Positive electrode material composition, secondary battery and electric device
By using a combination of phosphates and ternary cathode materials in lithium-ion batteries, single crystal structure and doping elements are used to improve the high-temperature storage performance and cycle stability of the battery, solving the problem of high-temperature storage performance of existing lithium-ion batteries. Solve the problem of insufficient energy and achieve higher energy density and longer service life.
Patent Information
- Application Number
- CN202410888120.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-07
AI Technical Summary
Existing lithium-ion batteries have insufficient storage performance at high temperatures. In particular, the cycle stability and energy density of the cathode material composition do not perform well at high temperatures, and are limited by the cycle stability of the ternary cathode material.
A combination of a phosphate cathode material and a ternary cathode material is used. The phosphate material is single crystal or has a single crystal core, and the ternary material is single crystal or has a single crystal core. By adjusting the particle size distribution and doping of the material, The selection of heterogeneous elements improves the structural stability and high-temperature storage performance of the material.
It significantly improves the high-temperature storage performance and cycle stability of lithium-ion batteries, increases the energy density and charging capacity of the battery, and extends the service life of the battery.
Smart Images

Figure CN118738338A_ABST
Abstract
Description
[0001] This application is a divisional application based on patent application 202380009727.3 filed on March 7, 2023 and entitled “A positive electrode material composition, secondary battery and electrical device”. Technical Field
[0002] The present application relates to the field of battery technology, and in particular to a positive electrode material composition, a secondary battery and an electrical device. Background Art
[0003] Lithium-ion battery is a secondary battery (rechargeable battery) that mainly relies on the movement of lithium ions between the positive electrode and the negative electrode to work. During the charging and discharging process, Li ions are intercalated and deintercalated between the two electrodes: when charging, Li ions are deintercalated from the positive electrode and intercalated into the negative electrode through the electrolyte, and the negative electrode is in a lithium-rich state; the opposite is true during discharge.
[0004] At present, there are many methods to improve the cycle performance of lithium-ion batteries, such as doping or coating the positive electrode materials to slow down the deterioration of the crystal structure of the positive electrode materials during the cycle; or combining positive electrode materials with different advantages to improve the cycle performance and energy density of the battery. For example, lithium iron phosphate positive electrode materials and ternary positive electrode materials are combined. However, usually the combination of the two still takes the ternary positive electrode material as the main body. Due to the limitation of the cycle stability of the ternary positive electrode material, the cycle stability of the combination is not improved enough, especially the high-temperature storage performance is not good enough. Summary of the invention
[0005] The present application provides a positive electrode material composition, a secondary battery and an electrical device to improve the high-temperature storage performance of the battery.
[0006] According to the first aspect of the present application, a positive electrode material composition is provided, including a phosphate positive electrode material and a ternary positive electrode material, the weight of the phosphate positive electrode material is denoted as W1, the weight of the ternary positive electrode material is denoted as W2, α=W1 / (W1+W2), 3%≤α≤50%, the phosphate positive electrode material is a single crystal material or has a single crystal core, and the ternary positive electrode material is a single crystal or has a single crystal core.
[0007] Although phosphate cathode materials have low energy density, their material structure has the strong stability of phosphate polyanion materials, good cycle stability, and lifespan advantages; ternary cathode materials have high energy density, but layered transition metal oxides face material losses such as phase change / Li-Ni mixing / oxygen release and structural collapse during the cycle, resulting in a worse lifespan of ternary cathode materials than phosphate cathode materials. The phosphate cathode materials of this application are single crystal materials or have a single crystal core, and the ternary cathode materials are single crystals or have a single crystal core, which further improves the cycle performance of the cathode materials; and the single crystal has a small BET specific surface area, a stable structure, a large compaction density, and better high-temperature storage performance.
[0008] In any embodiment of the first aspect, the particle size distribution of the positive electrode material composition satisfies the following relationship: 8>Aα+B(1-α)>1, wherein A is D of the phosphate positive electrode material. V 50, B is D of ternary cathode material V 50. Further improve the particle size matching effect between phosphate cathode materials and ternary cathode materials, thereby significantly improving high-temperature storage performance.
[0009] In any embodiment of the first aspect, D of the phosphate positive electrode material V 50 is 0.8~8μm, and DV 90 <30μm, so as to improve the processing feasibility and high temperature stability of the positive electrode material composition.
[0010] In a first embodiment of the first aspect, the BET specific surface area of the phosphate positive electrode material is 8 to 20 m 2 / g, which can further improve the structural stability, compaction density and high-temperature storage performance of the positive electrode material composition.
[0011] In a first embodiment of the first aspect, the chemical formula of the phosphate positive electrode material is Li 1+x Mn 1- y A y P 1-z R z O 4, in the chemical formula, x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, and the values of x, y and z satisfy the following conditions: the chemical formula is kept electrically neutral; A includes one or more elements in the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, optionally A includes one or more elements in the group consisting of Fe, Ti, V, Ni, Co and Mg, R includes one or more elements in the group consisting of B, Si, N, S, F, Cl and Br, optionally, R includes an element in the group consisting of B, Si, N and S. Doping element A and element R in phosphates helps to improve the structural stability of phosphate positive electrode materials and the rate performance of secondary batteries having them.
[0012] In a second embodiment of the first aspect, the chemical formula of the phosphate positive electrode material is Li a A x Mn 1- y B y P 1-z C z O 4-n D n , wherein A includes one or more elements in the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W, B includes one or more elements in the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, C includes one or more elements in the group consisting of B (boron), S, Si and N, D includes one or more elements in the group consisting of S, F, Cl and Br, a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, n is selected from the range of 0.001 to 0.1, and the phosphate positive electrode material is electrically neutral. By doping the above-mentioned specific elements at the above four positions at the same time with specific amounts, the rate performance, cycle performance and / or high temperature stability of the phosphate positive electrode material can be significantly improved.
[0013] In any embodiment of the first aspect, the phosphate cathode material optionally includes a single crystal core and a coating layer covering the single crystal core, wherein the single crystal core has a chemical formula of Li 1+x Mn 1-y A y P 1-z R z O 4 or chemical formula Li a A x Mn 1-yB y P 1-z C z O 4-n D n The coating layer may be one or more layers of pyrophosphate, phosphate, or carbon. The functional coating layer can effectively inhibit the dissolution of transition metals and reduce the surface side reactions of phosphate cathode materials.
[0014] In any embodiment of the first aspect, D of the ternary positive electrode material V 50 is 2~8μm, and D V 99≤18μm. The particle size affects the gram capacity after mixing and controls the D V 50 and D V 99, which helps to shorten the lithium ion diffusion path and bulk diffusion impedance, reduce the polarization of the material, and has a more significant effect on improving the capacity after mixing.
[0015] In any embodiment of the first aspect, the BET specific surface area of the ternary positive electrode material is 0.42 to 1.5 m 2 / g. It can further improve the structural stability, compaction density and high-temperature storage performance of the positive electrode material.
[0016] In any embodiment of the first aspect, the ternary positive electrode material is a single crystal NCM ternary positive electrode material or a single crystal NCA ternary positive electrode material. Optionally, the Ni molar content in the ternary positive electrode material is 50% to 99.5%, and the Co molar content is 0.5% to 49.5%; further optionally, the Ni molar content is 60% to 88%, and the Co molar content is 5% to 35%. The Ni molar content affects the capacity of the ternary positive electrode material and has a great influence on the energy density improvement of the blended material. The Co molar content improves the electronic conductivity and ionic conductivity of the system, which can effectively improve the charging capacity of the ternary positive electrode material.
[0017] In any embodiment of the first aspect, the above-mentioned ternary cathode material has a chemical formula Li a’ Ni b’ Co c’ M1 d’ M2 e’ O f’ R′ g’, wherein, 0.75 ≤ a' ≤ 1.2, 0 < b' < 1, 0 < c' < 1, 0 < d' < 1, 0 ≤ e' ≤ 0.2, 1 ≤ f' ≤ 2.5, 0 ≤ g' ≤ 1, f' + g' ≤ 3, M1 is Mn element and / or Al element, M2 is one or more elements selected from Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R' is one or more elements selected from N, F, S, Cl. Element doping is used to improve the cycle performance and rate performance of the ternary cathode material.
[0018] According to the second aspect of the present application, a secondary battery is provided. The secondary battery includes a positive electrode sheet, and the positive electrode sheet includes a positive electrode active material, which is any one of the positive electrode material compositions in the first aspect above. The secondary battery with the positive electrode material composition of the present application effectively improves the high-temperature storage performance on the basis of having high energy density and cycle performance.
[0019] According to the third aspect of the present application, an electrical device is provided, including a secondary battery, and the secondary battery is selected from the secondary batteries in the second aspect. The electrical device has better working stability at high temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required to be used in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained according to the drawings without creative efforts.
[0021] Figure 1 It is a schematic diagram of a secondary battery according to an embodiment of the present application.
[0022] Figure 2 is Figure 1 The exploded view of the secondary battery according to an embodiment of the present application shown.
[0023] Figure 3 It is a schematic diagram of a battery module according to an embodiment of the present application.
[0024] Figure 4 It is a schematic diagram of a battery pack according to an embodiment of the present application.
[0025] Figure 5 is Figure 4 The exploded view of the battery pack according to an embodiment of the present application shown.
[0026] Figure 6 It is a schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source.
[0027] In the drawings, the drawings are not drawn to scale.
[0028] Description of reference numerals:
[0029] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION
[0030] The following detailed description and drawings of the embodiments of the present application are used to illustrate the principles of the present application, but cannot be used to limit the scope of the present application, that is, the present application is not limited to the described embodiments.
[0031] Hereinafter, the embodiments of the positive electrode material composition, secondary battery and electric device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0032] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0033] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0034] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0035] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0036] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0037] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0038] [Secondary battery]
[0039] Secondary batteries, also known as rechargeable batteries or storage batteries, refer to batteries that can continue to be used by recharging the active materials after the battery is discharged.
[0040] Normally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions (such as lithium ions) are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte is between the positive electrode sheet and the negative electrode sheet, mainly to conduct active ions.
[0041] [Cathode material]
[0042] One embodiment of the present application provides a positive electrode material composition, including a phosphate positive electrode material and a ternary positive electrode material, the weight of the phosphate positive electrode material is denoted as W1, the weight of the ternary positive electrode material is denoted as W2, α=W1 / (W1+W2), 3%≤α≤50%, the phosphate positive electrode material is a single crystal material or has a single crystal core, and the ternary positive electrode material is a single crystal or has a single crystal core.
[0043] Although phosphate cathode materials have low energy density, their material structure has the strong stability of phosphate polyanion materials, good cycle stability, and lifespan advantages; ternary cathode materials have high energy density, but layered transition metal oxides face material losses such as phase change / Li-Ni mixing / oxygen release and structural collapse during the cycle, resulting in a worse lifespan of ternary cathode materials than phosphate cathode materials. The phosphate cathode materials of this application are single crystal materials or have a single crystal core, and the ternary cathode materials are single crystals or have a single crystal core, which further improves the cycle performance of the cathode materials; and the single crystal has a small BET specific surface area, a stable structure, a large compaction density, and better high-temperature storage performance.
[0044] As α increases within the above range, the cycle ability of the positive electrode material composition is enhanced.
[0045] Terminology Note:
[0046] Phosphate cathode materials: not only LiMnPO 4 , and also includes lithium iron manganese phosphate (LiMn x Fe 1-x PO 4 ) series of positive electrode materials, lithium aluminum manganese phosphate (LiMn x Al 1-x PO 4 ) series of positive electrode materials, such as LiMn x Fe 1-x PO 4 , doped LiMn x Fe 1-x PO 4 , LiMn with coating layer x Fe 1-x PO 4 .
[0047] Polycrystalline: refers to the positive electrode material existing in the form of agglomerates;
[0048] Single crystal: There is no primary particle agglomeration, and its particle size is generally 10-50 times larger than the primary particle size of agglomerated materials (polycrystalline), with high internal crystallinity and no excess pores.
[0049] When the positive electrode material composition exists in the positive electrode plate, the positive electrode plate is cut by argon ion polishing, and the element analysis is performed on the planed surface. Then, the main element ratios of the phosphate positive electrode material and the ternary material are compared respectively, and then the corresponding weights are calculated through the ratios.
[0050] In some embodiments, the particle size distribution of the positive electrode material composition satisfies the following relationship: 8>Aα+B(1-α)>1, wherein A is the DV of the phosphate positive electrode material. 50 , B is the DV of the ternary cathode material 50 . Further improve the particle size matching effect between phosphate cathode materials and ternary cathode materials, thereby significantly improving high-temperature storage performance.
[0051] In some embodiments, D of the phosphate cathode material V 50 is 0.8 to 8 μm, such as 0.8 μm, 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm, and D V 90<30μm, so as to improve the processing feasibility and high temperature stability of the positive electrode material composition.
[0052] In some embodiments, the BET specific surface area of the phosphate cathode material is 8 to 20 m 2 / g, for example, 8m 2 / g, 10m 2 / g, 12m 2 / g, 15m 2 / g or 20m 2 / g, which can further improve the structural stability, compaction density and high-temperature storage performance of the positive electrode material composition.
[0053] In some embodiments, the chemical formula of the phosphate cathode material is Li 1+x Mn 1-y A y P 1-z R z O 4, in the chemical formula, x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, z is any value in the range of 0.001-0.100, and the values of x, y and z satisfy the following conditions: the chemical formula is electrically neutral; A includes one or more elements in the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be one or more elements in the group consisting of Fe, Ti, V, Ni, Co and Mg, and R is one or more elements selected from the group consisting of B, Si, N, S, F, Cl and Br, and optionally, R is an element selected from the group consisting of B, Si, N and S. The element A doped in the manganese position of lithium manganese iron phosphate helps to reduce the lattice change rate of lithium manganese iron phosphate during lithium insertion and extraction, improves the structural stability of lithium manganese iron phosphate positive electrode materials, greatly reduces the dissolution of manganese and reduces the oxygen activity of the particle surface. The element R doped at the phosphorus position helps to change the difficulty of the Mn-O bond length change, thereby reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the rate performance of the secondary battery.
[0054] In some embodiments, the chemical formula of the phosphate cathode material is Li a A x Mn 1-y B y P 1-z C z O 4-n D n, wherein A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W, B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, C includes one or more elements selected from the group consisting of B (boron), S, Si and N, D includes one or more elements selected from the group consisting of S, F, Cl and Br, a is selected from the range of 0.9 to 1.1, for example, 0.97, 0.977, 0.984, 0.988, 0.99, 0.991, 0.992, 0.993, 0.994, 0.995, 0.996, 0.997, 0.998, 1.01, and x is selected from the range of 0.001 to 0.1 , for example, 0.001, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, y is selected from the range of 0.001 to 0.5, for example, 0.001, 0.005, 0.02, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.34, 0.345, 0.349, 0.35, 0.4, 0.5, z is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, n is selected from the range of 0.001 to 0.1, for example, 0.001, 0.005, 0.08, 0.1, and the phosphate positive electrode material is electrically neutral. A, B, C and D are respectively 4 The Li, Mn, P and O doped elements are added to the phosphates. Without wishing to be bound by theory, it is now believed that the performance improvement of phosphates is related to reducing the lattice change rate of phosphates during lithium insertion and extraction and reducing surface activity. Reducing the lattice change rate can reduce the lattice constant difference between the two phases at the grain boundary, reduce interfacial stress, and enhance Li + The transmission capacity at the interface improves the rate performance of the positive electrode active material. However, high surface activity can easily lead to serious side reactions at the interface, aggravating gas production, electrolyte consumption and interface damage, thereby affecting the battery's cycle performance. The above-mentioned phosphate positive electrode material reduces the lattice change rate by doping at the Li and Mn positions. Mn doping also effectively reduces the surface activity, thereby inhibiting Mn dissolution and side reactions at the interface between the positive electrode active material and the electrolyte. P-site doping makes the change rate of the Mn-O bond length faster, reduces the migration barrier of the small polaron of the material, and is beneficial to electronic conductivity. O-site doping has a good effect on reducing side reactions at the interface. P-site and O-site doping also affect the Mn dissolution and kinetic properties of anti-site defects. Therefore, doping reduces the concentration of anti-site defects in the material, improves the kinetic properties and gram capacity of the material, and can also change the morphology of the particles, thereby improving the compaction density. The applicant unexpectedly discovered that by in the compound LiMnPO 4By doping the Li, Mn, P and O positions with specific elements in specific amounts at the same time, significantly improved rate performance can be obtained, while the dissolution of Mn and the doping elements at the Mn position is significantly reduced, significantly improved cycle performance and / or high temperature stability are obtained, and the gram capacity and compaction density of the material can also be improved.
[0055] In some embodiments, the phosphate-based cathode material optionally includes a single crystal core and a functional coating layer covering the single crystal core, wherein the single crystal core has a chemical formula of Li 1+x Mn 1-y A y P 1-z R z O 4 The functional coating layer can be one or more layers of pyrophosphate, phosphate, and carbon. Since the migration barrier of transition metals in pyrophosphate is relatively high (>1eV), the dissolution of transition metals can be effectively inhibited. Phosphates have excellent lithium ion conductivity and can reduce the surface impurity lithium content. The carbon layer can effectively improve the LiMnPO 4 It not only has good conductivity and desolvation ability, but also acts as a "barrier" to further hinder the migration of manganese ions into the electrolyte and reduce the corrosion of the electrolyte to the active materials; at the same time, the above-mentioned carbon layer in the mixture can also optimize the conductive network around the ternary positive electrode material and improve the mixing uniformity of the phosphate positive electrode material and the ternary positive electrode material.
[0056] In some embodiments, D of the above ternary cathode material V 50 is 2~8μm, and D V 99≤18μm. The particle size affects the gram capacity after mixing and controls the D V 50 and D V 99, which helps to shorten the lithium ion diffusion path and bulk diffusion impedance, reduce the polarization of the material, and has a more significant effect on improving the capacity after mixing.
[0057] In some embodiments, the BET specific surface area of the ternary cathode material is 0.42 to 1.5 m 2 / g. The structural stability, compaction density and high-temperature storage performance of the positive electrode material composition can be further improved.
[0058] In some embodiments, the ternary cathode material is a single-crystal NCM ternary cathode material or a single-crystal NCA ternary cathode material. Optionally, the molar content of Ni in the ternary cathode material is 50% to 99.5%, such as 50%, 55%, 60%, 70%, 80%, 88%, 90%, 95% or 99.5%, and the molar content of Co is 0.5% to 49.5%, such as 0.5%, 5%, 10%, 20%, 30%, 35%, 40%, 45% or 50%. Further optionally, the molar content of Ni is 60% to 88%, and the molar content of Co is 5% to 35%. The molar content of Ni affects the capacity performance of the ternary cathode material and has a great impact on improving the energy density of the blended material. Increasing the molar content of Co can improve the electronic conductivity and ionic conductivity of the system, and can effectively improve the charging ability of the ternary cathode material.
[0059] In some embodiments, the ternary cathode material has the chemical formula Li a’ Ni b’ Co c’ M1 d’ M2 e’ O f’ R′ g’ , where 0.75 ≤ a’ ≤ 1.2, 0 < b’ < 1, 0 < c’ < 1, 0 < d’ < 1, 0 ≤ e’ ≤ 0.2, 1 ≤ f’ ≤ 2.5, 0 ≤ g’ ≤ 1, f’ + g’ ≤ 3, M1 is Mn element and / or Al element, M2 is one or more elements selected from Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R′ is one or more elements selected from N, F, S, Cl. Element doping is used to improve the cycle performance and rate performance of the ternary cathode material.
[0060] Both the above-mentioned phosphate cathode material and ternary cathode material of the present application can be commercial materials or can be prepared, such as a series of single-crystal lithium iron manganese phosphate cathode materials produced by Shenzhen Defang Nano-tech Co., Ltd. (referred to as Defang Nano in the examples); a series of single-crystal ternary cathode materials produced by Ningbo Ronbay New Energy Technology Co., Ltd. (referred to as Ronbay in the examples).
[0061] [Positive electrode plate]
[0062] The positive electrode plate generally includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, and the positive electrode film layer includes a positive electrode active material.
[0063] As an example, the positive electrode current collector has two surfaces opposite to each other in its own thickness direction, and the positive electrode film layer is provided on any one or both of the two opposite surfaces of the positive electrode current collector.
[0064] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0065] In some embodiments, the positive electrode active material adopts any positive electrode material composition provided in this application.
[0066] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0067] In some embodiments, the positive electrode film layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0068] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0069] [Negative electrode]
[0070] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0071] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0072] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0073] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0074] In some embodiments, the negative electrode film layer may further include a binder. As an example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0075] In some embodiments, the negative electrode film layer may further include a conductive agent. As an example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0076] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0077] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0078] [Electrolytes]
[0079] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0080] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.
[0081] In some embodiments, the electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0082] In some embodiments, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0083] In some embodiments, the electrolyte may further include additives. As examples, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0084] [Isolation film]
[0085] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0086] In some embodiments, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0087] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0088] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0089] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0090] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.
[0091] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0092] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0093] Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.
[0094] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0095] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0096] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0097] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0098] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0099] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.
[0100] [Example]
[0101] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be obtained commercially.
[0102] Sources of positive electrode materials, including phosphate positive electrode materials LiMn 0.6 Fe 0.4 PO 4 The cathode materials were purchased from Defang Nano and Rongbai Technology, and the remaining cathode materials were prepared using the following method.
[0103] Preparation Example 1: Li 0.999 Mn 0.60 Fe 0.393 V 0.004 Co 0.003 P 0.999 S 0.001 O 4 Preparation
[0104] (1) Preparation of co-doped lithium manganese iron phosphate core
[0105] Preparation of Fe, Co and V co-doped manganese oxalate: 689.5 g manganese carbonate (MnCO 3 455.2 g ferrous carbonate (as FeCO 3 4.6 g cobalt sulfate (in terms of CoSO 4 4.9 g vanadium dichloride (in VCl 2 The mixture was transferred to a reactor and 5 liters of deionized water and 1260.6 g of oxalic acid dihydrate (in C 2 H 2 O 4 .2H 2 O, the same below). The reactor was heated to 80°C and stirred at a speed of 600 rpm for 6 hours until the reaction was terminated (no bubbles were generated), to obtain a manganese oxalate suspension co-doped with Fe, Co, V and S. The suspension was then filtered, the filter cake was dried at 120°C, and then ground with an air mill, ground, classified, and passed through a 325-mesh sieve to obtain Fe, Co and V co-doped manganese oxalate dihydrate particles.
[0106] Preparation of Fe, Co, V and S co-doped lithium manganese iron phosphate: dihydrate manganese oxalate particles (1793.4 g) obtained in the previous step, 369.0 g lithium carbonate (Li 2 CO 3 1.6 g of 60% dilute sulfuric acid (60% H 2 SO 4 1148.9 g ammonium dihydrogen phosphate (NH 4 H 2 PO 4 The slurry was transferred to a spray drying device for spray drying and granulation, and the drying temperature was set to 250° C. and dried for 4 hours to obtain a powder. In a nitrogen (90 volume %) + hydrogen (10 volume %) protective atmosphere, the powder was sintered at 700° C. for 4 hours to obtain 1572.1 g of Fe, Co, V and S co-doped lithium manganese iron phosphate.
[0107] Preparation Example 2: Li 0.994 Mo 0.001 Mn 0.65 Fe 0.35 P 0.999 Si 0.001 O 3.999 F 0.001 Preparation
[0108] 1) Preparation of positive electrode active materials
[0109] Preparation of doped manganese oxalate: 1.3 mol of MnSO 4 ﹒ H 2 O, 0.7 mol FeSO 4 ﹒ H 2 O is fully mixed in a mixer for 6 hours. The mixture is transferred to a reactor, and 10L of deionized water and 2mol of dihydrated oxalic acid (in terms of oxalic acid) are added. The reactor is heated to 80°C and stirred at a speed of 600rpm for 6 hours. The reaction is terminated (no bubbles are generated) to obtain an Fe-doped manganese oxalate suspension. The suspension is then filtered, and the filter cake is dried at 120°C, then ground, graded, and sieved through a 325-mesh sieve, and ground to the target particle size as required to obtain Fe-doped manganese oxalate particles.
[0110] Preparation of doped lithium manganese iron phosphate: 1 mol of the above manganese oxalate particles, 0.497 mol of lithium carbonate, 0.001 mol of Mo(SO 4 ) 3 , an aqueous solution of 85% phosphoric acid containing 0.999 mol of phosphoric acid, 0.001 mol of H 4 SiO 4 , 0.0005 mol NH 4 HF 2 and 0.005 mol sucrose were added to 20 L of deionized water. The mixture was transferred to a sand mill and fully ground and stirred for 10 hours to obtain a slurry. The slurry was transferred to a spray drying device for spray drying and granulation, and the drying temperature was set to 250°C and dried for 4 hours to obtain particles. In a nitrogen (90 volume %) + hydrogen (10 volume %) protective atmosphere, the above powder was sintered at 700°C for 10 hours to obtain carbon-coated Li 0.994 Mo 0.001 Mn 0.65 Fe 0.35 P 0.999 Si 0.001 O 3.999 F 0.001 .
[0111] The volume particle size distribution and specific surface area of the obtained materials were adjusted by adjusting the heating temperature of the reactor, the mesh size of the sieve and the sintering temperature of the above-mentioned Preparation Examples 1 and 2, and this application will no longer describe the preparation process of each material one by one.
[0112] The appearance of the positive electrode material was observed by scanning electron microscopy to determine that the lithium manganese iron phosphate positive electrode material and the ternary positive electrode material in each embodiment were single crystal particles (a single crystal particle is a complete crystal sphere, while a polycrystalline particle is a large sphere formed by the aggregation of multiple small primary particles).
[0113] The particle size of the lithium manganese iron phosphate positive electrode material and the ternary positive electrode material in each embodiment is determined by powder laser particle size test: refer to the national standard GB / T19077-2016, wherein deionized water is used as the solvent, and ultrasound is used for 5 minutes before the test.
[0114] Powder specific surface area (BET) test: The test refers to GB / T 19587-2004. Before the test, the powder is placed in a vacuum oven at 200°C and dried for ≥2h. The required amount of powder is weighed>20g.
[0115] Powder primary particle size test: Confirm the primary particle size by testing the powder by SEM.
[0116] Gram capacity test: The button cells prepared above were placed at a constant temperature of 25°C for 5 minutes, discharged to 2.5V at 0.1C, and after standing for 5 minutes, charged to 4.3V or 4.25V (Ni content > 70%, upper limit voltage is 4.25V) at 0.1C cross-current constant voltage, and then charged at 4.3V or 4.25V at a constant voltage to a current ≤0.05mA, and stood for 5 minutes. The charging capacity at this time is recorded as C0, and then discharged to 2.5V at 0.1C. The discharge capacity at this time is the initial discharge capacity, recorded as D0.
[0117] The gram capacity of the positive electrode active material is obtained by dividing the tested discharge capacity value (ie, the initial discharge capacity D0) by the mass of the positive electrode active material in the button cell.
[0118] The gram capacity, D V 50. D V 90. The BET specific surface area is recorded in Table 1.
[0119] Table 1
[0120]
[0121]
[0122] Among them, NCM-18 is a secondary particle, and the rest are single crystal particles.
[0123] The compositions of the positive electrode material compositions of the embodiments and comparative examples are shown in Table 2 (wherein the proportion of LMFP is the mass proportion of LMFP and NCM).
[0124] Table 2
[0125]
[0126]
[0127]
[0128] The electrical performance was tested in the following manner.
[0129] (1) Preparation of mixed electrode stack batteries:
[0130] Preparation of mixed positive electrode: The positive electrode active composition in the above embodiments and comparative examples is used as the positive electrode active material (the mixing ratio is based on the mass ratio of the two, mA+mB=100%), polyvinylidene fluoride (PVDF), and conductive carbon are added to a certain amount of N-methylpyrrolidone (NMP), and the mass ratio of active material: PVDF: conductive carbon is 90:5:5, and stirred in a drying room to form a uniform slurry, and the viscosity is controlled to be 3000-10000mPa·S, and the above slurry is coated on aluminum foil, and dried and cold pressed to form a positive electrode sheet;
[0131] Preparation of graphite negative electrode: artificial graphite is used as the negative electrode active material, sodium carboxymethyl cellulose (CMC), conductive carbon and styrene-butadiene rubber (SBR) in a mass ratio of 94:1.5:2:2.5, a certain amount of deionized water is added, and the mixture is stirred in a drying room to form a uniform slurry, and the viscosity is controlled to be 2000-12000 mPa·S. The slurry is coated on a copper foil, and the negative electrode coating mass refers to the matching relationship with the positive electrode (94%*negative electrode coating mass*graphite gram capacity=1.15*90%*positive electrode coating mass*mixed positive electrode gram capacity, where the gram capacity refers to the gram capacity information of the material for the third cycle of the powder cycle of the lithium half-battery), and the negative electrode sheet is made after drying and cold pressing;
[0132] The electrolyte used was 1 mol / L LiPF6 / (ethylene carbonate (EC) + diethyl carbonate (DEC) + dimethyl carbonate (DMC)) (volume ratio 1:1:1) + 5 wt.% fluoroethylene carbonate (FEC);
[0133] A porous polymer film made of polyethylene (PE) is used as the isolation membrane.
[0134] In the drying room, the battery is assembled into stacked cells for testing through processes such as pole punching / cleaning pole ears / stacking / welding / top sealing / liquid injection / pre-forming / vacuuming / forming / molding.
[0135] (2) Initial gram capacity test of laminated battery:
[0136] The laminated batteries prepared as above were placed in a constant temperature environment of 25°C for 5 minutes, discharged to 2.5V at 1 / 3C, and after standing for 5 minutes, charged to 4.3V or 4.25V (Ni content>70%, upper limit voltage is 4.25V) at 1 / 3C cross-current constant voltage, and then charged at 4.3V or 4.25V at constant voltage to a current ≤0.05mA, and stood for 5 minutes. The charging capacity at this time was recorded as C0, and then discharged to 2.5V at 1 / 3C0. The discharge capacity at this time was the initial discharge capacity, recorded as D0.
[0137] The tested discharge capacity value (ie, the initial discharge capacity D0) is divided by the mass of the positive electrode active material in the secondary battery to obtain the full-electric initial gram capacity of the positive electrode active material.
[0138] (3) Cycling performance test of secondary battery at 25℃:
[0139] Each of the secondary batteries prepared above was charged to 4.3V or 4.25V at 0.5C0 at 2.5-4.3V or 4.25V under a constant temperature environment of 25°C, then charged at a constant voltage at 4.3V or 4.25V to a current ≤0.05mA, left to stand for 5min, and then discharged to 2.5V at 0.5C, and the capacity was recorded as Dn (n=1, 2, 3...), and the above operation was repeated for more than 5000 cycles to determine the capacity fading value. The capacity fading was calculated as the cell fading degree (State of health SOH) according to the ratio of Dn / D3, and the number of cycles of each cell when the cell was attenuated to 80% SOH was compared as the examination index of the cycle capacity.
[0140] (4) Storage capacity
[0141] In a constant temperature environment of 60℃, the battery was charged from 2.5V to 4.25-4.3V at 0.5C, then charged at a constant voltage of 4.25-4.4V to a current of ≤0.05mA, discharged at 0.5C to 2.5V, and the discharge capacity D0 was recorded. Then, the battery was charged at a constant voltage of 4.25-4.4V to a current of ≤0.05mA, and the battery was left to stand for 480 days. During the standing period, three cycles were performed continuously every 10 days. Each cycle was first discharged at 0.5C to 2.5V and then charged at a constant voltage of 4.25-4.4V to a current of ≤0.05mA. The discharge capacity of the third cycle was recorded as Dn (n=1,2,3...), where n represents the nth 10 days of standing. The value of Dn divided by D0 was taken as the degree of cell attenuation at the nth 10 days of high-temperature storage, and the number of days of high-temperature storage when the cell attenuated to 80% was recorded.
[0142] (5) Charging capacity experiment:
[0143] First, perform a capacity test on the soft-pack laminated battery. The process is as follows: Constant current charge at 0.33C until the full charge voltage V1 is reached, then switch to constant voltage charging. When the charging current decreases to 0.05C, the constant voltage charging ends. Subsequently, discharge at 0.33C until the full discharge voltage V2. Repeat this process 3 times and take the capacity result of the 3rd time as the standard. At the same time, the specific capacity of the positive electrode can be calculated using the result of the 3rd time.
[0144] Perform charging tests on the soft-pack laminated battery at different rates (C1 < C2 < C3 < C4 < …… < Cn). During the test, the charging rate needs to increase from small to large, and the full battery voltage and the negative electrode voltage of the soft-pack laminated battery need to be monitored simultaneously during the charging process. The detailed process is as follows: Charge the soft-pack laminated battery at C1 until the full charge voltage V1 or the negative electrode voltage reaches 0V, extract the SOC value of the battery at the end of charging, and then discharge at 0.33C until the full discharge voltage V2. Repeating the above process can obtain the SOC values at the end of charging at different rates. Among them, Cn at 100% SOC charging is the charging capacity of the battery cell in this solution.
[0145] The test results are recorded in Table 3.
[0146] Table 3
[0147]
[0148]
[0149] From the data comparison of Examples 1 - 4, it can be seen that too high or too low a proportion of the phosphate-based cathode material will cause deterioration of the storage life. At the same time, an increase in the proportion of the phosphate-based cathode material can increase the cycle life but will deteriorate the charging capacity. From the comparison of Examples 5 to 8 and 14 to 16, it can be seen that an increase in D V 50 will deteriorate the charging capacity, but it can improve the cycle and storage. However, too large a D V 50 will also affect the performance. From the comparison of Examples 9 to 12, it can be seen that too small a BET of the phosphate-based cathode material deteriorates the cycle and charging capacity. From the data comparison of Examples 18 to 21, it can be seen that too small a BET of the ternary cathode material deteriorates the charging capacity, cycle, and storage performance. From the data comparison of Examples 22 to 29, it can be seen that too much Ni content will increase the specific capacity but will deteriorate the charging capacity, cycle, and storage, and too much Co content will improve the charging capacity and storage but will deteriorate the specific capacity and cycle performance.
[0150] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A positive electrode material composition, wherein: It includes phosphate positive electrode materials and ternary positive electrode materials, the weight of the phosphate positive electrode material is recorded as W1, the weight of the ternary positive electrode material is recorded as W2, α=W1 / (W1+W2), 3%≤α≤50%, the phosphate positive electrode material is a single crystal material or has a single crystal core, and the ternary positive electrode material is a single crystal or has a single crystal core.
2. The positive electrode material composition according to claim 1, wherein The particle size distribution of the positive electrode material composition satisfies the following relationship: 8>Aα+B(1-α)>1, wherein A is the D of the phosphate positive electrode material. V 50, B is D of the ternary positive electrode material V 50.
3. The positive electrode material composition according to claim 1 or 2, wherein: The D of the phosphate positive electrode material V 50 is 0.8μm~8μm, and D V 90<30μm.
4. The positive electrode material composition according to any one of claims 1 to 2, wherein The BET specific surface area of the phosphate positive electrode material is 8 m 2 / g~20m 2 / g.
5. The positive electrode material composition according to claim 1, wherein The chemical formula of the phosphate positive electrode material is Li 1+x Mn 1-y A y P 1-z R z O4, wherein x is any value in the range of -0.100-0.100, y is any value in the range of 0.001-0.500, and z is any value in the range of 0.001-0.100, and the values of x, y and z satisfy the following conditions: the chemical formula is electrically neutral; A includes one or more elements in the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and R includes one or more elements in the group consisting of B, Si, N, S, F, Cl and Br; Alternatively, the chemical formula of the phosphate cathode material is Li a A x Mn 1-y B y P 1-z C z O 4-n D n , wherein A includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W, B includes one or more elements selected from the group consisting of Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, C includes one or more elements selected from the group consisting of B, S, Si and N, D includes one or more elements selected from the group consisting of S, F, Cl and Br, a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, n is selected from the range of 0.001 to 0.1, and the phosphate positive electrode material is electrically neutral.
6. The positive electrode material composition according to claim 5, wherein The chemical formula of the phosphate positive electrode material is Li 1+x Mn 1-y A y P 1-z R z When O4, the A includes one or more elements selected from the group consisting of Fe, Ti, V, Ni, Co and Mg.
7. The cathode material composition according to claim 5, wherein: The R includes an element selected from the group consisting of B, Si, N, and S.
8. The cathode material composition according to claim 5, wherein The chemical formula of the phosphate positive electrode material is Li 1+x Mn 1-y A y P 1-z When RzO4, x in the chemical formula is -0.001 or -0.
006.
9. The cathode material composition according to claim 5, wherein: The chemical formula of the phosphate positive electrode material is Li a A x Mn 1-y B y P 1-z C z O 4-n D n When a in the chemical formula is 0.994 to 1.1, and / or; y is 0.35~0.
5.
10. The positive electrode material composition according to any one of claims 5 to 9, wherein The phosphate positive electrode material comprises a single crystal core and a coating layer covering the single crystal core, wherein the single crystal core has the chemical formula Li 1+x Mn 1-y A y P 1- z R z O4 or the chemical formula Li a A x Mn 1-y B y P 1-z C z O 4-n D n The coating layer may optionally be one or more layers of pyrophosphate, phosphate, or carbon.
11. The positive electrode material composition according to any one of claims 1 to 2, wherein The D of the ternary cathode material V 50 is 2μm~8μm, and D V 99≤18μm.
12. The positive electrode material composition according to any one of claims 1 to 2, wherein The BET specific surface area of the ternary positive electrode material is 0.42 m 2 / g~1.5m 2 / g.
13. The positive electrode material composition according to any one of claims 1 to 2, wherein The ternary positive electrode material is a single crystal NCM ternary positive electrode material or a single crystal NCA ternary positive electrode material.
14. The positive electrode material composition according to claim 13, wherein The molar content of Ni in the ternary positive electrode material is 50% to 99.5%, and the molar content of Co is 0.5% to 49.5%.
15. The positive electrode material composition according to claim 14, wherein: The molar content of Ni in the ternary positive electrode material is 60% to 88%, and the molar content of Co is 5% to 35%.
16. The positive electrode material composition according to any one of claims 1 to 2, wherein The ternary cathode material has the chemical formula Li a’ Ni b’ Co c’ M1 d’ M2 e’ O f’ R′ g’ , where 0.75 ≤ a’ ≤ 1.2, 0 < b’ < 1, 0 < c’ < 1, 0 < d’ < 1, 0 ≤ e’ ≤ 0.2, 1 ≤ f’ ≤ 2.5, 0 ≤ g’ ≤ 1, f’ + g’ ≤ 3, M1 is Mn element and / or Al element, M2 is one or more elements selected from Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R′ is one or more elements selected from N, F, S, Cl.
17. A secondary battery, comprising a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode active material, wherein: The positive electrode active material is the positive electrode material composition according to any one of claims 1 to 16.
18. An electrical device comprising a secondary battery, wherein: The secondary battery is selected from the secondary battery described in claim 17.
Citation Information
Patent Citations
Mixed positive material of lithium-ion power battery
CN103618084A
Positive material, positive plate and lithium ion battery
CN108777298A
Mixed positive electrode material, positive electrode plate, manufacturing method of positive electrode plate and battery
CN114079046A
Composite positive electrode material, positive electrode plate, manufacturing method of positive electrode plate and battery
CN114079047A
Cited By
Positive electrode material, positive electrode plate, battery and electric device
CN121054653A