)acrylic resin is dissolved in ethyl acetate to form a 20% by mass solution, its viscosity at 25°C is preferably 20 Pa·s or less, more preferably 0.1 to 15 Pa·s. A (meth)acrylic resin having a viscosity at 25°C within this range contributes to improved durability and reworkability of optical laminates and laminates with optical films that include a pressure-sensitive adhesive layer formed using this resin. This viscosity can be measured using a Brookfield viscometer.

[0124] The glass transition temperature (Tg) of the (meth)acrylic resin is, for example, -60 to 20° C., preferably -50 to 15° C., more preferably -45 to 10° C., and further preferably -40 to 0° C. The glass transition temperature can be measured using a differential scanning calorimeter (DSC).

[0125] The (meth)acrylic resin may contain two or more (meth)acrylate polymers. Examples of such (meth)acrylate polymers include relatively low molecular weight (meth)acrylate polymers having a weight average molecular weight of 50,000 to 300,000, which are mainly composed of the structural unit (I) derived from the (meth)acrylate.

[0126] (Meth)acrylic resins can generally be produced by known polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization. In the production of (meth)acrylic resins, polymerization is generally carried out in the presence of a polymerization initiator. The amount of polymerization initiator used is generally 0.001 to 5 parts by mass relative to 100 parts by mass of all monomers constituting the (meth)acrylic resin. (Meth)acrylic resins can also be produced by polymerization using active energy rays such as ultraviolet rays.

[0127] The adhesive composition preferably contains a crosslinking agent. Examples of the crosslinking agent include conventional crosslinking agents (e.g., isocyanate compounds, epoxy compounds, aziridine compounds, metal chelate compounds, peroxides, etc.). In particular, isocyanate compounds are preferred from the viewpoints of the pot life and crosslinking speed of the adhesive composition, and the durability of the optical laminate and the laminate with the optical film.

[0128] An isocyanate compound is a compound having at least two isocyanate groups (-NCO) in its molecule. Specifically, examples include toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, naphthalene diisocyanate, and triphenylmethane triisocyanate. Examples also include adducts obtained by reacting these isocyanate compounds with polyols such as glycerol and trimethylolpropane, and dimers and trimers of these isocyanate compounds. Two or more isocyanate compounds may be used in combination.

[0129] The content of the crosslinking agent in the adhesive composition is, for example, 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 1 part by mass relative to 100 parts by mass of the (meth)acrylic resin.

[0130] The adhesive composition may further contain a silane compound. Examples of the silane compound include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylethoxydimethylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. The silane compound may include oligomers derived from the above-mentioned silane compounds.

[0131] The content of the silane compound in the adhesive composition is generally 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin. If the content of the silane compound is 0.01 parts by mass or greater, the adhesion between the adhesive layer and the adherend tends to be improved, while if the content is 10 parts by mass or less, the bleeding of the silane compound from the adhesive layer tends to be suppressed.

[0132] The adhesive composition may further include an antistatic agent. As the antistatic agent, known antistatic agents can be mentioned, and ionic antistatic agents are suitable. As cationic components constituting the ionic antistatic agent, organic cations and inorganic cations can be mentioned. As organic cations, pyridinium cations, imidazolium cations, ammonium cations, sulfonium cations, phosphonium cations, etc. can be mentioned. As inorganic cations, alkali metal cations such as lithium cations, potassium cations, sodium cations, and cesium cations, alkaline earth metal cations such as magnesium cations and calcium cations can be mentioned. As anionic components constituting the ionic antistatic agent, any one of inorganic anions and organic anions can be mentioned. From the perspective of excellent antistatic performance, anionic components containing fluorine atoms are preferred. As anionic components containing fluorine atoms, hexafluorophosphate anion (PF6 - ), bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N - ]、bis(fluorosulfonyl)imide anion [(FSO2)2N - ] anions, etc.

[0133] From the viewpoint of excellent temporal stability of the antistatic performance of the pressure-sensitive adhesive composition, an ionic antistatic agent that is solid at room temperature is preferred.

[0134] The content of the antistatic agent in the pressure-sensitive adhesive composition is, for example, 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 1 to 7 parts by mass relative to 100 parts by mass of the (meth)acrylic resin.

[0135] The adhesive composition may contain additives such as ultraviolet absorbers, solvents, crosslinking catalysts, tackifying resins (tackifiers), and plasticizers, either alone or in combination. It is also useful to add an ultraviolet curable compound to the adhesive composition and then irradiate the adhesive layer with ultraviolet light to cure it, thereby forming a harder adhesive layer.

[0136] The adhesive layer can be formed by, for example, dissolving or dispersing the adhesive composition in a solvent to prepare a solvent-containing adhesive composition, applying the solvent-containing adhesive composition to the surface of the layer where the adhesive layer is to be provided, and drying the solvent-containing adhesive composition.

[0137] The thickness of the adhesive layer is usually 0.1 μm to 30 μm, preferably 3 μm to 30 μm, more preferably 5 μm to 25 μm, and particularly preferably 5 μm to 10 μm.

[0138] Since the thickness of the first liquid crystal phase difference layer of the optical laminate is small, the thickness of the optical laminate is also reduced. When the optical laminate has an adhesive layer, it is preferred that the storage modulus G' of the adhesive layer at a temperature of 23°C is also small. As a result, it is easy to suppress the occurrence of scratches in the first liquid crystal phase difference layer 11 during product processing, etc. The storage modulus G' of the adhesive layer at a temperature of 23°C is preferably 5 MPa or less, more preferably 1 MPa or less, further preferably 0.5 MPa or less, further preferably 0.2 MPa or less, and particularly preferably 0.1 MPa or less. The storage modulus G' of the adhesive layer at a temperature of 23°C is generally 0.001 MPa or more, and can be 0.01 MPa or more. The storage modulus G' can be measured at a temperature of 23°C according to JIS K7244-6 using a viscoelasticity measuring device (manufactured by Physica, MCR300) by a torsional shear method (normal force FN: 1 N, strain γ: 1%, frequency: 1 Hz).

[0139] (Adhesive layer)

[0140] The adhesive layer may have the functions of bonding the polarizer to the polarizer protective film, bonding the optical film to the first liquid crystal retardation layer, bonding the components constituting the optical film (e.g., the polarizing plate and the second liquid crystal retardation layer), etc. The adhesive layer may be formed from an adhesive composition.

[0141] Examples of adhesive compositions include water-based adhesive compositions and curable adhesive compositions that cure by heating or exposure to active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. Examples of water-based adhesive compositions include compositions in which a polyvinyl alcohol-based resin or a urethane resin as a main component is dissolved in water, and compositions in which a polyvinyl alcohol-based resin or a urethane resin as a main component is dispersed in water. Water-based adhesive compositions may further contain curable components such as polyaldehydes, melamine-based compounds, zirconium oxide compounds, zinc compounds, glyoxal compounds, and water-soluble epoxy resins, as well as crosslinking agents. Examples of the water-based adhesive composition include the adhesive composition described in JP-A-2010-191389, the adhesive composition described in JP-A-2011-107686, the composition described in JP-A-2020-172088, and the composition described in JP-A-2005-208456.

[0142] The curable adhesive composition is preferably an active energy ray-curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. The active energy ray-curable adhesive composition is more preferably a photocurable adhesive composition that is cured by irradiation with ultraviolet rays or visible light. Examples of active energy ray-curable adhesive compositions and photocurable adhesive compositions include cationic polymerizable adhesive compositions containing a cationic polymerizable compound as a curable compound, free radical polymerizable adhesive compositions containing a free radical polymerizable compound as a curable compound, and mixed adhesive compositions containing both a cationic polymerizable compound and a free radical polymerizable compound as curable compounds.

[0143] The cationically polymerizable compound is a compound or oligomer that is cured by cation polymerization reaction when irradiated with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or heated. Specific examples thereof include epoxy compounds, oxetane compounds, and vinyl compounds.

[0144] Examples of epoxy compounds include alicyclic epoxy compounds (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule) such as 3,4-epoxycyclohexylmethyl 3',4'-epoxycyclohexanecarboxylate; aromatic epoxy compounds (compounds having an aromatic ring and an epoxy group in the molecule) such as diglycidyl ether of bisphenol A; and aliphatic epoxy compounds (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule) such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether.

[0145] Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.

[0146] The cationic polymerization type adhesive composition preferably contains a cationic polymerization initiator. The cationic polymerization initiator may be a thermal cationic polymerization initiator or a photocationic polymerization initiator. Examples of cationic polymerization initiators include aromatic diazonium salts such as benzene diazonium hexafluoroantimonate; aromatic iodonium salts such as diphenyl iodonium tetrakis(pentafluorophenyl)borate; aromatic sulfonium salts such as triphenylsulfonium hexafluorophosphate; iron-arene complexes such as ditoluene-cyclopentadienyl iron (II) hexafluoroantimonate, etc. The content of the cationic polymerization initiator in the adhesive composition is generally 0.1 to 10 parts by mass relative to 100 parts by mass of the cationic polymerizable compound. Two or more cationic polymerization initiators may be included.

[0147] Examples of the cationically polymerizable adhesive composition include the cationically polymerizable compositions described in JP-A-2021-113969.

[0148] Free radical polymerizable compounds are compounds or oligomers that cure by undergoing a free radical polymerization reaction upon irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or upon heating. Specifically, compounds having an ethylenically unsaturated bond are exemplified. Examples of compounds having an ethylenically unsaturated bond include (meth)acrylic compounds having one or more (meth)acryloyl groups in the molecule and vinyl compounds having one or more vinyl groups in the molecule.

[0149] Examples of the (meth)acrylic compound include (meth)acrylic oligomers having at least two (meth)acryloyl groups in a molecule obtained by reacting two or more (meth)acrylic acid ester monomers, (meth)acrylamide monomers, and functional group-containing compounds having at least one (meth)acryloyloxy group in the molecule.

[0150] The radical polymerization adhesive composition preferably contains a radical polymerization initiator. The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator. Examples of radical polymerization initiators include: acetophenone-based initiators such as acetophenone and 3-methylacetophenone; benzophenone-based initiators such as benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; thioxanthone-based initiators such as 4-isopropylthioxanthone; xanthone, fluorenone, and the like. The content of the radical polymerization initiator in the adhesive composition is typically 0.1 to 10 parts by mass per 100 parts by mass of the radical polymerizable compound. Two or more radical polymerization initiators may be included.

[0151] Examples of the radical polymerizable adhesive composition include radical polymerizable compositions described in JP-A-2016-126345, JP-A-2016-153474, and International Publication No. 2017 / 183335.

[0152] Active energy ray-curable adhesive compositions and photocurable adhesive compositions may contain additives such as ion trapping agents, antioxidants, chain transfer agents, tackifiers, thermoplastic resins, fillers, flow regulators, plasticizers, defoamers, antistatic agents, leveling agents, and solvents as needed.

[0153] The bonding of two layers using an adhesive layer can be carried out as follows: an adhesive composition is applied to at least one bonding surface selected from the respective bonding surfaces of the two layers, the two layers are overlapped with the aid of the coating layer of the adhesive composition, and after bonding them from top and bottom using a bonding roller, the coating layer is dried, irradiated with active energy rays to cure it, or heated to cure it.

[0154] Before forming the coating layer of the adhesive composition, at least one of the bonding surfaces of the two layers may be subjected to an adhesion-facilitating treatment such as saponification treatment, corona treatment, plasma treatment, primer treatment, or anchor coating treatment.

[0155] The coating layer of the adhesive composition can be formed using various coating methods such as a die coater, a comma coater, a gravure coater, a wire bar coater, and a knife coater.

[0156] The irradiation intensity of the active energy ray during irradiation is determined according to the composition of the active energy ray-curable adhesive composition or the photocurable adhesive composition and is not particularly limited, but is preferably 10 mW / cm 2 Above 1000mW / cm 2The following should be noted that the irradiation intensity is preferably an intensity in the wavelength region effective for activating a photopolymerization initiator such as a photocationic polymerization initiator or a photoradical polymerization initiator. Irradiation is performed once or multiple times at such an intensity so that the cumulative light amount is preferably 10 mJ / cm 2 More than 100 mJ / cm 2 Above and 1000mJ / cm 2 the following.

[0157] The light source used for polymerization and curing of active energy ray-curable adhesive compositions and photocurable adhesive compositions is not particularly limited, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.

[0158] The thickness of the adhesive layer formed from the water-based adhesive composition may be, for example, 5 μm or less, preferably 1 μm or less, more preferably 0.5 μm or less, and may be 0.01 μm or more, preferably 0.05 μm or more.

[0159] The thickness of the adhesive layer formed from the active energy ray-curable adhesive composition or the photocurable adhesive composition can be, for example, 10 μm or less, preferably 5 μm or less, more preferably 3 μm or less, and can be 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more.

[0160] <First Liquid Crystal Retardation Layer, Second Liquid Crystal Retardation Layer>

[0161] The first liquid crystal retardation layer and the second liquid crystal retardation layer respectively include a first polymer layer and a second polymer layer (hereinafter also referred to as "polymer layer"), each of which is a polymer containing a polymerizable liquid crystal compound. The first liquid crystal retardation layer may be a multilayer structure of the first polymer layer and the first orientation layer, and the second liquid crystal retardation layer may be a multilayer structure of the second polymer layer and the second orientation layer.

[0162] The first liquid crystal phase difference layer is formed by coating a first liquid crystal phase difference layer forming composition comprising a polymerizable liquid crystal compound on a first substrate layer or a first orientation layer to form an oriented polymer of the polymerizable liquid crystal compound. The second liquid crystal phase difference layer is formed by coating a second liquid crystal phase difference layer forming composition comprising a polymerizable liquid crystal compound on a second substrate layer or a second orientation layer to form an oriented polymer of the polymerizable liquid crystal compound. The formation of the liquid crystal phase difference layer in this way is preferred in terms of thinness and the ability to arbitrarily design wavelength dispersion characteristics. The first liquid crystal phase difference layer forming composition and the second liquid crystal phase difference layer forming composition may each independently further comprise a solvent, a photopolymerization initiator, a photosensitizer, an antioxidant, a leveling agent, a sealing agent, and the like.

[0163] The liquid crystal phase difference layer (the first liquid crystal phase difference layer or the second liquid crystal phase difference layer) is usually a film formed by solidifying a polymerizable liquid crystal compound in an oriented state. In order to produce a phase difference in the visible surface, it usually includes a polymer layer (the first polymer layer or the second polymer layer) formed by a solidified film formed by polymerizing polymerizable groups in a state where the polymerizable liquid crystal compound is oriented horizontally relative to the surface of the substrate layer (the first substrate layer or the second substrate layer). In this case, when the polymerizable liquid crystal compound is a rod-shaped liquid crystal, a positive A plate can be used, and when the polymerizable liquid crystal compound is a disc-shaped liquid crystal, a negative A plate can be used.

[0164] The optical stack and the stack with an optical film may include a polarizing element and a first liquid crystal phase difference layer, and have an anti-reflection function. In order to make the optical stack and the stack with an optical film highly realize the anti-reflection function, it is sufficient to have a λ / 4 plate function (i.e., a phase difference function of π / 2) in the entire visible light region. Specifically, it is preferred to have a λ / 4 layer with inverse wavelength dispersion, or it is preferred to combine two or more liquid crystal phase difference layers with different orientations. For example, a liquid crystal phase difference layer with a λ / 2 plate function (i.e., a phase difference function of π) can be combined with a liquid crystal phase difference layer with a λ / 4 plate function (i.e., a phase difference function of π / 2).

[0165] From the perspective of being able to compensate for the anti-reflection function in the oblique direction, the optical laminate and the laminate with an optical film preferably further include a layer having anisotropy in the thickness direction (positive C plate). In addition, each liquid crystal retardation layer can be tilted or cholesteric.

[0166] When the optical laminate or laminate with an optical film has an antireflection function and functions as a circular polarizing plate, the first liquid crystal retardation layer is preferably a λ / 4 liquid crystal retardation layer that provides a phase difference of λ / 4. When the optical laminate or laminate with an optical film has a first liquid crystal retardation layer and a second liquid crystal retardation layer and functions as a circular polarizing plate, [i] the first liquid crystal retardation layer and the second liquid crystal retardation layer may be a combination of a λ / 4 liquid crystal retardation layer and a λ / 2 liquid crystal retardation layer that provides a phase difference of λ / 2, or [ii] the first liquid crystal retardation layer and the second liquid crystal retardation layer may be a combination of a positive C plate and a λ / 4 liquid crystal retardation layer.

[0167] Regarding the λ / 4 function in the entire visible light region, if the in-plane phase difference relative to light of wavelength λnm is set to R(λ), it is preferred to satisfy the optical characteristics shown in the following formula (1), and it is preferred to satisfy the optical characteristics shown in the following formula (1), the following formula (2), and the following formula (3).

[0168] 100nm<Re(550)<160nm (1)

[0169] Re(450) / Re(550)≤1.0 (2)

[0170] 1.00≤Re(650) / Re(550) (3)

[0171] [In formulas (1) to (3),

[0172] Re(450) represents the in-plane phase difference value (in-plane retardation) with respect to light of wavelength 450 nm.

[0173] Re(550) represents the in-plane phase difference value with respect to light with a wavelength of 550 nm.

[0174] Re(650) represents the in-plane retardation value relative to light with a wavelength of 650 nm.]

[0175] If the "Re(450) / Re(550)" of the liquid crystal retardation layer exceeds 1.0, light leakage on the short wavelength side of the elliptically polarizing plate having the liquid crystal retardation layer increases. The value of "Re(450) / Re(550)" is preferably 0.7 or more and 1.0 or less, more preferably 0.80 or more and 0.95 or less, further preferably 0.80 or more and 0.92 or less, and particularly preferably 0.82 or more and 0.88 or less. The value of "Re(450) / Re(550)" can be arbitrarily adjusted by adjusting the mixing ratio of the polymerizable liquid crystal compound, the stacking angle of multiple liquid crystal retardation layers, and the phase difference value.

[0176] The in-plane phase difference value of the liquid crystal phase difference layer can be adjusted according to the thickness of the liquid crystal phase difference layer. Since the in-plane phase difference value is determined by the following formula (4), in order to obtain the desired in-plane phase difference value (Re(λ)), it is sufficient to adjust Δn(λ) and thickness d. The thickness of the liquid crystal phase difference layer is usually less than 10 μm, preferably greater than 0.3 μm and less than 5 μm, more preferably greater than 0.5 μm and less than 5 μm, and further preferably greater than 1 μm and less than 3 μm. The thickness of the liquid crystal phase difference layer can be measured using an interference film thickness meter, a laser microscope or a stylus film thickness meter. Δn(λ) in formula (4) depends on the molecular structure of the polymerizable liquid crystal compound described later.

[0177] Re(λ)=d×Δn(λ) (4)

[0178] [Where Re(λ) represents the in-plane retardation at a wavelength of λ nm, d represents the film thickness, and Δn(λ) represents the birefringence at a wavelength of λ nm.]

[0179] As one method for achieving antireflection performance, a structure combining a positive wavelength dispersion λ / 2 layer with a positive wavelength dispersion λ / 4 layer is known. For example, this can be achieved by combining a layer having the optical characteristics shown in Formulas (5), (7), and (8) with a layer having the optical characteristics shown in Formulas (6), (7), and (8) with a specific slow axis relationship.

[0180] 100nm<Re(550)<160nm (5)

[0181] 200nm<Re(550)<320nm (6)

[0182] Re(450) / Re(550)≥1.00 (7)

[0183] 1.00≥Re(650) / Re(550) (8)

[0184] [In formulas (5) to (8),

[0185] Re(450) represents the in-plane phase difference value with respect to light with a wavelength of 450 nm.

[0186] Re(550) represents the in-plane phase difference value with respect to light with a wavelength of 550 nm.

[0187] Re(650) represents the in-plane retardation value relative to light with a wavelength of 650 nm.]

[0188] As a method for combining the above layers, known methods such as Japanese Unexamined Patent Application Publication No. 2015-163935 and WO2013 / 137464 can be cited. From the perspective of compensation, it is preferable to use a λ / 2 liquid crystal retardation layer of a polymer preferably containing a discotic polymeric liquid crystal compound and a λ / 4 liquid crystal retardation layer of a polymer containing a rod-like polymeric liquid crystal compound.

[0189] As the discotic polymeric liquid crystal compound, for example, a compound containing a group represented by formula (W) (hereinafter, sometimes referred to as a polymeric liquid crystal compound) can be cited.

[0190] [Chemical formula 2]

[0191] n

[0192] [In formula (W), R 40 represents the following formulas (W-1) to (W-5).

[0193] [Chemical formula 3]

[0194]

[0195] [In formulas (W-1) to (W-5),

[0196] X 40 and Z 40 represent an alkanediyl group having 1 to 12 carbon atoms (Japanese: アルカンジイル基), and the hydrogen atoms contained in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and the hydrogen atoms contained in the alkoxy group may be substituted with a halogen atom. In addition, -CH2- constituting the alkanediyl group may be replaced with -O- or -CO-.

[0197] m2 represents an integer.]]

[0198] As the rod-like polymeric liquid crystal compound, for example, compounds represented by formula (II), formula (III), formula (IV), formula (V), formula (VI) or formula (VII) can be cited.

[0199] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12 (II)

[0200] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11(III)

[0201] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12(IV) ​​​

[0202] P11-B11-E11-B12-A11-B13-A12-B14-A13-F11 (V)

[0203] P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12 (VI)

[0204] P11-B11-E11-B12-A11-B13-A12-F11 (VII)

[0205] [In formulas (II) to (VII),

[0206] A11 to A14 each independently represent a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. The hydrogen atoms contained in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, or a nitro group. The hydrogen atoms contained in the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms may be substituted with a fluorine atom.

[0207] B11 and B17 each independently represent -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, or -CO-NR 16 -、-NR 16 -CO-, -CO-, -CS- or a single bond. R 16 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0208] B12 to B16 each independently represent -C≡C-, -CH=CH-, -CH2-CH2-, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -、-NR 16 -C(=O)-, -OCH2-, -OCF2-, -CH2O-, -CF2O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH- or a single bond.

[0209] E11 and E12 each independently represent an alkanediyl group having 1 to 12 carbon atoms, wherein the hydrogen atoms contained in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and the hydrogen atoms contained in the alkoxy group may be substituted with a halogen atom. Furthermore, the -CH2- group constituting the alkanediyl group may be replaced with -O- or -CO-.

[0210] F11 represents a hydrogen atom, an alkyl group having 1 to 13 carbon atoms, an alkoxy group having 1 to 13 carbon atoms, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxyl group, a hydroxymethyl group, a formyl group, a sulfo group (-SO3H), a carboxyl group, an alkoxycarbonyl group having 1 to 10 carbon atoms, or a halogen atom, and the -CH2- constituting the alkyl group and the alkoxy group may be substituted by -O-.

[0211] P11 and P12 each independently represent a polymerizable group.]

[0212] In addition to the above-mentioned combination of a positive wavelength dispersion λ / 2 layer and a positive wavelength dispersion λ / 4 layer, tilted alignment and cholesteric alignment can be used without particular limitation as long as they achieve an anti-reflection function. Examples of such structures include those described in WO2021 / 060378, WO2021 / 132616, and WO2021 / 132624.

[0213] The positive C plate is not particularly limited as long as it has anisotropy in the thickness direction. However, when tilt orientation or cholesteric orientation is not performed, the positive C plate has the optical properties represented by the following formula (9).

[0214] nx≈ny<nz (9)

[0215] [In formula (9),

[0216] nx represents the principal refractive index of the positive C plate at a wavelength λ [nm] within the plane.

[0217] Ny represents the refractive index of the positive C plate at a wavelength λ [nm] in the same plane as nx and in a direction perpendicular to nx.

[0218] nz(λ) represents the refractive index of the positive C plate at a wavelength of λ [nm] in the thickness direction.

[0219] In the case of nx≈ny, nx can be set as the refractive index in any direction within the plane of the positive C plate.]

[0220] The in-plane retardation value Re(550) of the positive C plate at a wavelength of 550 nm is generally in the range of 0 nm to 10 nm, preferably in the range of 0 nm to 5 nm. Furthermore, the thickness direction retardation value Rth(550) at a wavelength of 550 nm is generally in the range of -170 nm to -10 nm, preferably -150 nm to -20 nm, and more preferably -100 nm to -40 nm. If the thickness direction retardation value is within this range, the anti-reflection properties in the self-tilt direction can be further improved.

[0221] When the positive C plate is a liquid crystal retardation layer, the thickness thereof is usually 10 μm or less, preferably 5 μm or less, and more preferably 0.3 μm or more and 3 μm or less.

[0222] The positive C plate is preferably a liquid crystal retardation layer. More preferably, it is a rod-shaped polymerizable liquid crystal compound. Examples of the rod-shaped polymerizable liquid crystal compound include compounds represented by formulas (II) to (VII).

[0223] (Polymerizable liquid crystal compound constituting the liquid crystal phase difference layer)

[0224] The polymerizable liquid crystal compound contained in the first liquid crystal phase difference layer forming composition and the second liquid crystal phase difference layer forming composition (hereinafter also referred to as the "liquid crystal phase difference layer forming composition") refers to a liquid crystal compound having a polymerizable group, in particular a photopolymerizable group. As the polymerizable liquid crystal compound, a conventionally known polymerizable liquid crystal compound can be used. A photopolymerizable group refers to a group that can participate in a polymerization reaction through reactive species, such as active free radicals, acids, etc., generated by a photopolymerization initiator. Examples of photopolymerizable groups include vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, and oxetane. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane, and oxetane are preferred, and acryloyloxy is more preferred. The polymerizable liquid crystal compound may be a thermotropic liquid crystal or a lyotropic liquid crystal. From the perspective of being able to perform dense film thickness control, a thermotropic liquid crystal is preferred. In addition, as a phase-ordered structure in a thermotropic liquid crystal, it may be a nematic liquid crystal or a smectic liquid crystal. Furthermore, it may be a rod-shaped liquid crystal or a disc-shaped liquid crystal. The polymerizable liquid crystal compound may be used alone or in combination of two or more.

[0225] As a polymerizable liquid crystal compound, from the viewpoint of exhibiting reverse wavelength dispersion, it is preferred to use a liquid crystal having a mesomorphic structure in a T-type or H-type which further has birefringence in a direction perpendicular to the long axis of the molecule. From the viewpoint of obtaining stronger dispersion, a T-type liquid crystal is more preferred. Specifically, as the structure of the T-type liquid crystal, for example, a compound represented by the following formula (VIII) can be cited.

[0226] [Chemical Formula 4]

[0227]

[0228] [In formula (VIII),

[0229] Ar represents a divalent aromatic group which may have a substituent. The divalent aromatic group preferably contains at least one of a nitrogen atom, an oxygen atom, and a sulfur atom. When the divalent group Ar contains two or more aromatic groups, the two or more aromatic groups may be bonded to each other via a divalent bonding group such as a single bond, -CO-O-, or -O-.

[0230] G 1 and G 2 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. Here, hydrogen atoms contained in the divalent aromatic group or divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and carbon atoms constituting the divalent aromatic group or divalent alicyclic hydrocarbon group may be replaced with an oxygen atom, a sulfur atom, or a nitrogen atom.

[0231] L 1 、L 2 、B 1 and B 2 Each is independently a single bond or a divalent linking group.

[0232] k and l each independently represent an integer from 0 to 3 and satisfy the relationship 1≤k+1. Here, in the case of 2≤k+1, B 1 and B 2 , G 1 and G 2 They can be the same as or different from each other.

[0233] E 1 and E 2 Each independently represents an alkanediyl group having 1 to 17 carbon atoms, wherein the hydrogen atoms contained in the alkanediyl group may be substituted by halogen atoms, and the -CH2- contained in the alkanediyl group may be replaced by -O-, -S-, or -COO-. When there are multiple -O-, -S-, or -COO- groups, they are not adjacent to each other.

[0234] P 1 and P 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.]

[0235] G 1 and G 2Each independently preferably is a 1,4-phenylenediyl group which may be substituted with at least one substituent selected from a halogen atom and an alkyl group having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group which may be substituted with at least one substituent selected from a halogen atom and an alkyl group having 1 to 4 carbon atoms. More preferably, it is a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group. Particularly preferably, it is an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group.

[0236] In addition, it is preferable that there are multiple G 1 and G 2 At least one of them is a divalent alicyclic hydrocarbon group, and more preferably 1 or L 2 Bonded G 1 and G 2 At least one of them is a divalent alicyclic hydrocarbon group.

[0237] L 1 and L 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -、-R a3 COOR a4 -、-R a5 OCOR a6 -、R a7 OC=OOR a8 -、-N=N-、-CR c =CR d -, or -C≡C-. Here, R a1 ~R a8 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms, R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 More preferably, each independently represents a single bond, -O Ra2-1 -、-CH2-、-CH2CH2-、-COOR a4-1 -, or OCOR a6-1 -. Here, R a2-1 、R a4-1 、R a6-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and L 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or -OCO-.

[0238] B 1 and B 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -、-R a11 COOR a12 -、-R a13 OCOR a14 -, or -R a15 OC=OOR a16 -. Here, R a9 ~R a16 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B 2 More preferably, each independently represents a single bond, -OR a10-1 -、-CH2-、-CH2CH2-、-COOR a12 -1 -, or -OCOR a14-1 -. Here, R a10-1 、R a12-1 、R a14-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and B 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or -OCOCH2CH2-.

[0239] From the viewpoint of exhibiting reverse wavelength dispersion, k and 1 are preferably in the range of 2≤k+1≤6, preferably k+1=4, and more preferably k=2 and 1=2. k=2 and 1=2 are preferred because they form a symmetrical structure.

[0240] E 1 and E 2 Each independently of the above, an alkanediyl group having 1 to 17 carbon atoms is preferred, and an alkanediyl group having 4 to 12 carbon atoms is more preferred.

[0241] As P 1 or P 2 The polymerizable group shown in the figure includes epoxy, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxiranyl and oxetanyl. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxiranyl and oxetanyl are preferred, and acryloyloxy is more preferred.

[0242] Ar preferably has at least one selected from an aromatic hydrocarbon ring that may have a substituent, an aromatic heterocycle that may have a substituent, and an electron-withdrawing group. As the aromatic hydrocarbon ring, for example, a benzene ring, a naphthalene ring, an anthracene ring, etc. can be enumerated, preferably a benzene ring, a naphthalene ring. As the aromatic heterocycle, a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, and a phenanthroline ring, etc. can be enumerated. Wherein, preferably there is a thiazole ring, a benzothiazole ring or a benzofuran ring, further preferably there is a benzothiazolyl group. In addition, when Ar comprises a nitrogen atom, the nitrogen atom preferably has π electrons.

[0243] In formula (VIII), the total number of π electrons contained in the divalent aromatic group represented by Ar is N π It is preferably 8 or more, more preferably 10 or more, further preferably 14 or more, and particularly preferably 16 or more. It is preferably 30 or less, more preferably 26 or less, and further preferably 24 or less.

[0244] Preferred examples of the aromatic group represented by Ar include the following groups.

[0245] [Chemical Formula 5]

[0246]

[0247] In formulas (Ar-1) to (Ar-23),

[0248] *Mark indicates a connection portion.

[0249] Z 0 、Z 1 and Z 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms.

[0250] Q 1 and Q 2 Each independently represents -CR 2’ R 3’ -、-S-、-NH-、-NR 2’ -、-CO- or O-,R 2’ and R3’ Each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0251] J 1 and J 2 Each independently represents a carbon atom or a nitrogen atom.

[0252] Y 1 、Y 2 and Y 3 Each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group which may be substituted.

[0253] W 1 and W 2 Each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom.

[0254] m represents an integer from 0 to 6.

[0255] As Y 1 、Y 2 and Y 3 Examples of the aromatic hydrocarbon group in the group include aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as phenyl, naphthyl, anthracenyl, phenanthrenyl, and biphenyl. Phenyl and naphthyl are preferred, and phenyl is more preferred. Examples of the aromatic heterocyclic group include aromatic heterocyclic groups having 4 to 20 carbon atoms, such as furyl, pyrrolyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl, which contain at least one heteroatom such as a nitrogen atom, an oxygen atom, or a sulfur atom. Furyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl are preferred.

[0256] Y 1 、Y 2 and Y 3 Each independently may be a polycyclic aromatic hydrocarbon group or a polycyclic aromatic heterocyclic group which may be substituted. A polycyclic aromatic hydrocarbon group refers to a fused polycyclic aromatic hydrocarbon group or a group derived from an aggregate of aromatic rings. A polycyclic aromatic heterocyclic group refers to a fused polycyclic aromatic heterocyclic group or a group derived from an aggregate of aromatic rings.

[0257] Z 0 、Z 1 and Z 2 Each of them is independently preferably a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkoxy group having 1 to 12 carbon atoms, 0 More preferably, a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group, Z 1 and Z 2 More preferred are a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, and a cyano group.

[0258] Q 1 and Q 2 -NH-, -S-, -NR-2’ -、-O-,R 2’ A hydrogen atom is preferred, and among them, -S-, -O-, and -NH- are particularly preferred.

[0259] Among formulae (Ar-1) to (Ar-23), formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.

[0260] In the formulas (Ar-16) to (Ar-23), Y 1 The nitrogen atom and Z 0 Together they form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include those previously described as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. The aromatic heterocyclic group may have a substituent. In addition, Y 1 The nitrogen atom and Z 0 Together, they represent the aforementioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group, for example, a benzofuran ring, a benzothiazole ring, a benzoxazole ring, and the like.

[0261] Among the polymerizable liquid crystal compounds, compounds having a maximum absorption wavelength of 300 to 400 nm are preferred. When a photopolymerization initiator is included in the composition for forming a liquid crystal phase difference layer, it is possible to carry out polymerization reaction and gelation of the polymerizable liquid crystal compound during long-term storage. However, if the maximum absorption wavelength of the polymerizable liquid crystal compound is 300 to 400 nm, even if it is exposed to ultraviolet light during storage, it is possible to effectively suppress the generation of reactive species from the photopolymerization initiator and the polymerization reaction and gelation of the polymerizable liquid crystal compound caused by the reactive species. Therefore, it is advantageous in terms of the long-term stability of the polymerizable liquid crystal composition, and it is possible to improve the orientation and uniformity of the film thickness of the obtained polymer layer (liquid crystal cured film). It should be noted that the maximum absorption wavelength of the polymerizable liquid crystal compound can be measured using an ultraviolet-visible spectrophotometer in a solvent. The solvent is a solvent that can dissolve the polymerizable liquid crystal compound, and for example, chloroform can be mentioned.

[0262] Relative to 100 parts by mass of the solid content of the composition for forming a liquid crystal phase difference layer, the content of the polymerizable liquid crystal compound in the composition for forming a liquid crystal phase difference layer is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and further preferably 90 to 95 parts by mass. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous from the perspective of the orientation of the obtained polymer layer (liquid crystal cured film). It should be noted that, in this specification, the solid content of the composition for forming a liquid crystal phase difference layer refers to all components after removing volatile components such as organic solvents from the composition for forming a liquid crystal phase difference layer.

[0263] The composition for forming a liquid crystal retardation layer may further contain reactive additives such as a solvent, a leveling agent, a polymerization initiator, a photosensitizer, an antioxidant, a crosslinking agent, and an adhesion agent. From the viewpoint of processability, it preferably contains a solvent and a leveling agent.

[0264] The composition for forming a liquid crystal phase difference layer may contain a solvent. Generally, the viscosity of the polymerizable liquid crystal compound is high, so by preparing a composition for forming a liquid crystal phase difference layer that is soluble in a solvent, coating becomes easy, and as a result, a liquid crystal phase difference layer is easily formed in most cases. As a solvent, a solvent that can completely dissolve the polymerizable liquid crystal compound is preferably a solvent that is inactive in the polymerization reaction of the polymerizable liquid crystal compound.

[0265] Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorinated solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These solvents may be used alone or in combination of two or more.

[0266] The content of the solvent is preferably 50 to 98% by mass relative to the total amount of the composition for forming a liquid crystal phase difference layer. In other words, the content of the solid component in the composition for forming a liquid crystal phase difference layer is preferably 2 to 50% by mass, more preferably 5 to 30% by mass. If the content of the solid component is less than 50% by mass, the viscosity of the composition for forming a liquid crystal phase difference layer decreases, so the thickness of the liquid crystal phase difference layer becomes roughly uniform, thereby there is a trend that the liquid crystal phase difference layer is not easy to produce unevenness. In addition, the content of the solid component can be determined taking into account the thickness of the liquid crystal phase difference layer to be manufactured.

[0267] The composition for forming a liquid crystal phase difference layer may contain a leveling agent. A leveling agent is an additive that adjusts the fluidity of the composition for forming a liquid crystal phase difference layer and makes the film obtained by coating the composition flatter. Examples thereof include organically modified silicone-based, polyacrylate-based, and perfluoroalkyl-based leveling agents. Among them, polyacrylate-based leveling agents and perfluoroalkyl-based leveling agents are preferred for horizontal orientation, while organically modified silicone-based leveling agents and perfluoroalkyl-based leveling agents are preferred for vertical orientation.

[0268] When the composition for forming a liquid crystal phase difference layer contains a leveling agent, it is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the content of the polymerizable liquid crystal compound. If the content of the leveling agent is within the above range, there is a tendency to easily make the polymerizable liquid crystal compound horizontally oriented and the resulting liquid crystal phase difference layer smoother. If the content of the leveling agent exceeds the above range relative to the content of the polymerizable liquid crystal compound, there is a tendency that the resulting liquid crystal phase difference layer is prone to unevenness. It should be noted that the composition for forming a liquid crystal phase difference layer may contain two or more leveling agents.

[0269] The composition for forming a liquid crystal retardation layer may contain a polymerization initiator. A polymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound or the like. As the polymerization initiator, a photopolymerization initiator that generates active free radicals under the action of light is preferred because it is independent of the phase state of the thermotropic liquid crystal.

[0270] As long as the photopolymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound, any known photopolymerization initiator can be used. Specifically, photopolymerization initiators capable of generating active free radicals or acids by the action of light can be mentioned, with photopolymerization initiators that generate free radicals by the action of light being preferred. Photopolymerization initiators can be used alone or in combination of two or more.

[0271] As the photopolymerization initiator, a known photopolymerization initiator can be used. For example, as a photopolymerization initiator that generates active free radicals, self-cleavable benzoin-based compounds, acetophenone-based compounds, hydroxyacetophenone-based compounds, α-aminoacetophenone-based compounds, oxime ester-based compounds, acylphosphine oxide-based compounds, azo-based compounds, etc. can be used. Hydrogen-abstracting benzophenone-based compounds, alkylphenone-based compounds, benzoin ether-based compounds, benzyl ketal-based compounds, dibenzocycloheptenone-based compounds, anthraquinone-based compounds, xanthone-based compounds, thioxanthone-based compounds, halogenated acetophenone-based compounds, dialkoxyacetophenone-based compounds, halogenated bisimidazole-based compounds, halogenated triazine-based compounds, triazine-based compounds, etc. can be used. As a photopolymerization initiator that generates an acid, iodonium salts and sulfonium salts can be used. From the viewpoint of excellent reaction efficiency at low temperatures, self-cleavage type photopolymerization initiators are preferred, and acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, and oxime ester compounds are particularly preferred.

[0272] The content of the polymerization initiator in the composition for forming a liquid crystal retardation layer can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound, and is generally 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization initiator is within the above range, polymerization can be carried out without disturbing the alignment of the polymerizable liquid crystal compound.

[0273] The composition for forming a liquid crystal retardation layer may contain a sensitizer. A photosensitizer is preferably used as the sensitizer. Examples of such sensitizers include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and anthracene containing an alkoxy group (e.g., dibutoxyanthracene, etc.); phenothiazine and rubrene.

[0274] When the composition for forming a liquid crystal retardation layer contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the composition can be further promoted. The amount of the sensitizer used is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0275] The liquid crystal retardation layer may contain an antioxidant from the viewpoint of stably progressing the polymerization reaction. The antioxidant can control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.

[0276] The antioxidant may be, for example, a primary antioxidant selected from phenolic antioxidants, amine antioxidants, quinone antioxidants, and nitroso antioxidants, or a secondary antioxidant selected from phosphorus antioxidants and sulfur antioxidants.

[0277] When the composition for forming a liquid crystal retardation layer contains an antioxidant, the content of the antioxidant is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. The antioxidant may be used alone or in combination of two or more. If the content of the antioxidant is within the above range, polymerization can be performed without disturbing the alignment of the polymerizable liquid crystal compound.

[0278] The composition for forming a liquid crystal phase difference layer may contain a reactive additive. As a reactive additive, it is preferred to have a carbon-carbon unsaturated bond, an active hydrogen reactive group, or a mercapto group in its molecule. It should be noted that the "active hydrogen reactive group" referred to here refers to a group that is reactive to a group having active hydrogen such as a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), and glycidyl, oxazoline, carbodiimide, aziridine, imide, isocyanate, thioisocyanate, maleic anhydride, etc. are representative examples thereof. The number of reactive groups possessed by the reactive additive is generally 1 to 20, preferably 1 to 10.

[0279] (Method for Manufacturing Liquid Crystal Retardation Layer)

[0280] The liquid crystal phase difference layer can be manufactured by coating a liquid crystal phase difference layer forming composition (a first liquid crystal phase difference layer forming composition or a second liquid crystal phase difference layer forming composition) on a substrate layer (a first substrate layer or a second substrate layer) or an orientation layer (a first orientation layer or a second orientation layer) formed on a substrate layer.

[0281] As the method for applying the composition for forming liquid crystal phase difference layer on substrate layer or orientation layer, extrusion coating method, direct gravure coating method, reverse gravure coating method, CAP coating method, slit coating method, micro gravure method, die coating method, ink jet method etc. can be enumerated. In addition, the method etc. of coating using the coating machines such as dip coater, rod coater, spin coater etc. can also be enumerated. Wherein, in the case of being continuously coated with roller to roller (Roll to Roll) form, it is preferably to utilize the coating method of micro gravure method, ink jet method, slit coating method, die coating method, in the case of being coated on single substrates such as glass, the spin coating method of preferred uniformity is high. In the case of being coated with roller to roller (Roll to Roll) form, it is also possible to form orientation layer by coating composition for forming orientation layer on substrate layer etc., further continuously coating liquid crystal phase difference layer forming composition on the obtained orientation layer.

[0282] Examples of drying methods for removing the solvent contained in the composition for forming a liquid crystal phase difference layer include natural drying, ventilation drying, heat drying, reduced pressure drying, and combinations thereof. Natural drying or heat drying are preferred. The drying temperature is preferably in the range of 0 to 200°C, more preferably in the range of 20 to 150°C, and even more preferably in the range of 50 to 130°C. The drying time is preferably 10 seconds to 10 minutes, more preferably 30 seconds to 5 minutes. The composition for forming an alignment layer can also be dried in the same manner.

[0283] As a method for polymerizing the polymerizable liquid crystal compound contained in the composition for forming a liquid crystal phase difference layer, photopolymerization is preferred. Photopolymerization is implemented by irradiating an active energy ray to a laminate coated with a composition for forming a liquid crystal phase difference layer comprising a polymerizable liquid crystal compound on a substrate layer or on an orientation layer. As the active energy ray irradiated, it is appropriately selected according to the type of polymerizable liquid crystal compound contained in the dry film (particularly the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator in the case of a photopolymerization initiator, and their amount. Specifically, one or more active energy rays selected from visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and gamma rays can be cited. Among them, from the aspect of easily controlling the progress of the polymerization reaction and the aspect of the device widely used in the art that can be used as a photopolymerization device, ultraviolet light is preferred, and the type of polymerizable liquid crystal compound is preferably selected in a manner that can utilize ultraviolet light for photopolymerization.

[0284] Examples of light sources for active energy rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.

[0285] The UV radiation intensity is usually 10mW / cm 2 Above 3000mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in the wavelength region effective for activating the cationic polymerization initiator or the free radical polymerization initiator. The ultraviolet irradiation time is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and even more preferably 10 seconds to 1 minute. If irradiated once or multiple times with such an ultraviolet irradiation intensity, the cumulative light amount is usually 10 mJ / cm 2 Above and 3000mJ / cm 2 Below, preferably 50mJ / cm 2 Above and 2000mJ / cm 2Below, more preferably 100mJ / cm 2 Above and 1000mJ / cm 2 If the accumulated light intensity is below this range, the curing of the polymerizable liquid crystal compound becomes insufficient, and good transferability may not be achieved. On the other hand, if the accumulated light intensity is above this range, the optical film including the liquid crystal retardation layer may be colored.

[0286] (Phase difference body)

[0287] The phase difference body includes at least one liquid crystal phase difference layer. The optical laminate and the optical film may include a phase difference body. For example, the first liquid crystal phase difference layer included in the optical laminate and the second liquid crystal phase difference layer included in the optical film may constitute the phase difference body.

[0288] (Base layer (first base layer, second base layer))

[0289] Examples of the substrate layer include glass substrates and film substrates, with film substrates being preferred. From the perspective of continuous production, long roll films are more preferred. The substrate layer is preferably a transparent substrate layer. Examples of the resin constituting the film substrate include: polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylates; polyacrylates; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonates; polysulfones; polyethersulfones; polyetherketones; polyphenylene sulfides and polyphenylene oxides; and other plastics. Among these, from the perspective of transparency when used in optical film applications, a film substrate composed of a resin selected from triacetyl cellulose, cyclic olefin resins, polymethacrylates, and polyethylene terephthalate is more preferred.

[0290] Examples of commercially available cellulose ester substrates include "FUJITAC Film" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M," "KC8UY," and "KC4UY" (all manufactured by Konica Minolta Opto Co., Ltd.).

[0291] Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona GmbH (Germany)), "ARTON" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by ZEON Corporation of Japan), and "APEL" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Such cyclic olefin resins can be formed into films by known methods such as solvent casting and melt extrusion to form substrates. Commercially available cyclic olefin resin substrates can also be used. Examples of commercially available cyclic olefin resin substrates include "Esushina" (registered trademark), "SCA40" (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), "ZeonorFilm" (registered trademark) (manufactured by Optes Co., Ltd.), and "Arton Film" (registered trademark) (manufactured by JSR Corporation).

[0292] The thickness of the second substrate layer is preferably thin enough to allow practical handling. However, if it is too thin, there is a tendency for reduced strength and poor processability. The thickness of the second substrate layer is generally 5 μm to 300 μm, preferably 10 μm to 200 μm, and more preferably 10 to 50 μm. In addition, by peeling off the second substrate layer and transferring the liquid crystal retardation layer, a further thinning effect can be achieved.

[0293] (Orientation Layers (First Orientation Layer, Second Orientation Layer))

[0294] The alignment layer has an alignment regulating force for aligning the polymerizable liquid crystal compound in a desired direction.

[0295] The orientation layer facilitates the liquid crystal orientation of the polymerizable liquid crystal compound. The state of liquid crystal orientation such as horizontal orientation, vertical orientation, mixed orientation, and tilted orientation varies according to the properties of the orientation layer and the polymerizable liquid crystal compound, and their combination can be selected arbitrarily. For example, if the orientation film is a material that exhibits horizontal orientation as an orientation limiting force, the polymerizable liquid crystal compound can form a horizontal orientation or a mixed orientation. If it is a material that exhibits vertical orientation, the polymerizable liquid crystal compound can form a vertical orientation or a tilted orientation. Expressions such as horizontal and vertical indicate the direction of the optical axis of the oriented polymerizable liquid crystal compound when the plane of the liquid crystal phase difference layer is used as a reference. For example, vertical orientation refers to having an optical axis of the oriented polymerizable liquid crystal compound in a direction perpendicular to the plane of the liquid crystal phase difference layer. The vertical mentioned here refers to 90°±20° relative to the plane of the liquid crystal phase difference layer.

[0296] Regarding the orientation restraining force, when the orientation layer is formed of an aligning polymer, it can be arbitrarily adjusted by the surface state and rubbing conditions, and when it is formed of a photoaligning polymer, it can be arbitrarily adjusted by polarized light irradiation conditions, etc. In addition, the liquid crystal orientation can also be controlled by selecting the physical properties such as the surface tension and liquid crystallinity of the polymerizable liquid crystal compound.

[0297] As an orientation layer formed between the substrate layer and the liquid crystal phase difference layer, it is preferably an orientation layer that is insoluble in the solvent used when forming the liquid crystal phase difference layer on the orientation layer and has heat resistance during the heat treatment for removing the solvent and orienting the liquid crystal. As the orientation layer, an orientation layer comprising an oriented polymer, a photo-alignment layer, a groove-aligned film, a stretched film stretched along the orientation direction, etc. can be cited. In the case of an elongated roll film, a photo-alignment layer is preferred from the viewpoint of being able to easily control the orientation direction.

[0298] The thickness of the alignment layer is usually in the range of 10 nm to 5000 nm, preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 30 to 300 nm.

[0299] As the oriented polymer used in the rubbing orientation layer, there can be mentioned: polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule and polyamic acid as their hydrolyzates, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinyl pyrrolidone, polyacrylic acid and polyacrylates, etc. Among them, polyvinyl alcohol is preferred. These oriented polymers can be used alone or in combination of two or more.

[0300] Examples of the rubbing method include a method in which a film of an oriented polymer formed on the surface of a substrate layer by applying an oriented polymer composition to a substrate and annealing the oriented polymer composition is brought into contact with a rotating rubbing roller wound with a rubbing cloth.

[0301] The photo-alignment layer comprises a polymer, oligomer, or monomer having a photoreactive group. The photo-alignment layer obtains an alignment restraining force by irradiating polarized light. From the perspective of being able to arbitrarily control the direction of the alignment restraining force by selecting the polarization direction of the irradiated polarized light, a photo-alignment layer is more preferred.

[0302] A photoreactive group refers to a group that generates liquid crystal orientation ability by irradiation with light. Specifically, it is a group that generates a photoreaction that is the origin of the liquid crystal orientation ability, such as an orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction of a molecule generated by irradiation with light. Among the photoreactive groups, from the aspect of excellent orientation, a group that undergoes dimerization reaction or photocrosslinking reaction is preferred. As a photoreactive group capable of the above-mentioned reaction, a photoreactive group having an unsaturated bond, particularly a double bond, is preferably a group having at least one selected from a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond).

[0303] As photoreactive groups having C=C bonds, for example, vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolinium groups, chalcone groups and cinnamoyl groups can be cited. From the viewpoint of easy control of reactivity and the viewpoint of exhibiting orientation restriction force during photo-orientation, chalcone groups and cinnamoyl groups are preferred. As photoreactive groups having C=N bonds, groups having structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups having N=N bonds, groups having azobenzene, azonaphthyl groups, aromatic heterocyclic azo groups, disazo groups and formazan groups, and groups with oxidized azobenzene as the basic structure can be cited. As photoreactive groups having C=O bonds, benzophenone groups, coumarin groups, anthraquinone groups and maleimide groups can be cited. These groups may have a substituent such as an alkyl group, an alkoxy group, an aryl group, an allyloxy group, a cyano group, an alkoxycarbonyl group, a hydroxyl group, a sulfonic acid group, or a haloalkyl group.

[0304] When irradiating polarized light, it can be in the form of directly irradiating polarized light from the film surface, or it can be in the form of irradiating polarized light from the substrate layer side and transmitting the polarized light. In addition, the polarized light is particularly preferably substantially parallel light. Regarding the polarized light irradiated, it is preferably polarized light in a wavelength region in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) with a wavelength range of 250 to 400 nm is particularly preferred. As the light source used in the polarized light irradiation, xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF can be mentioned, and high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are more preferred. These lamps are preferred because the luminous intensity of ultraviolet light with a wavelength of 313 nm is large. The light from the light source is irradiated through an appropriate polarizer, thereby enabling polarized light to be irradiated. As the polarizer, a polarizing filter, a polarizing prism such as Glan-Thomson or Glan-Taylor, or a wire-grid polarizer can be used.

[0305] From the perspective of easily adjusting the transmittance Tx of the first liquid crystal retardation layer with a substrate to the above range, the first liquid crystal retardation layer preferably does not include a first orientation layer. When a first orientation layer is provided, a material constituting the first orientation layer is preferably a material with low absorbance at a wavelength of 280 to 340 nm.

[0306] Polarizing Plate

[0307] A polarizing plate is a film with anisotropic light absorption, typically a film containing a polarizing element that uniaxially orients a dichroic dye. To uniaxially orient the dichroic dye, a film (i.e., a polarizer) can be made by uniaxially stretching a polymer such as a polyvinyl alcohol (PVA) resin impregnated with iodine or an organic dichroic dye, or by orienting the dichroic dye and a polymerizable liquid crystal compound to form an optically anisotropic layer (i.e., a liquid crystal polarizer). Specifically, the polarizing function is exhibited by utilizing the anisotropic absorption of light by the dichroic dye contained in the stretched polymer or polymerizable liquid crystal compound.

[0308] The polarizing plate may include a polarizing element, and may have a polarizing element protective film or layer on one or both sides of the polarizing element.

[0309] The polarization performance of the polarizing plate can be measured using a spectrophotometer. For example, in the range of visible light, i.e., a wavelength of 380nm to 780nm, a device equipped with a prism polarizer on a spectrophotometer can be used to measure the transmittance (T1) in the transmission axis direction (direction perpendicular to the orientation) and the transmittance (T2) in the absorption axis direction (orientation direction) by the double beam method. Regarding the polarization performance in the visible light range, the following formulas (Formula 1) and (Formula 2) are used to calculate the single transmittance and polarization degree at each wavelength, and the visibility (Japanese: visual sensitivity) is further corrected using the 2-degree field of view (C light source) of JIS Z 8701, thereby being able to calculate the visibility-corrected single transmittance (Ty') and the visibility-corrected polarization degree (Py). In addition, based on the transmittance measured in the same way, the color matching function of the C light source is used to calculate L * a * b * Chromaticity a in the (CIE) color system * and b * , thereby obtaining the color tone of the polarizing plate alone (single color tone), the color tone of the polarizing plates arranged in parallel (parallel color tone), and the color tone of the polarizing plates arranged orthogonally (orthogonal color tone). * and b * The closer the value is to 0, the more neutral the color tone can be judged to be.

[0310] Single body transmittance (%) = (T1 + T2) / 2 (Formula 1)

[0311] Polarization degree (%) = (T1-T2) / (T1+T2)×100 (Equation 2)

[0312] The polarizing plate's corrected polarization index Py is typically 80% or higher, preferably 90% or higher, more preferably 95% or higher, even more preferably 98% or higher, and particularly preferably 99% or higher. A value of 99.9% or higher allows for suitable use in liquid crystal displays. Increasing the corrected polarization index Py of the polarizing plate is beneficial in improving the antireflection function of the optical laminate. If the corrected polarization index Py is less than 80%, the optical laminate may not exhibit its antireflection function when used as an antireflection film.

[0313] The larger the visibility-corrected single transmittance Ty' of the polarizing plate, the greater the clarity of the white display. However, as can be seen from the relationship between (Equation 1) and (Equation 2), if the single transmittance is excessively increased, there is a problem of reduced polarization. Therefore, it is preferably 30% or more and 60% or less, more preferably 35% or more and 55% or less, further preferably 38% or more and 50% or less, and even more preferably 40% or more and 45% or less. If the visibility-corrected single transmittance Ty' becomes too large, the visibility-corrected polarization degree Py becomes too small, and sometimes the anti-reflection function of the optical laminate when used as an anti-reflection film becomes insufficient.

[0314] (Polarization element)

[0315] As described above, examples of the polarizing element include polarizing plates and liquid crystal polarizing plates. The polarizing element is preferably a polarizing plate.

[0316] (Polarizing Plate)

[0317] Polarizers, which are films obtained by uniaxially stretching a polymer such as a polyvinyl alcohol (PVA) resin film impregnated with iodine or an organic dichroic dye, can generally be manufactured through the following steps: uniaxially stretching the polyvinyl alcohol resin film; dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine to adsorb the dichroic dye; treating the polyvinyl alcohol resin film adsorbed with the dichroic dye with a crosslinking agent such as an aqueous solution containing boric acid; and washing the film with water after treatment with the crosslinking agent such as an aqueous solution containing boric acid. Polarizers may contain a crosslinking agent.

[0318] The thickness of the polarizer is usually 30 μm or less, preferably 18 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less. The thickness is usually 1 μm or more, for example 5 μm or more.

[0319] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When uniaxial stretching is performed after dyeing, it can be performed before or during the boric acid treatment. Of course, uniaxial stretching can also be performed in multiple stages as shown here. Uniaxial stretching can be performed by: uniaxial stretching in the film conveying direction between rollers with different peripheral speeds; uniaxial stretching in the film conveying direction using heated rollers; stretching in the width direction using a tenter frame, etc. Uniaxial stretching can be performed by dry stretching in the air or by wet stretching in a state where the polyvinyl alcohol-based resin film is swollen using a solvent such as water. The stretching ratio is generally 3 to 8 times. Alternatively, an aqueous solution containing polyvinyl alcohol can be applied to the thermoplastic resin film, followed by drying, and then stretched together with the thermoplastic resin film by the above-mentioned method.

[0320] The polyvinyl alcohol-based resin film can be dyed with a dichroic dye by, for example, immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye. Specifically, iodine and a dichroic organic dye can be used as the dichroic dye.

[0321] (Method for Manufacturing Polarizing Plate)

[0322] Polarizers are generally manufactured through the following steps: a step of uniaxially stretching a polyvinyl alcohol resin film (hereinafter also referred to as a "PVA film"); a step of dyeing the PVA film with a dichroic dye to adsorb the dichroic dye; a step of cross-linking the PVA film adsorbed with the dichroic dye by treating it with an aqueous solution containing boric acid; and a step of washing the cross-linking treatment with the aqueous solution containing boric acid (hereinafter also referred to as a "boric acid treatment").

[0323] The uniaxial stretching of the PVA film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When uniaxial stretching is performed after dyeing, it can be performed before or during the boric acid treatment. Of course, uniaxial stretching can also be performed in multiple stages as shown here. Uniaxial stretching can be performed by a method of uniaxially stretching the film in the direction of film transport between rollers of different peripheral speeds, a method of uniaxially stretching the film in the direction of film transport using a heated roller, a method of stretching the film in the width direction using a tenter, etc. In addition, uniaxial stretching can be performed by dry stretching in the air, or by wet stretching in a state where the PVA film is swollen using a solvent such as water. The stretching ratio is usually 3 to 8 times.

[0324] The dyeing of the PVA film using a dichroic pigment can be carried out, for example, by immersing the PVA film in an aqueous solution containing a dichroic pigment. Specifically, iodine or a dichroic organic dye can be used as the dichroic pigment. It should be noted that the PVA film is preferably immersed in water to swell the film before dyeing.

[0325] When iodine is used as the dichroic pigment, a method for dyeing is generally adopted in which the PVA film is immersed in an aqueous solution containing iodine and potassium iodide. The iodine content in the aqueous solution is generally 0.01 to 1 part by mass relative to 100 parts by mass of water, and the potassium iodide content is generally 0.5 to 20 parts by mass relative to 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is generally 20 to 40°C. In addition, the immersion time in the aqueous solution (dyeing time) is generally 20 to 1800 seconds.

[0326] On the other hand, when a dichroic organic dye is used as a dichroic pigment, a method of dyeing is usually adopted in which the PVA film is immersed in an aqueous solution containing a water-soluble dichroic organic dye. The content of the dichroic organic dye in the aqueous solution is usually 0.0001 to 10 parts by mass relative to 100 parts by mass of water, preferably 0.001 to 1 part by mass. The dye aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing auxiliary. The temperature of the dichroic organic dye aqueous solution used in dyeing is usually 20 to 80°C. In addition, the immersion time (dyeing time) in the aqueous solution is usually 10 to 1800 seconds.

[0327] The boric acid treatment after dyeing with a dichroic pigment can be carried out by immersing the dyed PVA film in an aqueous solution containing boric acid. The content of boric acid in the aqueous solution containing boric acid is generally 2 to 15 parts by mass relative to 100 parts by mass of water, preferably 5 to 12 parts by mass. When iodine is used as the dichroic pigment, the aqueous solution containing boric acid preferably contains potassium iodide. The content of potassium iodide in the aqueous solution containing boric acid is generally 0.1 to 15 parts by mass relative to 100 parts by mass of water, preferably 5 to 12 parts by mass. The immersion time in the aqueous solution containing boric acid is generally 60 to 1200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the aqueous solution containing boric acid is generally above 50°C, preferably 50 to 85°C, and more preferably 60 to 80°C.

[0328] The boric acid-treated PVA film is typically washed with water. For example, the boric acid-treated PVA film can be immersed in water. The water temperature during the washing process is typically 5 to 40°C. The immersion time is typically 1 to 120 seconds.

[0329] After washing, drying treatment is implemented to obtain a polarizer. Drying treatment can be carried out using a hot air dryer or a far-infrared heater. The temperature of the drying treatment is usually 30 to 100° C., preferably 50 to 80° C. The time of the drying treatment is usually 60 to 600 seconds, preferably 120 to 600 seconds. By drying treatment, the moisture content in the polarizer is reduced to a practical level. Its moisture content is usually 5 to 20% by mass relative to the total mass of the polarizer, preferably 8 to 15% by mass. If the moisture content is 5% by mass or more, the polarizer has sufficient flexibility, thereby being able to suppress damage or breakage after drying. In addition, if the moisture content is 20% by mass or less, the polarizer has sufficient thermal stability.

[0330] As described above, a polarizing plate in which a dichroic dye is adsorbed and oriented on a PVA film can be produced.

[0331] The polarizing plate obtained as described above can be produced into a polarizing plate by further laminating a polarizing element protective film or a protective layer on one or both surfaces thereof.

[0332] (Liquid crystal polarizer)

[0333] Liquid crystal polarizers, i.e., optically anisotropic layers comprising polymers of polymerizable liquid crystal compounds containing dichroic dyes, are suitable for applications such as flexible displays because they can arbitrarily control color tones, can be significantly thinned, and are non-contractile due to the absence of stretching and relaxation caused by heat.

[0334] The liquid crystal polarizer is formed by applying a liquid crystal polarizer forming composition on a third substrate layer or on a third orientation layer formed on the third substrate layer, so that the dichroic pigment contained in the liquid crystal polarizer forming composition is oriented. The thickness of the liquid crystal polarizer is preferably 0.1 μm or more and 5 μm or less, more preferably 0.3 μm or more and 4 μm or less, and further preferably 0.5 μm or more and 3 μm or less. If the thickness is less than the above range, the desired light absorption may not be obtained, and if the thickness is greater than the above range, there is a tendency that the orientation restriction force based on the third orientation layer is reduced and orientation defects are easily generated. In addition, the liquid crystal polarizer forming composition may further include a solvent, a photopolymerization initiator, a photosensitizer, an inhibitor, a leveling agent, and an adhesion improver.

[0335] For a liquid crystal polarizer in which the dichroic dye and the polymerizable liquid crystal compound are horizontally aligned relative to the third substrate layer, the ratio of the absorbance A1(λ) in the alignment direction for light of wavelength λ nm to the absorbance A2(λ) in the perpendicular direction within the alignment plane (dichroic ratio) is preferably 7 or greater, more preferably 20 or greater, and even more preferably 40 or greater. The larger the value of this ratio, the more excellent the absorption selectivity of the liquid crystal polarizer. Although it also depends on the type of dichroic dye, when the polymerizable liquid crystal compound constituting the liquid crystal polarizer is cured in a nematic liquid crystal phase, the above ratio is approximately 5 to 10.

[0336] By mixing two or more dichroic pigments with different absorption wavelengths, liquid crystal polarizers with various hues can be produced, and liquid crystal polarizers with absorption across the entire visible light range can be produced. By producing liquid crystal polarizers with such absorption characteristics, they can be used in a variety of applications.

[0337] (Polymerizable liquid crystal compound constituting liquid crystal polarizer)

[0338] A polymerizable liquid crystal compound refers to a compound having a polymerizable group and liquid crystal properties. A polymerizable group refers to a group that participates in the polymerization reaction, preferably a photopolymerizable group. Here, a photopolymerizable group refers to a group that can participate in the polymerization reaction through active free radicals, acids, etc. generated by the photopolymerization initiator described later. Examples of polymerizable groups include: vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxiranyl, oxetane, etc. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxiranyl and oxetane are preferred, with methacryloyloxy or acryloyloxy being more preferred. The liquid crystal properties may be thermotropic or lyotropic. When mixed with a dichroic pigment described later, thermotropic liquid crystals are preferred. A polymerizable liquid crystal compound may be a monomer or a polymer obtained by polymerizing a dimer or more.

[0339] In the case where the polymerizable liquid crystal compound is a thermotropic liquid crystal, it can be a thermotropic liquid crystal compound showing a nematic liquid crystal phase, or it can be a thermotropic liquid crystal compound showing a smectic liquid crystal phase. From the viewpoint of being able to present high dichroism, the liquid crystal state shown by the polymerizable liquid crystal compound is preferably a smectic phase. If it is a high-order smectic phase, it is more preferred from the viewpoint of high performance. Among them, it is more preferred to form a high-order smectic polymerizable liquid crystal compound of smectic B phase, smectic D phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase or smectic L phase, and further preferably a high-order smectic polymerizable liquid crystal compound forming a smectic B phase, smectic F phase or smectic I phase. If the liquid crystal phase formed by the polymerizable liquid crystal compound is these high-order smectic phases, it is possible to manufacture a liquid crystal polarizer having higher polarization performance. In addition, the liquid crystal polarizer having high polarization performance can obtain a Bragg peak of a high-order structure such as a hexagonal phase (Japanese: hexagonal phase) and a crystalline phase in X-ray diffraction measurement. The Bragg peak is a peak derived from the periodic structure of molecular orientation, and its periodic interval can be obtained as From the viewpoint of obtaining higher polarization characteristics, the liquid crystal polarizer preferably includes a polymer of a polymerizable liquid crystal compound in which the polymerizable liquid crystal compound is aligned in a smectic phase.

[0340] The polymerizable liquid crystal compound may be used alone or in combination of two or more. As long as the effect of the present invention is not impaired, the composition for forming a liquid crystal polarizer containing other compounds described later may also contain other polymerizable liquid crystal compounds other than the polymerizable liquid crystal compound, but from the viewpoint of obtaining a liquid crystal polarizer with a high degree of orientation order, the polymerizable liquid crystal compound (polymerizable liquid crystal compound other than other polymerizable liquid crystal compounds) relative to the total mass of all polymerizable liquid crystal compounds contained in the composition for forming a liquid crystal polarizer is preferably 51% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more.

[0341] The content of the polymerizable liquid crystal compound in the composition for forming a liquid crystal polarizer is preferably 40 to 99.9% by mass, more preferably 60 to 99% by mass, and further preferably 70 to 99% by mass relative to the solid content of the polymerizable liquid crystal composition. If the content of the polymerizable liquid crystal compound is within the above range, there is a tendency for the orientation of the polymerizable liquid crystal compound to increase. It should be noted that, in this specification, the solid content refers to the total amount of the components after removing the solvent from the composition for forming a liquid crystal polarizer.

[0342] (Dichroic pigments that make up liquid crystal polarizers)

[0343] A dichroic dye is a dye having a property where the absorbance along the long axis of the molecule differs from the absorbance along the short axis. Dichroic dyes preferably have the property of absorbing visible light, and more preferably have an absorption maximum wavelength (λMAX) in the wavelength range of 380 to 680 nm. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, with azo dyes being preferred. Azo dyes include monoazo dyes, disazo dyes, triazo dyes, tetrazo dyes, and stilbene azo dyes, with disazo dyes and triazo dyes being preferred. Dichroic dyes can be used alone or in combination. To achieve absorption across the entire visible light range, a combination of two or more dichroic dyes is preferred, and a combination of three or more dichroic dyes is more preferred.

[0344] Examples of the azo dye include compounds represented by formula (VIII) (hereinafter, sometimes also referred to as “compound (VIII)”).

[0345] T 1 -A 1 (-N=NA 2 ) p -N=NA 3 -T 2 (VIII)

[0346] [In formula (VIII),

[0347] A 1 、A 2 and A 3 Each independently represents an optionally substituted 1,4-phenylene group, an optionally substituted naphthalene-1,4-diyl group, an optionally substituted phenylbenzoate group, an optionally substituted 4,4'-diphenylvinylene group, or an optionally substituted divalent heterocyclic group.

[0348] T 1 and T 2 They are independently electron-withdrawing groups or electron-donating groups, and are located at substantially 180° relative to the azo bond plane.

[0349] p represents an integer from 0 to 4. When p is 2 or more, each A 2 They may be the same or different. Within the range showing absorption in the visible region, the -N=N- bond may be replaced by a -C=C-, -COO-, -NHCO-, or -N=CH- bond.]

[0350] From the perspective of obtaining good light absorption properties, the content of the dichroic pigment (the total amount when multiple types are included) is generally 1 to 60 parts by mass, preferably 1 to 40 parts by mass, and more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the dichroic pigment is less than this range, light absorption becomes insufficient and sufficient polarization performance cannot be obtained. If it is more than this range, the orientation of the liquid crystal molecules may be hindered.

[0351] The liquid crystal polarizer can be manufactured by applying a liquid crystal polarizer forming composition on the third substrate layer or on the third orientation layer formed on the third substrate layer. The liquid crystal polarizer forming composition may further contain additives such as a solvent, a leveling agent, a polymerization initiator, a photosensitizer, an antioxidant, a cross-linking agent, and a reactive additive such as a bonding agent. From the viewpoint of processability, it is preferred to contain a solvent and a leveling agent. These additives can use the additives described in the composition for forming a liquid crystal phase difference layer.

[0352] Examples of methods for applying the liquid crystal polarizer-forming composition, drying to remove the solvent contained in the liquid crystal polarizer-forming composition, and polymerizing the polymerizable liquid crystal compound contained in the liquid crystal polarizer-forming composition include the methods described in the method for producing a liquid crystal retardation layer. Examples of the third substrate layer and the third orientation layer include the first substrate layer and the second substrate layer described in the method for producing a liquid crystal retardation layer, and the layers described in the first orientation layer and the second orientation layer.

[0353] A polarizing plate can be produced by laminating a polarizing element protective film or protective layer on one or both sides of a liquid crystal polarizer.

[0354] (Polarizing element protective film)

[0355] The polarizer protective film has the function of protecting the surface of the polarizer. The polarizer and the polarizer protective film can be directly stacked with each other. Here, "direct stacking" includes: a method of stacking on the polarizer by the self-adhesiveness of the polarizer protective film and a method of stacking by means of an adhesive layer (adhesive layer or adhesive layer). In order to improve the adhesion with the polarizer, the polarizer protective film can be subjected to a surface treatment (for example, a corona treatment, etc.), or a thin layer such as a primer layer (also referred to as an "easy bonding layer") can be formed.

[0356] As a polarizing element protective film, for example, a resin film having excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, and stretchability can be used. The resin film can be a thermoplastic resin film. Specific examples of the resin constituting such a resin film include: cellulose resins such as triacetyl cellulose; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyethersulfone resins; polysulfone resins; polycarbonate resins; polyamide resins such as nylon and aromatic polyamide; polyimide resins; polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; cyclic polyolefin resins having a ring system and norbornene structure (also referred to as "norbornene resins"); (meth) acrylic resins such as polymethyl methacrylate; polyarylate resins; polystyrene resins; polyvinyl alcohol resins, and mixtures thereof. Polarizing element protective films of this material can be easily obtained from the market. Other examples include (meth)acrylic, urethane, (meth)acrylic urethane, epoxy, silicone, and other thermosetting and UV-curing resins. In this specification, (meth)acrylic acid refers to either acrylic acid or methacrylic acid. The same applies to (meth)acrylate and (meth)acryloyl.

[0357] Examples of the chain polyolefin resin include, in addition to homopolymers of chain olefins such as polyethylene resin (polyethylene resin as a homopolymer of ethylene, copolymers mainly composed of ethylene) and polypropylene resin (polypropylene resin as a homopolymer of propylene, copolymers mainly composed of propylene), copolymers containing two or more chain olefins.

[0358] Cyclic polyolefin resins are a general term for resins polymerized using cyclic olefins as polymerized units. Examples include the resins described in Japanese Patent Application Laid-Open No. 1-240517, Japanese Patent Application Laid-Open No. 3-14882, and Japanese Patent Application Laid-Open No. 3-122137. Specific examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (typically random copolymers) of cyclic olefins with chain olefins such as ethylene and propylene, graft polymers obtained by modifying these with unsaturated carboxylic acids or their derivatives, and hydrogenated products thereof. Of these, norbornene resins using norbornene monomers such as norbornene and polycyclic norbornene monomers as cyclic olefins are preferred.

[0359] Polyester resins are resins with ester bonds in their main chains and are generally polycondensates of polycarboxylic acids or their derivatives with polyols. Examples of polycarboxylic acids or their derivatives include divalent dicarboxylic acids or their derivatives, such as terephthalic acid, isophthalic acid, dimethyl terephthalate, and dimethyl naphthalate. Examples of polyols include divalent diols, such as ethylene glycol, propylene glycol, butanediol, neopentyl glycol, and cyclohexanedimethanol. A representative example of a polyester resin is polyethylene terephthalate, a polycondensate of terephthalic acid and ethylene glycol.

[0360] Cellulose ester resins are esters of cellulose and fatty acids. Specific examples of cellulose ester resins include cellulose triacetate, cellulose diacetate, cellulose tripropionate, and cellulose dipropionate. Other examples include copolymers comprising multiple polymerized units comprising these cellulose ester resins, and resins in which some of the hydroxyl groups have been modified with other substituents. Among these, cellulose triacetate (triacetyl cellulose) is particularly preferred.

[0361] (Meth)acrylic resins are resins whose main constituent monomers are compounds having (meth)acryloyl groups. Specific examples of (meth)acrylic resins include: poly(meth)acrylates such as polymethyl methacrylate; methyl methacrylate-(meth)acrylic acid copolymers; methyl methacrylate-(meth)acrylic acid copolymers; methyl methacrylate-(meth)acrylic acid copolymers; methyl methacrylate-acrylate-(meth)acrylic acid copolymers; methyl (meth)acrylate-styrene copolymers (MS resins, etc.); copolymers of methyl methacrylate and compounds having alicyclic hydrocarbon groups (e.g., methyl methacrylate-cyclohexyl methacrylate copolymers, methyl methacrylate-norbornyl (meth)acrylate copolymers, etc.). Poly(meth)acrylic acid C such as polymethyl methacrylate is preferably used. 1-6 As the polymer containing an alkyl ester as a main component, it is more preferable to use a methyl methacrylate-based resin containing methyl methacrylate as a main component (50 to 100% by weight, preferably 70 to 100% by weight).

[0362] Polycarbonate resins include polymers in which monomer units are bonded via carbonate groups. Polycarbonate resins may include resins called modified polycarbonates, which have modified polymer backbones, and copolycarbonates. Examples of polycarbonate resins include those described in Japanese Patent Application Laid-Open No. 2012-31370.

[0363] The thickness of the polarizer protective film is preferably 0.1 μm to 60 μm, more preferably 0.5 μm to 40 μm, and even more preferably 1 μm to 30 μm.

[0364] Polarizer protective film can be used in a manner more close to the visible side than polarizer. Therefore, surface treatments such as hard coating, anti-reflection treatment, anti-adhesion treatment, anti-glare treatment can be implemented to polarizer protective film as needed. Further / or, polarizer protective film can also be implemented as needed to process as follows, that is, the visibility when viewing through polarized sunglasses is improved (representatively, giving (elliptical) circular polarization function, giving ultra-high phase difference). By implementing such processing, even when viewing the display screen through polarized lenses such as polarized sunglasses, excellent visibility can be achieved. Therefore, the polarizer plate equipped with the polarizer protective film with phase difference can also be suitable for use in image display devices that can be used outdoors.

[0365] By stretching the film containing the above-mentioned thermoplastic resin, a polarizing element protective film can be produced. As stretching treatment, uniaxial stretching, biaxial stretching, etc. can be mentioned. As stretching directions, the mechanical flow direction (MD) of the unstretched film, the direction (TD) perpendicular thereto, the direction oblique to the mechanical flow direction (MD), etc. can be mentioned. Biaxial stretching can be simultaneous biaxial stretching in two stretching directions, or it can be sequential biaxial stretching in which the film is stretched in a prescribed direction and then stretched in other directions. The stretching treatment can be carried out, for example, by using two or more pairs of clamping rollers with increased circumferential speed on the outlet side to stretch along the longitudinal direction (mechanical flow direction: MD), or by holding both side ends of the unstretched film with a chuck and extending it in a direction (TD) perpendicular to the mechanical flow direction. At this time, by adjusting the thickness of the film or adjusting the stretching ratio, the phase difference value and the wavelength dispersion can be controlled. In addition, by adding a wavelength dispersion modifier to the resin, the wavelength dispersion value can be controlled.

[0366] The polarizing element protective film may contain any appropriate additives according to the purpose. Examples of additives include: hindered phenol-based, phosphorus-based, sulfur-based antioxidants, light stabilizers, ultraviolet absorbers, weathering stabilizers, heat stabilizers and other stabilizers; reinforcing materials such as glass fiber and carbon fiber; near-infrared absorbers; flame retardants such as tris(dibromopropyl) phosphate, triallyl phosphate, and antimony oxide; antistatic agents such as anionic, cationic, and nonionic surfactants; colorants such as inorganic pigments, organic pigments, and dyes; organic fillers and inorganic fillers; resin modifiers; plasticizers; lubricants; phase difference reducing agents, etc. The type, combination, and content of the additives contained can be appropriately set according to the purpose and desired characteristics.

[0367] In order to give desired surface optical properties or other features, a coating layer (surface treatment layer) can be provided on the outer surface of the polarizer protective film. The specific example of the surface treatment layer includes a hard coat, an anti-glare layer, an anti-reflection layer, an antistatic layer, an antifouling layer. The method for forming the surface treatment layer is not particularly limited, and known methods can be used. The surface treatment layer can be formed on one side of the polarizer protective film, and can also be formed on both sides.

[0368] The hard coat layer has the function of increasing the surface hardness of the polarizer protective film and is provided for purposes such as preventing surface scratches. The hard coat layer preferably has a pencil hardness of H or higher as measured by the pencil hardness test specified in JIS K 5600-5-4:1999 "General Test Methods for Coatings - Part 5: Mechanical Properties of Coatings - Section 4: Scratch Hardness (Pencil Method)" (measured by placing the optical film having the hard coat layer on a glass plate).

[0369] The material forming the hard coat layer is generally a material that cures by heat or light. For example, organic hard coat materials such as silicone-based, melamine-based, epoxy-based, (meth)acrylic, and urethane (meth)acrylate-based materials, and inorganic hard coat materials such as silica can be mentioned. Among them, urethane (meth)acrylate-based or multifunctional (meth)acrylate-based hard coat materials are preferably used due to their good adhesion to the polarizer protective film and excellent productivity.

[0370] The hard coat layer may contain various fillers as desired to adjust the refractive index, increase the flexural modulus, stabilize the volume shrinkage, or even improve heat resistance, antistatic properties, anti-glare properties, etc. The hard coat layer may also contain additives such as antioxidants, UV absorbers, light stabilizers, antistatic agents, leveling agents, and defoaming agents.

[0371] To further enhance strength, the hard coat layer may contain additives. The additives are not limited, but examples include inorganic microparticles, organic microparticles, or mixtures thereof. To enhance hardness, the thicker the hard coat layer, the better. However, if it is too thick, it will easily break when cut. Therefore, the hard coat layer is preferably 1 μm to 20 μm, or 2 μm to 10 μm. The thickness of the hard coat layer is preferably 3 μm to 7 μm.

[0372] The anti-glare layer is a layer having fine concavo-convex shapes on its surface, and is preferably formed using the above-mentioned material for forming the hard coat layer.

[0373] An anti-glare layer having a fine concavo-convex shape on its surface can be formed by the following methods: 1) a method of forming a coating film containing microparticles on a stretched film and providing concavo-convex shapes based on the microparticles; 2) a method of forming a coating film containing or not containing microparticles on a stretched film and then pressing it against a mold (roller, etc.) having a concavo-convex shape on the surface to transfer the concavo-convex shape (also called embossing method), etc.

[0374] An antireflection layer is a layer that reduces the reflection of external light from the surface of the polarizer protective film, typically exhibiting a visible light reflectivity of 1.5% or less. This reflectivity is typically achieved by laminating a high-refractive-index layer with a low-refractive-index layer, using the methods and materials described in Japanese Patent Application Laid-Open No. 2021-6929. By adjusting the refractive indices and thicknesses of the layers, the reflected light from each layer can be canceled, resulting in an excellent antireflection function.

[0375] About the anti-reflection layer comprising a high refractive index layer and a low refractive index layer, if a coating composition that can form a high refractive index layer and a low refractive index layer is used to manufacture the anti-reflection layer, the operation is extremely simple, so it is preferred. Here, an example of a coating composition that can form a high refractive index layer and a low refractive index layer is given. The coating composition is liquid, comprising a suitable curable resin and an additive as needed. The coating composition (high refractive index layer forming composition) that can form a high refractive index layer is, for example, a curable resin such as urethane acrylate and an acetophenone system, a benzophenone system, a benzyl dimethyl ketal system, an α-hydroxyalkyl phenone system, an α-aminoalkyl phenone system, a thioxanthone system, etc. The initiator (photopolymerization initiator) for photopolymerization is dissolved in a solvent such as methyl ethyl ketone, methyl isobutyl ketone. In order to make the coating property better, a leveling agent, preferably a fluorine-based leveling agent, can be included. In addition, as a coating type composition (low refractive index layer forming composition) that can form a low refractive index layer, it is in the binder resin of polyethylene glycol diacrylate, pentaerythritol (tri / tetra) acrylate and the like as a curable resin, an initiator (photopolymerization initiator) for photopolymerization such as acetophenone system, benzophenone system, benzyl dimethyl ketal system, α-hydroxyalkyl phenone system, α-aminoalkyl phenone system, thioxanthone system is dissolved in a solution formed by a solvent such as 1-methoxy-2-propyl acetate, methyl isobutyl ketone and the like, and silicon dioxide particles are dispersed. In order to make coating property better, a fluorine-based leveling agent can be included. It should be noted that the coating type composition that can form a high refractive index layer and a low refractive index layer respectively listed here is only an example, and preferably, according to the characteristic of the anti-reflection layer to be formed, a high refractive index layer forming composition and a low refractive index layer forming composition are optimized respectively.

[0376] The antireflection layer may include, for example, a low refractive index layer, or may have a multilayer structure further including a high refractive index layer and / or a medium refractive index layer between the polarizer protective film and the low refractive index layer.

[0377] The low refractive index layer can be formed by applying a coating liquid containing a cured product of the aforementioned curable resin, a light-transmitting resin such as a metal alkoxide polymer, and inorganic particles, and then curing the coating layer as needed. Examples of the inorganic particles include low refractive index particles such as LiF (refractive index 1.4), MgF (refractive index 1.4), 3NaF·AlF (refractive index 1.4), AlF (refractive index 1.4), and Na3AlF6 (refractive index 1.33), as well as hollow silica particles.

[0378] The antistatic layer is provided for the purpose of imparting conductivity to the surface of the polarizer protective film and suppressing the effects of static electricity. The antistatic layer can be formed, for example, by applying a resin composition containing a conductive substance (antistatic agent) to the polarizer protective film. For example, an antistatic hard coat can be formed by coexisting an antistatic agent with the above-mentioned hard coat forming material.

[0379] The antifouling layer is provided to impart hydrophobicity, oleophobicity, perspiration resistance, and antifouling properties. Suitable materials for forming the antifouling layer are fluorine-containing organic compounds. Examples of fluorine-containing organic compounds include fluorocarbons, perfluorosilanes, and polymer compounds thereof. The antifouling layer can be formed using methods such as physical vapor deposition (PVD), CVD, and wet coating, typically exemplified by evaporation and sputtering, depending on the material being formed. The average thickness of the antifouling layer is typically about 1 to 50 nm, preferably 3 to 35 nm.

[0380] (Protective layer)

[0381] The polarizing plate may have a protective layer on one or both sides of the polarizing element. When a liquid crystal polarizer is used as the polarizing element and the liquid crystal polarizer is laminated with other films using an adhesive, the protective layer on the surface of the liquid crystal polarizer can prevent low-molecular components such as unreacted polymerizable liquid crystal compounds and dichroic dyes in the liquid crystal polarizer from diffusing into other layers.

[0382] The protective layer preferably has a small thickness as long as it can inhibit the diffusion of unreacted polymerizable liquid crystal compounds, dichroic dyes, and other low-molecular components in the liquid crystal polarizer into other layers. The thickness of the protective layer is preferably 0.1 μm to 10 μm, more preferably 0.1 μm to 5 μm, and even more preferably 0.1 μm to 3 μm.

[0383] The protective layer is preferably a polymer with a large cross-linking density or a water-soluble polymer with a high hydrophilic interaction. For example, it is formed by comprising at least one selected from (meth) acrylic resin, epoxy resin, oxetane resin, carbamate resin, melamine resin, and polyvinyl alcohol resin. Among them, from the viewpoint of excellent curability and easy formation, it is preferably formed by comprising at least one selected from (meth) acrylic resin, epoxy resin, oxetane resin, carbamate resin, and melamine resin, and more preferably by comprising at least one selected from (meth) acrylic resin and carbamate resin. In addition, from the viewpoint of hydrophilicity, polyvinyl alcohol resin is preferred.

[0384] [Example]

[0385] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. Unless otherwise specified, "%" and "parts" in Examples and Comparative Examples refer to "mass %" and "mass parts," respectively.

[0386] <Production of Polarizing Plate a>

[0387] (Production of Polarizing Plate a)

[0388] A polyvinyl alcohol film having an average degree of polymerization of approximately 2400, a saponification degree of 99.9 mol% or more, and a thickness of 75 μm was immersed in pure water at 30°C, and then immersed in an aqueous solution having an iodine / potassium iodide / water ratio of 0.02 / 2 / 100 at 30°C for iodine dyeing (dyeing step). The polyvinyl alcohol film that had undergone the dyeing step was then immersed in an aqueous solution having a potassium iodide / boric acid / water ratio of 12 / 5 / 100 at 56.5°C for boric acid treatment (boric acid treatment step).

[0389] The polyvinyl alcohol film that had undergone the boric acid treatment was washed with pure water at 8°C and then dried at 65°C to obtain Polarizer A, in which iodine was adsorbed on the polyvinyl alcohol and oriented. Stretching was performed during the iodine dyeing and boric acid treatment steps. The total stretching ratio during this stretching was 5.3 times, and the resulting Polarizer A had a thickness of 27 μm.

[0390] (Production of Polarizing Plate a)

[0391] A cyclic polyolefin resin (COP) film (ZEONOR ZF14, manufactured by ZEON Japan, 13 μm thick) was bonded to one side of polarizer a using an aqueous adhesive. A saponified triacetyl cellulose film (trade name: KC4UYTAC, manufactured by KONICA MINOLTA, 40 μm thick) was bonded to the other side of polarizer a using an aqueous adhesive. The resulting bond was dried at 60°C for 2 minutes while maintaining a tension of 430 N / m to obtain polarizer a. The aqueous adhesive was prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (Kuraray Poval KL318, manufactured by Kuraray) and 1.5 parts of a water-soluble polyamide epoxy resin (Sumirez Resin 650, manufactured by Sumika Chemtex, a 30% solids aqueous solution) to 100 parts of water.

[0392] <Production of Polarizing Plate (b)>

[0393] Saponified triacetyl cellulose films (trade name: KC4UYTAC, manufactured by Konica Minolta, 40 μm thick) were bonded to both sides of polarizer a using the aqueous adhesive used in the preparation of polarizing plate a. The resulting bonded product was dried at 60°C for 2 minutes while maintaining a tension of 430 N / m. This yielded polarizing plate b having triacetyl cellulose (TAC) films as polarizer protective films on both sides.

[0394] <Preparation of the first liquid crystal phase difference layer (1)>

[0395] (Preparation of the first liquid crystal retardation layer forming composition (1))

[0396] To 100 parts of the polymerizable liquid crystal compound Paliocolor LC242 (manufactured by BASF Japan) shown below, 0.1 parts of a leveling agent "BYK-361N" (manufactured by BYK-Chemie) and 2.5 parts of a photopolymerization initiator "Omnirad 907" (manufactured by IGM Resin BV) were added. Furthermore, to 100 parts of the polymerizable liquid crystal compound, 400 parts of propylene glycol-1-monomethyl ether-2-acetate (PGME) were added, and the mixture was stirred at 80°C for 1 hour to prepare a first liquid crystal retardation layer-forming composition (1).

[0397] Polymeric liquid crystal compound Paliocolor LC242:

[0398] [Chemical Formula 6]

[0399]

[0400] (Preparation of the first liquid crystal phase difference layer (1) with a substrate)

[0401] A triacetyl cellulose (TAC) film (KC4UY (thickness 40 μm) manufactured by Konica Minolta Co., Ltd.) cut into a rectangular shape as the first substrate layer (1) was subjected to a rubbing treatment at an angle of 15° to the longitudinal direction of the TAC film, and a first liquid crystal phase difference layer forming composition (1) was applied thereon by a bar coater. The obtained coating layer was dried at 100°C for 1 minute and then cooled to room temperature to obtain a dried film. Next, the dried film was irradiated with 1000 mJ / cm2 of a high-pressure mercury lamp ("Unicure VB-15201BY-A" manufactured by USHIO Electric Co., Ltd.) in a nitrogen atmosphere. 2 The invention relates to a method for preparing a first liquid crystal phase difference layer (1) with a substrate, wherein the first polymer layer (1) (horizontally oriented liquid crystal solidified film) is formed by curing the polymerizable liquid crystal compound in a state of being oriented in a horizontal direction in the plane relative to the first substrate layer (1), and obtaining a first liquid crystal phase difference layer (1) with a substrate comprising the first substrate layer (1) / the first liquid crystal phase difference layer (1) (the first polymer layer (1)).

[0402] The thickness of the obtained first polymer layer (1) was measured using a laser microscope and found to be 1.0 μm. The in-plane phase difference value of the first liquid crystal phase difference layer (1) with a substrate was measured using KOBRA-WR manufactured by Oji Instruments Co., Ltd. As a result, the in-plane phase difference value at a wavelength of 550 nm was Re(550) = 140 nm. It should be noted that the phase difference value of the TAC film serving as the first substrate layer (1) at a wavelength of 550 nm is approximately 0, and therefore has no effect on the optical properties. The orientation angle is 15° relative to the longitudinal direction of the first substrate layer (1). The first liquid crystal phase difference layer (1) has positive wavelength dispersion.

[0403] <Preparation of the first liquid crystal phase difference layer (2)>

[0404] (Preparation of the first liquid crystal phase difference layer (2) with a substrate)

[0405] On the first substrate layer (1) described in the preparation of the first liquid crystal phase difference layer (1) with a substrate, the first liquid crystal phase difference layer (2) is formed according to the preparation steps of the third optical anisotropic layer described in paragraphs

[0136] and

[0137] of International Publication No. 2021 / 060378, thereby obtaining the first liquid crystal phase difference layer (2) with a substrate comprising the first substrate layer (1) / the first liquid crystal phase difference layer (2) (the first polymer layer (2)).

[0406] <Preparation of the first liquid crystal phase difference layer (3)>

[0407] (Preparation of Vertical Alignment Layer Forming Composition (1) (Alignment Layer Forming Composition))

[0408] As a composition (1) for forming a vertical alignment layer, a mixture of 2-phenoxyethyl acrylate, tetrahydrofurfuryl acrylate, dipentaerythritol triacrylate and bis(2-vinyloxyethyl) ether in a ratio of 1:1:4:5 was used, and LUCIRIN TPO as a polymerization initiator was added in a ratio of 4%.

[0409] (Preparation of the first liquid crystal phase difference layer forming composition (2))

[0410] The first liquid crystal retardation layer-forming composition (2) was prepared by preparing a photopolymerizable nematic liquid crystal compound (RMM28B manufactured by Merck) and a solvent so that the solid content was 1 to 1.5 g. The solvent used was a mixed solvent prepared by mixing methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), and cyclohexanone (CHN) at a mass ratio (MEK:MIBK:CHN) of 35:30:35.

[0411] (Preparation of the first liquid crystal phase difference layer (3) with a substrate)

[0412] A polyethylene terephthalate (PET) film having a thickness of 38 μm was prepared as the first substrate layer (2). A vertical alignment layer forming composition (1) was applied to one side of the first substrate layer (2) to a thickness of 3 μm and irradiated with 200 mJ / cm 2 The first orientation layer (1) is produced as a vertical orientation layer by irradiating ultraviolet rays.

[0413] The first liquid crystal phase difference layer forming composition (2) is applied to the first orientation layer (1) by die coating. The coating amount is 4 to 5 g (wet). The drying temperature is set to 75°C and the drying time is set to 120 seconds to dry the coating. Then, the coating is irradiated with ultraviolet light (UV) to polymerize the polymerizable liquid crystal compound to form a first polymer layer (3), thereby obtaining a first liquid crystal phase difference layer (3) with a substrate comprising a first substrate layer (2) / a first liquid crystal phase difference layer (3) (a first orientation layer (1) / a first polymer layer (3)).

[0414] The first liquid crystal phase difference layer (3) with a substrate is a positive C plate. The thickness of the first liquid crystal phase difference layer (3) is 4 μm. After the first liquid crystal phase difference layer (3) with a substrate is bonded to the glass with the aid of an adhesive, the first substrate layer (3) is peeled off and the in-plane phase difference value of the first liquid crystal phase difference layer (3) is measured. The measurement is performed using "KOBRA-WPR" manufactured by Oji Instruments Co., Ltd. The in-plane phase difference value at a wavelength of 550 nm is Re (550) = 1 nm, and the phase difference value in the thickness direction at a wavelength of 550 nm is Rth (550) = -100 nm. The first liquid crystal phase difference layer (3) has positive wavelength dispersion.

[0415] <Preparation of the First Liquid Crystal Retardation Layer (c1)>

[0416] (Preparation of Oriented Polymer Composition (c1) (Oriented Layer-Forming Composition (c1)))

[0417] Water was added to commercially available polyvinyl alcohol (polyvinyl alcohol 1000 completely saponified type, manufactured by Wako Pure Chemical Industries, Ltd.), and the mixture was heated at 100° C. for 1 hour to obtain an oriented polymer composition (c1).

[0418] (Preparation of the First Liquid Crystal Retardation Layer (c1) with a Substrate)

[0419] An oriented polymer composition (c1) was applied to a triacetylcellulose (TAC) film (manufactured by Konica Minolta Co., Ltd., KC8UY (thickness 80 μm)) cut into a rectangular shape as the first substrate layer (c1), and the film was heated and dried to form a first oriented layer (c1) with a thickness of 100 nm. The surface of the first oriented layer (c1) was subjected to a friction treatment at an angle of 15° to the longitudinal direction of the above-mentioned TAC film, and the first liquid crystal phase difference layer forming composition (1) was applied thereon using a rod coater. The obtained coating layer was dried at 100°C for 1 minute and then cooled to room temperature to obtain a dry film. Next, a high-pressure mercury lamp ("Unicure VB-15201BY-A" manufactured by USHIO Electric Co., Ltd.) was used to irradiate the dry film with 1000 mJ / cm 2 The invention relates to a method for preparing a first liquid crystal phase difference layer (c1) with a substrate, wherein the first liquid crystal phase difference layer (c1) is formed by curing the polymerizable liquid crystal compound in a state of being oriented in a horizontal direction in the plane relative to the first substrate layer (c1) (a horizontally oriented liquid crystal cured film), and a first liquid crystal phase difference layer (c1) with a substrate comprising the first substrate layer (c1) / the first liquid crystal phase difference layer (c1) (the first oriented layer (c1) / the first polymer layer (c1)) is obtained.

[0420] The thickness of the obtained first polymer layer (c1) was measured using a laser microscope and found to be 1.0 μm. The in-plane phase difference value of the first liquid crystal phase difference layer (c1) with a substrate was measured using KOBRA-WR manufactured by Oji Instruments Co., Ltd. As a result, the in-plane phase difference value at a wavelength of 550 nm was Re(550)=140 nm. It should be noted that the phase difference value of the TAC film serving as the first substrate layer (c1) at a wavelength of 550 nm is approximately 0, and therefore has no effect on the optical properties. The orientation angle is 15° relative to the longitudinal direction of the first substrate layer (c1). The first liquid crystal phase difference layer (c1) has positive wavelength dispersion.

[0421] [Measurement of Light Transmittance Tx of the First Liquid Crystal Retardation Layer with Substrate]

[0422] The transmittance Tx of the first liquid crystal retardation layer with a substrate obtained above at a wavelength of 317 nm was measured using an ultraviolet-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation). The results are shown in Tables 1 to 3.

[0423] [Measurement of Thickness of First Base Material Layer]

[0424] The thickness of the first base material layer was measured using a contact-type film thickness meter (Nikon: DIGIMICRO MH-15M). The results are shown in Tables 1 to 3.

[0425] <Preparation of the Second Liquid Crystal Retardation Layer (1)>

[0426] (Preparation of the Second Liquid Crystal Retardation Layer-Forming Composition (1))

[0427] A polymerizable liquid crystal compound (A1) and a polymerizable liquid crystal compound (A2) having the structures shown below were prepared. The polymerizable liquid crystal compound (A1) and the polymerizable liquid crystal compound (A2) were prepared according to the method described in Japanese Patent Application Laid-Open No. 2010-244038.

[0428] Polymerizable liquid crystal compound (A1):

[0429] [Chemical Formula 7]

[0430]

[0431] Polymerizable liquid crystal compound (A2):

[0432] [Chemical Formula 8]

[0433]

[0434] The polymerizable liquid crystal compound (A1) and the polymerizable liquid crystal compound (A2) were mixed at a mass ratio of 80:20 to obtain a mixture. To 100 parts of the obtained mixture, 0.1 parts of a leveling agent "Megafac F-556" (manufactured by DIC Corporation), 2.5 parts of "Omnirad 907" (manufactured by IGM Resin BV) as a photopolymerization initiator, and 0.1 parts of the ionic compound (B) shown below were added. Furthermore, 650 parts of cyclopentanone were added to 100 parts of the mixture, and the mixture was stirred at a temperature of 80°C for 1 hour to prepare a second liquid crystal retardation layer-forming composition (1).

[0435] Ionic compound (B)

[0436] [Chemical Formula 9]

[0437]

[0438] (Preparation of the Second Liquid Crystal Retardation Layer (1) with a Substrate)

[0439] A cycloolefin polymer (COP) film (ZF14, 13 μm thick, manufactured by ZEON Corporation of Japan) cut into rectangular shapes as the second substrate layer (1) was subjected to corona treatment using a corona treatment device (AGF-B 10; manufactured by Kasuga Electric Co., Ltd.), and then an oriented polymer composition (c1) was applied thereto. After heat drying, a second oriented polymer layer (1) having a thickness of 100 nm was formed. The surface of the second oriented layer (1) was rubbed at an angle of 75° to the longitudinal direction of the COP film, and a second liquid crystal retardation layer forming composition (1) was applied thereto using a bar coater. The film was dried at 120°C for 2 minutes to obtain a dried film. The dried film was irradiated with an exposure dose of 1000 mJ / cm2 using a high-pressure mercury lamp ("Unicure VB-15201BY-A" manufactured by USHIO Electric Co., Ltd.) at a temperature of 80°C in a nitrogen atmosphere. 2 The second liquid crystal retardation layer (1) with a substrate is formed by applying ultraviolet light (365 nm reference) to the second polymer layer (1) solidified in a state where the optical axis of the polymerizable liquid crystal compound is oriented in a horizontal direction relative to the in-plane of the second substrate layer (1), thereby obtaining a second liquid crystal retardation layer (1) with a substrate as an optical film. The second liquid crystal retardation layer (1) with a substrate has a layer structure of second substrate layer (1) / second liquid crystal retardation layer (1) (second orientation layer (1) / second polymer layer (1)).

[0440] The thickness of the obtained second polymer layer (1) was measured using a laser microscope and found to be 1.8 μm. The in-plane phase difference value of the second liquid crystal phase difference layer (1) with a substrate was measured using KOBRA-WR manufactured by Oji Instruments Co., Ltd. As a result, the in-plane phase difference value at a wavelength of 550 nm was Re(550) = 270 nm. It should be noted that the phase difference value of the COP film serving as the second substrate layer (1) at a wavelength of 550 nm is approximately 0, and therefore has no effect on the optical properties of the second liquid crystal phase difference layer (1) with a substrate. The orientation angle is 75° relative to the longitudinal direction of the second substrate layer (1). The second liquid crystal phase difference layer (1) has positive wavelength dispersion.

[0441] <Preparation of the Second Liquid Crystal Retardation Layer (2)>

[0442] (Preparation of the photo-alignment film-forming composition (2) (alignment layer-forming composition))

[0443] A photo-alignment material having the following structure (weight average molecular weight: 50,000, m:n=50:50) was prepared according to the method described in Japanese Patent Application Laid-Open No. 2021-196514. Two parts of the photo-alignment material and 98 parts of cyclopentanone (solvent) were mixed as components, and the resulting mixture was stirred at 80° C. for 1 hour to prepare a photo-alignment film-forming composition (2).

[0444] Photo-oriented materials:

[0445] [Chemical Formula 10]

[0446]

[0447] (Preparation of the Second Liquid Crystal Retardation Layer-Forming Composition (2))

[0448] A polymerizable liquid crystal compound (A3) and a polymerizable liquid crystal compound (A4) having the structures shown below were prepared. The polymerizable liquid crystal compound (A3) was prepared in the same manner as described in JP-A-2019-003177. The polymerizable liquid crystal compound (A4) was prepared in the same manner as described in JP-A-2009-173893.

[0449] Polymerizable liquid crystal compound (A3):

[0450] [Chemical Formula 11]

[0451]

[0452] Polymerizable liquid crystal compound (A4):

[0453] [Chemical Formula 12]

[0454]

[0455] 1 mg of the polymerizable liquid crystal compound (A3) was dissolved in 10 mL of chloroform to obtain a solution. The resulting solution was added to a measuring cuvette with a 1 cm optical path length, and a measuring sample was added. The measuring sample was placed in an ultraviolet-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation) to measure the absorption spectrum. The wavelength of maximum absorbance was read from the obtained absorption spectrum. The maximum absorption wavelength λmax within the wavelength range of 300 to 400 nm was 356 nm.

[0456] The polymerizable liquid crystal compound (A3) and the polymerizable liquid crystal compound (A4) were mixed at a mass ratio of 90:10 to obtain a mixture. 0.1 parts of a leveling agent "BYK-361N" (manufactured by BM Chemie) and 3 parts of a photopolymerization initiator "Irgacure OXE-03" (manufactured by BASF Japan Co., Ltd.) were added to 100 parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so as to obtain a solid content concentration of 13%. The mixture was stirred at a temperature of 80° C. for 1 hour to prepare a second liquid crystal phase difference layer forming composition (2).

[0457] (Preparation of the Second Liquid Crystal Retardation Layer (2) with a Substrate)

[0458] A composition for forming a photo-alignment film (2) was applied to a biaxially stretched polyethylene terephthalate (PET) film (Diafoil, manufactured by Mitsubishi Plastics Co., Ltd.) as the second substrate layer (2) using a rod coater. The resulting coating layer was dried at 120°C for 2 minutes and then cooled to room temperature to form a dry film. Subsequently, 100 mJ (313 nm reference) of polarized ultraviolet light was irradiated using a UV irradiation device (SPOT CURE SP-9; manufactured by USHIO Electric Co., Ltd.) to obtain a photo-alignment film as the second alignment layer (2). The thickness of the second alignment layer (2) measured using an ellipsometer M-220 manufactured by JASCO Corporation was 100 nm.

[0459] The second liquid crystal retardation layer forming composition (2) was applied onto the second orientation layer (2) using a bar coater, and dried by heating at 120°C for 2 minutes, followed by cooling to room temperature to obtain a dry film. Next, the dry film was irradiated with an exposure dose of 500 mJ / cm2 using a high-pressure mercury lamp ("Unicure VB-15201BY-A" manufactured by USHIO Electric Co., Ltd.) in a nitrogen atmosphere. 2The second polymer layer (2) (horizontally oriented liquid crystal cured film) is formed by curing the polymerizable liquid crystal compound in a state of being oriented in a horizontal direction in the plane relative to the second substrate layer (2) by ultraviolet rays (365 nm reference), thereby obtaining a second liquid crystal phase difference layer (2) with a substrate as an optical film. The second liquid crystal phase difference layer (2) with a substrate has a layer structure of second substrate layer (2) / second liquid crystal phase difference layer (2) (second orientation layer (2) / second polymer layer (2)). The thickness of the second polymer layer (2) measured using a laser microscope LEXT OLS4100 manufactured by Olympus Corporation was 2.0 μm.

[0460] The second liquid crystal phase difference layer (2) with a substrate is subjected to a corona treatment on the second liquid crystal phase difference layer (2) side, and is bonded to glass with a 25 μm pressure-sensitive adhesive manufactured by LINTEC, and the second substrate layer (2) is peeled off and removed. The in-plane phase difference value is measured using KOBRA-WR manufactured by Oji Instruments Co., Ltd. It should be noted that the in-plane phase difference value for light with a wavelength of 450 nm, 550 nm and 650 nm is obtained by using the Cauchy dispersion formula obtained from the measurement results of the in-plane phase difference value for light with a wavelength of 448.2 nm, 498.6 nm, 548.4 nm, 587.3 nm, 628.7 nm and 748.6 nm.

[0461] As a result, the in-plane phase difference values ​​of the second liquid crystal phase difference layer (2) are Re(450)=122nm, Re(550)=140nm, and Re(650)=144nm. The relationship between the in-plane phase difference values ​​at each wavelength is as follows. The second liquid crystal phase difference layer (2) has reverse wavelength dispersion.

[0462] Re(450) / Re(550)=0.87

[0463] Re(650) / Re(550)=1.03

[0464] [Wherein, Re(450) represents the in-plane retardation value relative to light with a wavelength of 450 nm, Re(550) represents the in-plane retardation value relative to light with a wavelength of 550 nm, and Re(650) represents the in-plane retardation value relative to light with a wavelength of 650 nm.]

[0465] [Measurement of Light Transmittance of Second Liquid Crystal Retardation Layer]

[0466] After the second liquid crystal phase difference layer side of the second liquid crystal phase difference layer with a substrate obtained above was bonded to glass via an adhesive layer, the second substrate layer was peeled off to obtain a measurement sample (1). For the laminate of glass and the adhesive layer used in the preparation of the measurement sample (1), the transmittance at a wavelength of 317 nm was measured using an ultraviolet-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation), and this was used as a baseline. The transmittance of the measurement sample (1) at a wavelength of 317 nm was measured in the same manner as above, and the obtained measured value was used as the transmittance of the second liquid crystal phase difference layer. The results are shown in Tables 1 to 3.

[0467] <Preparation of a photocurable adhesive composition>

[0468] The following components were blended and mixed, and then degassed to prepare an adhesive composition as a photocurable adhesive composition.

[0469] Neopentyl glycol diglycidyl ether (cationically polymerizable compound) (trade name: EX-211L, manufactured by Nagase ChemteX Co., Ltd.): 30 parts

[0470] 3-Ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (cationically polymerizable compound) (trade name: OXT-221, manufactured by Toagosei Co., Ltd.): 13 parts

[0471] Bisphenol A type epoxy resin (cationic polymerizable compound) (trade name: EP-4100E, ADEKA Co., Ltd., viscosity 13 Pa·s (temperature 25° C.)): 45 parts

[0472] Aromatic-containing oxetane compound (cationic polymerizable compound) (trade name: TCM-104, manufactured by TRONLY): 12 parts

[0473] Photopolymerization initiator (photocationic polymerization initiator) (trade name: CPI-100P, manufactured by San-Apro Co., Ltd., 50% propylene carbonate solution): 2.25 parts (solid content)

[0474] 1,4-Diethoxynaphthalene (photosensitizing agent): 1 part

[0475] [Measurement of Maximum Absorption Wavelength of Photopolymerization Initiator]

[0476] The maximum absorption wavelength of the photopolymerization initiator used in the adhesive composition was dissolved in methanol and measured using an ultraviolet-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation). The photopolymerization initiator has a maximum absorption wavelength at 305 nm.

[0477] <Adhesive Sheet Production>

[0478] (Preparation of Adhesive Composition)

[0479] A mixed solution of 100 parts of ethyl acetate, 99.0 parts of butyl acrylate, 0.5 parts of 2-hydroxyethyl acrylate, and 0.5 parts of acrylic acid was placed in a reaction vessel equipped with a condenser, a nitrogen inlet tube, a thermometer, and a stirrer. While replacing the air in the apparatus with nitrogen to remove oxygen, the internal temperature was raised to 55°C. Then, the entire amount of a solution prepared by dissolving 0.12 parts of azobisisobutyronitrile (polymerization initiator) in 10 parts of ethyl acetate was added. After the addition of the polymerization initiator, the temperature was maintained at that temperature for 1 hour. Subsequently, while maintaining the internal temperature at 54-56°C, ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr. The addition of ethyl acetate was stopped when the concentration of the (meth)acrylic resin reached 35% by mass. The temperature was further maintained at that temperature until 6 hours had passed from the start of the addition of ethyl acetate. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20% by mass, thereby preparing an acrylic resin solution (1). The obtained acrylic resin had a weight-average molecular weight (Mw) of 1.7 million and a molecular weight distribution (Mw / Mn) of 3.9. Mw and Mn were measured using a GPC apparatus equipped with two TSKgel GMHHR-H(S) columns connected in series, using tetrahydrofuran as the eluent, under the following conditions: a sample concentration of 2 mg / mL, a sample introduction volume of 100 μL, a temperature of 40°C, and a flow rate of 1 mL / min, in terms of standard polystyrene.

[0480] To 80 parts of the solid content of the acrylic resin solution (1), 20 parts (solid content) of a difunctional acrylate (obtained from Shin-Nakamura Chemical Co., Ltd.; product number "A-DOG"), 2.5 parts of a crosslinking agent (Mitsui Chemicals: trade name "D-101E" (an ethyl acetate solution of a trimethylolpropane adduct of toluene diisocyanate (solid content concentration 75% by mass)) in terms of active ingredient, 1.5 parts of a photopolymerization initiator (Ciba Specialty Chemicals: trade name "Irgacure 500"), and 0.3 parts of a silane coupling agent (Shin-Etsu Chemical Co., Ltd.: trade name "KBM-403") were added, and ethyl acetate was further added so that the solid content concentration became 13% to obtain an adhesive composition.

[0481] A-DOG is a diacrylate of an acetal compound of hydroxypivalaldehyde and trimethylolpropane, and has the following structure.

[0482] [Chemical Formula 13]

[0483]

[0484] (Preparation of Adhesive Layer)

[0485] The adhesive composition prepared above was applied to the release-treated surface of a separator made of polyethylene terephthalate film [MRV(V04) manufactured by Mitsubishi Chemical (thickness: 38 μm)] using an applicator to a thickness of 5 μm after drying. The mixture was then dried at 100°C for 1 minute to produce an adhesive layer. The surface of the resulting adhesive layer opposite the separator was then bonded to the release-treated surface of a separator made of polyethylene terephthalate film [MRF manufactured by Mitsubishi Chemical (thickness: 38 μm)]. The adhesive sheet was then irradiated with ultraviolet light under the following conditions to produce the adhesive sheet.

[0486] UV irradiation conditions

[0487] ·Use Fusion UV lamp system (Fusion UV Systems) H Bulb

[0488] Cumulative light intensity 250mJ / cm 2

[0489] [Example 1]

[0490] (Production of Phase Difference Body (1))

[0491] The first liquid crystal phase difference layer (1) side of the first liquid crystal phase difference layer (1) with a substrate and the second liquid crystal phase difference layer (1) side of the second liquid crystal phase difference layer (1) with a substrate are subjected to corona treatment respectively. The adhesive composition prepared above is applied to one corona-treated surface, and the first liquid crystal phase difference layer (1) of the first liquid crystal phase difference layer (1) with a substrate and the second liquid crystal phase difference layer (1) of the second liquid crystal phase difference layer (1) with a substrate are bonded together. Ultraviolet rays are irradiated from the first liquid crystal phase difference layer (1) with a substrate to cure the adhesive composition and form an adhesive layer (1) as a first adhesive layer. The UVA with a wavelength of 320nm to 390nm becomes 400mJ / cm 2 The method of irradiating ultraviolet rays was used. A phase difference body (1) as an optical laminate having a layer structure of second substrate layer (1) / second liquid crystal phase difference layer (1) (second orientation layer (1) / second polymer layer (1)) / adhesive layer (1) / first liquid crystal phase difference layer (1) / first substrate layer (1) was obtained. The thickness of the adhesive layer (1) was 2.0 μm.

[0492] (Production of optical layered body (1))

[0493] The TAC film side of the polarizing plate a is subjected to a corona treatment, and the surface of the adhesive sheet obtained above from which one spacer has been peeled is adhered, and then the other spacer is peeled off to expose the adhesive layer. The second liquid crystal phase difference layer (1) (second polymer layer (1)) exposed by peeling off the second substrate layer (1) of the phase difference body (1) is subjected to a corona treatment and adhered to the above-exposed adhesive layer (second adhesive layer) to obtain an optical laminate (1). The second orientation layer (1) is also peeled off together with the second substrate layer (1). The layer structure of the optical laminate (1) is polarizing plate a / adhesive layer / second liquid crystal phase difference layer (1) (second polymer layer (1)) / adhesive layer (1) / first liquid crystal phase difference layer (1) / first substrate layer (1).

[0494] (Production of a laminate with an optical film (1))

[0495] The first substrate layer (1) is peeled off from the optical laminate (1) to obtain a laminate (1) with an optical film. The laminate (1) with an optical film has a layer structure of polarizing plate a / adhesive layer / second liquid crystal retardation layer (1) (second polymer layer (1)) / adhesive layer (1) / first liquid crystal retardation layer (1).

[0496] [Examples 2 to 4]

[0497] Optical laminates (2) to (4) and laminates with optical films (2) to (4) were obtained by following the same steps as in Example 1 except that the amount of ultraviolet light irradiated to cure the adhesive composition from the side of the first liquid crystal phase difference layer (1) with a substrate was changed to the amount shown in Table 1 to form adhesive layers (2) to (4).

[0498] [Example 5]

[0499] An optical laminate (5) and an optical film-attached laminate (5) were obtained by the same procedure as in Example 3 except that the thickness of the adhesive layer was changed to the thickness shown in Table 1 to form the adhesive layer (5).

[0500] [Example 6]

[0501] (Production of Phase Difference Body (6))

[0502] A phase difference body (6) was obtained according to the procedure of Example 1 except that the adhesive layer (1) was replaced with the adhesive composition prepared above to form an adhesive layer (6) having a thickness of 3.5 μm. The phase difference body (6) had a layer structure of second substrate layer (1) / second liquid crystal phase difference layer (1) (second orientation layer (1) / second polymer layer (1)) / adhesive layer (6) / first liquid crystal phase difference layer (1) / first substrate layer (1).

[0503] (Production of optical laminate (6) and laminate (6) with optical film)

[0504] An optical layered body (6) and a layered body (6) with an optical film were obtained according to the procedure of Example 1 except that the layered body (6) was used instead of the layered body (1).

[0505] [Example 7]

[0506] (Production of Phase Difference Body (7))

[0507] The first liquid crystal phase difference layer (2) side of the first liquid crystal phase difference layer (2) with a substrate and the second liquid crystal phase difference layer (2) side of the second liquid crystal phase difference layer (2) with a substrate are subjected to corona treatment respectively. The adhesive composition prepared above is applied to one corona-treated surface, and the first liquid crystal phase difference layer (2) of the first liquid crystal phase difference layer (2) with a substrate and the second liquid crystal phase difference layer (2) of the second liquid crystal phase difference layer (2) with a substrate are bonded together. Ultraviolet rays are irradiated from the first liquid crystal phase difference layer (2) with a substrate to cure the adhesive composition and form an adhesive layer (7) as a first adhesive layer. The UVA with a wavelength of 320nm to 390nm becomes 400mJ / cm 2 The method of irradiating ultraviolet rays was used. A phase difference body (7) as an optical laminate having a layer structure of second substrate layer (2) / second liquid crystal phase difference layer (2) (second orientation layer (2) / second polymer layer (2)) / adhesive layer (7) / first liquid crystal phase difference layer (2) / first substrate layer (2) was obtained. The thickness of the adhesive layer (7) was 2.0 μm.

[0508] (Production of optical laminate (7))

[0509] The TAC film side of the polarizing plate a is subjected to corona treatment, and the surface of the adhesive sheet obtained above after peeling off one spacer is adhered, and then the other spacer is peeled off to expose the adhesive layer. The second liquid crystal phase difference layer (2) (second polymer layer (2)) exposed by peeling off the second substrate layer (2) of the phase difference body (3) is subjected to corona treatment and adhered to the above-mentioned exposed adhesive layer (second adhesive layer) to obtain an optical laminate (7). The second orientation layer (2) is also peeled off together with the second substrate layer (2). The layer structure of the optical laminate (7) is polarizing plate a / adhesive layer / second liquid crystal phase difference layer (2) (second polymer layer (2)) / adhesive layer (7) / first liquid crystal phase difference layer (2) / first substrate layer (1).

[0510] (Production of a laminate with an optical film (7))

[0511] The first substrate layer (1) is peeled off from the optical laminate (7) to obtain a laminate (7) with an optical film. The laminate (7) with an optical film has a layer structure of polarizing plate / adhesive layer / second liquid crystal retardation layer (2) (second polymer layer (2)) / adhesive layer (7) / first liquid crystal retardation layer (2).

[0512] [Example 8]

[0513] (Production of Phase Difference Body (8))

[0514] A phase difference body (8) was obtained according to the procedure of Example 7, except that the adhesive layer (7) was replaced with the adhesive composition prepared above to form an adhesive layer (8) having a thickness of 3.5 μm. The phase difference body (8) had a layer structure of second substrate layer (2) / second liquid crystal phase difference layer (2) (second orientation layer (2) / second polymer layer (2)) / adhesive layer (8) / first liquid crystal phase difference layer (2) / first substrate layer (1).

[0515] (Production of optical laminate (8) and laminate (8) with optical film)

[0516] An optical layered body (8) and a layered body (8) with an optical film were obtained according to the procedure of Example 7 except that the layered body (8) was used instead of the layered body (3).

[0517] [Example 9]

[0518] (Production of Phase Difference Body (9))

[0519] The first liquid crystal phase difference layer (3) side of the first liquid crystal phase difference layer (3) with a substrate and the second liquid crystal phase difference layer (2) side of the second liquid crystal phase difference layer (2) with a substrate are subjected to corona treatment respectively. The adhesive composition prepared above is applied to one corona-treated surface, and the first liquid crystal phase difference layer (3) of the first liquid crystal phase difference layer (3) with a substrate and the second liquid crystal phase difference layer (2) of the second liquid crystal phase difference layer (2) with a substrate are bonded together. Ultraviolet rays are irradiated from the first liquid crystal phase difference layer (3) side with a substrate to cure the adhesive composition and form an adhesive layer (9) as a first adhesive layer. The UVA with a wavelength of 320nm to 390nm becomes 400mJ / cm 2 The method of irradiating ultraviolet rays is as follows. A phase difference body (9) as an optical laminate having a layer structure of the second substrate layer (2) / the second liquid crystal phase difference layer (2) (the second orientation layer (2) / the second polymer layer (2)) / the adhesive layer (9) / the first liquid crystal phase difference layer (3) (the first polymer layer (3) / the first orientation layer (1)) / the first substrate layer (2) is obtained. The thickness of the adhesive layer (9) is 2.0 μm.

[0520] (Production of optical laminate (9))

[0521] The TAC film side of the polarizing plate a is subjected to corona treatment, and the surface of the adhesive sheet obtained above from which one spacer is peeled is adhered, and then the other spacer is peeled off to expose the adhesive layer. The second liquid crystal phase difference layer (2) (second polymer layer (2)) exposed by peeling off the second substrate layer (2) of the phase difference body (9) is subjected to corona treatment and adhered to the above-exposed adhesive layer (second adhesive layer) to obtain an optical laminate (5). The second orientation layer (2) is also peeled off together with the second substrate layer (2). The layer structure of the optical laminate (9) is polarizing plate a / adhesive layer / second liquid crystal phase difference layer (2) (second polymer layer (2)) / adhesive layer (9) / first liquid crystal phase difference layer (3) (first polymer layer (3) / first orientation layer (1)) / first substrate layer (2).

[0522] (Production of a laminate (9) with an optical film)

[0523] The first substrate layer (3) is peeled off from the optical laminate (5) to obtain a laminate (9) with an optical film. The first orientation layer (1) is also peeled off at the same time as the first substrate layer (2). The laminate (9) with an optical film has a layer structure of polarizing plate / adhesive layer / second liquid crystal phase difference layer (2) (second polymer layer (2)) / adhesive layer (9) / first liquid crystal phase difference layer (3) (first polymer layer (3)).

[0524] [Example 10]

[0525] (Production of Phase Difference Body (10))

[0526] A phase difference body (10) was obtained according to the procedure of Example 9, except that the adhesive layer (9) was replaced with the adhesive composition prepared above to form an adhesive layer (10) having a thickness of 3.5 μm. The phase difference body (10) had a layer structure of second substrate layer (2) / second liquid crystal phase difference layer (2) (second orientation layer (2) / second polymer layer (2)) / adhesive layer (10) / first liquid crystal phase difference layer (3) (first polymer layer (3) / first orientation layer (1)) / first substrate layer (2).

[0527] (Production of optical laminate (10) and laminate (10) with optical film)

[0528] An optical layered body (6) and a layered body with an optical film (10) were obtained according to the procedure of Example 9 except that the layered body (10) was used instead of the layered body (9).

[0529] [Comparative Example 1]

[0530] (Fabrication of Phase Difference Body (c1))

[0531] The first liquid crystal phase difference layer (c1) side of the first liquid crystal phase difference layer (c1) with a substrate and the second liquid crystal phase difference layer (1) side of the second liquid crystal phase difference layer (1) with a substrate are subjected to corona treatment respectively. The adhesive composition prepared above is applied to one corona-treated surface, and the second liquid crystal phase difference layer (1) of the second liquid crystal phase difference layer (1) with a substrate is bonded to the first liquid crystal phase difference layer (c1) with a substrate. Ultraviolet rays are irradiated from the first liquid crystal phase difference layer (c1) side with a substrate to cure the adhesive composition and form an adhesive layer (c1). The UVA with a wavelength of 320nm to 390nm becomes 400mJ / cm 2 The method of irradiating ultraviolet rays was used. A phase difference body (c1) having a layer structure of second substrate layer (1) / second liquid crystal phase difference layer (1) (second orientation layer (1) / second polymer layer (1)) / adhesive layer (c1) / first liquid crystal phase difference layer (c1) (first polymer layer (c1) / first orientation layer (c1)) / first substrate layer (c1) was obtained. The thickness of the adhesive layer (c1) was 2.0 μm.

[0532] (Production of optical layered body (c1))

[0533] A corona treatment is applied to one TAC film side of the polarizing plate b, and the surface of the adhesive sheet obtained above from which one spacer has been peeled is adhered, and then the other spacer is peeled off to expose the adhesive layer. A corona treatment is applied to the second liquid crystal phase difference layer (1) (second polymer layer (1)) exposed by peeling off the second substrate layer (1) of the phase difference body (c1), and adhered to the above-exposed adhesive layer (second adhesive layer) to obtain an optical laminate (c1). The second orientation layer (1) is also peeled off together with the second substrate layer (1). The layer structure of the optical laminate (c1) is polarizing plate b / adhesive layer / second liquid crystal phase difference layer (1) (second polymer layer (1)) / adhesive layer (1) / first liquid crystal phase difference layer (c1) (first polymer layer (c1) / first orientation layer (c1)) / first substrate layer (c1).

[0534] (Production of a laminate (c1) with an optical film)

[0535] The first substrate layer (c1) is peeled off from the optical laminate (c1) to obtain a laminate (1) with an optical film. The first orientation layer (c1) is peeled off at the same time as the first substrate layer (c1). The laminate (1) with an optical film has a layer structure of polarizing plate b / adhesive layer / second liquid crystal phase difference layer (1) (second polymer layer (1)) / adhesive layer (1) / first liquid crystal phase difference layer (1) (first polymer layer (1)).

[0536] [Example 11]

[0537] When preparing an optical laminate, the corona-treated surface of the polarizing plate a is bonded to the corona-treated surface of the second liquid crystal phase difference layer (1) (second polymer layer (1)) exposed by peeling off the second substrate layer (1) of the phase difference body (1) using the adhesive composition prepared above, and the adhesive is cured by irradiating ultraviolet light from the phase difference body (1) side from which the second substrate layer is peeled off, thereby forming an adhesive layer serving as a second adhesive layer. An optical laminate (11) and a laminate (11) with an optical film are obtained by the same procedure as in Example 1 except that the UVA with a wavelength of 320 nm to 390 nm becomes 400 mJ / cm 2 The thickness of the adhesive layer as the second adhesive layer was 2.5 μm.

[0538] [Example 12]

[0539] When preparing an optical laminate, the UVA with a wavelength of 320 nm to 390 nm is 600 mJ / cm 2 In the same manner as in Example 11, an optical laminate (12) and a laminate (12) with an optical film were obtained, except that ultraviolet rays were irradiated from the side of the phase difference body (1) from which the second substrate layer was peeled off.

[0540] [Examples 13 to 15]

[0541] Optical layered bodies (13) to (15) and layered bodies with optical films (13) to (15) were obtained by the same procedure as in Example 11 except that phase difference bodies (6) to (8) were used in the production of the optical layered bodies.

[0542] [Measurement of Thickness of Adhesive Layer]

[0543] The thickness of the adhesive layer was measured using a laser microscope manufactured by KEYENCE. The results are shown in Tables 1 to 3.

[0544] [Measurement of light transmittance Ty of optical film]

[0545] In the optical laminate and the laminate with an optical film, the polarizing plate / adhesive layer (second adhesive layer) / second liquid crystal retardation layer constituted the optical film. The transmittance Ty of this optical film at a wavelength of 317 nm was measured using an ultraviolet-visible spectrophotometer ("UV-2450" manufactured by Shimadzu Corporation) and compared with the transmittance Tx of the first liquid crystal retardation layer with a substrate at a wavelength of 317 nm. The results are shown in Tables 1 to 3.

[0546] [Measurement of the Remaining Amount of Photopolymerization Initiator in the Adhesive Layer]

[0547] Using a phase difference body, the proportion of the photopolymerization initiator contained in the adhesive layer is calculated according to the following steps. First, the first substrate layer and the second substrate layer are peeled off from the phase difference body, and the laminated body of the layer structure of the second liquid crystal phase difference layer / adhesive layer / first liquid crystal phase difference layer is freeze-pulverized and filtered after being dissolved in a solvent (acetonitrile) to obtain a test solution. The obtained test solution is subjected to high performance liquid chromatography, and the photopolymerization initiator is quantified based on the peak area of ​​the component derived from the photopolymerization initiator. The measurement conditions are as follows.

[0548] Device: LC-20A series (manufactured by Shimadzu Corporation)

[0549] Column: Kinetex 2.6 μm C18 (4.6 mm φ × 100 mm, manufactured by Phenomenex)

[0550] Mobile phase: Liquid A; water with 0.05% trifluoroacetic acid added

[0551] Solution B: Acetonitrile with 0.05% trifluoroacetic acid

[0552] Elution conditions: Gradient B concentration: 10% - 30 minutes - 100% (10 minutes hold)

[0553] Mobile phase flow rate: 1.0 mL / min

[0554] Column temperature: 40°C

[0555] Detector: UV detector (wavelength: 254nm)

[0556] Sample injection volume: 5μL

[0557] The ratio of the component derived from the photopolymerization initiator was calculated according to the following formula.

[0558] Content of initiator component in adhesive [%]

[0559] = (amount per unit volume of the component derived from the photopolymerization initiator of the adhesive layer in the test solution [mg / mL]) ÷ (amount of powder when preparing the test solution [mg]) × (amount of solvent used when preparing the test solution [mL]) ÷ (thickness of the adhesive layer [μm]) × (thickness of the entire laminate after peeling off the first and second substrate layers [μm]) × 100

[0560] [Scratch resistance test]

[0561] For a laminate with an optical film (equivalent to Figure 2 The first liquid crystal phase difference layer side surface of the optical laminate (after the first substrate layer is peeled off) was subjected to a test by applying steel wool #0000 with a load of 250 g / cm 2The scratch resistance test was repeated 10 times. The haze of the laminate with the optical film was then measured according to JIS K 7136. The change in haze before and after the scratch resistance test was calculated (ΔHz [%] = (haze after the scratch resistance test) - (haze before the scratch resistance test)). Evaluation was performed according to the following criteria. The results are shown in Tables 1 to 3.

[0562] A: ΔHz is less than 2%.

[0563] B: ΔHz is 2% or more and less than 4%.

[0564] C: ΔHz is 4% or more.

[0565] [Evaluation of heat wrinkles]

[0566] The optical film-coated laminate was cut into a size of 0.5 m (total width in the TD direction) x 0.5 m (in the MD direction) and placed on an inspection table. The MD direction corresponds to the absorption axis of the polarizer, and the TD direction is perpendicular to the MD direction. A fluorescent lamp emitting three wavelengths of light was placed above the inspection table, parallel to the TD direction. The galvanized iron-like irregularities in the MD direction of the optical film laminate were observed from a distance of 50 cm and evaluated according to the following criteria. The results are shown in Tables 1 to 3.

[0567] A: No unevenness was observed.

[0568] B: Concavities and convexities are slightly observed.

[0569] C: Concavities and convexities can be seen.

[0570] [Evaluation of Adhesion]

[0571] The exposed surface of the optical laminate after peeling off the first substrate layer is bonded to the glass via an adhesive layer. Next, 100 (10×10) 1 mm square grids are cut from the polarizing plate side so as to penetrate the optical laminate on the glass (the optical laminate with the first substrate layer peeled off) to form a measurement sample (2). Under the conditions of a temperature of 23°C and a relative humidity of 55%, an adhesive tape with a width of 24 mm (cellophane adhesive tape CT405AP-24, manufactured by Nichiban) is attached so as to cover the entire 100 grids formed on the measurement sample (2), and then the adhesive tape is peeled off in a direction of 45° relative to the grid surface. The number of grids remaining on the glass of the measurement sample (2) is counted and evaluated according to the following criteria. The results are shown in Tables 1 to 3.

[0572] A: The number of remaining cross cuts is 80 or more and 100 or less.

[0573] B: The number of remaining cross cuts is 50 or more and less than 80.

[0574] C: The number of remaining cross cuts is 0 or more and less than 50.

[0575] [Table 1]

[0576]

[0577] [Table 2]

[0578]

[0579] [Table 3]

[0580]

[0581] Description of Reference Numerals

[0582] 1 to 3: optical laminate, 11: first liquid crystal phase difference layer, 13: first liquid crystal phase difference layer with substrate, 16: first substrate layer, 20: optical film, 21: second liquid crystal phase difference layer (optical film), 23: second liquid crystal phase difference layer with substrate (optical film), 26: second substrate layer, 31: first adhesive layer (adhesive layer), 32: second adhesive layer, 50: polarizing plate (optical film).

Claims

1. An optical laminate comprising a bonding adhesive layer and a first liquid crystal retardation layer with a substrate, The adhesive layer is a cured layer of a photocurable adhesive composition. The first liquid crystal retardation layer with a substrate includes a first liquid crystal retardation layer and a first substrate layer in order from the adhesive layer side. The first liquid crystal retardation layer includes a first polymer layer containing a polymer of a polymerizable liquid crystal compound. The first substrate layer is releasable relative to the first liquid crystal retardation layer. The first liquid crystal retardation layer with a substrate has a light transmittance Tx of 20% or more at a wavelength of 317 nm.

2. The optical layered body according to claim 1, wherein: The light transmittance Ts of the first substrate layer at a wavelength of 317 nm is 20% or more.

3. The optical layered body according to claim 1 or 2, wherein: The first substrate layer is a film substrate, The resin constituting the film substrate is triacetyl cellulose.

4. The optical layered body according to claim 1 or 2, wherein: The first substrate layer has a thickness of 40 μm or less.

5. The optical layered body according to claim 1 or 2, wherein: The first liquid crystal retardation layer has positive wavelength dispersion.

6. The optical layered body according to claim 1 or 2, wherein: The first liquid crystal retardation layer is the first polymer layer.

7. The optical layered body according to claim 1 or 2, wherein: The adhesive composition comprises a photopolymerization initiator, The remaining amount of the photopolymerization initiator in the tackiness adhesive layer is 0.050 mass % or less.

8. The optical layered body according to claim 1 or 2, wherein: The thickness of the adhesive layer is 2 μm or more.

9. The optical layered body according to claim 1 or 2, wherein: The adhesive composition comprises a photopolymerization initiator, The photopolymerization initiator has a maximum absorption wavelength within a wavelength range of 280 nm to 340 nm. 10 . The optical laminate according to claim 1 , further comprising an optical film on the side of the tackiness adhesive layer opposite to the first liquid crystal retardation layer side.

11. The optical layered body according to claim 10, wherein: The optical film includes at least one of a polarizing plate including a polarizing element and a second liquid crystal retardation layer. The second liquid crystal retardation layer includes a second polymer layer containing a polymer of a polymerizable liquid crystal compound.

12. The optical layered body according to claim 10, wherein: The light transmittance Ty of the optical film is the same as or smaller than the light transmittance Tx of the first liquid crystal retardation layer with a substrate.

13. A method for producing an optical laminate, which is the method for producing an optical laminate according to claim 1 or 2, the method comprising: Step S1, forming a coating layer of the adhesive composition on the first liquid crystal retardation layer side of the first liquid crystal retardation layer with a substrate; as well as In step S2, the coating layer formed in the step S1 is irradiated with light via the first liquid crystal retardation layer with a substrate, thereby forming the adhesive layer.

14. The method for producing an optical layered body according to claim 13, wherein: The light is ultraviolet light, The cumulative amount of light irradiated to the coating layer in step S2 is 10 mJ / cm 2 Above and 1000mJ / cm 2 the following.