Positive electrode active material composition, positive electrode plate, battery and electric device

By using first and second positive electrode active materials with different crystal forms in the positive electrode active material of the battery and controlling their particle size distribution to make them densely packed, combined with specific element doping and coating layers, the problem of high energy density and long life battery in the prior art has been solved, and high energy density and long life battery performance has been achieved.

CN118738342AActive Publication Date: 2024-10-01CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410947464.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-01
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Existing cathode active materials cannot simultaneously meet the requirements of high energy density, low cost, and good service life. Simply mixing cathode active materials with different crystal forms cannot effectively improve the compaction density and battery performance.

Method used

A composition comprising a first positive electrode active material and a second positive electrode active material with different crystal forms is used. By controlling their particle size distribution curves, the two materials are made to pack tightly, thereby improving the actual packing density and compaction density efficiency. Specific element doping and coating layers are used to improve the material performance.

Benefits of technology

This achieves high energy density and longer lifespan for the battery, while reducing production costs and improving battery cycle performance and high-temperature stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738342A_ABST
    Figure CN118738342A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode active material composition, a positive electrode plate, a battery and a power utilization device, the positive electrode active material composition comprises a first positive electrode active material and a second positive electrode active material with a crystal form different from that of the first positive electrode active material, and the first positive electrode active material comprises phosphate, a particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is marked as a first peak, the volume distribution particle size corresponding to the maximum peak intensity of the first peak is marked as Dv1, the volume distribution peak with the secondary maximum peak intensity is marked as a second peak, and the volume distribution particle size corresponding to the secondary maximum peak intensity of the first peak is marked as Dv1. The volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, namely 0 lt; dv1-Dv2 / Dv1 < = 50.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a positive electrode active material composition, a positive electrode sheet, a battery and an electrical device. Background Art

[0002] In recent years, batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the continuous expansion of battery application fields, the demand for battery energy density and service life is getting higher and higher. Summary of the invention

[0003] The present application provides a positive electrode active material composition, a positive electrode plate, a battery and an electrical device, which can enable the battery to have high energy density, low cost and good service life.

[0004] In a first aspect, the present application provides a positive electrode active material composition, comprising a first positive electrode active material and a second positive electrode active material having a crystal form different from that of the first positive electrode active material, wherein the first positive electrode active material comprises phosphate, and a particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, a volume distribution peak with a maximum peak intensity is recorded as a first peak, and a volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, a volume distribution peak with a second maximum peak intensity is recorded as a second peak, and a volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, then 0<|Dv1-Dv2| / Dv1≤50.

[0005] By making the positive electrode active material composition include a first positive electrode active material and a second positive electrode active material with different crystal forms, and making the particle size distribution curve of the positive electrode active material composition satisfy 0<|Dv1-Dv2| / Dv1≤50, the first positive electrode active material and the second positive electrode active material can be tightly stacked, thereby improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and further enabling the battery using the positive electrode active material composition to have a higher energy density and a longer service life.

[0006] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 12.5 μm.

[0007] In any embodiment, the volume distribution particle size Dv50 of the second positive electrode active material is 2.5 μm to 16.5 μm.

[0008] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:

[0009] 0.1≤|Dv1-Dv2| / Dv1≤50, optionally, 0.46≤|Dv1-Dv2| / Dv1≤39.6; and / or,

[0010] 0.3 μm ≤ Dv1 ≤ 17.8 μm, optionally, 0.35 μm ≤ Dv1 ≤ 12.1 μm; and / or,

[0011] 0.3μm≤Dv2≤17.8μm, optionally, 0.46μm≤Dv2≤14.2μm.

[0012] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thereby enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.

[0013] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:

[0014] 0.1≤|Dv1-Dv2| / Dv1≤6.0, optionally, 0.34≤|Dv1-Dv2| / Dv1≤3.8; and / or,

[0015] 2.0 μm ≤ Dv1 ≤ 12.5 μm, optionally, 3.0 μm ≤ Dv1 ≤ 12.3 μm; and / or,

[0016] 2.0μm≤Dv2≤15.0μm, optionally, 3.4μm≤Dv2≤14.3μm.

[0017] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thereby enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.

[0018] The second aspect of the present application provides a positive electrode active material composition, the positive electrode active material composition comprising a first positive electrode active material and a second positive electrode active material having a crystal form different from the first positive electrode active material, the first positive electrode active material comprising a phosphate, the particle size distribution curve of the positive electrode active material composition having at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, and the volume distribution peak with the second maximum peak intensity is recorded as the second peak. The volume distribution particle size of the first positive electrode active material is Dv50, which is 0.25 μm to 3.5 μm, and 0.3 μm ≤ Dv1 ≤ 17.8 μm, and 0.3 μm ≤ Dv2 ≤ 17.8 μm; or the volume distribution particle size of the first positive electrode active material is Dv50, which is 3.5 μm to 12.5 μm, and 2.0 μm ≤ Dv1 ≤ 12.5 μm, and 2.0 μm ≤ Dv2 ≤ 15.0 μm.

[0019] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thereby enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.

[0020] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and 0.35 μm≤Dv1≤12.1 μm, 0.46 μm≤Dv2≤14.2 μm. Thus, the battery using the positive electrode active material composition can further have a higher energy density and / or a longer service life.

[0021] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and 3.0 μm≤Dv1≤12.3 μm, 3.4 μm≤Dv2≤14.3 μm. Thus, the battery using the positive electrode active material composition can further have a higher energy density and / or a longer service life.

[0022] In any embodiment, the morphology of the first cathode active material includes one or more of single crystal and polycrystalline, and the morphology of the second cathode active material includes one or more of single crystal and polycrystalline.

[0023] In any embodiment, the volume distribution particle size Dv50 of the single-crystalline first positive electrode active material is 0.25 μm to 3.5 μm, and optionally 0.35 μm to 2.5 μm.

[0024] In any embodiment, the volume distribution particle size Dv10 of the single-crystalline first positive electrode active material is 0.05 μm to 1.5 μm, and can be 0.1 μm to 1.0 μm.

[0025] In any embodiment, the volume distribution particle size Dv50 of the polycrystalline first positive electrode active material is 3.5 μm to 12.5 μm, and optionally 3.8 μm to 10.5 μm.

[0026] In any embodiment, the volume distribution particle size Dv10 of the polycrystalline first positive electrode active material is 0.1 μm to 5.0 μm, and optionally 0.5 μm to 4.5 μm.

[0027] In any embodiment, the volume distribution particle size Dv50 of the single-crystalline second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 8.5 μm.

[0028] In any embodiment, the volume distribution particle size Dv10 of the single-crystal second positive electrode active material is 0.3 μm to 8 μm, and can be 1.0 μm to 3.5 μm.

[0029] In any embodiment, the volume distribution particle size Dv50 of the second positive electrode active material having a polycrystalline morphology is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 15.5 μm.

[0030] In any embodiment, the volume distribution particle size Dv10 of the second positive electrode active material having a polycrystalline morphology is 0.5 μm to 12 μm, and optionally 1.0 μm to 8.5 μm.

[0031] When the volume distribution particle size of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density, and can also reduce side reactions, lower interface impedance, and extend the battery life.

[0032] In any embodiment, based on the total weight of the positive electrode active material composition, the weight content of the first positive electrode active material is recorded as w a The weight content of the second positive electrode active material is recorded as w b , then w a is selected from the range of 0.5% to 99.5%, optionally selected from the range of 2% to 95%; and / or, w b Selected from the range of 0.5% to 99.5%, optionally selected from the range of 5% to 98%.

[0033] When the content of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density and / or a longer service life.

[0034] In any embodiment, the powder compaction density P1 of the first positive electrode active material at 30000N is 1.89 g / cm 3 Above, optional 1.95g / cm 3 Above, 1.98g / cm2 is optional 3 Above, further optional 2.0g / cm 3 Above, further optional 2.2g / cm 3 Above, further optionally 2.2 g / cm 3 Above and 2.8g / cm 3 Below or 2.2g / cm 3 Above and 2.65g / cm 3 the following.

[0035] In any embodiment, the powder compaction density P2 of the second positive electrode active material at 30000N is greater than or equal to 2.90g / cm 3 , can be selected as greater than or equal to 3.1g / cm 3 , more preferably greater than or equal to 3.3 g / cm 3 .

[0036] When the powder compaction density of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density.

[0037] In any embodiment, the BET specific surface area of ​​the second positive electrode active material is less than or equal to 1.73 m 2 / g, can be selected to be less than or equal to 1.5m 2 / g, 0.28m 2 / g to 1.5m 2 / g. This can reduce side reactions and improve the cycle performance of the battery.

[0038] In any embodiment, the first positive electrode active material comprises a compound represented by formula (I),

[0039] Li a A x Mn 1-y M 1 y P 1-z M 2 z O 4-n D n (I)

[0040] A includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; M 1It includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB and Group VIII; C includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D includes one or more elements selected from Group VIA and Group VIIA; a is selected from the range of 0.85 to 1.15; x is selected from the range of 0 to 0.1; y is selected from the range of 0.001 to 0.999; z is selected from the range of 0 to 0.5; n is selected from the range of 0 to 0.5.

[0041] By doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping element at the Mn position, obtaining improved cycle performance and / or high temperature stability, and the gram capacity and compaction density of the material are also improved.

[0042] In any embodiment, A includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W.

[0043] In any embodiment, M 1 It includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be optionally selected from one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge.

[0044] In any embodiment, M 2 Includes one or more elements selected from B (boron), S, Si and N.

[0045] In any embodiment, D includes one or more elements selected from S, F, Cl and Br.

[0046] In any embodiment, A includes any one element selected from Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include any one element selected from Mg and Nb.

[0047] In any embodiment, M 1It includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and can be optionally included at least two elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and can be optionally included at least two elements selected from Fe, Ti, V, Ni, Co and Mg, and can be further optionally included at least two elements selected from Fe, Ti, V, Co and Mg, and can be further optionally included Fe and one or more elements selected from Ti, V, Co and Mg.

[0048] In any embodiment, M 2 Includes any one element selected from B (boron), S, Si and N, and S is optional.

[0049] In any embodiment, D includes any one element selected from S, F, Cl and Br, and may be F.

[0050] By selecting the Li-position doping element within the above range, the lattice change rate during the delithiation process can be further reduced, thereby further improving the rate performance of the battery. By selecting the Mn-position doping element within the above range, the electronic conductivity can be further improved and the lattice change rate can be further reduced, thereby improving the rate performance and gram capacity of the battery. By selecting the P-position doping element within the above range, the rate performance of the battery can be further improved. By selecting the O-position doping element within the above range, the side reactions of the interface can be further reduced and the high temperature performance of the battery can be improved.

[0051] In any embodiment, a is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01.

[0052] In any embodiment, x is selected from the range of 0.001 to 0.005.

[0053] In any embodiment, y is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5.

[0054] In any embodiment, z is selected from the range of 0.001 to 0.5, alternatively selected from the range of 0.001 to 0.1, more alternatively selected from the range of 0.001 to 0.005.

[0055] In any embodiment, n is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.

[0056] By selecting the y value within the above range, the gram capacity and rate performance of the first positive electrode active material can be further improved. By selecting the x value within the above range, the kinetic performance of the first positive electrode active material can be further improved. By selecting the z value within the above range, the rate performance of the battery can be further improved. By selecting the n value within the above range, the high temperature performance of the battery can be further improved.

[0057] In any embodiment, x is 0, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.5, and n is 0; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0.

[0058] By doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, especially doping a specific element in a specific amount at the Mn position and P position of LiMnPO4 or at the Li position, Mn position, P position and O position of LiMnPO4, it is possible to improve the rate performance, reduce the dissolution of Mn and the doping element at the Mn position, improve the cycle performance and / or high temperature stability, and increase the gram capacity and compaction density of the first positive electrode active material.

[0059] In any embodiment, y:z is selected from the range of 0.002 to 999, and may be selected from the range of 0.025 to 999 or the range of 0.002 to 500, and may be selected from the range of 0.2 to 600. Thus, the defects of the first positive electrode active material can be reduced, and the integrity of the framework structure of the first positive electrode active material can be improved, thereby effectively improving the structural stability of the first positive electrode active material, and further improving the cycle stability of the battery.

[0060] In any embodiment, z:n is selected from the range of 0.002 to 500, and can be selected from the range of 0.2 to 100, and can be selected from the range of 0.2 to 50. Thus, the defects of the first positive electrode active material can be further reduced, the integrity of the framework structure of the first positive electrode active material can be further improved, the structural stability of the first positive electrode active material can be effectively improved, and the cycle stability of the battery can be improved.

[0061] In any embodiment, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; M 1Includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; M 2 It includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.1.

[0062] By doping specific elements in specific amounts at the Li position, Mn position, P position and O position of the compound LiMnPO4 at the same time, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping elements at the Mn position, thereby obtaining improved cycle performance and / or high temperature stability, and the gram capacity and compaction density of the first positive electrode active material can also be improved.

[0063] In any embodiment, M 1 It includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and may optionally include one or more elements selected from the group consisting of Zn, Fe, Ti, V, Ni, Co and Mg; M 2 It includes one or more elements selected from B (boron), Si, N and S; a is selected from the range of 0.9 to 1.1, x is 0, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is 0.

[0064] By doping specific elements at specific amounts at both the Mn and P positions of the compound LiMnPO4, the rate performance can be improved, the dissolution of Mn and the doping elements at the Mn position can be reduced, the cycle performance and / or high temperature stability can be improved, and the gram capacity and compaction density of the first positive electrode active material can be increased.

[0065] In any embodiment, (1-y):y is in the range of 0.1-999, and may be in the range of 0.1-10 or in the range of 0.67-999, and may be in the range of 1 to 10, and may be in the range of 1 to 4, and may be in the range of 1.5 to 3. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material may be further improved.

[0066] In any embodiment, a:x is in the range of 1 to 1200, optionally in the range of 9 to 1100, and more optionally in the range of 190 to 998. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.

[0067] In any embodiment, z:(1-z) is 1:9 to 1:999, and can be 1:499 to 1:249. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.

[0068] In any embodiment, the first positive electrode active material includes a core and a shell coating the core, the core includes the compound represented by formula (I); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

[0069] By arranging a coating layer with ionic conductivity and / or electronic conductivity on the surface of the inner core, a first positive electrode active material with a core-shell structure is provided. Applying the first positive electrode active material to a battery can improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.

[0070] In any embodiment, the one or more coating layers each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.

[0071] In any embodiment, the shell comprises a coating layer; optionally, the coating layer comprises one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.

[0072] The above materials can be used to obtain a coating layer with ionic conductivity and / or electronic conductivity, thereby improving the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.

[0073] In any embodiment, the shell includes a first coating layer coating the core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer; more optionally, the first coating layer includes one or more selected from pyrophosphate, phosphate, oxide and boride, and the second coating layer includes one or more selected from carbon and doped carbon. The use of a first coating layer of a specific material and a second coating layer of a specific material can further improve the rate performance, further reduce the dissolution of Mn and Mn-doped elements, thereby improving the cycle performance and / or high temperature stability of the battery.

[0074] In any embodiment, the shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; optionally, the first coating layer, the second coating layer, and the third coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer; more optionally, the first coating layer includes pyrophosphate, the second coating layer includes one or more selected from phosphate, oxide, and boride, and the third coating layer includes one or more selected from carbon and doped carbon. The use of a first coating layer of a specific material, a second coating layer of a specific material, and a third coating layer of a specific material further improves the rate performance, further reduces the dissolution of Mn and Mn-position doping elements, thereby improving the cycle performance and / or high temperature stability of the battery, and further improves the gram capacity and compaction density of the first positive electrode active material.

[0075] In any embodiment, the pyrophosphate is M b (P2O7) c ; and / or, the phosphate is X m (PO4) q ; and / or, the doping element in the doped carbon includes one or more selected from Group IIIA, Group VA, Group VIA and Group VIIA; and / or, the oxide is M' d O e ; and / or, the boride is Z v B w ; and / or, the polymer includes one or more elements selected from polysaccharides and their derivatives, polysiloxanes; M, X and Z each independently include one or more elements selected from Group IA, Group IIA, Group IIIA, Group IB, Group IIB, Group IVB, Group VB, Group VIIB and Group VIII; b is selected from the range of 1 to 4; c is selected from the range of 1 to 6; m is selected from the range of 1 to 2; q is selected from the range of 1 to 4; M′ includes one or more elements selected from alkali metals, alkaline earth metals, transition metals, Group IIIA elements, Group IVA elements, lanthanides and Sb; d is greater than 0 and less than or equal to 2; e is greater than 0 and less than or equal to 5; v is selected from the range of 1 to 7; w is selected from the range of 1 to 2.

[0076] By using the above materials as the coating layer, the dissolution of Mn and Mn-doping elements can be further reduced, the gram capacity and compaction density of the first positive electrode active material can be further increased, and the rate performance, high-temperature cycle performance and high-temperature storage performance of the battery can be further improved.

[0077] In any embodiment, M, X and Z each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, Mn and Al.

[0078] In any embodiment, the doping element in the doped carbon includes one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine.

[0079] In any embodiment, M′ includes one or more elements selected from Li, Be, B, Na, Mg, Al, Si, P, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, W, La and Ce, and can optionally include one or more elements selected from Mg, Al, Si, Zn, Zr and Sn.

[0080] In any embodiment, the polysiloxane is selected from one or more of linear polysiloxane and cyclic polysiloxane.

[0081] In any embodiment, the polysaccharide is selected from one or more of plant polysaccharides and marine polysaccharides.

[0082] By using the above-mentioned specific material as the coating layer, the dissolution of Mn and Mn-doped elements can be further reduced, and the high-temperature cycle performance and high-temperature storage performance of the battery can be further improved.

[0083] In any embodiment, the first positive electrode active material includes a core and a shell covering the core, wherein the core includes Li a Mn 1-y M 1 y P 1-z M 2 z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, M 1 The M 2 The shell comprises a first coating layer covering the inner core and a second coating layer covering the first coating layer, wherein the first coating layer comprises pyrophosphate MP2O7 and phosphate XPO4, and M and X each independently comprise one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; and the second coating layer comprises carbon.

[0084] In any embodiment, the first positive electrode active material includes a core and a shell covering the core, wherein the core includes Li a Mn 1-y M 1 y P 1-z M 2 z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, M 1 The M 2 The shell comprises a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer, wherein the first coating layer comprises pyrophosphate Li f QP2O7 and / or Q g (P2O7) h , 0≤f≤2, 1≤g≤4, 1≤h≤6, the pyrophosphate Li f QP2O7 and / or Q g (P2O7) h wherein Q independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; the second coating layer comprises crystalline phosphate XPO4, and X comprises one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; the third coating layer comprises carbon.

[0085] By doping lithium manganese phosphate with specific elements and coating its surface, the dissolution of Mn during lithium insertion and extraction can be effectively reduced, while promoting the migration of lithium ions, thereby improving the rate performance of the battery and enhancing the battery's cycle performance and high-temperature performance.

[0086] In any embodiment, the one or more coating layers in the shell that are farthest from the core each independently include one or more selected from polysiloxane, polysaccharide and polysaccharide derivatives. Thus, the uniformity of the coating can be improved, and the interface side reactions caused by high voltage can be effectively blocked, thereby improving the high-temperature cycle performance and high-temperature storage performance of the first positive electrode active material; and the coating layer has good ionic conductivity, which helps to improve the gram capacity of the first positive electrode active material and reduce the heat generation of the battery.

[0087] In any embodiment, the polysiloxane comprises a structural unit represented by formula (i),

[0088]

[0089] R1 and R2 are independently selected from H, -COOH, -OH, -SH, -CN, -SCN, amino, phosphate, carboxylate, amide, aldehyde, sulfonyl, polyether segment, C1-C20 aliphatic, C1-C20 halogenated aliphatic, C1-C20 heteroaliphatic, C1-C20 halogenated heteroaliphatic, C6-C20 aromatic, C6-C20 halogenated aromatic, C2-C20 heteroaromatic and C2-C20 halogenated heteroaromatic; optionally, R1 and R2 are independently selected from H, amino, phosphate, polyether segment, C1-C8 alkyl, C1-C8 halogenated alkyl, C1-C8 heteroalkyl, C1-C8 halogenated heteroalkyl, C2-C8 alkenyl and C2-C8 halogenated alkenyl.

[0090] In any embodiment, the polysiloxane further comprises an end-capping group, and the end-capping group comprises one or more of the following functional groups: polyether, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl, C2-C8 haloalkenyl, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy, C2-C8 epoxy, hydroxyl, C1-C8 hydroxyalkyl, amino, C1-C8 aminoalkyl, carboxyl, C1-C8 carboxylalkyl.

[0091] In any embodiment, the polysiloxane includes polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl functionalized polysiloxane, epoxy-terminated polysiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, polymethylchloropropylsiloxane, hydroxy-terminated polydimethylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, aminoethylaminopropyl polydimethylsiloxane, terminal polyether polydimethylsiloxane, side chain aminopropyl polysiloxane. , aminopropyl-terminated polydimethylsiloxane, side chain phosphate grafted polydimethylsiloxane, side chain polyether grafted polydimethylsiloxane, 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, cyclic polymethylvinylsiloxane, hexadecylcyclooctasiloxane, tetradecamethylcycloheptasiloxane, cyclic polydimethylsiloxane or more.

[0092] In any embodiment, the number average molecular weight of the polysiloxane, the polysaccharide and the polysaccharide derivative is independently below 300,000, optionally 10,000 to 200,000, more optionally 20,000 to 120,000, further optionally 400 to 80,000.

[0093] In any embodiment, the mass percentage of polar functional groups in the polysiloxane is α, 0≤α<50%, optionally, 5%≤α≤30%.

[0094] In any embodiment, the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH and its salts, -R-OH, -SO3H and its salts, -R-OH, -R-SO3H and its salts, sulfate, alkoxy, R represents an alkylene group, optionally representing a C1 to C5 alkylene group; optionally, the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH, -COOLi, -COONa, -COOK, -SO3H, -SO3Li, -SO3Na, -SO3K, -CH2-SO3H, -CH2-SO3Li, -CH2-SO3Na, -CH2-SO3K, methoxy, ethoxy.

[0095] In any embodiment, the polysaccharide includes one or more selected from pectin, carboxymethyl starch, hydroxypropyl starch, dextrin, cellulose ether, carboxymethyl chitosan, hydroxyethyl cellulose, carboxymethyl cellulose, carboxypropyl methyl cellulose, guar gum, sesbania gum, gum arabic, lithium alginate, sodium alginate, potassium alginate, fucoidan, agar, carrageenan, carrageenan, xanthan gum and fenugreek gum.

[0096] In any embodiment, the mass percentage of the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivative is independently 20% to 85%, optionally 30% to 78%.

[0097] In any embodiment, the lattice mismatch between the material of the core and the material of the shell is less than 10%. Thus, the contact between the core and the shell (or coating layer) can be good to prevent the shell (or coating layer) from falling off.

[0098] In any embodiment, based on the total weight of the first positive electrode active material, the manganese content is in the range of 10 wt%-35 wt%, optionally in the range of 13.3 wt%-33.2 wt%, more optionally in the range of 15 wt%-30 wt%, and further optionally in the range of 17 wt%-20 wt%; and / or, the phosphorus content is in the range of 12 wt%-25 wt%, optionally in the range of 15 wt%-20 wt%, and more optionally in the range of 16.8 wt%-19.5 wt%; and / or, the weight ratio of manganese to phosphorus is in the range of 0.71-1.85, optionally in the range of 0.90-1.25, and more optionally in the range of 0.95-1.20.

[0099] Limiting the content of manganese within the above range can further improve the stability and density of the first positive electrode active material, thereby improving the battery's cycling, storage and compaction properties; and can maintain a higher voltage platform, thereby improving the battery's energy density.

[0100] Limiting the content of phosphorus within the above range can effectively reduce the influence of small polaron conductivity on the conductivity of the first positive electrode active material, and can further improve the stability of the lattice structure, thereby improving the overall stability of the first positive electrode active material.

[0101] Limiting the weight ratio of manganese to phosphorus within the above range can further reduce manganese dissolution, improve the stability and gram capacity of the first positive electrode active material, and improve the cycle performance and storage performance of the battery; it can also reduce impurities, enable the first positive electrode active material to maintain a higher discharge voltage platform, and enable the battery to have a high energy density.

[0102] In any embodiment, the surface of the first positive electrode active material is coated with one or more of carbon and doped carbon; optionally, the surface of the first positive electrode active material is coated with carbon, thereby improving the conductivity of the first positive electrode active material.

[0103] In any embodiment, the doping element in the doped carbon includes one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine.

[0104] In any embodiment, the coating amount of the shell is 0.1 wt % to 6 wt %, based on the weight of the core.

[0105] In any embodiment, the coating amount of the first coating layer is greater than 0 and less than or equal to 7% by weight, optionally greater than 0 and less than or equal to 6% by weight, more optionally greater than 0 and less than or equal to 5.5% by weight or 4-5.6% by weight, and further optionally greater than 0 and less than or equal to 2% by weight, based on the weight of the core; and / or, the coating amount of the second coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, more optionally 2-4% by weight or 3-5% by weight, based on the weight of the core; and / or, the coating amount of the third coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, and more optionally greater than 0 and less than or equal to 2% by weight, based on the weight of the core.

[0106] In any embodiment, the shell also includes a fourth coating layer coating the third coating layer and a fifth coating layer coating the fourth coating layer; the coating amounts of the fourth coating layer and the fifth coating layer are each independently 0.01 wt % to 10 wt %, optionally 0.05 wt % to 10 wt %, more optionally 0.1 wt % to 5 wt %, further 0.1 wt % to 2 wt %, based on the weight of the core.

[0107] The coating amount of each coating layer is preferably within the above range, so that the core can be fully coated and the kinetic performance of the battery can be further improved without sacrificing the gram capacity of the first positive electrode active material.

[0108] In any embodiment, the shell is located on 40% to 90% of the surface of the core, and optionally 60% to 80% of the surface, so that the core can be fully coated, thereby improving the dynamic performance of the battery.

[0109] In any embodiment, the shell has a thickness of 1-15 nm.

[0110] In any embodiment, the thickness of the first coating layer is 1-10nm, optionally 2-10nm; and / or the thickness of the second coating layer is 2-25nm, optionally 2-15nm, and more optionally 3-15nm; and / or the thickness of the third coating layer is 2-25nm, optionally 5-25nm.

[0111] In any embodiment, the one or more coating layers each independently include one or more selected from pyrophosphate, phosphate and oxide, and one or more selected from the pyrophosphate, phosphate and oxide are crystalline; optionally, the crystallinity of the pyrophosphate, the phosphate and the oxide is each independently 10% to 100%, and more optionally 50% to 100%.

[0112] Pyrophosphates and phosphates with a certain degree of crystallinity are not only conducive to fully utilizing the pyrophosphate coating to reduce manganese dissolution and the phosphate coating's excellent ability to conduct lithium ions and reduce interface side reactions, but also enable the pyrophosphate coating and the phosphate coating to better lattice match, thereby achieving a close bond between the coatings.

[0113] In any embodiment, in the shell, the weight ratio of pyrophosphate to phosphate and the weight ratio of pyrophosphate to oxide are independently 1:3 to 3:1, and can be 1:3 to 1:1. Thus, by having pyrophosphate and phosphate in a suitable weight ratio range or pyrophosphate and oxide in a suitable weight ratio range, manganese dissolution can be effectively reduced, surface impurity lithium content can be effectively reduced, and interface side reactions can be reduced, thereby improving the high temperature storage performance and high temperature cycle performance of the battery.

[0114] In any embodiment, the one or more coating layers independently include carbon, and the carbon is a mixture of SP2 carbon and SP3 carbon; optionally, in the carbon, the molar ratio of the SP2 carbon to the SP3 carbon is any value in the range of 0.07-13, more preferably any value in the range of 0.1-10, and further preferably any value in the range of 2.0-3.0. By selecting the form of carbon in the carbon coating layer, the comprehensive electrical performance of the battery can be improved.

[0115] In any embodiment, the one or more coating layers independently include doped carbon, and the mass content of the doping element in the doped carbon is less than 30%; optionally, the mass content of the doping element in the doped carbon is less than 20%. The doping elements within the above content range can not only fully improve the conductivity of the pure carbon layer, but also effectively avoid excessive surface activity caused by excessive doping of the doping elements, thereby effectively controlling the interface side reactions caused by excessive doping of the coating layer.

[0116] In any embodiment, the one or more coating layers each independently include doped carbon, in which the doping element is nitrogen and / or sulfur, and the mass content of the doping element in the doped carbon is 1% to 15%; or, the doping element is phosphorus, boron and / or fluorine, and the mass content of the doping element in the doped carbon is 0.5% to 5%; optionally, the doping element is nitrogen, phosphorus, sulfur, boron or fluorine.

[0117] Since nitrogen atoms and sulfur atoms are closer to the atomic radius of carbon atoms and are not easy to destroy the carbon skeleton, when the doping amount of nitrogen atoms and sulfur atoms is within the above relatively wide range, the conductivity of the doped carbon layer can be fully exerted, and the lithium ion transmission and lithium ion desolvation ability can be promoted.

[0118] Since the atomic radius of phosphorus atoms, boron atoms and / or fluorine atoms is different from that of carbon atoms, excessive doping can easily destroy the carbon skeleton. Therefore, when the doping amount of phosphorus atoms, boron atoms and / or fluorine atoms is within the relatively small range mentioned above, the conductivity of the doped carbon layer can be fully exerted, and the lithium ion transmission and lithium ion desolvation capabilities can be promoted.

[0119] In any embodiment, the one or more coating layers independently include pyrophosphate, the pyrophosphate has a lattice spacing range of 0.293-0.470nm, optionally 0.297-0.462nm or 0.293-0.326nm, and more optionally 0.300-0.310nm, and a crystal orientation (111) angle range of 18.00°-32.57°, optionally 18.00°-32.00° or 26.41°-32.57°, more optionally 19.211°-30.846°, and further optionally 29.00°-30.00°.

[0120] In any embodiment, the one or more coating layers independently include phosphate, the phosphate has a lattice spacing range of 0.244-0.425nm, optionally 0.345-0.358nm, and a crystal orientation (111) angle range of 20.00°-37.00°, optionally 24.25°-26.45°.

[0121] As a result, the impurity phase in the coating layer can be effectively reduced, thereby improving the material's gram capacity, cycle performance and rate performance.

[0122] In any embodiment, the first coating layer or the second coating layer comprises a phosphate.

[0123] In any embodiment, the lattice change rate of the first positive electrode active material before and after complete lithium deintercalation is 50% or less, optionally 9.8% or less, more optionally 8.1% or less, further optionally 7.5% or less, further optionally 6% or less, further optionally 4% or less, further optionally 3.8% or less, further optionally 2.0-3.8%. By reducing the lattice change rate, Li ion transmission can be made easier, that is, the migration ability of Li ions in the first positive electrode active material is stronger, which is conducive to improving the rate performance of the battery.

[0124] In any embodiment, the Li / Mn antisite defect concentration of the first positive electrode active material is 5.3% or less, optionally 5.1% or less, more optionally 4% or less, further optionally 2.2% or less, further optionally 2% or less, further optionally 1.5%-2.2% or 0.5% or less. By reducing the Li / Mn antisite defect concentration, it is beneficial to improve the gram capacity and rate performance of the first positive electrode active material.

[0125] In any embodiment, the surface oxygen valence state of the first positive electrode active material is below -1.55, optionally below -1.82, more optionally below -1.88, further optionally below -1.90 or -1.98 to -1.88, further optionally -1.98 to -1.89, further optionally -1.98 to -1.90. By reducing the surface oxygen valence state, the interface side reaction between the first positive electrode active material and the electrolyte can be reduced, thereby improving the cycle performance and high temperature stability of the battery.

[0126] In any embodiment, the positive electrode active material composition satisfies 0.0004≤w a ×y×(3.4-V B )≤0.063, optionally, 0.0015≤w a ×y×(3.4-V B )≤0.045,w a represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition, y is 1 mol of M in the compound represented by formula (I) 1 Molar amount of element, V B M in the compound represented by formula (I) 1 The voltage platform of an element, in V (volts). When the positive electrode active material composition further meets the above conditions, it is beneficial for the positive electrode sheet to have both high compaction density and high compaction density efficiency, and it is beneficial for the battery to have both high energy density and long service life.

[0127] In any embodiment, the second positive electrode active material includes a layered oxide. By properly combining the first positive electrode active material and the second positive electrode active material, the actual packing density of the positive electrode active material composition can be improved, the compaction density and compaction density efficiency of the positive electrode sheet can be improved, and the battery using the positive electrode active material composition can have a higher energy density and a longer service life.

[0128] In any embodiment, the second positive electrode active material comprises a compound represented by formula (II),

[0129] Li a1 A 1 b1 Ni c1 Co d1 B 1 e1 C 1 f1 O 2-g1 D 1 g1 , (II)

[0130] A1 Includes one or more elements selected from Group IA, Group IIA, Group VIII, Group VIB, and Group IIB; B 1 including Mn and / or Al; C 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group VIA, Group IIB, Group IIIB, Group IVB, Group VB, Group VIB, and Group VIII; D 1 It includes one or more elements selected from Group VIA and Group VIIA; a1 is selected from the range of 0.8 to 1.2; b1 is selected from the range of 0 to 0.2; c1 is selected from the range of 0 to 1; d1 is selected from the range of 0 to 1; e1 is selected from the range of 0 to 1; f1 is selected from the range of 0 to 0.1; g1 is selected from the range of 0 to 0.1; and c1+d1+e1+f1=1.

[0131] In any embodiment, A 1 It includes one or more elements selected from Na, K, Mg, Rb, Zn and Zr.

[0132] In any embodiment, C 1 It includes one or more elements selected from Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Fe, Zn, Ba, Mo, V, Ce, Nb, Sb, Ta, Ge, Nb, Sc, Ba, B, S and Y, and can optionally include one or more elements selected from Al, Ti, Zr, Nb, Sr, Sc, Sb, Y, Ba, B.

[0133] In any embodiment, D 1 The invention comprises one or more elements selected from N, S, F, Cl and Br, and may optionally comprise S and / or F.

[0134] In any embodiment, a1 is selected from the range of 0.9 to 1.1.

[0135] In any embodiment, b1 is selected from the range of 0 to 0.1.

[0136] In any embodiment, c1 is selected from the range of 0.314 to 0.990, and can be optionally selected from the range of 0.500 to 0.990.

[0137] In any embodiment, d1 is selected from the range of 0 to 0.320, and may be selected from the range of 0 to 0.150.

[0138] In any embodiment, e1 is selected from the range of 0.001 to 0.450, and can be optionally selected from the range of 0.005 to 0.4.

[0139] In any embodiment, f1 is selected from the range of 0.001 to 0.1, and can be optionally selected from the range of 0.001 to 0.05.

[0140] In any embodiment, g1 is selected from the range of 0 to 0.01, and can be optionally selected from the range of 0.01 to 0.05.

[0141] In any embodiment, the second positive electrode active material includes a core and a shell coating the core, the core includes the compound represented by formula (II); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

[0142] In any embodiment, in the shell of the second positive electrode active material, the one or more coating layers each independently include one or more selected from phosphate, pyrophosphate, carbon, doped carbon, oxide, and fast ion conductor, and may optionally include one or more selected from phosphate, pyrophosphate, and oxide.

[0143] In any embodiment, the shell of the second positive electrode active material includes a coating layer; optionally, the coating layer includes one or more selected from phosphate, pyrophosphate, and oxide.

[0144] In any embodiment, the shell of the second positive electrode active material includes a first coating layer coating the inner core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from phosphates, pyrophosphates, and oxides; more optionally, the first coating layer includes one or more selected from phosphates and oxides, and the second coating layer includes one or more selected from pyrophosphates and oxides.

[0145] In any embodiment, the coating amount of the shell of the second positive electrode active material is 0.005 wt % to 1 wt %, optionally 0.01 wt % to 0.5 wt %, based on the weight of the core; and / or the thickness of the shell is 2 nm to 200 nm, optionally 5 nm to 50 nm.

[0146] The third aspect of the present application provides a positive electrode plate, including a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes the positive electrode active material composition of the first aspect of the present application or the positive electrode active material composition of the second aspect.

[0147] In any embodiment, the content of the positive electrode active material composition in the positive electrode film layer is 90 wt % to 99.5 wt %, and more preferably 95 wt % to 99.5 wt %, based on the total weight of the positive electrode film layer.

[0148] In any embodiment, the positive electrode film layer further includes a third positive electrode active material, and the third positive electrode active material includes one or more of a lithium-rich oxide material, a lithium iron phosphate material, a spinel-type lithium manganate material, and their respective modified compounds, and the modification methods include doping and / or surface coating modification.

[0149] In any embodiment, the third positive electrode active material includes a compound represented by formula (III),

[0150] Li 1+p1 A 2 q1 B 2 r1 O s1 , (III)

[0151] 0.05 ≤ p1 < 0.2, 0.10 < q1 ≤ 0.95, 0 ≤ r1 ≤ 0.2, and 2 ≤ s1 < 3, A 2 includes one or more elements selected from Co, Ni, Mn, and Al; B 2 includes one or more elements selected from Mg, Ti, Cr, Zr, Nb, Fe, Mo, Cu, Sb, V, P, and F.

[0152] In any embodiment, the third positive electrode active material includes a core and a shell coating the core, and the core includes the compound represented by formula (III); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

[0153] In any embodiment, one or more of the coating layers in the shell coating the compound represented by formula (III) independently includes one or more selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly intercalating and deintercalating lithium ions.

[0154] In any embodiment, the coating amount of the shell coating the compound represented by formula (III) is 0.1 wt% to 5 wt%, optionally 0.5 wt% to 2 wt%, based on the weight of the core; and / or, the thickness of the shell coating the compound represented by formula (III) is 2 nm to 200 nm, optionally 5 nm to 50 nm.

[0155] In any embodiment, the third positive electrode active material includes a compound represented by formula (IV),

[0156] Li a2 A 3 x2 B 3 y2 P 1-z2 C 3z2 O 4-n2 D 3 n2 , (IV)

[0157] A 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; C 3 Includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D 3 It includes one or more elements selected from Group VIA and Group VIIA; a2 is selected from the range of 0.85 to 1.15; x2 is selected from the range of 0 to 0.1; y2 is selected from the range of 0.001 to 0.999; z2 is selected from the range of 0 to 0.5; and n2 is selected from the range of 0 to 0.5.

[0158] In any embodiment, A 3 It includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and can optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W.

[0159] In any embodiment, B 3 It includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and can be optionally selected from one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge.

[0160] In any embodiment, C 3 Includes one or more elements selected from B (boron), S, Si and N.

[0161] In any embodiment, D 3 Includes one or more elements selected from S, F, Cl and Br.

[0162] In any embodiment, a2 is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01.

[0163] In any embodiment, x2 is selected from the range of 0.001 to 0.005.

[0164] In any embodiment, y2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5.

[0165] In any embodiment, z2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, and more optionally selected from the range of 0.001 to 0.005.

[0166] In any embodiment, n2 is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.

[0167] In any embodiment, the third positive electrode active material includes a core and a shell covering the core, the core includes the compound represented by formula (IV); and the shell is the same as the shell covering the compound represented by formula (I).

[0168] In any embodiment, the third positive electrode active material includes a compound represented by formula (V),

[0169] LiMn t1 A 4 2-t1 O4, (V)

[0170] t1 is selected from the range of 0 to 2, A 4 Includes one or more elements selected from Ni, Cr, Al, Zr, V, Ti, Mo, Ru, Mg, Nb, Ba, Si, P, W, Co, Cu and Zn.

[0171] In any embodiment, the third positive electrode active material includes a core and a shell coating the core, the core includes the compound represented by formula (V); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

[0172] In any embodiment, one or more coating layers in the shell coating the compound represented by formula (V) independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly inserting and deinserting lithium ions.

[0173] In any embodiment, the coating amount of the shell coating the compound represented by formula (V) is 0.1 wt% to 5 wt%, optionally 0.5 wt% to 2 wt%, based on the weight of the core; and / or the thickness of the shell coating the compound represented by formula (V) is 2 nm to 200 nm, optionally 5 nm to 50 nm.

[0174] In any embodiment, the positive electrode film layer includes a positive electrode binder and / or a positive electrode conductor.

[0175] In any embodiment, the positive electrode binder includes a vinylidene fluoride homopolymer and / or copolymer. More optionally, the comonomer includes one or more of tetrafluoroethylene, hexafluoropropylene, and propylene.

[0176] In any embodiment, the weight average molecular weight of the positive electrode binder is 300,000 to 2,000,000.

[0177] In any embodiment, the positive electrode film layer further includes functional additives, and the functional additives include one or more of a dispersant, a plasticizer, a pore former, a water removal additive, an acid removal additive, and a lithium supplement.

[0178] In any embodiment, the positive electrode plate also includes a functional coating, which is located between the positive electrode collector and the positive electrode film layer and / or on the surface of the positive electrode film layer facing away from the positive electrode collector, and the functional coating includes one or more of conductive carbon, water removal additives, acid removal additives, and lithium supplements.

[0179] A fourth aspect of the present application provides a battery, comprising the positive electrode active material composition of the first aspect of the present application, the positive electrode active material composition of the second aspect, or the positive electrode plate of the third aspect of the present application.

[0180] In any embodiment, the battery includes an electrolyte, and the electrolyte includes one or more of a liquid electrolyte, an all-solid electrolyte, and a gel electrolyte.

[0181] In any embodiment, the liquid electrolyte includes a lithium salt, a non-aqueous solvent for dissolving the lithium salt, and an optional additive; optionally, the lithium salt includes one or more selected from LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2, LiBF2C2O4, and LiPO2F2.

[0182] In any embodiment, the concentration of the lithium salt is 0.5-1.5 mol / L.

[0183] In any embodiment, the non-aqueous solvent includes one or more selected from propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethylene sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, acid anhydride, N-methylpyrrolidone, acetonitrile, cyclopentane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, and tetrahydrofuran.

[0184] In any embodiment, the additive includes one or more selected from cyclic carbonate compounds containing carbon-carbon double bonds, halogen-substituted cyclic carbonate compounds, nitrile and polynitrile compounds, phosphazene compounds, aromatic hydrocarbons and halogenated aromatic hydrocarbon compounds, isocyanate compounds, acid anhydride compounds, sulfate compounds, sulfite compounds, sulfonate compounds, disulfonate compounds, borate compounds, phosphate compounds, amide compounds, carbodiimide compounds, crown ethers and azacrown ether compounds, and their respective derivatives, optionally including vinylene carbonate, 1,2,3-tris(2-cyanoethoxy)propane, 1-aza-12-crown 4-ether, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, tris(hexafluoroisopropyl)borate, tris(2,2,3,3-tetrafluoropropyl)borate, and tris(pentafluorophenyl)borate. .

[0185] In any embodiment, the battery includes a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, the negative electrode film layer includes a negative electrode active material, and the negative electrode active material includes one or more of a carbon-based material, a silicon-based material, a tin-based material and lithium titanate; optionally, the negative electrode active material includes a carbon-based material, or a combination of a carbon-based material and a silicon-based material.

[0186] In any embodiment, the porosity of the negative electrode film layer is 20% to 50%.

[0187] In any embodiment, the negative electrode active material includes a carbon-based material, and the carbon-based material includes graphite, or a combination of graphite and hard carbon.

[0188] In any embodiment, the negative electrode active material includes a combination of a carbon-based material and a silicon-based material, the carbon-based material includes graphite, or a combination of graphite and hard carbon, and the content of the silicon element in the negative electrode active material is greater than 0 and less than or equal to 30 weight %, based on the total weight of the negative electrode active material.

[0189] In any embodiment, the negative electrode plate further includes a functional coating, which is located between the negative electrode collector and the negative electrode film layer and / or on the surface of the negative electrode film layer facing away from the negative electrode collector; optionally, the functional coating includes carbon.

[0190] In any embodiment, the negative electrode film layer also includes a lithium replenishing material. Optionally, the lithium replenishing material includes one or more of lithium foil, lithium strip, lithium powder, and a pre-lithiation agent. Optionally, the pre-lithiation agent includes one or more of Li-aromatic hydrocarbons, complexes of Li-aromatic hydrocarbons and ether solvents, and may further include one or more of naphthalene lithium and biphenyl lithium-dimethyl ether.

[0191] In any embodiment, the negative electrode plate includes a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer respectively arranged on two surfaces of the negative electrode current collector. Optionally, the thickness ratio of the first negative electrode film layer to the second negative electrode film layer is 5:95 to 95:5.

[0192] In any embodiment, the battery includes a negative electrode sheet, and the negative electrode sheet does not include a negative electrode active material capable of inserting and extracting lithium ions.

[0193] In any embodiment, the negative electrode plate includes a lithium plate or a lithium alloy plate.

[0194] In any embodiment, the negative electrode sheet includes a mesh or foam three-dimensional skeleton layer.

[0195] In any embodiment, the battery includes a separator including a porous substrate.

[0196] In any embodiment, the isolation membrane further comprises a coating located on at least one surface of the porous substrate. Optionally, the coating comprises one or more of inorganic heat-resistant particles and organic heat-resistant particles.

[0197] In any embodiment, the porosity of the isolation film is 10%-40%.

[0198] A fifth aspect of the present application provides an electrical device, comprising the battery of the fourth aspect of the present application.

[0199] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0200] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some implementation methods of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0201] Figure 1 It is a schematic diagram of an embodiment of a battery cell of the present application.

[0202] Figure 2 It is an exploded schematic diagram of an embodiment of a battery cell of the present application.

[0203] Figure 3 It is a schematic diagram of an embodiment of a battery module of the present application.

[0204] Figure 4 It is a schematic diagram of an embodiment of the battery pack of the present application.

[0205] Figure 5 yes Figure 4 An exploded schematic diagram of an embodiment of a battery pack is shown.

[0206] Figure 6 It is a schematic diagram of an embodiment of an electrical device including the battery of the present application as a power source.

[0207] Figure 7 is a particle size distribution curve of the positive electrode active material composition of Example 11.

[0208] In the drawings, the drawings may not be drawn according to the actual scale. The reference numerals are as follows: 1 battery pack, 2 upper box, 3 lower box, 4 battery module, 5 battery cell, 51 housing, 52 electrode assembly, 53 cover plate. DETAILED DESCRIPTION

[0209] Below, the embodiments of the positive electrode active material composition, positive electrode sheet, battery and electric device of the present application are specifically disclosed with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0210] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0211] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0212] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0213] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0214] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0215] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0216] If not otherwise specified, in this application, the terms "first", "second", "third", "fourth", "fifth", etc. are used to distinguish different objects rather than to describe a specific order or a primary and secondary relationship.

[0217] In the present application, the terms "plurality" and "multiple" refer to two or more.

[0218] In various places of this specification, the substituents of compounds are disclosed in groups or ranges. It is clearly expected that this description includes each individual subcombination of members of these groups and ranges. For example, it is clearly expected that the term "C1-C6 alkyl" discloses C1, C2, C3, C4, C5, C6, C1-C6, C1-C5, C1-C4, C1-C3, C1-C2, C2-C6, C2-C5, C2-C4, C2-C3, C3-C6, C3-C5, C3-C4, C4-C6, C4-C5 and C5-C6 alkyl individually.

[0219] Unless otherwise specified, the terms used in this application have the commonly understood meanings that are commonly understood by those skilled in the art.

[0220] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured by various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise specified, the test temperature of each parameter is 25°C.

[0221] Unless otherwise specified, the ratio parameters involved in this application are compared in the same unit. For example, the ratio of the volume distribution particle size of A to that of B is 1:1, and the units of the volume distribution particle size of A and B are the same.

[0222] In the present application, the term "compacted density efficiency" refers to the ratio of the compacted density of the membrane layer to the theoretical compacted density of the active material powder.

[0223] In the present application, the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material may be tested for element content using inductively coupled plasma emission spectroscopy (ICP).

[0224] The battery mentioned in the embodiments of the present application refers to a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module or a battery pack.

[0225] A battery cell is the smallest unit of a battery, which can independently realize the functions of charging and discharging. A battery cell can be cylindrical, flat, rectangular or other shapes, etc., which are not limited in the embodiments of the present application. Figure 1 The battery cell 5 is a rectangular parallelepiped structure as an example.

[0226] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed connection through a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a case and battery cells, and the battery cells or battery modules are accommodated in the case. In some embodiments, the case may serve as part of the chassis structure of the vehicle. For example, part of the case may become at least a part of the floor of the vehicle, or part of the case may become at least a part of the crossbeam and longitudinal beam of the vehicle.

[0227] In some embodiments, the battery may be an energy storage device, which includes an energy storage container, an energy storage cabinet, and the like.

[0228] The battery cells mentioned in the embodiments of the present application include lithium-ion primary battery cells, lithium-ion secondary battery cells, lithium metal battery cells, negative electrode-free lithium metal battery cells, etc., which are not limited in the embodiments of the present application.

[0229] A battery cell generally includes an electrode assembly, which generally includes a positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet. The electrode assembly may be a wound structure or a laminated structure, which is not limited in the present application.

[0230] The battery cell may further include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte. The outer package may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS).

[0231] In some embodiments, Figure 2As shown, the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The electrode assembly 52 is encapsulated in the receiving cavity. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, which can be adjusted according to needs.

[0232] In some embodiments, battery cells may be assembled into a battery module. The battery module may contain multiple battery cells, and the specific number may be adjusted according to the application and capacity of the battery module. Figure 3 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 3 As shown, in the battery module 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.

[0233] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.

[0234] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0235] Figure 4 and Figure 5 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 4 and Figure 5 As shown, the battery pack 1 may include a box body and a plurality of battery modules 4 disposed in the box body. The box body includes an upper box body 2 and a lower box body 3, and the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the box body in any manner.

[0236] The positive electrode sheet includes positive electrode active materials. As an important component of the battery, the performance of positive electrode active materials is an important factor restricting the energy density and service life of the battery. At present, no positive electrode active material that can meet the requirements of low cost, high capacity and few side reactions has been developed.

[0237] In view of this, the inventors propose a positive electrode active material composition, which can make the battery have high energy density, low cost and good service life.

[0238] The positive electrode active material composition provided in the embodiment of the present application includes a first positive electrode active material and a second positive electrode active material with a different crystal form from the first positive electrode active material, wherein the first positive electrode active material includes phosphate. The different crystal forms of the first positive electrode active material and the second positive electrode active material refer to that the first positive electrode active material and the second positive electrode active material have different crystal systems.

[0239] The particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, then 0<|Dv1-Dv2| / Dv1≤50. "||" represents an absolute value.

[0240] The first positive electrode active material includes phosphate, which is usually an olivine structure and has a generally low production cost. However, the compaction density of the first positive electrode active material is relatively low, and it is difficult to meet the requirements of high energy density batteries. Combining it with another positive electrode active material with a high compaction density can increase the compaction density of the positive electrode sheet, but simply mixing the two positive electrode active materials usually does not improve the compaction density and compaction density efficiency of the positive electrode sheet, making it difficult to fully utilize the capacity of the battery, and also affecting the battery's service life.

[0241] The inventors have found that by making the positive electrode active material composition include a first positive electrode active material and a second positive electrode active material with different crystal forms, and making the particle size distribution curve of the positive electrode active material composition satisfy 0<|Dv1-Dv2| / Dv1≤50, the first positive electrode active material and the second positive electrode active material can be tightly stacked, thereby improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and further enabling the battery using the positive electrode active material composition to have a higher energy density and a longer service life.

[0242] The particle size distribution curve of the positive electrode active material composition can be adjusted by adjusting one or more parameters of the volume distribution particle size, volume particle size distribution width, mass content, etc. of each of the first positive electrode active material and the second positive electrode active material.

[0243] In some embodiments, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 12.5 μm.

[0244] In some embodiments, the volume distribution particle size Dv50 of the second positive electrode active material is 2.5 μm to 16.5 μm.

[0245] In some embodiments, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:

[0246] 0.1≤|Dv1-Dv2| / Dv1≤50, optionally, 0.46≤|Dv1-Dv2| / Dv1≤39.6; and / or,

[0247] 0.3 μm ≤ Dv1 ≤ 17.8 μm, optionally, 0.35 μm ≤ Dv1 ≤ 12.1 μm; and / or,

[0248] 0.3μm≤Dv2≤17.8μm, optionally, 0.46μm≤Dv2≤14.2μm.

[0249] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thereby enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.

[0250] In some embodiments, the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies:

[0251] 0.1≤|Dv1-Dv2| / Dv1≤6.0, optionally, 0.34≤|Dv1-Dv2| / Dv1≤3.8; and / or,

[0252] 2.0 μm ≤ Dv1 ≤ 12.5 μm, optionally, 3.0 μm ≤ Dv1 ≤ 12.3 μm; and / or,

[0253] 2.0μm≤Dv2≤15.0μm, optionally, 3.4μm≤Dv2≤14.3μm.

[0254] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thereby enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.

[0255] The present application also provides a positive electrode active material composition, the positive electrode active material composition comprising a first positive electrode active material and a second positive electrode active material having a crystal form different from the first positive electrode active material, the first positive electrode active material comprising a phosphate, the particle size distribution curve of the positive electrode active material composition having at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, and the volume distribution peak with the second maximum peak intensity is recorded as the second peak. The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and 0.3 μm≤Dv1≤17.8 μm, 0.3 μm≤Dv2≤17.8 μm; or the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and 2.0 μm≤Dv1≤12.5 μm, 2.0 μm≤Dv2≤15.0 μm.

[0256] This allows the first positive electrode active material and the second positive electrode active material to be stacked more densely, further improving the actual stacking density of the positive electrode active material composition, improving the compaction density and compaction density efficiency of the positive electrode sheet, and thereby enabling the battery using the positive electrode active material composition to have a higher energy density and / or a longer service life.

[0257] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and 0.35 μm≤Dv1≤12.1 μm, 0.46 μm≤Dv2≤14.2 μm. Thus, the battery using the positive electrode active material composition can further have a higher energy density and / or a longer service life.

[0258] In any embodiment, the volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and 3.0 μm≤Dv1≤12.3 μm, 3.4 μm≤Dv2≤14.3 μm. Thus, the battery using the positive electrode active material composition can further have a higher energy density and / or a longer service life.

[0259] The additional technical features described below are applicable to both the positive electrode active material composition of the first aspect and the positive electrode active material composition of the second aspect herein.

[0260] In some embodiments, the morphology of the first positive electrode active material includes one or more of single crystal and polycrystalline, and the morphology of the second positive electrode active material includes one or more of single crystal and polycrystalline.

[0261] The term "single crystal" also includes quasi-single crystals (also called quasi-single crystals), which generally refer to particles formed by the aggregation of a small number of primary particles. Polycrystalline refers to secondary particles formed by the aggregation of multiple primary particles.

[0262] In some embodiments, the volume distribution particle size Dv50 of the single-crystalline first positive electrode active material is 0.25 μm to 3.5 μm, and optionally 0.35 μm to 2.5 μm.

[0263] In some embodiments, the volume distribution particle size Dv10 of the single-crystalline first positive electrode active material is 0.05 μm to 1.5 μm, and optionally 0.1 μm to 1.0 μm.

[0264] In some embodiments, the volume distribution particle size Dv50 of the polycrystalline first positive electrode active material is 3.5 μm to 12.5 μm, and optionally 3.8 μm to 10.5 μm.

[0265] In some embodiments, the volume distribution particle size Dv10 of the polycrystalline first positive electrode active material is 0.1 μm to 5.0 μm, and optionally 0.5 μm to 4.5 μm.

[0266] In some embodiments, the volume distribution particle size Dv50 of the single-crystalline second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 8.5 μm.

[0267] In some embodiments, the volume distribution particle size Dv10 of the single-crystal second positive electrode active material is 0.3 μm to 8 μm, and may be 1.0 μm to 3.5 μm.

[0268] In some embodiments, the volume distribution particle size Dv50 of the polycrystalline second positive electrode active material is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 15.5 μm.

[0269] In some embodiments, the volume distribution particle size Dv10 of the polycrystalline second positive electrode active material is 0.5 μm to 12 μm, and optionally 1.0 μm to 8.5 μm.

[0270] When the volume distribution particle size of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density, and can also reduce side reactions, lower interface impedance, and extend the battery life.

[0271] In some embodiments, the morphology of the first positive electrode active material includes single crystals, for example, the number of single crystals may account for more than 80% or more than 90%. The first positive electrode active material with a polycrystalline morphology has a higher specific surface area, which will increase hygroscopicity and process time costs during the production process, thereby increasing the production cost of the battery.

[0272] In some embodiments, the morphology of the second positive electrode active material includes polycrystalline, for example, the amount of polycrystalline may account for more than 80% or more than 90%. The second positive electrode active material with polycrystalline morphology may have a larger particle size and a higher powder compaction density, thereby helping to improve the energy density of the battery.

[0273] In some embodiments, based on the total weight of the positive electrode active material composition, the weight content of the first positive electrode active material is recorded as w a , then w a Selected from the range of 0.5% to 99.5%, optionally selected from the range of 2% to 95%.

[0274] In some embodiments, based on the total weight of the positive electrode active material composition, the weight content of the second positive electrode active material is recorded as w b , then w b Selected from the range of 0.5% to 99.5%, optionally selected from the range of 5% to 98%.

[0275] When the content of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density and / or a longer service life.

[0276] In some embodiments, the powder compaction density P1 of the first positive electrode active material at 30000N is 1.89 g / cm 3 Above, optional 1.95g / cm 3 Above, 1.98g / cm2 is optional 3 Above, further optional 2.0g / cm 3 Above, further optional 2.2g / cm 3 Above, further optionally 2.2 g / cm 3 Above and 2.8g / cm 3 Below or 2.2g / cm 3 Above and 2.65g / cm 3 the following.

[0277] In some embodiments, the powder compaction density P2 of the second positive electrode active material at 30000N is greater than or equal to 2.90 g / cm 3 , can be selected as greater than or equal to 3.1g / cm 3 , more preferably greater than or equal to 3.3 g / cm 3 .

[0278] When the powder compaction density of the first positive electrode active material and / or the second positive electrode active material is within the above range, the battery can have a higher energy density.

[0279] In some embodiments, the BET specific surface area of ​​the second positive electrode active material is less than or equal to 1.73 m 2 / g, can be selected to be less than or equal to 1.5m 2 / g, 0.28m 2 / g to 1.5m 2 / g. This can reduce side reactions and improve the cycle performance of the battery.

[0280] The specific surface area of ​​a material is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured by nitrogen adsorption specific surface area analysis test method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The test instrument can be the Tri-Star 3020 specific surface area pore size analysis tester from Micromeritics, USA.

[0281] The powder compaction density of the material (eg, the first positive electrode active material, the second positive electrode active material, etc.) can be measured according to GB / T24533-2009.

[0282] The volume distribution particle sizes Dv10 and Dv50 of materials (such as the first positive electrode active material, the second positive electrode active material, etc.) have well-known meanings in the art, which respectively represent the particle sizes corresponding to the cumulative volume distribution percentages of the materials reaching 10% and 50%, and can be measured using instruments and methods known in the art. For example, it can be measured with a laser particle size analyzer with reference to GB / T 19077-2016. The test instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK. Deionized water can be used as the solvent for the test, and the material can be ultrasonically treated for 5 minutes before the test.

[0283] The particle size distribution curve of the positive electrode active material composition can be measured with reference to GB / T 19077-2016 using a laser particle size analyzer. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK. Deionized water can be used as the solvent during the test, and the material can be ultrasonically treated for 5 minutes before the test.

[0284] In some embodiments, the first positive electrode active material includes a compound represented by formula (I),

[0285] Li a A x Mn 1-y M 1 y P 1-z M 2 zO 4-n D n (I)

[0286] A includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; M 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; M 2 It includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D includes one or more elements selected from Group VIA and Group VIIA; a is selected from the range of 0.85 to 1.15; x is selected from the range of 0 to 0.1; y is selected from the range of 0.001 to 0.999; z is selected from the range of 0 to 0.5; and n is selected from the range of 0 to 0.5.

[0287] Unless otherwise specified, in the above chemical formula, when A is more than two elements, the above limitation on the numerical range of x is not only a limitation on the stoichiometric number of each element as A, but also a limitation on the sum of the stoichiometric numbers of each element as A. For example, when A is more than two elements A1, A2...An, the stoichiometric numbers x1, x2...xn of A1, A2...An each need to fall within the numerical range of x defined in the present application, and the sum of x1, x2...xn also needs to fall within the numerical range.

[0288] Similarly, for other symbols mentioned in the embodiments of the present application (such as B, C, D, M, M', X, Z, P, Q, A 1 , B 1 , C 1 , D 1 , A 2 , B 2 , A 3 , A 4 When there are two or more elements (such as ), the numerical range of the stoichiometric number in the present application also has the above meaning.

[0289] The first positive electrode active material is obtained by element doping in the compound LiMnPO4, wherein A, M 1 , C and M 2 They are the elements doped at the Li, Mn, P and O positions of the compound LiMnPO4. Without wishing to be bound by theory, it is now believed that the performance improvement of lithium manganese phosphate is related to reducing the lattice change rate of lithium manganese phosphate during lithium insertion and extraction and reducing surface activity. Reducing the lattice change rate can reduce the lattice constant difference between the two phases at the grain boundary, reduce the interface stress, and enhance Li +The transmission capacity at the interface improves the rate performance of the first positive electrode active material. However, high surface activity can easily lead to serious side reactions at the interface, aggravating gas production, electrolyte consumption and interface damage, thereby affecting the cycle performance of the battery. The lattice change rate can be reduced by doping at Li and / or Mn positions. Mn doping can also effectively reduce surface activity, thereby reducing Mn dissolution and side reactions at the interface between the first positive electrode active material and the electrolyte. P-position doping makes the change rate of the Mn-O bond length faster, reduces the migration barrier of the small polaron of the material, and is beneficial to improve the electronic conductivity. O-position doping has a good effect on reducing side reactions at the interface. P-position and / or O-position doping also affects the Mn dissolution and kinetic properties of anti-site defects. Therefore, doping reduces the concentration of anti-site defects in the material, improves the kinetic properties and gram capacity of the material, and can also change the morphology of the particles, thereby improving the compaction density. The inventors unexpectedly discovered that by doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping element at the Mn position, obtaining improved cycle performance and / or high temperature stability, and the gram capacity and compaction density of the material are also improved.

[0290] In some embodiments, A includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; and / or,

[0291] M 1 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; and / or,

[0292] M 2 comprising one or more elements selected from B (boron), S, Si and N; and / or,

[0293] D includes one or more elements selected from S, F, Cl and Br.

[0294] In some embodiments, A includes any one element selected from Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include any one element selected from Mg and Nb; and / or,

[0295] M 1 comprising one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and optionally comprising at least two elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and more optionally comprising at least two elements selected from Fe, Ti, V, Ni, Co and Mg, and further optionally comprising at least two elements selected from Fe, Ti, V, Co and Mg, and further optionally comprising Fe and one or more elements selected from Ti, V, Co and Mg; and / or,

[0296] M 2 comprising any one element selected from B (boron), S, Si and N, optionally S; and / or,

[0297] D includes any one element selected from S, F, Cl and Br, and may be F.

[0298] By selecting the Li-position doping element within the above range, the lattice change rate during the delithiation process can be further reduced, thereby further improving the rate performance of the battery. By selecting the Mn-position doping element within the above range, the electronic conductivity can be further improved and the lattice change rate can be further reduced, thereby improving the rate performance and gram capacity of the battery. By selecting the P-position doping element within the above range, the rate performance of the battery can be further improved. By selecting the O-position doping element within the above range, the side reactions of the interface can be further reduced and the high temperature performance of the battery can be improved.

[0299] In some embodiments, a is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or,

[0300] x is selected from the range of 0.001 to 0.005; and / or,

[0301] y is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or,

[0302] z is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, more optionally selected from the range of 0.001 to 0.005; and / or,

[0303] n is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.

[0304] By selecting the y value within the above range, the gram capacity and rate performance of the first positive electrode active material can be further improved. By selecting the x value within the above range, the kinetic performance of the first positive electrode active material can be further improved. By selecting the z value within the above range, the rate performance of the battery can be further improved. By selecting the n value within the above range, the high temperature performance of the battery can be further improved.

[0305] In some embodiments, x is 0, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.5, and n is 0; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0.

[0306] Therefore, by doping a specific element in a specific amount at the Mn position of the compound LiMnPO4 and optionally at the Li position, P position and / or O position, especially doping a specific element in a specific amount at the Mn position and P position of LiMnPO4 or at the Li position, Mn position, P position and O position of LiMnPO4, it is possible to improve the rate performance, reduce the dissolution of Mn and the doping element at the Mn position, improve the cycle performance and / or high temperature stability, and increase the gram capacity and compaction density of the first positive electrode active material.

[0307] In some embodiments, y:z is selected from the range of 0.002 to 999, and may be selected from the range of 0.025 to 999 or the range of 0.002 to 500, and may be selected from the range of 0.2 to 600, such as 0.2, 0.25, 1, 2, 3, 4, 5, 6, 8, 10, 12, 13, 15, 17, 20, 70, 80, 84, 67, 91, 100, 134, 150, 182, 200, 250, 300, 320, 350, 400, 420, 450, 500, 600, 999 or a range consisting of any two of the above values. Thus, the defects of the first positive electrode active material can be reduced, and the integrity of the framework structure of the first positive electrode active material can be improved, thereby effectively improving the structural stability of the first positive electrode active material, and then improving the cycle stability of the battery.

[0308] In some embodiments, z:n is selected from the range of 0.002 to 500, and may be selected from the range of 0.2 to 100, and may be selected from the range of 0.2 to 50, such as 0.2, 0.8, 1, 1.25, 4, 5, 50, or a range consisting of any two of the above values. Thus, the defects of the first positive electrode active material can be further reduced, the integrity of the framework structure of the first positive electrode active material can be further improved, the structural stability of the first positive electrode active material can be effectively improved, and the cycle stability of the battery can be improved.

[0309] In some embodiments, (1-y):y is in the range of 0.1-999, optionally in the range of 0.1-10 or in the range of 0.67-999, more optionally in the range of 1 to 10, further optionally in the range of 1 to 4, and further optionally in the range of 1.5 to 3; and / or, a:x is in the range of 1 to 1200, optionally in the range of 9 to 1100, and more optionally in the range of 190-998.

[0310] Here, y represents the sum of the stoichiometric numbers of the doping elements at the Mn position. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.

[0311] In some embodiments, z:(1-z) is 1:9 to 1:999, and can be 1:499 to 1:249. When the above conditions are met, the energy density and cycle performance of the first positive electrode active material can be further improved.

[0312] In some embodiments, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo, and W; M 1 Includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; M 2 It includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.1.

[0313] By doping specific elements in specific amounts at the Li position, Mn position, P position and O position of the compound LiMnPO4 at the same time, improved rate performance can be obtained, while reducing the dissolution of Mn and the doping elements at the Mn position, thereby obtaining improved cycle performance and / or high temperature stability, and the gram capacity and compaction density of the first positive electrode active material can also be improved.

[0314] In some embodiments, M 1It includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and may optionally include one or more elements selected from the group consisting of Zn, Fe, Ti, V, Ni, Co and Mg; M 2 It includes one or more elements selected from B (boron), Si, N and S; a is selected from the range of 0.9 to 1.1, x is 0, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is 0.

[0315] By doping specific elements at specific amounts at both the Mn and P positions of the compound LiMnPO4, the rate performance can be improved, the dissolution of Mn and the doping elements at the Mn position can be reduced, the cycle performance and / or high temperature stability can be improved, and the gram capacity and compaction density of the first positive electrode active material can be increased.

[0316] In some embodiments, the first positive electrode active material includes a core and a shell coating the core, wherein the core includes the compound represented by the above formula (I). The shell includes one or more coating layers. Each coating layer has ionic conductivity and / or electronic conductivity. In practice, each coating layer may be completely coated or partially coated.

[0317] By arranging a coating layer with ionic conductivity and / or electronic conductivity on the surface of the inner core, a first positive electrode active material with a core-shell structure is provided. Applying the first positive electrode active material to a battery can improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.

[0318] In some embodiments, one or more coating layers each independently include one or more selected from the group consisting of pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer.

[0319] In some embodiments, the shell comprises a coating; optionally, the coating comprises one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.

[0320] The above materials can be used to obtain a coating layer with ionic conductivity and / or electronic conductivity, thereby improving the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.

[0321] In some embodiments, the shell includes a first coating layer coating the inner core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.

[0322] Using the above materials as the materials for the coating layer and providing two coating layers can further improve the high temperature cycle performance, cycle stability and high temperature storage performance of the battery.

[0323] In some embodiments, the first coating layer includes one or more selected from pyrophosphate, phosphate, oxide, and boride, and the second coating layer includes one or more selected from carbon and doped carbon.

[0324] The use of a first coating layer of a specific material and a second coating layer of a specific material can further improve the rate performance and further reduce the dissolution of Mn and Mn-doped elements, thereby improving the cycle performance and / or high temperature stability of the battery.

[0325] In some embodiments, the shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; optionally, the first coating layer, the second coating layer, and the third coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride, and polymer. "Polymer" can be either an oligomer or a polymer, and the embodiments of the present application are not limited to this.

[0326] Using the above materials as the materials for the coating layer and providing three layers of coating layers can further reduce the dissolution of Mn and Mn-doped elements, and further improve the high-temperature cycle performance, cycle stability and high-temperature storage performance of the battery.

[0327] In some embodiments, the first coating layer includes pyrophosphate, the second coating layer includes one or more selected from phosphates, oxides, and borides, and the third coating layer includes one or more selected from carbon and doped carbon.

[0328] The use of a first coating layer of a specific material, a second coating layer of a specific material, and a third coating layer of a specific material further improves the rate performance, further reduces the dissolution of Mn and Mn-doping elements, thereby improving the battery's cycle performance and / or high temperature stability, and further increases the gram capacity and compaction density of the first positive electrode active material.

[0329] In some embodiments, the pyrophosphate is b (P2O7) c and / or,

[0330] Phosphate is X m (PO4) q and / or,

[0331] The doping element in the doped carbon includes one or more elements selected from Group IIIA, Group VA, Group VIA and Group VIIA; and / or,

[0332] Oxide is M'd O e and / or,

[0333] Boride is Z v B w and / or,

[0334] The polymer includes one or more selected from polysaccharides and their derivatives, and polysiloxanes;

[0335] M, X and Z each independently include one or more elements selected from Group IA, Group IIA, Group IIIA, Group IB, Group IIB, Group IVB, Group VB, Group VIIB and Group VIII;

[0336] b is selected from the range of 1 to 4, c is selected from the range of 1 to 6; m is selected from the range of 1 to 2, q is selected from the range of 1 to 4;

[0337] M′ comprises one or more elements selected from alkali metals, alkaline earth metals, transition metals, Group IIIA elements, Group IVA elements, lanthanides and Sb;

[0338] d is greater than 0 and less than or equal to 2, e is greater than 0 and less than or equal to 5;

[0339] v is selected from the range of 1-7, and w is selected from the range of 1-2.

[0340] By using the above materials as the coating layer, the dissolution of Mn and Mn-doping elements can be further reduced, the gram capacity and compaction density of the first positive electrode active material can be further increased, and the rate performance, high-temperature cycle performance and high-temperature storage performance of the battery can be further improved.

[0341] In some embodiments, M, X and Z each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, Mn and Al; and / or,

[0342] The doping element in the doped carbon includes one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine; and / or,

[0343] M′ comprises one or more elements selected from Li, Be, B, Na, Mg, Al, Si, P, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, W, La and Ce, and may optionally comprise one or more elements selected from Mg, Al, Si, Zn, Zr and Sn; and / or

[0344] The polysiloxane is selected from one or more of linear polysiloxane and cyclic polysiloxane; and / or,

[0345] The polysaccharide is selected from one or more of plant polysaccharides and marine polysaccharides.

[0346] By using the above-mentioned specific material as the coating layer, the dissolution of Mn and Mn-doped elements can be further reduced, and the high-temperature cycle performance and high-temperature storage performance of the battery can be further improved.

[0347] In some embodiments, the first positive electrode active material includes a core and a shell covering the core.

[0348] The kernel includes Li a Mn 1-y M 1 y P 1-z M 2 z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, M 1 The M 2 Includes one or more elements selected from B (boron), S, Si and N.

[0349] The shell includes a first coating layer coating the inner core and a second coating layer coating the first coating layer, the first coating layer includes pyrophosphate MP2O7 and phosphate XPO4, M and X each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; the second coating layer contains carbon.

[0350] The first positive electrode active material may be a core-shell structure having two coating layers, and the element M doped at the manganese position of the lithium manganese phosphate 1 It helps to reduce the lattice change rate of lithium manganese phosphate during lithium insertion and extraction, improve the structural stability of the first positive electrode active material, greatly reduce the dissolution of manganese and reduce the oxygen activity on the particle surface. 2It helps to change the difficulty of the change of the Mn-O bond length, thereby reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the rate performance of the battery. The first coating layer of the first positive electrode active material includes pyrophosphate and phosphate. Since the migration barrier of transition metals in pyrophosphate is relatively high (>1eV), the dissolution of transition metals can be effectively reduced. Phosphates have excellent lithium ion conductivity and can reduce the surface impurity lithium content. In addition, since the second coating layer is a carbon-containing layer, it can effectively improve the conductivity and desolvation ability of LiMnPO4. In addition, the "barrier" effect of the second coating layer can further reduce the migration of manganese ions into the electrolyte and reduce the corrosion of the electrolyte to the second active material. Therefore, by performing specific element doping and surface coating on lithium manganese phosphate, the dissolution of Mn in the process of lithium insertion and extraction can be effectively reduced, while promoting the migration of lithium ions, thereby improving the rate performance of the battery and improving the cycle performance and high temperature performance of the battery.

[0351] In some embodiments, the first positive electrode active material includes a core and a shell covering the core.

[0352] The kernel includes Li a Mn 1-y M 1 y P 1-z M 2 z O4, a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, M 1 The M 2 Includes one or more elements selected from B (boron), S, Si and N.

[0353] The shell includes a first coating layer coating the inner core, a second coating layer coating the first coating layer, and a third coating layer coating the second coating layer.

[0354] The first coating layer includes pyrophosphate Li f QP2O7 and / or Q g (P2O7) h , 0≤f≤2, 1≤g≤4, 1≤h≤6, pyrophosphate Li f QP2O7 and / or Q g (P2O7) h The Qs in each independently include one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al.

[0355] The second coating layer includes crystalline phosphate XPO4, and X includes one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al.

[0356] The third coating layer includes carbon.

[0357] The first positive electrode active material is a core-shell structure, wherein the manganese site and phosphorus site of the core are doped with elements M 1 and element M 2 , which can not only effectively reduce manganese dissolution, thereby reducing manganese ions migrating to the negative electrode, reducing the electrolyte consumed by SEI film decomposition, and improving the battery's cycle performance, but also promote Mn-O bond adjustment, reduce lithium ion migration barriers, promote lithium ion migration, and improve the battery's rate performance; by coating the core with a first coating layer including pyrophosphate, the migration resistance of manganese can be further increased, its dissolution can be reduced, and the surface impurity lithium content and the contact between the core and the electrolyte can be reduced, thereby reducing interfacial side reactions and gas production, and improving the battery's high-temperature storage performance and cycle performance; by further coating with a phosphate coating layer with excellent lithium ion conductivity, the interfacial side reactions on the surface of the first positive electrode active material can be effectively reduced, thereby improving the battery's high-temperature cycle and storage performance; by further coating with a carbon layer as the third coating layer, the battery's kinetic performance can be further improved. In addition, in the core, the element M doped at the manganese position 1 It also helps to reduce the lattice change rate of lithium manganese phosphate during the process of lithium insertion and extraction, improve the structural stability of the first positive electrode active material, greatly reduce the dissolution of manganese and reduce the oxygen activity on the particle surface; the element M doped at the phosphorus position 2 It also helps to change the difficulty of the Mn-O bond length change, thereby improving electronic conductivity and reducing the lithium ion migration barrier, promoting lithium ion migration, and improving the battery's rate performance.

[0358] In addition, the entire core system maintains electrical neutrality, which can minimize defects and impurities in the first positive electrode active material. If there is an excess of transition metal (such as manganese) in the first positive electrode active material, since the material system itself has a relatively stable structure, the excess transition metal is likely to precipitate in the form of a single substance or form an impurity phase inside the lattice. Maintaining electrical neutrality can minimize such impurities. In addition, making the system electrically neutral can also generate lithium vacancies in the material in some cases, thereby making the kinetic performance of the first positive electrode active material more excellent.

[0359] In some embodiments, the one or more coating layers in the shell that are farthest from the core each independently include one or more selected from polysiloxane, polysaccharide, and polysaccharide derivatives.

[0360] As a result, the uniformity of the coating can be improved, and the interfacial side reactions caused by high voltage can be effectively blocked, thereby improving the high-temperature cycle performance and high-temperature storage performance of the first positive electrode active material; and the coating layer has good ionic conductivity, which helps to improve the gram capacity of the first positive electrode active material while reducing the heat generation of the battery.

[0361] In some embodiments, the polysiloxane comprises a structural unit represented by the following formula (i):

[0362]

[0363] R1 and R2 are independently selected from H, -COOH, -OH, -SH, -CN, -SCN, amino, phosphate, carboxylate, amide, aldehyde, sulfonyl, polyether segment, C1-C20 aliphatic, C1-C20 halogenated aliphatic, C1-C20 heteroaliphatic, C1-C20 halogenated heteroaliphatic, C6-C20 aromatic, C6-C20 halogenated aromatic, C2-C20 heteroaromatic and C2-C20 halogenated heteroaromatic;

[0364] Optionally, R1 and R2 are independently selected from H, amino, phosphate, polyether segment, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl and C2-C8 haloalkenyl.

[0365] In some embodiments, the polysiloxane further comprises an end-capping group, which includes one or more of the following functional groups: polyether, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl, C2-C8 haloalkenyl, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy, C2-C8 epoxy, hydroxyl, C1-C8 hydroxyalkyl, amino, C1-C8 aminoalkyl, carboxyl, C1-C8 carboxylalkyl.

[0366] In some embodiments, the polysiloxane includes polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl functionalized polysiloxane, epoxy-terminated polysiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, polymethylchloropropylsiloxane, hydroxy-terminated polydimethylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, aminoethylaminopropyl polydimethylsiloxane, terminal polyether polydimethylsiloxane, side chain aminopropyl polysiloxane, One or more of aminopropyl-terminated polydimethylsiloxane, side chain phosphate grafted polydimethylsiloxane, side chain polyether grafted polydimethylsiloxane, 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, cyclic polymethylvinylsiloxane, hexadecylcyclooctasiloxane, tetradecamethylcycloheptasiloxane, and cyclic polydimethylsiloxane.

[0367] In some embodiments, the number average molecular weight of polysiloxane, polysaccharide and polysaccharide derivative is independently below 300,000, optionally 10,000 to 200,000, more optionally 20,000 to 120,000, further optionally 400 to 80,000.

[0368] The number average molecular weight of polysiloxane, polysaccharide and polysaccharide derivatives can be measured by methods known in the art, such as gel permeation chromatography (GPC). The testing instrument can be a PL-GPC 220 high temperature gel permeation chromatograph.

[0369] In some embodiments, the mass percentage of polar functional groups in the polysiloxane is α, 0≤α<50%, optionally, 5%≤α≤30%.

[0370] "The mass percentage of polar functional groups in polysiloxane" refers to the mass proportion of polar functional groups in R1, R2 and end groups in polysiloxane. Polar functional groups include -COOH, -OH, -SH, -CN, -SCN, amino groups (including -NH2, -NH-), phosphate groups, carboxylate groups (-COO-), amide groups (-CONH-), aldehyde groups (-CHO), sulfonyl groups (-S(=O)2-), polyether segments, halogens, alkoxy groups, and epoxy groups. One or more of the following. When the above polar functional groups are directly connected to silicon atoms, α means the mass fraction of these polar functional groups in polysiloxane; when the above polar functional groups are not directly connected to silicon atoms, α means the sum of the mass fractions of polar functional groups and divalent to tetravalent methyl groups (such as -CH2, -CH-, -C-, etc.) directly connected thereto in polysiloxane, where "divalent to tetravalent methyl groups" means carbon atoms directly connected to polar functional groups and located between polar functional groups and silicon atoms, as well as other non-polar functional groups connected to carbon atoms. Taking polymethyltrifluoropropylsiloxane as an example, α means the mass percentage of -CF3 therein, excluding ethylene therein; taking polymethylchloropropylsiloxane as an example, α means the mass percentage of -CH2Cl, excluding ethylene therein; taking hydroxypropyl-terminated polydimethylsiloxane as an example, α means the mass percentage of -CH2OH. The mass percentage of polar functional groups in the polysiloxane can be determined by methods known in the art, such as titration (eg, acid-base titration, redox titration, precipitation titration), infrared spectroscopy, and nuclear magnetic resonance spectroscopy.

[0371] In some embodiments, the substituents attached to the sugar units in the polysaccharides and polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH and its salts, -R-OH, -SO3H and its salts, -R-OH, -R-SO3H and its salts, sulfate, alkoxy, R represents an alkylene group, optionally representing a C1 to C5 alkylene group.

[0372] Optionally, the substituents attached to the sugar units in the polysaccharides and polysaccharide derivatives each independently include one or more of the group consisting of the following functional groups: -OH, -COOH, -COOLi, -COONa, -COOK, -SO3H, -SO3Li, -SO3Na, -SO3K, -CH2-SO3H, -CH2-SO3Li, -CH2-SO3Na, -CH2-SO3K, methoxy, ethoxy.

[0373] The term "substituents attached to the sugar unit" includes all groups attached to the sugar unit backbone.

[0374] In some embodiments, the polysaccharide includes one or more selected from pectin, carboxymethyl starch, hydroxypropyl starch, dextrin, cellulose ether, carboxymethyl chitosan, hydroxyethyl cellulose, carboxymethyl cellulose, carboxypropyl methyl cellulose, guar gum, sesbania gum, gum arabic, lithium alginate, sodium alginate, potassium alginate, fucoidan, agar, carrageenan, carrageenan, xanthan gum and fenugreek gum.

[0375] In some embodiments, the mass percentage of the substituents attached to the sugar units in the polysaccharide and polysaccharide derivatives is independently 20% to 85%, and optionally 30% to 78%. The mass percentage of the substituents attached to the sugar units in the polysaccharide and polysaccharide derivatives can be determined by methods known in the art, such as titration (e.g., acid-base titration, redox titration, precipitation titration), infrared spectroscopy, and nuclear magnetic resonance spectroscopy.

[0376] In some embodiments, the lattice mismatch between the material of the core and the material of the shell is less than 10%, thereby enabling good contact between the core and the shell (or coating layer) to prevent the shell (or coating layer) from falling off.

[0377] In some embodiments, based on the weight of the positive electrode active material,

[0378] The manganese content is in the range of 10 wt% to 35 wt%, optionally in the range of 13.3 wt% to 33.2 wt%, more optionally in the range of 15 wt% to 30 wt%, further optionally in the range of 17 wt% to 20 wt%; and / or,

[0379] The phosphorus content is in the range of 12 wt% to 25 wt%, optionally in the range of 15 wt% to 20 wt%, and more optionally in the range of 16.8 wt% to 19.5 wt%; and / or,

[0380] The weight ratio of manganese element to phosphorus element ranges from 0.71 to 1.85, and can be selected from 0.90 to 1.25, and more preferably from 0.95 to 1.20.

[0381] In the case where manganese is contained only in the core of the first positive electrode active material, the content of manganese may correspond to the content of the core.

[0382] Limiting the content of manganese within the above range can further improve the stability and density of the first positive electrode active material, thereby improving the battery's cycling, storage and compaction properties; and can maintain a higher voltage platform, thereby improving the battery's energy density.

[0383] Limiting the content of phosphorus within the above range can effectively reduce the influence of small polaron conductivity on the conductivity of the first positive electrode active material, and can further improve the stability of the lattice structure, thereby improving the overall stability of the first positive electrode active material.

[0384] Limiting the weight ratio of manganese to phosphorus within the above range can further reduce manganese dissolution, improve the stability and gram capacity of the first positive electrode active material, and improve the cycle performance and storage performance of the battery; it can also reduce impurities, enable the first positive electrode active material to maintain a higher discharge voltage platform, and enable the battery to have a high energy density.

[0385] The measurement of manganese and phosphorus can be carried out by conventional technical means in the art. In particular, the following method is used to determine the content of manganese and phosphorus: the material is dissolved in dilute hydrochloric acid (concentration 10-30%), the content of each element in the solution is tested by ICP, and then the content of manganese is measured and converted to obtain its weight percentage.

[0386] In some embodiments, the surface of the first positive electrode active material is coated with one or more of carbon and doped carbon; alternatively, the surface of the first positive electrode active material is coated with carbon, thereby improving the conductivity of the first positive electrode active material.

[0387] In some embodiments, the doping element in the doped carbon includes one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine, so as to facilitate the control of the performance of the doped carbon layer.

[0388] In some embodiments, the coating amount of the shell (only one coating layer) is 0.1 wt % to 6 wt %, based on the weight of the core. The coating amount of the coating layer is preferably within the above range, which can fully coat the core and further improve the kinetic performance of the battery without sacrificing the gram capacity of the first positive electrode active material.

[0389] In some embodiments, the coating amount of the first coating layer is greater than 0 and less than or equal to 7% by weight, optionally greater than 0 and less than or equal to 6% by weight, more optionally greater than 0 and less than or equal to 5.5% by weight or 4-5.6% by weight, further optionally greater than 0 and less than or equal to 2% by weight, based on the weight of the kernel; and / or,

[0390] The coating amount of the second coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, and more optionally 2-4% by weight or 3-5% by weight, based on the weight of the kernel; and / or,

[0391] The coating amount of the third coating layer is greater than 0 and less than or equal to 6 wt %, optionally greater than 0 and less than or equal to 5.5 wt %, and more optionally greater than 0 and less than or equal to 2 wt %, based on the weight of the core.

[0392] In some embodiments, the shell further includes a fourth coating layer coating the third coating layer and a fifth coating layer coating the fourth coating layer.

[0393] The coating amounts of the fourth coating layer and the fifth coating layer are each independently 0.01 to 10 wt %, optionally 0.05 to 10 wt %, more optionally 0.1 to 5 wt %, further 0.1 to 2 wt %, based on the weight of the core.

[0394] The coating amount of each coating layer is preferably within the above range, so that the core can be fully coated and the kinetic performance of the battery can be further improved without sacrificing the gram capacity of the first positive electrode active material.

[0395] In some embodiments, the shell is located on 40% to 90% of the surface of the core, and optionally 60% to 80% of the surface, thereby being able to fully coat the core, thereby improving the dynamic performance of the battery.

[0396] In some embodiments, the shell (which is just one coating layer) has a thickness of 1-15 nm.

[0397] In some embodiments, the thickness of the first coating layer is 1-10 nm, optionally 2-10 nm; and / or,

[0398] The thickness of the second coating layer is 2-25 nm, optionally 2-15 nm, more optionally 3-15 nm; and / or,

[0399] The thickness of the third cladding layer is 2-25 nm, and can be 5-25 nm.

[0400] In some embodiments, the thickness of the first coating layer can be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, or about 10 nm, or any range thereof.

[0401] In some embodiments, the thickness of the second coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, or within any range of the above values.

[0402] In some embodiments, the thickness of the third coating layer may be about 2nm, about 3nm, about 4nm, about 5nm, about 6nm, about 7nm, about 8nm, about 9nm, about 10nm, about 11nm, about 12nm, about 13nm, about 14nm, about 15nm, about 16nm, about 17nm, about 18nm, about 19nm, about 20nm, about 21nm, about 22nm, about 23nm, about 24nm or about 25nm, or within any range of any of the above values.

[0403] The first coating layer has the above thickness range, which can further reduce the adverse effect on the kinetic properties of the first positive electrode active material.

[0404] The second coating layer has the above-mentioned thickness range, so that the surface structure of the second coating layer is stable and the side reaction with the electrolyte is small, so the interface side reaction can be effectively reduced, thereby improving the high temperature performance of the battery.

[0405] The third coating layer has the above-mentioned thickness range, which can enhance the conductivity of the first positive electrode active material and improve the compaction density of the positive electrode sheet prepared using the first positive electrode active material.

[0406] The thickness test of the coating layer is mainly carried out by FIB. The specific method may include the following steps: randomly selecting a single particle from the first positive electrode active material powder to be tested, cutting a thin slice with a thickness of about 100nm from the middle position or near the middle position of the selected particle, and then performing TEM test on the thin slice, measuring the thickness of the coating layer, measuring 3-5 positions, and taking the average value.

[0407] In some embodiments, the one or more coating layers each independently include one or more selected from pyrophosphate, phosphate, and oxide, and the one or more selected from pyrophosphate, phosphate, and oxide is crystalline.

[0408] Optionally, the crystallinity of the pyrophosphate, phosphate and oxide is each independently from 10% to 100%, more preferably from 50% to 100%.

[0409] Herein, crystalline means that the crystallinity is above 50%, i.e., 50%-100%. That is, when the crystalline pyrophosphate and crystalline phosphate of the present application appear, it means that the crystallinity is 50% to 100%.

[0410] Pyrophosphates and phosphates with a certain degree of crystallinity are not only conducive to fully utilizing the pyrophosphate coating to reduce manganese dissolution and the phosphate coating's excellent ability to conduct lithium ions and reduce interface side reactions, but also enable the pyrophosphate coating and the phosphate coating to better lattice match, thereby achieving a close bond between the coatings.

[0411] It should be noted that the crystallinity can be adjusted by adjusting the process conditions of the sintering process, such as the sintering temperature, the sintering time, etc. The crystallinity can be measured by methods known in the art, such as X-ray diffraction, density method, infrared spectroscopy, differential scanning calorimetry, and nuclear magnetic resonance absorption method. A specific method for testing the crystallinity of the first positive electrode active material by X-ray diffraction method may include the following steps:

[0412] Take a certain amount of the first positive electrode active material powder and measure the total scattering intensity by X-ray. It is the sum of the scattering intensities of all matter in space and is only related to the intensity of the primary rays, the chemical structure of the first positive electrode active material powder, and the total number of electrons participating in the diffraction, i.e. the mass, but has nothing to do with the order state of the sample. Then separate the crystalline scattering and the non-crystalline scattering from the diffraction pattern, and the degree of crystallinity is the ratio of the scattering of the crystalline part to the total scattering intensity.

[0413] In some embodiments, in the shell, the weight ratio of pyrophosphate to phosphate and the weight ratio of pyrophosphate to oxide are independently 1:3 to 3:1, and can be 1:3 to 1:1. Thus, by having pyrophosphate and phosphate in a suitable weight ratio range or pyrophosphate and oxide in a suitable weight ratio range, manganese dissolution can be effectively reduced, surface impurity lithium content can be effectively reduced, and interface side reactions can be reduced, thereby improving the high temperature storage performance and high temperature cycle performance of the battery.

[0414] In some embodiments, one or more coating layers independently include carbon, and the carbon is a mixture of SP2 carbon and SP3 carbon. Optionally, the molar ratio of SP2 carbon to SP3 carbon in the carbon is any value in the range of 0.07-13, and can be any value in the range of 0.1-10, and can be any value in the range of 2.0-3.0.

[0415] In some embodiments, the molar ratio of SP2 carbon to SP3 carbon may be about 0.1, about 0.2, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, or about 10, or any range of any of the above values.

[0416] In the present application, "about" a certain numerical value indicates a range, which means a range of ±10% of the numerical value.

[0417] By selecting the form of carbon in the carbon coating, the comprehensive electrical performance of the battery can be improved. Specifically, by using a mixed form of SP2 carbon and SP3 carbon and limiting the ratio of SP2 carbon to SP3 carbon within a certain range, the following situations can be avoided: if the carbon in the coating is all amorphous SP3, the conductivity is poor; if it is all graphitized SP2, although the conductivity is good, there are few lithium ion pathways, which is not conducive to lithium deintercalation. In addition, limiting the molar ratio of SP2 carbon to SP3 carbon within the above range can not only achieve good conductivity, but also promote the transmission of lithium ions, which is beneficial to the realization of battery functions and its cycle performance.

[0418] The mixing ratio of the SP2 form and the SP3 form of carbon can be controlled by sintering conditions such as sintering temperature and sintering time. The molar ratio of SP2 form carbon to SP3 form carbon can be measured by Raman spectroscopy. The specific test method is as follows: by peak separation of the energy spectrum of the Raman test, Id / Ig (where Id is the peak intensity of the SP3 form carbon, and Ig is the peak intensity of the SP2 form carbon) is obtained to confirm the molar ratio of the two.

[0419] In some embodiments, one or more coating layers independently include doped carbon, and the mass content of the doped element in the doped carbon is less than 30%; optionally, the mass content of the doped element in the doped carbon is less than 20%. The doping element within the above content range can not only fully improve the conductivity of the pure carbon layer, but also effectively avoid excessive surface activity caused by excessive doping of the doping element, thereby effectively controlling the interface side reaction caused by excessive doping of the coating layer.

[0420] In some embodiments, one or more coating layers each independently include doped carbon, wherein the doped carbon

[0421] The doping element is nitrogen and / or sulfur, and the mass content of the doping element in the doped carbon is 1% to 15%; or,

[0422] The doping element is phosphorus, boron and / or fluorine, and the mass content of the doping element in the doped carbon is 0.5% to 5%;

[0423] Optionally, the doping element is nitrogen, phosphorus, sulfur, boron or fluorine.

[0424] Since nitrogen atoms and sulfur atoms are closer to the atomic radius of carbon atoms and are not easy to destroy the carbon skeleton, when the doping amount of nitrogen atoms and sulfur atoms is within the above relatively wide range, the conductivity of the doped carbon layer can be fully exerted, and the lithium ion transmission and lithium ion desolvation ability can be promoted.

[0425] Since the atomic radius of phosphorus atoms, boron atoms and / or fluorine atoms is different from that of carbon atoms, excessive doping can easily destroy the carbon skeleton. Therefore, when the doping amount of phosphorus atoms, boron atoms and / or fluorine atoms is within the relatively small range mentioned above, the conductivity of the doped carbon layer can be fully exerted, and the lithium ion transmission and lithium ion desolvation capabilities can be promoted.

[0426] In some embodiments, one or more coating layers independently include pyrophosphate, the interplanar spacing of the pyrophosphate is in the range of 0.293-0.470 nm, optionally 0.297-0.462 nm or 0.293-0.326 nm, more optionally 0.300-0.310 nm, and the angle of the crystal direction (111) is in the range of 18.00°-32.57°, optionally 18.00°-32.00° or 26.41°-32.57°, more optionally 19.211°-30.846°, and further optionally 29.00°-30.00°; and / or,

[0427] The one or more coating layers independently include phosphate, the interplanar spacing of the phosphate is in the range of 0.244-0.425 nm, optionally 0.345-0.358 nm, and the angle of the crystal direction (111) is in the range of 20.00°-37.00°, optionally 24.25°-26.45°;

[0428] Optionally, the first coating layer or the second coating layer comprises a phosphate.

[0429] The first coating layer and the second coating layer in the first positive electrode active material are both made of crystalline materials, and their interplanar spacing and angle ranges are within the above ranges. Thus, the impurity phase in the coating layer can be effectively reduced, thereby improving the material's gram capacity, cycle performance, and rate performance.

[0430] In some embodiments, the lattice change rate of the first positive electrode active material before and after complete lithium deintercalation is less than 50%, optionally less than 9.8%, more optionally less than 8.1%, further optionally less than 7.5%, further optionally less than 6%, further optionally less than 4%, further optionally less than 3.8%, and further optionally less than 2.0-3.8%.

[0431] By reducing the lattice change rate, Li ion transmission can be made easier, that is, the mobility of Li ions in the first positive electrode active material is stronger, which is beneficial to improve the rate performance of the battery. The lattice change rate can be measured by methods known in the art, such as X-ray diffraction (XRD) patterns.

[0432] In some embodiments, the Li / Mn antisite defect concentration of the first positive electrode active material is less than 5.3%, optionally less than 5.1%, more optionally less than 4%, further optionally less than 2.2%, further optionally less than 2%, further optionally less than 1.5%-2.2% or less than 0.5%.

[0433] The so-called Li / Mn antisite defect refers to the Li + With Mn 2+ The positions of Li / Mn are interchanged. The Li / Mn antisite defect concentration refers to the number of Li / Mn antisite defects in the first positive electrode active material. 2+ Li exchange + Occupy + The percentage of total antisite defect Mn 2+ Will hinder Li + The transport of Li / Mn antisite defects can improve the gram capacity and rate performance of the first positive electrode active material by reducing the concentration of Li / Mn antisite defects. The concentration of Li / Mn antisite defects can be measured by methods known in the art, such as XRD.

[0434] In some embodiments, the surface oxygen valence state of the first positive electrode active material is below -1.55, optionally below -1.82, more optionally below -1.88, further optionally below -1.90 or -1.98 to -1.88, further optionally -1.98 to -1.89, further optionally -1.98 to -1.90.

[0435] By reducing the surface oxygen valence state, the interfacial side reaction between the first positive electrode active material and the electrolyte can be reduced, thereby improving the cycle performance and high temperature stability of the battery. The surface oxygen valence state can be measured by methods known in the art, such as by electron energy loss spectroscopy (EELS).

[0436] In some embodiments, the positive electrode active material composition satisfies 0.0004≤w a ×y×(3.4-V B )≤0.063, optionally, 0.0015≤w a ×y×(3.4-V B )≤0.045.

[0437] w a It represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition.

[0438] y is 1 mol of M in the compound represented by formula (I) 1 The molar amount of the element can be determined by inductively coupled plasma emission spectroscopy (ICP).

[0439] VB M in the compound represented by formula (I) 1 The voltage platform of the element, in V (volts). B The test can be performed as follows: at 25°C, let the battery stand for 10 minutes, and discharge it at 0.33C to the lower cut-off voltage; after standing for 10 minutes, charge the battery at a constant current of 0.33C to the upper cut-off voltage, and continue to charge at a constant voltage until the current is ≤0.05C; after standing for 10 minutes, discharge the battery at 0.33C to the lower cut-off voltage, and obtain the discharge capacity of the battery, which is recorded as C0; after standing for 10 minutes, charge the battery at a constant current of 0.04C0 to the upper cut-off voltage, and continue to charge at a constant voltage until the current is ≤0.05C0; after standing for 10 minutes, discharge the battery at 0.04C0 to the lower cut-off voltage, and obtain the discharge capacity of the battery, which is recorded as C1. A discharge differential capacity dQ / dV curve is drawn according to the discharge curve, and the peak less than 3.4V on the dQ / dV curve is taken as M 1 The peak of the element, the voltage corresponding to the peak is V B .

[0440] The battery is a battery including a positive electrode active material composition.

[0441] When the positive electrode active material composition further meets the above conditions, it is beneficial for the positive electrode sheet to have both high compaction density and high compaction density efficiency, and it is beneficial for the battery to have both high energy density and long service life.

[0442] In some embodiments, the second positive active material includes a layered oxide.

[0443] The second positive electrode active material has a high compaction density, but the cost is high and during the use of the battery, there are usually more side reactions and the crystal structure stability is relatively poor. By reasonably matching the above-mentioned first positive electrode active material with the second positive electrode active material, the actual stacking density of the positive electrode active material composition can be improved, the compaction density and compaction density efficiency of the positive electrode sheet can be improved, and the battery using the positive electrode active material composition can have a higher energy density and a longer service life.

[0444] In some embodiments, the second positive electrode active material includes a compound represented by formula (II),

[0445] Li a1 A 1 b1 Ni c1 Co d1 B 1 e1 C 1 f1 O 2-g1 D 1 g1 , (II)

[0446] A 1 Includes one or more elements selected from Group IA, Group IIA, Group VIII, Group VIB, and Group IIB; B 1 including Mn and / or Al; C 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group VIA, Group IIB, Group IIIB, Group IVB, Group VB, Group VIB, and Group VIII; D 1 It includes one or more elements selected from Group VIA and Group VIIA; a1 is selected from the range of 0.8 to 1.2; b1 is selected from the range of 0 to 0.2; c1 is selected from the range of 0 to 1; d1 is selected from the range of 0 to 1; e1 is selected from the range of 0 to 1; f1 is selected from the range of 0 to 0.1; g1 is selected from the range of 0 to 0.1; and c1+d1+e1+f1=1.

[0447] In some embodiments, A 1 including one or more elements selected from the group consisting of Na, K, Mg, Rb, Zn, and Zr; and / or,

[0448] C 1 including one or more elements selected from the group consisting of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Fe, Zn, Ba, Mo, V, Ce, Nb, Sb, Ta, Ge, Nb, Sc, Ba, B, S and Y, and optionally including one or more elements selected from the group consisting of Al, Ti, Zr, Nb, Sr, Sc, Sb, Y, Ba, B; and / or,

[0449] D 1 comprising one or more elements selected from N, S, F, Cl and Br, and optionally comprising S and / or F; and / or,

[0450] a1 is selected from the range of 0.9 to 1.1; and / or,

[0451] b1 is selected from the range of 0 to 0.1; and / or,

[0452] c1 is selected from the range of 0.314 to 0.990, and may be selected from the range of 0.500 to 0.990; and / or,

[0453] d1 is selected from the range of 0 to 0.320, and may be selected from the range of 0 to 0.150; and / or,

[0454] e1 is selected from the range of 0.001 to 0.450, and may be selected from the range of 0.005 to 0.4; and / or,

[0455] f1 is selected from the range of 0.001 to 0.1, and may be selected from the range of 0.001 to 0.05; and / or,

[0456] g1 is selected from the range of 0 to 0.01, and can be optionally selected from the range of 0.01 to 0.05.

[0457] In some embodiments, the second positive electrode active material includes a core and a shell coating the core, wherein the core includes a compound represented by formula (II); the shell includes one or more coating layers; and each coating layer has ionic conductivity and / or electronic conductivity.

[0458] In some embodiments, one or more coating layers each independently include one or more selected from phosphate, pyrophosphate, carbon, doped carbon, oxide, and fast ion conductor, and may optionally include one or more selected from phosphate, pyrophosphate, and oxide.

[0459] In some embodiments, one or more coating layers each independently include one or more elements selected from Al, Zr, Mg, Ba, Cd, Zn, Ti, Co, W, Y, Si, Sn, B, P, S, and C.

[0460] In some embodiments, the fast ion conductor includes Li 3x3 La 2 / 3-x3 M 2 a3 TiN 2 z3 O3、Li 2+2x4 Zn 1-x4 GeO4、LiM 3 2(PO4)3, one or more, M 2 Includes one or more elements selected from Ba, Sr, N 2 Includes one or more elements selected from Al, Zr, M 3 It is one or more elements selected from Zr, Ti, Ge, and Hf, 0.04≤x3≤0.167, 0≤a3≤1, 0≤z3≤1, and -0.3≤x4≤0.8.

[0461] In some embodiments, the shell of the second positive electrode active material includes a coating layer; optionally, the coating layer includes one or more selected from phosphate, pyrophosphate, and oxide.

[0462] In some embodiments, the shell of the second positive electrode active material includes a first coating layer coating the inner core and a second coating layer coating the first coating layer; optionally, the first coating layer and the second coating layer each independently include one or more selected from phosphates, pyrophosphates, and oxides.

[0463] Optionally, the first coating layer includes one or more selected from phosphates and oxides, and the second coating layer includes one or more selected from pyrophosphates and oxides. Optionally, the oxide in the first coating layer is an oxide of one or more elements selected from Al, Zr, Mg, Ti, Co, Y, Ba, and Cd. Optionally, the oxide in the second coating layer is an oxide of one or more elements selected from B, Sn, S, and P.

[0464] In some embodiments, the coating amount of the shell of the second positive active material is 0.005 wt % to 1 wt %, optionally 0.01 wt % to 0.5 wt %, based on the weight of the core.

[0465] In some embodiments, the shell of the second positive active material has a thickness of 2 nm to 200 nm, optionally 5 nm to 50 nm.

[0466] The first positive electrode active material and the second positive electrode active material may be prepared by a sintering method. The shells of the first positive electrode active material and the second positive electrode active material may be prepared by a liquid phase coating method.

[0467] [Positive electrode]

[0468] The positive electrode sheet provided in the embodiment of the present application includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes the above-mentioned positive electrode active material composition. The positive electrode current collector has two surfaces opposite to each other in its own thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0469] In some embodiments, the content of the positive electrode active material composition in the positive electrode film layer is 50-99.5% by weight, optionally 90-99.5% by weight, or 95-99.5% by weight, based on the total weight of the positive electrode film layer.

[0470] In some embodiments, the positive electrode film layer also includes a third positive electrode active material, which includes one or more of a lithium-rich oxide material, a lithium iron phosphate material, a spinel lithium manganese oxide material, and their respective modified compounds, and the modification method includes doping and / or surface coating modification.

[0471] In some embodiments, the third positive electrode active material includes a compound represented by formula (III),

[0472] Li 1+p1 A 2 q1 B 2 r1 O s1 , (III)

[0473] 0.05 ≤ p1 < 0.2, 0.10 < q1 ≤ 0.95, 0 ≤ r1 ≤ 0.2, and 2 ≤ s1 < 3, A 2 comprises one or more elements selected from Co, Ni, Mn, and Al; B 2 comprises one or more elements selected from Mg, Ti, Cr, Zr, Nb, Fe, Mo, Cu, Sb, V, P, and F.

[0474] In some embodiments, the third positive electrode active material comprises one or more selected from 1.11 Li 0.22 Ni 0.58 Mn 0.02 Ti 1.2 O2, Li 0.6 Mn 0.2 Ni 1.16 O2, Li 0.22 Ni 0.6 Mn 1.16 O2, Li 0.13 Ni 0.06 Co 0.59 Mn 1.1 O2 and Li 0.2 Ni 0.2 Co 0.48 Mn

[0475] O2.

[0476] In some embodiments, the third positive electrode active material comprises a core and a shell coating the core, the core comprising a compound represented by formula (III); the shell comprises one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

[0477] Phosphates, pyrophosphates, and solid electrolytes can improve the ionic transport properties of the third positive electrode active material.

[0478] Conductive polymers can form a uniform film with high electronic conductivity, improving charge transfer at the interface between the positive electrode and the electrolyte. At the same time, conductive polymers can adapt to the volume change of the material, thereby reducing crack formation.

[0479] Materials capable of reversibly intercalating and deintercalating lithium ions can include some different types of positive electrode active materials.

[0480] In some embodiments, the coating amount of the shell coating the compound represented by formula (III) is 0.1 wt% to 5 wt%, optionally 0.5 wt% to 2 wt%, based on the weight of the core.

[0481] In some embodiments, the thickness of the shell encapsulating the compound of formula (III) is 2 nm to 200 nm, and optionally 5 nm to 50 nm.

[0482] In some embodiments, the third positive electrode active material includes a compound represented by formula (IV),

[0483] Li a2 A 3 x2 B 3 y2 P 1-z2 C 3 z2 O 4-n2 D 3 n2 , (IV)

[0484] A 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; C 3 Includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D 3 It includes one or more elements selected from Group VIA and Group VIIA; a2 is selected from the range of 0.85 to 1.15; x2 is selected from the range of 0 to 0.1; y2 is selected from the range of 0.001 to 0.999; z2 is selected from the range of 0 to 0.5; and n2 is selected from the range of 0 to 0.5.

[0485] In some embodiments, A 3 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; and / or,

[0486] B 3 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; and / or,

[0487] C 3 comprising one or more elements selected from B (boron), S, Si and N; and / or,

[0488] D 3 comprising one or more elements selected from S, F, Cl and Br; and / or,

[0489] a2 is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or,

[0490] x2 is selected from the range of 0.001 to 0.005; and / or,

[0491] y2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or,

[0492] z2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, more optionally selected from the range of 0.001 to 0.005; and / or,

[0493] n2 is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.005.

[0494] In some embodiments, the third positive electrode active material includes a core and a shell covering the core, wherein the core includes a compound represented by formula (IV); the shell is the same as the shell covering the compound represented by formula (I), and will not be repeated here.

[0495] In some embodiments, the third positive electrode active material includes a compound represented by formula (V),

[0496] LiMn t1 A 4 2-t1 O4, (V)

[0497] t1 is selected from the range of 0 to 2, A 4 Includes one or more elements selected from Ni, Cr, Al, Zr, V, Ti, Mo, Ru, Mg, Nb, Ba, Si, P, W, Co, Cu and Zn.

[0498] In some embodiments, the third positive electrode active material includes a core and a shell coating the core, the core includes a compound represented by formula (V); the shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

[0499] In some embodiments, the one or more coating layers each independently include one or more selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly intercalating and deintercalating lithium ions.

[0500] Phosphates, pyrophosphates, and solid electrolytes can improve the ion transport properties of the third positive electrode active material.

[0501] Conductive polymers can form uniform films with high electronic conductivity, improve charge transfer at the cathode-electrolyte interface, and accommodate volume changes in materials, thereby reducing crack formation.

[0502] The material capable of reversibly intercalating and deintercalating lithium ions may include several different kinds of positive electrode active materials.

[0503] In some embodiments, the coating amount of the shell coating the compound represented by formula (V) is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core.

[0504] In some embodiments, the shell encapsulating the compound represented by formula (V) has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.

[0505] The third positive electrode active material can be prepared by a sintering method. The shell can be prepared by a liquid phase coating method.

[0506] In some embodiments, the positive electrode film layer may include a positive electrode binder.

[0507] In some embodiments, the positive electrode binder may include a vinylidene fluoride homopolymer and / or copolymer. Optionally, the comonomer may include one or more of tetrafluoroethylene, hexafluoropropylene, and propylene. Optionally, the weight proportion of the comonomer is ≤1%. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer.

[0508] In some embodiments, the positive electrode binder may include one or more of polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.

[0509] In some embodiments, the weight average molecular weight of the positive electrode binder may be 300,000 to 2,000,000.

[0510] In some embodiments, the positive electrode film layer may include a positive electrode conductive agent. As an example, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, which is not limited in the present application.

[0511] In some embodiments, the positive electrode film layer may further include functional additives, which may include one or more of a dispersant, a plasticizer, a pore former, a water removal additive, an acid removal additive, and a lithium supplement.

[0512] The dispersant may include an abc type block copolymer, wherein the a block includes polyvinyl pyrrolidone, the b block includes polyacrylic acid, and the c block includes one or more of a polytetrahydrofuran chain, a polyethylene oxide chain, a polyethylene glycol chain, a polypropylene glycol chain, and a polyoxypropylene triol chain. Optionally, the ratio of the average degree of polymerization of the a block to the b block is greater than 10:1. Optionally, the ratio of the average degree of polymerization of the a block to the c block is (0.1-10):1. Optionally, the weight average molecular weight of the dispersant is 2000 to 100,000.

[0513] The plasticizer may include one or more of a strong solvent type (PP-SS) plasticizer, a low temperature resistant type (PP-LT) plasticizer, a low volatility type (PP-LV) plasticizer, a low diffusion type (SP-LD) plasticizer, a heat stable type (SP-Stab) plasticizer, and a flame retardant type (SP-FR) plasticizer.

[0514] Strong solvent type (PP-SS) plasticizers can provide strong plasticizing properties, and may include, for example, phthalates, non-phthalates (such as benzoates, tricresyl phosphate, etc.).

[0515] Low temperature resistant (PP-LT) plasticizers can also provide good low temperature resistance, for example, can include aliphatic dibasic acid esters.

[0516] Low volatility (PP-LV) plasticizers also have relatively low volatility and may include, for example, trimellitates and polyesters.

[0517] Low-diffusivity (SP-LD) plasticizers also have lower diffusivity and, for example, may include polyesters.

[0518] The heat-stabilized (SP-Stab) plasticizer also has a heat-stabilizing function and may include, for example, epoxy compounds.

[0519] Flame retardant (SP-FR) plasticizers also have flame retardant functions and may include, for example, phosphate esters and halogenated hydrocarbons.

[0520] The lithium supplement may include one or more of lithium-rich oxides (such as Li2NiO2, Li5FeO4, etc.), nanocomposites and binary lithium compounds. Optionally, the number of Li atoms in the molecular formula of the lithium supplement is ≥1.5.

[0521] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0522] The positive electrode plate does not exclude other additional functional layers besides the positive electrode film layer. For example, in some embodiments, the positive electrode plate may also include a functional coating, which may be located between the positive electrode collector and the positive electrode film layer and / or located on the surface of the positive electrode film layer away from the positive electrode collector. As an example, the functional coating may include one or more of conductive carbon, a water removal additive, an acid removal additive, and a lithium supplement, which is not limited in the embodiments of the present application. In some embodiments, the thickness of the functional coating may be 0.1 μm-10 μm.

[0523] The positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material composition, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0524] [Negative electrode]

[0525] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material. As an example, the negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0526] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0527] In some embodiments, the thickness of the negative electrode current collector may be 3 μm-20 μm.

[0528] In some embodiments, the negative electrode active material may include one or more of a carbon-based material, a silicon-based material, a tin-based material, and lithium titanate. The carbon-based material may include one or more of graphite (e.g., artificial graphite, natural graphite, etc.), soft carbon, and hard carbon. The silicon-based material may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys.

[0529] In some embodiments, the negative electrode active material may include a carbon-based material, or a combination of a carbon-based material and a silicon-based material.

[0530] In some embodiments, the negative electrode active material may include a carbon-based material, and the carbon-based material includes graphite, or a combination of graphite and hard carbon. Optionally, the graphite may have a porous structure. Optionally, the gram capacity of the graphite may be greater than or equal to 340 mAh / g.

[0531] In some embodiments, the negative electrode active material may include a combination of a carbon-based material and a silicon-based material, the carbon-based material includes graphite, or a combination of graphite and hard carbon, and the content of silicon element in the negative electrode active material is greater than 0 and less than or equal to 30 weight %, based on the total weight of the negative electrode active material.

[0532] In some embodiments, the negative electrode film layer may include a negative electrode binder. As an example, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS), and the present application embodiment is not limited to this.

[0533] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. As an example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, which is not limited in the present application.

[0534] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC)).

[0535] In some embodiments, the porosity of the negative electrode film layer is 20% to 50%.

[0536] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. In some embodiments, the negative electrode plate may also include a functional coating, which may be located between the negative electrode current collector and the negative electrode film layer and / or located on the surface of the negative electrode film layer away from the negative electrode current collector. Optionally, the functional coating may include carbon.

[0537] In some embodiments, the negative electrode film layer may further include a lithium supplement material. Optionally, the lithium supplement material includes one or more of lithium foil, lithium ribbon, lithium powder, and a pre-lithiation agent. Optionally, the pre-lithiation agent may include one or more of Li-aromatic hydrocarbons, complexes of Li-aromatic hydrocarbons and ether solvents, and may optionally include one or more of lithium naphthalene, lithium biphenyl lithium-dimethyl ether (DME).

[0538] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer respectively disposed on two surfaces of the negative electrode current collector. The compositions of the first negative electrode film layer and the second negative electrode film layer may be the same or different; the thicknesses of the first negative electrode film layer and the second negative electrode film layer may be the same or different.

[0539] In some embodiments, a thickness ratio of the first negative electrode film layer to the second negative electrode film layer is 5:95 to 95:5.

[0540] The negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0541] In some embodiments, the negative electrode plate may not include a negative electrode active material capable of deintercalating and extracting lithium ions. For example, the negative electrode plate may include a lithium plate or a lithium alloy plate; or, the negative electrode plate may include a mesh or foam three-dimensional skeleton layer; or, the negative electrode plate may include a negative electrode current collector and a lithium-containing layer disposed on at least one surface of the negative electrode current collector.

[0542] [Electrolytes]

[0543] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to the needs. For example, the electrolyte may include one or more of a liquid electrolyte (also known as an electrolyte), a fully solid electrolyte, a gel electrolyte, or a plurality of electrolytes.

[0544] In some embodiments, the electrolyte is liquid and includes a lithium salt, a non-aqueous solvent in which the lithium salt is dissolved, and optional additives.

[0545] In some embodiments, the lithium salt may include one or more selected from LiPF6, LiBF4, LiN(SO2F)2, LiN(CF3SO2)2, LiClO4, LiAsF6, LiB(C2O4)2, LiBF2C2O4, and LiPO2F2.

[0546] In some embodiments, the concentration of the lithium salt may be 0.5-1.5 mol / L.

[0547] In some embodiments, the non-aqueous solvent may include one or more selected from propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethylene sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, acid anhydride, N-methylpyrrolidone, acetonitrile, cyclopentane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, and tetrahydrofuran.

[0548] In some embodiments, the additive may include one or more of a negative electrode film-forming additive, a positive electrode film-forming additive, an additive to improve battery overcharge performance, an additive to improve battery high temperature performance, an additive to improve battery low temperature power performance, a water removal additive, an acid removal additive, and an additive capable of complexing transition metal ions. As an example, the additive may include

[0549] One or more selected from cyclic carbonate compounds containing carbon-carbon double bonds, halogen-substituted cyclic carbonate compounds, nitrile and polynitrile compounds, phosphazene compounds, aromatic hydrocarbons and halogenated aromatic hydrocarbon compounds, isocyanate compounds, acid anhydride compounds, sulfate compounds, sulfite compounds, sulfonate compounds, disulfonate compounds, borate compounds, phosphate compounds, amide compounds, carbodiimide compounds, crown ethers and azacrown ether compounds, and their respective derivatives, optionally Including one or more of vinylene carbonate (VC), 1,2,3-tris(2-cyanoethoxy)propane (TCP), 1-aza-12-crown 4-ether (A12C4), N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, tris(hexafluoroisopropyl)borate, tris(2,2,3,3-tetrafluoropropyl)borate, and tris(pentafluorophenyl)borate.

[0550] In some embodiments, the content of the additive may be less than or equal to 10% based on the total weight of the electrolyte.

[0551] [Isolation film]

[0552] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0553] In some embodiments, the isolation membrane includes a porous substrate. The material of the porous substrate may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, polyester, and polyimide. The porous substrate may be a single-layer film or a multi-layer composite film, without particular limitation. When the porous substrate is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0554] In some embodiments, the isolation membrane may further include a coating layer located on at least one surface of the porous substrate. Optionally, the coating layer includes one or more of inorganic heat-resistant particles and organic heat-resistant particles.

[0555] In some embodiments, the isolation film has a porosity of 10%-40%.

[0556] In some embodiments, the isolation film may have a thickness of 3 μm-20 μm.

[0557] The present application also provides an electrical device, which includes at least one of the battery cells, battery modules, or battery packs provided in the present application. The battery cells, battery modules, or battery packs can be used as power sources for the electrical device, or as energy storage units for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0558] As an electrical device, a battery cell, a battery module or a battery pack can be selected according to its usage requirements.

[0559] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the power consumption device for high power and high energy density, a battery pack or a battery module can be used.

[0560] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a battery cell may be used as a power source.

[0561] Example

[0562] The following examples describe the disclosure of the present application in more detail, and these examples are only for illustrative purposes, as it is obvious to those skilled in the art that various modifications and variations are made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0563] The batteries of Examples 1-26 and Comparative Example 3 were prepared according to the following method.

[0564] Preparation of positive electrode

[0565] The first positive electrode active material and the second positive electrode active material shown in Table 1 and Table 2, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were fully stirred and mixed in a proper amount of solvent NMP at a mass ratio of 96:2:2 to form a uniform positive electrode slurry; the positive electrode slurry was evenly coated on the two surfaces of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.

[0566] Preparation of negative electrode

[0567] The negative electrode active material graphite, the binder styrene butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC-Na), and the conductive agent carbon black (Super P) are fully stirred and mixed in a proper amount of solvent deionized water at a mass ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet is obtained.

[0568] Preparation of electrolyte

[0569] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0570] Preparation of isolation membrane

[0571] A porous polyethylene membrane was used as the separator.

[0572] Preparation of batteries

[0573] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, and after drying, the electrolyte is injected, and the battery is obtained after vacuum packaging, standing, forming, shaping and other processes.

[0574] Comparative Example 1

[0575] The preparation method of the battery is the same as that of Example 1, except for the preparation of the positive electrode sheet.

[0576] The second positive electrode active material shown in Table 1, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were fully stirred and mixed in a proper amount of solvent NMP at a mass ratio of 96:2:2 to form a uniform positive electrode slurry; the positive electrode slurry was evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.

[0577] Comparative Example 2

[0578] The preparation method of the battery is the same as that of Example 1, except for the preparation of the positive electrode sheet.

[0579] The first positive electrode active material shown in Table 1, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were fully stirred and mixed in a proper amount of solvent NMP at a mass ratio of 96:2:2 to form a uniform positive electrode slurry; the positive electrode slurry was evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet was obtained.

[0580] In Table 1 and Table 2, NCM523 refers to LiNi 0.5 Co 0.2 Mn 0.3 O2, LMFP refers to carbon-coated LiMn 0.7 Fe 0.3 PO4.

[0581] The NCM523 and LMFP of each embodiment and comparative example can be commercially purchased, and then a variety of commercially available materials are screened by selecting a suitable sieve and then mixed in a predetermined ratio to obtain the material; or, the commercially available materials are first ball-milled to a suitable size, and then screened by selecting a suitable sieve, and then mixed in a predetermined ratio to obtain the material; or, a sintering method is adopted and the sintering process parameters (such as sintering temperature, sintering time, sintering atmosphere, etc.) and grinding parameters (such as grinding speed, grinding time, etc.) are adjusted, and a suitable sieve is selected for screening to obtain the material; or, a variety of materials of different sizes prepared by the sintering method are mixed in a predetermined ratio to obtain the material.

[0582] w a w represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition. bIt represents the weight content of the second positive electrode active material based on the total weight of the positive electrode active material composition.

[0583] P1 is the powder compaction density of the first positive electrode active material at 30000 N. P2 is the powder compaction density of the second positive electrode active material at 30000 N.

[0584] PD represents the compaction density of the positive electrode film.

[0585] Compacted density efficiency of positive electrode = PD / [(P1×W a )+(P2×W b )]. (P1×W a )+(P2×W b ) represents the theoretical compaction density of the positive electrode active material composition.

[0586] y is the molar amount of Fe element in LMFP, i.e. 0.3.

[0587] V B is the voltage platform of Fe element in LMFP, in V (volt).

[0588] In the particle size distribution curve of the positive electrode active material composition, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2.

[0589] Figure 7 is the particle size distribution curve of the positive electrode active material composition of Example 11, as shown in Figure 7 As shown, in the particle size distribution curve of the positive electrode active material composition, the peak on the left is the second peak (ie, the volume distribution peak with the second largest peak intensity), and the peak on the right is the first peak (ie, the volume distribution peak with the largest peak intensity).

[0590] The above parameters can be measured according to the test methods given above.

[0591] In Table 1, the first positive electrode active material is mainly single crystal, accounting for more than 90% in number. The second positive electrode active material of Examples 1-11 is mainly polycrystalline, accounting for more than 90% in number. The second positive electrode active material of Examples 12-16 is mainly single crystal, accounting for more than 90% in number.

[0592] In Table 2, the first positive electrode active material is mainly polycrystalline, accounting for more than 90% in number. The second positive electrode active material of Examples 17-21 is mainly single crystal, accounting for more than 90% in number. The second positive electrode active material of Examples 22-26 is mainly polycrystalline, accounting for more than 90% in number.

[0593] Test Section

[0594] At 25°C, charge the battery to 4.3V at 1C constant current, and continue to charge at constant voltage until the current reaches 0.05C. At this time, the battery is fully charged. Record the charging capacity at this time, which is the charging capacity of the first cycle. After the battery is left to stand for 5 minutes, discharge it to 2.8V at 1C constant current. This is a cycle charge and discharge process. Record the discharge capacity at this time, which is the discharge capacity of the first cycle. Perform a cyclic charge and discharge test on the battery according to the above method, and record the discharge capacity after each cycle until the discharge capacity of the battery decays to 80% of the discharge capacity of the first cycle. The number of cycles at this time is used to characterize the cycle performance of the battery. The higher the number of cycles of the battery, the better the service life.

[0595] It can be seen from the test results of Table 1 and Table 2 that when the particle size distribution curve of the positive electrode active material composition satisfies 0<|Dv1-Dv2| / Dv1≤50, the positive electrode sheet using the positive electrode active material composition can have both high compaction density and high compaction density efficiency, thereby enabling the secondary battery to have a high energy density while also enabling the secondary battery to have a long service life.

[0596] The preparation methods of the batteries of Examples 27-31 are similar to that of Example 4, except that the types of the first positive electrode active materials are different, as shown in Table 3 for details.

[0597] The first positive electrode active material of Examples 27-31 is obtained by a sintering method and by adjusting sintering process parameters (such as sintering temperature, sintering time, sintering atmosphere, etc.), grinding parameters (such as grinding speed, grinding time, etc.), and selecting a suitable screen for screening; or, by mixing a plurality of materials of different particle sizes prepared by the sintering method in a predetermined proportion.

[0598] It can be seen from the test results in Table 3 that by doping specific elements at the Mn position of LiMnPO4 and at the Li position, P position and / or O position, it is possible to dope specific elements at the Mn position and P position of LiMnPO4, or more preferably at the Li position, Mn position, P position and O position of LiMnPO4, the compaction density of the positive electrode sheet can be further improved, the energy density of the battery can be improved, and the cycle performance of the battery can be improved.

[0599] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

[0600]

[0601]

Claims

1. A positive electrode active material composition, in, The positive electrode active material composition includes a first positive electrode active material and a second positive electrode active material having a crystal form different from that of the first positive electrode active material, the first positive electrode active material includes phosphate, and the particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, then 0<|Dv1-Dv2| / Dv1≤50.

2. The positive electrode active material composition according to claim 1, in, The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 12.5 μm; and / or, The volume distribution particle size Dv50 of the second positive electrode active material is 2.5 μm to 16.5 μm.

3. The positive electrode active material composition according to claim 1 or 2, in, The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies: 0.1≤|Dv1-Dv2| / Dv1≤50, optionally, 0.46≤|Dv1-Dv2| / Dv1≤39.6; and / or, 0.3 μm ≤ Dv1 ≤ 17.8 μm, optionally, 0.35 μm ≤ Dv1 ≤ 12.1 μm; and / or, 0.3μm≤Dv2≤17.8μm, optionally, 0.46μm≤Dv2≤14.2μm.

4. The positive electrode active material composition according to claim 1 or 2, in, The volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and the particle size distribution curve of the positive electrode active material composition satisfies: 0.1≤|Dv1-Dv2| / Dv1≤6.0, optionally, 0.34≤|Dv1-Dv2| / Dv1≤3.8; and / or, 2.0 μm ≤ Dv1 ≤ 12.5 μm, optionally, 3.0 μm ≤ Dv1 ≤ 12.3 μm; and / or, 2.0μm≤Dv2≤15.0μm, optionally, 3.4μm≤Dv2≤14.3μm.

5. A positive electrode active material composition, in, The positive electrode active material composition includes a first positive electrode active material and a second positive electrode active material having a crystal form different from the first positive electrode active material, the first positive electrode active material includes phosphate, the particle size distribution curve of the positive electrode active material composition has at least two volume distribution peaks, the volume distribution peak with the maximum peak intensity is recorded as the first peak, and the volume distribution particle size corresponding to the maximum peak intensity of the first peak is recorded as Dv1, the volume distribution peak with the second maximum peak intensity is recorded as the second peak, and the volume distribution particle size corresponding to the maximum peak intensity of the second peak is recorded as Dv2, wherein, The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and 0.3 μm≤Dv1≤17.8 μm, 0.3 μm≤Dv2≤17.8 μm; or The volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and 2.0 μm≤Dv1≤12.5 μm, and 2.0 μm≤Dv2≤15.0 μm.

6. The positive electrode active material composition according to claim 5, in, The volume distribution particle size Dv50 of the first positive electrode active material is 0.25 μm to 3.5 μm, and 0.35 μm≤Dv1≤12.1 μm, and 0.46 μm≤Dv2≤14.2 μm.

7. The positive electrode active material composition according to claim 5, in, The volume distribution particle size Dv50 of the first positive electrode active material is 3.5 μm to 12.5 μm, and 3.0 μm≤Dv1≤12.3 μm, and 3.4 μm≤Dv2≤14.3 μm.

8. The positive electrode active material composition according to any one of claims 1 to 7, in, The morphology of the first positive electrode active material includes one or more of single crystal and polycrystalline, and the morphology of the second positive electrode active material includes one or more of single crystal and polycrystalline; Optionally, the volume distribution particle size Dv50 of the first positive electrode active material with a single crystal morphology is 0.25 μm to 3.5 μm, and optionally 0.35 μm to 2.5 μm; and / or, Optionally, the volume distribution particle size Dv10 of the first positive electrode active material with a single crystal morphology is 0.05 μm to 1.5 μm, and optionally 0.1 μm to 1.0 μm; and / or, Optionally, the volume distribution particle size Dv50 of the first positive electrode active material with polycrystalline morphology is 3.5 μm to 12.5 μm, and optionally 3.8 μm to 10.5 μm; and / or, Optionally, the volume distribution particle size Dv10 of the first positive electrode active material with polycrystalline morphology is 0.1 μm to 5.0 μm, and optionally 0.5 μm to 4.5 μm; and / or, Optionally, the volume distribution particle size Dv50 of the second positive electrode active material with single crystal morphology is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 8.5 μm; and / or, Optionally, the volume distribution particle size Dv10 of the second positive electrode active material with a single crystal morphology is 0.3 μm to 8 μm, and optionally 1.0 μm to 3.5 μm; and / or, Optionally, the volume distribution particle size Dv50 of the second positive electrode active material with polycrystalline morphology is 2.5 μm to 16.5 μm, and optionally 3.0 μm to 15.5 μm; Optionally, the volume distribution particle size Dv10 of the second positive electrode active material with a polycrystalline morphology is 0.5 μm to 12 μm, and optionally 1.0 μm to 8.5 μm.

9. The positive electrode active material composition according to any one of claims 1 to 8, in, Based on the total weight of the positive electrode active material composition, the weight content of the first positive electrode active material is recorded as w a The weight content of the second positive electrode active material is recorded as w b ,but w a Selected from the range of 0.5% to 99.5%, optionally selected from the range of 2% to 95%; and / or, w b Selected from the range of 0.5% to 99.5%, optionally selected from the range of 5% to 98%.

10. The positive electrode active material composition according to any one of claims 1 to 9, in, The powder compaction density P of the first positive electrode active material at 30000N is 1 1.89 g / cm 3 Above, optional 1.95g / cm 3 Above, 1.98g / cm2 is optional 3 Above, further optional 2.0g / cm 3 Above, further optional 2.2g / cm 3 Above, further optionally 2.2 g / cm 3 Above and 2.8g / cm 3 Below or 2.2g / cm 3 Above and 2.65g / cm 3 The following; and / or, The powder compaction density P of the second positive electrode active material at 30000N is 2 Greater than or equal to 2.90g / cm 3 , can be selected as greater than or equal to 3.1g / cm 3 , more preferably greater than or equal to 3.3 g / cm 3 and / or, The BET specific surface area of ​​the second positive electrode active material is less than or equal to 1.73 m 2 / g, can be selected to be less than or equal to 1.5m 2 / g, 0.28m 2 / g to 1.5m 2 / g.

11. The positive electrode active material composition according to any one of claims 1 to 10, in, The first positive electrode active material includes a compound represented by formula (I), Li a A x Mn 1-y M 1 y P 1-z M 2 z O 4-n D n (I) A includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; M 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; M 2 It includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D includes one or more elements selected from Group VIA and Group VIIA; a is selected from the range of 0.85 to 1.15; x is selected from the range of 0 to 0.1; y is selected from the range of 0.001 to 0.999; z is selected from the range of 0 to 0.5; and n is selected from the range of 0 to 0.

5.

12. The positive electrode active material composition according to claim 11, in, A includes one or more elements selected from Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; and / or, M 1 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; and / or, M 2 comprising one or more elements selected from B (boron), S, Si and N; and / or, D includes one or more elements selected from S, F, Cl and Br.

13. The positive electrode active material composition according to claim 11 or 12, in, A includes any one element selected from Zn, Al, Na, K, Mg, Nb, Mo and W, and may optionally include any one element selected from Mg and Nb; and / or, M 1 comprising one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and optionally comprising at least two elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge, and more optionally comprising at least two elements selected from Fe, Ti, V, Ni, Co and Mg, and further optionally comprising at least two elements selected from Fe, Ti, V, Co and Mg, and further optionally comprising Fe and one or more elements selected from Ti, V, Co and Mg; and / or, M 2 comprising any one element selected from B (boron), S, Si and N, optionally S; and / or, D includes any one element selected from S, F, Cl and Br, and may be F.

14. The positive electrode active material composition according to any one of claims 11 to 13, in, a is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or, x is selected from the range of 0.001 to 0.005; and / or, y is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or, z is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, more optionally selected from the range of 0.001 to 0.005; and / or, n is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.

005.

15. The positive electrode active material composition according to any one of claims 11 to 14, in, x is 0, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is 0, z is 0, and n is selected from the range of 0.001 to 0.1; or, x is 0, z is selected from the range of 0.001 to 0.5, and n is 0; or, x is selected from the range of 0.001 to 0.1, z is selected from the range of 0.001 to 0.5, and n is selected from the range of 0.001 to 0.

1.

16. The positive electrode active material composition according to any one of claims 11 to 15, in, y:z is selected from the range of 0.002 to 999, and may be selected from the range of 0.025 to 999 or the range of 0.002 to 500, and may be further selected from the range of 0.2 to 600.

17. The positive electrode active material composition according to any one of claims 11 to 16, in, z:n is selected from the range of 0.002 to 500, can be selected from the range of 0.2 to 100, and can be further selected from the range of 0.2 to 50.

18. The positive electrode active material composition according to any one of claims 11 to 17, in, A includes one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; M 1 Includes one or more elements selected from Ti, V, Zr, Fe, Ni, Mg, Co, Ga, Sn, Sb, Nb and Ge; M 2 It includes one or more elements selected from B (boron), S, Si and N; D includes one or more elements selected from S, F, Cl and Br; a is selected from the range of 0.9 to 1.1, x is selected from the range of 0.001 to 0.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is selected from the range of 0.001 to 0.

1.

19. The positive electrode active material composition according to any one of claims 11 to 17, in, M 1 It includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and may optionally include one or more elements selected from the group consisting of Zn, Fe, Ti, V, Ni, Co and Mg; M 2 It includes one or more elements selected from B (boron), Si, N and S; a is selected from the range of 0.9 to 1.1, x is 0, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, and n is 0.

20. The positive electrode active material composition according to any one of claims 11 to 19, in, (1-y): y is in the range of 0.1-999, optionally in the range of 0.1-10 or in the range of 0.67-999, more optionally in the range of 1 to 10, further optionally in the range of 1 to 4, and further optionally in the range of 1.5 to 3; and / or, a:x is in the range of 1 to 1200, and can be optionally in the range of 9 to 1100, and can be more optionally in the range of 190-998.

21. The positive electrode active material composition according to any one of claims 11 to 20, in, z:(1-z) is 1:9 to 1:999, and can be optionally 1:499 to 1:

249.

22. The positive electrode active material composition according to any one of claims 11 to 21, in, The first positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (I); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

23. The positive electrode active material composition according to claim 22, in, The one or more coating layers each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.

24. The positive electrode active material composition according to claim 22 or 23, in, The shell includes a coating; Optionally, the coating layer comprises one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer.

25. The positive electrode active material composition according to claim 22 or 23, in, The shell includes a first coating layer covering the core and a second coating layer covering the first coating layer; Optionally, the first coating layer and the second coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer; More optionally, the first coating layer includes one or more selected from pyrophosphate, phosphate, oxide and boride, and the second coating layer includes one or more selected from carbon and doped carbon.

26. The positive electrode active material composition according to claim 22 or 23, in, The shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer; Optionally, the first coating layer, the second coating layer and the third coating layer each independently include one or more selected from pyrophosphate, phosphate, carbon, doped carbon, oxide, boride and polymer; More optionally, the first coating layer includes pyrophosphate, the second coating layer includes one or more selected from phosphates, oxides and borides, and the third coating layer includes one or more selected from carbon and doped carbon.

27. The positive electrode active material composition according to any one of claims 23 to 26, in, The pyrophosphate is M b (P 2 O 7 ) c and / or, The phosphate is X m (PO 4 ) q and / or, The doping element in the doped carbon includes one or more elements selected from Group IIIA, Group VA, Group VIA and Group VIIA; and / or, The oxide is M' d O e and / or, The boride is Z v B w and / or, The polymer includes one or more selected from polysaccharides and their derivatives, and polysiloxanes; M, X and Z each independently include one or more elements selected from Group IA, Group IIA, Group IIIA, Group IB, Group IIB, Group IVB, Group VB, Group VIIB and Group VIII; b is selected from the range of 1 to 4; c is selected from the range of 1 to 6; m is selected from the range of 1 to 2; q is selected from the range of 1 to 4; M′ comprises one or more elements selected from alkali metals, alkaline earth metals, transition metals, Group IIIA elements, Group IVA elements, lanthanides and Sb; d is greater than 0 and less than or equal to 2; e is greater than 0 and less than or equal to 5; v is selected from the range of 1 to 7; w is selected from the range of 1 to 2.

28. The positive electrode active material composition according to claim 27, in, M, X and Z each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, Mn and Al; and / or, The doping element in the doped carbon includes one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine; and / or, M′ comprises one or more elements selected from Li, Be, B, Na, Mg, Al, Si, P, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, As, Se, Sr, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Te, W, La and Ce, and may optionally comprise one or more elements selected from Mg, Al, Si, Zn, Zr and Sn; and / or The polysiloxane is selected from one or more of linear polysiloxane and cyclic polysiloxane; and / or, The polysaccharide is selected from one or more of plant polysaccharides and marine polysaccharides.

29. The positive electrode active material composition according to any one of claims 22 to 23, 25, 27 to 28, in, The first positive electrode active material includes a core and a shell covering the core, The core includes Li a Mn 1-y M 1 y P 1-z M 2 z O 4 , a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, M 1 The M 2 including one or more elements selected from B (boron), S, Si and N; The shell includes a first coating layer covering the core and a second coating layer covering the first coating layer, wherein the first coating layer includes pyrophosphate MP 2 O 7 and phosphate XPO 4 , M and X each independently include one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; and the second coating layer contains carbon.

30. The positive electrode active material composition according to any one of claims 22 to 23, 26 to 28, in, The first positive electrode active material includes a core and a shell covering the core, The core includes Li a Mn 1-y M 1 y P 1-z M 2 z O 4 , a is selected from the range of 0.9 to 1.1, y is selected from the range of 0.001 to 0.5, z is selected from the range of 0.001 to 0.1, M 1 The M 2 including one or more elements selected from B (boron), S, Si and N; The shell includes a first coating layer covering the core, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer. The first coating layer includes pyrophosphate Li f QP 2 O 7 and / or Q g (P 2 O 7 ) h , 0≤f≤2, 1≤g≤4, 1≤h≤6, the pyrophosphate Li f QP 2 O 7 and / or Q g (P 2 O 7 ) h wherein Q independently comprises one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; The second coating layer includes crystalline phosphate XPO 4 , X includes one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al; The third coating layer includes carbon.

31. The positive electrode active material composition according to any one of claims 22 to 28, in, The one or more coating layers in the shell that are farthest from the core each independently include one or more selected from polysiloxane, polysaccharide and polysaccharide derivatives.

32. The positive electrode active material composition according to any one of claims 22 to 28 and 31, in, The polysiloxane comprises a structural unit represented by formula (i), R 1 and R 2 independently selected from H, -COOH, -OH, -SH, -CN, -SCN, amino, phosphate, carboxylate, amide, aldehyde, sulfonyl, polyether segment, C1-C20 aliphatic, C1-C20 halogenated aliphatic, C1-C20 heteroaliphatic, C1-C20 halogenated heteroaliphatic, C6-C20 aromatic, C6-C20 halogenated aromatic, C2-C20 heteroaromatic and C2-C20 halogenated heteroaromatic; Optionally, R 1 and R 2 Independently selected from H, amino group, phosphate group, polyether segment, C1-C8 alkyl group, C1-C8 haloalkyl group, C1-C8 heteroalkyl group, C1-C8 haloheteroalkyl group, C2-C8 alkenyl group and C2-C8 haloalkenyl group.

33. The positive electrode active material composition according to any one of claims 22 to 28, 31 to 32, in, The polysiloxane further comprises an end-capping group, which comprises one or more of the following functional groups: polyether, C1-C8 alkyl, C1-C8 haloalkyl, C1-C8 heteroalkyl, C1-C8 haloheteroalkyl, C2-C8 alkenyl, C2-C8 haloalkenyl, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy, C2-C8 epoxy, hydroxyl, C1-C8 hydroxyalkyl, amino, C1-C8 aminoalkyl, carboxyl, C1-C8 carboxylalkyl.

34. The positive electrode active material composition according to any one of claims 22 to 28, 31 to 33, in, The polysiloxane comprises polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl functionalized polysiloxane, epoxy-terminated polysiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, polymethylchloropropylsiloxane, hydroxy-terminated polydimethylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, aminoethylaminopropyl polydimethylsiloxane, terminal polyether polydimethylsiloxane, side-chain aminopropyl polysiloxane, aminopropyl One or more of end-capped polydimethylsiloxane, side chain phosphate grafted polydimethylsiloxane, side chain polyether grafted polydimethylsiloxane, 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, cyclic polymethylvinylsiloxane, hexadecylcyclooctasiloxane, tetradecamethylcycloheptasiloxane, and cyclic polydimethylsiloxane.

35. The positive electrode active material composition according to any one of claims 22 to 28 and 31 to 34, in, The number average molecular weight of the polysiloxane, the polysaccharide and the polysaccharide derivative is independently below 300,000, and may be 10,000 to 200,000, more preferably 20,000 to 120,000, and further preferably 400 to 80,000.

36. The positive electrode active material composition according to any one of claims 22 to 28 and 31 to 35, in, The mass percentage of the polar functional groups in the polysiloxane is α, 0≤α<50%, optionally, 5%≤α≤30%.

37. The positive electrode active material composition according to any one of claims 22 to 28 and 31 to 36, in, The substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the following functional groups: -OH, -COOH and salts thereof, -R-OH, -SO 3 H and its salts, -R-OH, -R-SO 3 H and its salts, sulfate ester groups, alkoxy groups, R represents an alkylene group, and optionally represents a C1-C5 alkylene group; Optionally, the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives each independently include one or more of the following functional groups: -OH, -COOH, -COOLi, -COONa, -COOK, -SO 3 H, -SO 3 Li, -SO 3 Na, -SO 3 K, -CH 2 -SO 3 H, -CH 2 -SO 3 Li, -CH 2 -SO 3 Na, -CH 2 -SO 3 K, methoxy, ethoxy.

38. According to any one of claims 22 to 28, 31 to 37, the positive electrode active material composition, the polysaccharide comprises one or more selected from pectin, carboxymethyl starch, hydroxypropyl starch, dextrin, cellulose ether, carboxymethyl chitosan, hydroxyethyl cellulose, carboxymethyl cellulose, carboxypropyl methyl cellulose, guar gum, sesbania gum, gum arabic, lithium alginate, sodium alginate, potassium alginate, fucoidan, agar, carrageenan, carrageenan, xanthan gum and fenugreek gum.

39. The positive electrode active material composition according to any one of claims 22 to 28 and 31 to 38, in, The mass percentage of the substituents attached to the sugar units in the polysaccharide and the polysaccharide derivatives is independently 20% to 85%, and optionally 30% to 78%.

40. The positive electrode active material composition according to any one of claims 22 to 39, in, The lattice mismatch between the material of the core and the material of the shell is less than 10%.

41. The positive electrode active material composition according to any one of claims 11 to 40, in, Based on the total weight of the first positive electrode active material, The manganese content is in the range of 10 wt% to 35 wt%, optionally in the range of 13.3 wt% to 33.2 wt%, more optionally in the range of 15 wt% to 30 wt%, further optionally in the range of 17 wt% to 20 wt%; and / or, The phosphorus content is in the range of 12 wt% to 25 wt%, optionally in the range of 15 wt% to 20 wt%, and more optionally in the range of 16.8 wt% to 19.5 wt%; and / or, The weight ratio of manganese element to phosphorus element ranges from 0.71 to 1.85, and can be selected from 0.90 to 1.25, and more preferably from 0.95 to 1.

20.

42. The positive electrode active material composition according to any one of claims 1 to 21, in, The surface of the first positive electrode active material is coated with one or more of carbon and doped carbon; optionally, the surface of the first positive electrode active material is coated with carbon.

43. The positive electrode active material composition according to claim 42, in, The doping elements in the doped carbon include one or more selected from nitrogen, phosphorus, sulfur, boron and fluorine.

44. The positive electrode active material composition according to any one of claims 22 to 24, 27 to 28, 31 to 43, in, The coating amount of the shell is 0.1 wt % to 6 wt % based on the weight of the core.

45. The positive electrode active material composition according to any one of claims 22 to 23, 25 to 41, in, The coating amount of the first coating layer is greater than 0 and less than or equal to 7% by weight, and can be greater than 0 and less than or equal to 6% by weight, and can be greater than 0 and less than or equal to 5.5% by weight or 4-5.6% by weight, and can be further greater than 0 and less than or equal to 2% by weight, based on the weight of the core; and / or, The coating amount of the second coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, and more optionally 2-4% by weight or 3-5% by weight, based on the weight of the core; and / or, The coating amount of the third coating layer is greater than 0 and less than or equal to 6% by weight, optionally greater than 0 and less than or equal to 5.5% by weight, and more optionally greater than 0 and less than or equal to 2% by weight, based on the weight of the core.

46. ​​The positive electrode active material composition according to any one of claims 22 to 23, 26 to 28, 30 to 41, 45, in, The shell further includes a fourth coating layer covering the third coating layer and a fifth coating layer covering the fourth coating layer; The coating amounts of the fourth coating layer and the fifth coating layer are each independently 0.01 wt % to 10 wt %, optionally 0.05 wt % to 10 wt %, more optionally 0.1 wt % to 5 wt %, further 0.1 wt % to 2 wt %, based on the weight of the core.

47. The positive electrode active material composition according to any one of claims 22 to 46, in, The shell is located on 40% to 90% of the surface of the inner core, optionally 60% to 80% of the surface.

48. The positive electrode active material composition according to any one of claims 22 to 24, 27 to 28, 31 to 44, 47, in, The shell has a thickness of 1-15 nm.

49. The positive electrode active material composition according to any one of claims 22 to 23, 25 to 41, 45 to 48, in, The thickness of the first coating layer is 1-10 nm, and can be 2-10 nm; and / or, The thickness of the second coating layer is 2-25 nm, optionally 2-15 nm, more optionally 3-15 nm; and / or, The thickness of the third coating layer is 2-25 nm, and can be optionally 5-25 nm.

50. The positive electrode active material composition according to any one of claims 22 to 49, in, The one or more coating layers each independently include one or more selected from pyrophosphate, phosphate and oxide, and the one or more selected from the pyrophosphate, phosphate and oxide are crystalline; Optionally, the crystallinity of the pyrophosphate, the phosphate and the oxide is each independently 10% to 100%, more preferably 50% to 100%.

51. The positive electrode active material composition according to any one of claims 22 to 50, in, In the shell, the weight ratio of pyrophosphate to phosphate and the weight ratio of pyrophosphate to oxide are each independently 1:3 to 3:1, and optionally 1:3 to 1:

1.

52. The positive electrode active material composition according to any one of claims 22 to 51, in, The one or more coating layers each independently include carbon, and the carbon is a mixture of SP2 carbon and SP3 carbon; Optionally, in the carbon, the molar ratio of the SP2 carbon to the SP3 carbon is any value in the range of 0.07-13, more preferably any value in the range of 0.1-10, and further preferably any value in the range of 2.0-3.

0.

53. The positive electrode active material composition according to any one of claims 22 to 52, in, The one or more coating layers each independently include doped carbon, and the mass content of the doping element in the doped carbon is less than 30%; optionally, the mass content of the doping element in the doped carbon is less than 20%.

54. The positive electrode active material composition according to any one of claims 22 to 53, in, The one or more coating layers each independently include doped carbon, in which: The doping element is nitrogen and / or sulfur, and the mass content of the doping element in the doped carbon is 1% to 15%; or, The doping element is phosphorus, boron and / or fluorine, and the mass content of the doping element in the doped carbon is 0.5% to 5%; Optionally, the doping element is nitrogen, phosphorus, sulfur, boron or fluorine.

55. The positive electrode active material composition according to any one of claims 22 to 54, in, The one or more coating layers independently include pyrophosphate, the interplanar spacing of the pyrophosphate is in the range of 0.293-0.470nm, optionally 0.297-0.462nm or 0.293-0.326nm, more optionally 0.300-0.310nm, and the angle of the crystal direction (111) is in the range of 18.00°-32.57°, optionally 18.00°-32.00° or 26.41°-32.57°, more optionally 19.211°-30.846°, and further optionally 29.00°-30.00°; and / or, The one or more coating layers independently include phosphate, the interplanar spacing of the phosphate is in the range of 0.244-0.425 nm, optionally 0.345-0.358 nm, and the angle of the crystal direction (111) is in the range of 20.00°-37.00°, optionally 24.25°-26.45°; Optionally, the first coating layer or the second coating layer comprises phosphate.

56. The positive electrode active material composition according to any one of claims 1 to 55, in, The lattice change rate of the first positive electrode active material before and after complete lithium deintercalation is 50% or less, optionally 9.8% or less, more optionally 8.1% or less, further optionally 7.5% or less, further optionally 6% or less, further optionally 4% or less, further optionally 3.8% or less, further optionally 2.0-3.8%; and / or, The Li / Mn antisite defect concentration of the first positive electrode active material is 5.3% or less, optionally 5.1% or less, more optionally 4% or less, further optionally 2.2% or less, further optionally 2% or less, further optionally 1.5%-2.2% or 0.5% or less; and / or, The surface oxygen valence state of the first positive electrode active material is -1.55 or less, optionally -1.82 or less, more optionally -1.88 or less, further optionally -1.90 or less or -1.98 to -1.88, further optionally -1.98 to -1.89, further optionally -1.98 to -1.

90.

57. The positive electrode active material composition according to any one of claims 8, 11 to 56, in, The positive electrode active material composition satisfies 0.0004≤w a ×y×(3.4-V B )≤0.063, optionally, 0.0015≤w a ×y×(3.4-V B )≤0.045, w a represents the weight content of the first positive electrode active material based on the total weight of the positive electrode active material composition, y is 1 mol of M in the compound represented by formula (I) 1 Molar amount of element, V B M in the compound represented by formula (I) 1 The voltage platform of the element, in V (volts).

58. The positive electrode active material composition according to any one of claims 1 to 57, in, The second positive electrode active material includes a layered oxide.

59. The positive electrode active material composition according to claim 58, in, The second positive electrode active material includes a compound represented by formula (II), Li a1 A 1 b1 Ni c1 Co d1 B 1 e1 C 1 f1 O 2-g1 D 1 g1 (II) A 1 Includes one or more elements selected from Group IA, Group IIA, Group VIII, Group VIB, and Group IIB; B 1 including Mn and / or Al; C 1 comprising one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group VIA, Group IIB, Group IIIB, Group IVB, Group VB, Group VIB, and Group VIII; D 1 It includes one or more elements selected from Group VIA and Group VIIA; a1 is selected from the range of 0.8 to 1.2; b1 is selected from the range of 0 to 0.2; c1 is selected from the range of 0 to 1; d1 is selected from the range of 0 to 1; e1 is selected from the range of 0 to 1; f1 is selected from the range of 0 to 0.1; g1 is selected from the range of 0 to 0.1; and c1+d1+e1+f1=1.

60. The positive electrode active material composition according to claim 59, in, A 1 including one or more elements selected from the group consisting of Na, K, Mg, Rb, Zn, and Zr; and / or, C 1 including one or more elements selected from the group consisting of Al, Mg, Ca, Na, Ti, W, Zr, Sr, Cr, Fe, Zn, Ba, Mo, V, Ce, Nb, Sb, Ta, Ge, Nb, Sc, Ba, B, S and Y, and optionally including one or more elements selected from the group consisting of Al, Ti, Zr, Nb, Sr, Sc, Sb, Y, Ba, B; and / or, D 1 comprising one or more elements selected from N, S, F, Cl and Br, and optionally comprising S and / or F; and / or, a1 is selected from the range of 0.9 to 1.1; and / or, b1 is selected from the range of 0 to 0.1; and / or, c1 is selected from the range of 0.314 to 0.990, and may be selected from the range of 0.500 to 0.990; and / or, d1 is selected from the range of 0 to 0.320, and may be selected from the range of 0 to 0.150; and / or, e1 is selected from the range of 0.001 to 0.450, and may be selected from the range of 0.005 to 0.4; and / or, f1 is selected from the range of 0.001 to 0.1, and may be selected from the range of 0.001 to 0.05; and / or, g1 is selected from the range of 0 to 0.01, and can be optionally selected from the range of 0.01 to 0.

05.

61. The positive electrode active material composition according to claim 59 or 60, in, The second positive electrode active material includes a core and a shell covering the core, The core comprises the compound represented by formula (II); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

62. The positive electrode active material composition according to claim 61, in, The one or more coating layers each independently include one or more selected from phosphate, pyrophosphate, carbon, doped carbon, oxide, and fast ion conductor, and may optionally include one or more selected from phosphate, pyrophosphate, and oxide.

63. The positive electrode active material composition according to claim 61 or 62, in, The shell includes a coating; Optionally, the coating layer includes one or more selected from phosphates, pyrophosphates, and oxides.

64. The positive electrode active material composition according to claim 61 or 62, in, The shell includes a first coating layer covering the core and a second coating layer covering the first coating layer; Optionally, the first coating layer and the second coating layer each independently include one or more selected from phosphates, pyrophosphates, and oxides; More optionally, the first coating layer includes one or more selected from phosphates and oxides, and the second coating layer includes one or more selected from pyrophosphates and oxides.

65. The positive electrode active material composition according to any one of claims 61 to 64, in, The coating amount of the shell is 0.005 wt % to 1 wt %, and optionally 0.01 wt % to 0.5 wt %, based on the weight of the core; and / or, The shell has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.

66. A positive electrode plate, comprising a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, the positive electrode film layer comprising a positive electrode active material, the positive electrode active material comprising the positive electrode active material composition according to any one of claims 1 to 65, optionally, the content of the positive electrode active material composition in the positive electrode film layer is 90 weight % to 99.5 weight %, more optionally 95 weight % to 99.5 weight %, based on the total weight of the positive electrode film layer.

67. The positive electrode sheet according to claim 66, in, The positive electrode film layer also includes a third positive electrode active material, which includes one or more of a lithium-rich oxide material, a lithium iron phosphate material, a spinel lithium manganese oxide material, and their respective modified compounds, and the modification method includes doping and / or surface coating modification.

68. The positive electrode sheet according to claim 67, in, The third positive electrode active material includes a compound represented by formula (III), Li 1+p1 A 2 q1 B 2 r1 O s1 (III) 0.05 ≤ p1 < 0.2, 0.10 < q1 ≤ 0.95, 0 ≤ r1 ≤ 0.2, and 2 ≤ s1 < 3, A 2 comprises one or more elements selected from Co, Ni, Mn, and Al; B 2 comprises one or more elements selected from Mg, Ti, Cr, Zr, Nb, Fe, Mo, Cu, Sb, V, P, and F.

69. The positive electrode sheet according to claim 68, in, The third positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (III); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

70. The positive electrode sheet according to claim 69, in, The one or more coating layers independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly inserting and deinserting lithium ions.

71. The positive electrode sheet according to claim 69 or 70, in, The coating amount of the shell is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core; and / or, The shell has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.

72. The positive electrode sheet according to claim 67, in, The third positive electrode active material includes a compound represented by formula (IV), Li a2 A 3 x2 B 3 y2 P 1-z2 C 3 z2 O 4-n2 D 3 n2 , (IV) A 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IIB, Group VB and Group VIB; B 3 Includes one or more elements selected from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, and Group VIII; C 3 Includes one or more elements selected from Group IIIA, Group IVA, Group VA and Group VIA; D 3 It includes one or more elements selected from Group VIA and Group VIIA; a2 is selected from the range of 0.85 to 1.15; x2 is selected from the range of 0 to 0.1; y2 is selected from the range of 0.001 to 0.999; z2 is selected from the range of 0 to 0.5; and n2 is selected from the range of 0 to 0.

5.

73. The positive electrode sheet according to claim 72, in, A 3 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, Ga, In, Cd, V, Ta, Cr, Zn, Al, Na, K, Mg, Nb, Mo and W, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; and / or, B 3 comprising one or more elements selected from the group consisting of Rb, Cs, Be, Ca, Sr, Ba, In, Pb, Bi, Cd, Hf, Ta, Cr, Ru, Rh, Pd, Os, Ir, Pt, Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, and optionally comprising one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge; and / or, C 3 comprising one or more elements selected from B (boron), S, Si and N; and / or, D 3 comprising one or more elements selected from S, F, Cl and Br; and / or, a2 is selected from the range of 0.9 to 1.1, optionally selected from the range of 0.97 to 1.01; and / or, x2 is selected from the range of 0.001 to 0.005; and / or, y2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.01 to 0.5, optionally selected from the range of 0.25 to 0.5; and / or, z2 is selected from the range of 0.001 to 0.5, optionally selected from the range of 0.001 to 0.1, more optionally selected from the range of 0.001 to 0.005; and / or, n2 is selected from the range of 0 to 0.1, optionally from the range of 0.001 to 0.

005.

74. The positive electrode sheet according to claim 72 or 73, in, The third positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (IV); The shell is a shell according to any one of claims 19 to 52.

75. The positive electrode sheet according to claim 67, in, The third positive electrode active material includes a compound represented by formula (V), LiMn t1 A 4 2-t1 O 4 , (V) t1 is selected from the range of 0 to 2, A 4 Includes one or more elements selected from Ni, Cr, Al, Zr, V, Ti, Mo, Ru, Mg, Nb, Ba, Si, P, W, Co, Cu and Zn.

76. The positive electrode sheet according to claim 75, in, The third positive electrode active material includes a core and a shell covering the core, The inner core comprises the compound represented by formula (V); The shell includes one or more coating layers; each coating layer has ionic conductivity and / or electronic conductivity.

77. The positive electrode sheet according to claim 76, in, The one or more coating layers independently include one or more materials selected from phosphates, pyrophosphates, solid electrolytes, conductive polymers, and materials capable of reversibly inserting and deinserting lithium ions.

78. The positive electrode sheet according to claim 76 or 77, in, The coating amount of the shell is 0.1 wt % to 5 wt %, optionally 0.5 wt % to 2 wt %, based on the weight of the core; and / or, The shell has a thickness of 2 nm to 200 nm, and optionally 5 nm to 50 nm.

79. The positive electrode sheet according to claim 78, in, The positive electrode film layer includes a positive electrode binder and / or a positive electrode conductor; Optionally, the positive electrode binder includes a vinylidene fluoride homopolymer and / or copolymer, and more optionally, the comonomer includes one or more of tetrafluoroethylene, hexafluoropropylene, and propylene; and / or, Optionally, the weight average molecular weight of the positive electrode binder is 300,000 to 2,000,000.

80. The positive electrode sheet according to claim 78 or 79, in, The positive electrode film layer further includes functional additives, wherein the functional additives include one or more of a dispersant, a plasticizer, a pore former, a water removal additive, an acid removal additive, and a lithium supplement; and / or, The positive electrode plate also includes a functional coating, which is located between the positive electrode collector and the positive electrode film layer and / or on the surface of the positive electrode film layer facing away from the positive electrode collector, and the functional coating includes one or more of conductive carbon, a water removal additive, an acid removal additive, and a lithium supplement.

81. A battery comprising the positive electrode active material composition according to any one of claims 1 to 65 or the positive electrode sheet according to any one of claims 66 to 80.

82. The battery according to claim 81, in, The battery includes an electrolyte, and the electrolyte includes one or more of a liquid electrolyte, an all-solid electrolyte, and a gel electrolyte.

83. The battery according to claim 82, in, The liquid electrolyte comprises a lithium salt, a non-aqueous solvent for dissolving the lithium salt, and an optional additive; Optionally, the lithium salt includes a selected from LiPF 6 , LiBF 4 、LiN(SO 2 F) 2 、LiN(CF 3 SO 2 ) 2 、LiClO 4 、LiAsF 6 、LiB(C 2 O 4 ) 2 , LiBF 2 C 2 O 4 、LiPO 2 F 2 One or more of; and / or, Optionally, the concentration of the lithium salt is 0.5-1.5 mol / L; and / or, Optionally, the non-aqueous solvent includes one or more selected from propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, ethyl acetate, methyl butyrate, ethyl butyrate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethylene sulfite, propylene sulfite, dimethyl sulfite, diethyl sulfite, acid anhydride, N-methylpyrrolidone, acetonitrile, cyclopentane, dimethyl sulfoxide, methyl sulfide, γ-butyrolactone, tetrahydrofuran; and / or, Optionally, the additive includes one or more selected from cyclic carbonate compounds containing carbon-carbon double bonds, halogen-substituted cyclic carbonate compounds, nitrile and polynitrile compounds, phosphazene compounds, aromatic hydrocarbons and halogenated aromatic hydrocarbon compounds, isocyanate compounds, acid anhydride compounds, sulfate compounds, sulfite compounds, sulfonate compounds, disulfonate compounds, borate compounds, phosphate compounds, amide compounds, carbodiimide compounds, crown ethers and azacrown ether compounds, and their respective derivatives, and optionally includes vinylene carbonate, 1,2,3-tris(2-cyanoethoxy)propane, 1-aza-12-crown 4-ether, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, tris(hexafluoroisopropyl)borate, tris(2,2,3,3-tetrafluoropropyl)borate, and tris(pentafluorophenyl)borate.

84. A battery according to any one of claims 81 to 83, in, The battery comprises a negative electrode plate, the negative electrode plate comprises a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer comprises a negative electrode active material, and the negative electrode active material comprises one or more of a carbon-based material, a silicon-based material, a tin-based material and lithium titanate; Optionally, the negative electrode active material includes a carbon-based material, or a combination of a carbon-based material and a silicon-based material; Optionally, the porosity of the negative electrode film layer is 20% to 50%.

85. The battery according to claim 84, in, The negative electrode active material includes a carbon-based material, and the carbon-based material includes graphite, or a combination of graphite and hard carbon; or The negative electrode active material includes a combination of a carbon-based material and a silicon-based material, the carbon-based material includes graphite, or a combination of graphite and hard carbon, and the content of the silicon element in the negative electrode active material is greater than 0 and less than or equal to 30 weight %, based on the total weight of the negative electrode active material.

86. The battery according to claim 84 or 85, in, The negative electrode plate further comprises a functional coating, wherein the functional coating is located between the negative electrode current collector and the negative electrode film layer and / or located on a surface of the negative electrode film layer away from the negative electrode current collector; optionally, the functional coating comprises carbon; and / or, The negative electrode film layer also includes a lithium replenishing material. Optionally, the lithium replenishing material includes one or more of lithium foil, lithium strip, lithium powder, and a pre-lithiation agent. Optionally, the pre-lithiation agent includes one or more of Li-aromatic hydrocarbons, complexes of Li-aromatic hydrocarbons and ether solvents, and may further include one or more of naphthalene lithium and biphenyl lithium-dimethyl ether.

87. A battery according to any one of claims 84 to 86, in, The negative electrode plate includes a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer respectively arranged on two surfaces of the negative electrode current collector. Optionally, the thickness ratio of the first negative electrode film layer to the second negative electrode film layer is 5:95 to 95:

5.

88. A battery according to any one of claims 81 to 83, in, The battery comprises a negative electrode plate, and the negative electrode plate does not comprise a negative electrode active material capable of inserting and removing lithium ions; Optionally, the negative electrode plate comprises a lithium plate or a lithium alloy plate; or, The negative electrode plate includes a mesh or foam three-dimensional skeleton layer.

89. The battery according to any one of claims 81 to 88, in, The battery includes a separator including a porous substrate.

90. The battery according to claim 89, in, The isolation membrane further comprises a coating located on at least one surface of the porous substrate. Optionally, the coating comprises one or more of inorganic heat-resistant particles and organic heat-resistant particles.

91. The battery according to claim 89 or 90, in, The porosity of the isolation film is 10%-40%.

92. An electrical device comprising the battery according to any one of claims 81 to 91.

Citation Information

Patent Citations

  • Lithium iron phosphate positive electrode active material, preparation method thereof, positive electrode plate and battery

    CN114068920A

  • Secondary battery

    CN115528296A

  • Secondary battery, electrolyte, and apparatus comprising the secondary battery

    US20220123366A1

Cited By

  • Solid-state battery, positive electrode sheet, positive electrode active material, preparation method, electric device and use

    WO2026098036A1