Nonaqueous electrolyte secondary battery
By dividing the positive electrode into 1/3 and 2/3 end regions and a central region in the width direction, and reducing the stiffness value through heat treatment, the problems of fracture of the positive electrode foil and deterioration of charge and discharge cycle characteristics of non-aqueous electrolyte secondary batteries are solved. problem, achieving higher capacity and improved long-life performance.
Patent Information
- Application Number
- CN202380025713.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-03-06
- Publication Date
- 2024-10-01
AI Technical Summary
After the high-density treatment of the positive electrode of the existing non-aqueous electrolyte secondary battery, the flexibility is improved, but the foil is prone to breakage, and the charge and discharge cycle characteristics are reduced.
A design is adopted to divide the positive electrode into 1/3 and 2/3 of the width direction of the end areas and the central area. The stiffness value of the end areas is reduced through heat treatment, so that the overall stiffness value is between 0.018N/mm and 0.040N/ mm range, inhibit foil breakage and maintain charge and discharge cycle characteristics.
It effectively suppresses the foil breakage of the positive electrode during the winding process, improves the stability of the charge and discharge cycle characteristics, and ensures the high capacity and long life performance of the battery.
Smart Images

Figure CN118743047A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery. Background Art
[0002] In recent years, nonaqueous electrolyte secondary batteries such as lithium ion secondary batteries are used in a wide range of applications such as notebook PCs, power tools, electric power-assisted bicycles, electric vehicles, etc. because of their high energy density. Wherein, it is desirable to develop nonaqueous electrolyte secondary batteries with higher capacity and excellent life performance. In order to cope with high capacity, it is known that the method of high densification of the positive electrode of nonaqueous electrolyte secondary batteries is used, but if the positive electrode is high densified, the flexibility of the positive electrode decreases, and there is a problem of the foil fracture of the positive electrode that can be produced when the positive electrode is wound.
[0003] Therefore, in order to improve the flexibility of the positive electrode, for example, Patent Documents 1 and 2 propose to perform a heat treatment on the positive electrode.
[0004] However, while the flexibility of the positive electrode increases by heat treatment, the binder contained in the positive electrode forms a film and becomes a resistance component in the positive electrode, which causes a problem that the charge and discharge cycle characteristics of the battery decrease.
[0005] Prior Art Literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2010-165564
[0008] Patent Document 2: International Publication No. 2010 / 029675 Summary of the invention
[0009] Therefore, an object of the present disclosure is to provide a non-aqueous electrolyte secondary battery capable of suppressing foil breakage when a positive electrode is wound and a decrease in charge and discharge cycle characteristics.
[0010] One method disclosed herein is a non-aqueous electrolyte secondary battery having a wound electrode body and a non-aqueous electrolyte, wherein the electrode body is formed by winding a positive electrode and a negative electrode with an insulator interposed therebetween, and is characterized in that the positive electrode comprises: a positive electrode collector; and a positive electrode composite material layer formed on the positive electrode collector, comprising a positive electrode active material and a binding material, wherein when the positive electrode is divided into a first end region having a width of 1 / 3 relative to the full width of the positive electrode from one end in the width direction of the positive electrode toward the center side, a second end region having a width of 1 / 3 relative to the full width of the positive electrode from the other end in the width direction of the positive electrode toward the center side, and a central region sandwiched between the first end region and the second end region, the stiffness values of the first end region and the second end region are lower than the stiffness value of the central region, and the stiffness value of the positive electrode as a whole is in the range of 0.018 N / mm to 0.040 N / mm.
[0011] According to one aspect of the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery capable of suppressing foil breakage when a positive electrode is wound and a decrease in charge and discharge cycle characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment.
[0013] Figure 2 It is a schematic plan view of the positive electrode before being wound.
[0014] Figure 3 This is a diagram for explaining a method for measuring a stiffness value by a ring stiffness method. DETAILED DESCRIPTION
[0015] An example of an embodiment will be described with reference to the drawings. The nonaqueous electrolyte secondary battery disclosed herein is not limited to the embodiment described below. The drawings referred to in the description of the embodiment are schematically described.
[0016] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment. Figure 1 The non-aqueous electrolyte secondary battery 10 shown includes a wound electrode body 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18 and 19 disposed above and below the electrode body 14, respectively, and a battery case 15 that accommodates the above components. The battery case 15 is composed of an outer can 16 and a sealing body 17 that seals the opening of the outer can 16.
[0017] The outer can 16 is, for example, a metal shell in a bottomed cylindrical shape. A gasket 28 is provided between the outer can 16 and the sealing body 17 to ensure the airtightness of the battery interior. The outer can 16 has, for example, an extension portion 22 that supports the sealing body 17, in which a part of the side portion extends inward. The extension portion 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and supports the sealing body 17 on its upper surface.
[0018] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and the insulating member 25 is interposed between the peripheral portions of the lower valve body 24 and the upper valve body 26. If the internal pressure of the non-aqueous electrolyte secondary battery 10 rises due to heat caused by an internal short circuit, for example, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cover 27 side, and the current path between the lower valve body 24 and the upper valve body 26 is cut off. If the internal pressure rises further, the upper valve body 26 breaks, and gas is discharged from the opening of the cover 27.
[0019] exist Figure 1 In the non-aqueous electrolyte secondary battery 10 shown, the positive electrode lead 20 attached to the positive electrode 11 passes through the through hole of the insulating plate 18 and extends to the sealing body 17 side, and the negative electrode lead 21 attached to the negative electrode 12 passes through the outside of the insulating plate 19 and extends to the bottom side of the outer can 16. The positive electrode lead 20 is connected to the lower surface of the filter 23 as the bottom plate of the sealing body 17 by welding or the like, and the cover 27 as the top plate of the sealing body 17 electrically connected to the filter 23 serves as a positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 serves as a negative terminal.
[0020] Hereinafter, each component of the nonaqueous electrolyte secondary battery 10 will be described in detail.
[0021] [positive electrode]
[0022] The positive electrode 11 includes a positive electrode current collector and a positive electrode composite material layer disposed on the positive electrode current collector. For the positive electrode current collector, a foil of a metal such as aluminum that is stable within the potential range of the positive electrode 11, a film having the metal disposed on the surface, etc. can be used. The positive electrode composite material layer includes a positive electrode active material and a binding material, and may include an additive such as a conductive material as required.
[0023] The positive electrode 11 of the present embodiment is manufactured, for example, as follows. First, a positive electrode composite material slurry containing a positive electrode active material, a conductive material, and a binding material is applied to a positive electrode current collector, and after the coating is dried, it is compressed to obtain a positive electrode having a positive electrode composite material layer formed on the positive electrode current collector. Then, as described later, the end region of the positive electrode is brought into contact with a heated roller, and the positive electrode is subjected to a heat treatment, thereby manufacturing the positive electrode 11 of the present embodiment. The thickness of the positive electrode current collector is, for example, not less than 10 μm. In addition, the thickness of the positive electrode composite material layer is, for example, not less than 20 μm. The density of the positive electrode composite material layer is, for example, 1.60 g / cm 3 above.
[0024] The positive electrode active material includes lithium metal composite oxides containing transition metal elements such as Co, Mn, and Ni. For example, lithium metal composite oxides are Li x CoO2、Li x NiO2、Li x MnO2、Li x Co y Ni 1-y O2、Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn2O4、Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3). They can be used alone or in combination. In order to achieve a high capacity of the non-aqueous electrolyte secondary battery, the positive electrode active material preferably contains Li x NiO2、Li x Co y Ni 1-y O2、Li x Ni 1-y M y O z Lithium nickel composite oxides such as (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3).
[0025] The binder material can be, for example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF) and other fluorine resins, polyacrylonitrile (PAN), polyimide (PI), acrylic resin, polyolefin resin, styrene butadiene rubber (SBR), nitrile rubber (NBR), carboxymethyl cellulose (CMC) or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. They can be used alone or in combination of two or more. The content of the binder in the positive electrode composite material layer is preferably 0.5% to 10% by mass, and more preferably 1% to 5% by mass.
[0026] Examples of the conductive material include carbon black (CB), acetylene black (AB), Ketjen black, carbon nanotubes (CNT), and carbon particles such as graphite. These may be used alone or in combination of two or more.
[0027] Figure 2 The arrow S shown in the figure indicates the winding axis direction of the electrode body 14 , and the arrow R orthogonal to the arrow S indicates the winding direction of the positive electrode 11 when the electrode body 14 is produced.
[0028] like Figure 2 As shown, the positive electrode 11 is divided into a first end region 11a having a width (X1) of 1 / 3 of the full width (W) of the positive electrode 11 from one end in the width direction of the positive electrode 11 along the winding axis direction of the electrode body 14 to the center side, a second end region 11b having a width (X2) of 1 / 3 of the full width (W) of the positive electrode 11 from the other end in the width direction of the positive electrode 11 along the winding axis direction of the electrode body 14 to the center side, and a center region 11c sandwiched between the first end region 11a and the second end region 11b. When the positive electrode 11 is divided into three parts in this way, the rigidity values of the first end region 11a and the second end region 11b are lower than the rigidity value of the center region 11c, and the rigidity value of the entire positive electrode 11 is in the range of 0.018N / mm to 0.040N / mm. The rigidity value is an index of flexibility, and the lower the rigidity value, the more flexible it is. The stiffness value is measured by the ring stiffness method described later.
[0029] As in the case of the positive electrode 11, by making the stiffness values of the first end region 11a and the second end region 11b lower than the stiffness value of the central region 11c, the flexibility of the end region is improved, so that even when the positive electrode 11 is wound to make the electrode body 14, the foil breakage of the positive electrode 11 can be suppressed. Here, the stiffness value can be controlled by heating the positive electrode 11. Specifically, by heating a part or the whole of the first end region 11a and the second end region 11b, the positive electrode collector and the like in the end region are softened, and the stiffness value can be reduced. The heating treatment is performed, for example, by bringing a part or the whole of the first end region 11a and the second end region 11b of the positive electrode 11 into contact with a heated roller.
[0030] However, it is necessary to heat treat a part or the whole of the first end region 11a and the second end region 11b so that the stiffness value of the positive electrode 11 as a whole is in the range of 0.018N / mm to 0.040N / mm. For example, if the heating temperature of the end region is low, the stiffness value of the positive electrode 11 as a whole may exceed 0.040N / mm. In this case, even if the stiffness values of the first end region 11a and the second end region 11b are lower than the stiffness value of the central region 11c, the foil of the positive electrode 11 may be broken. The heating temperature of the end region is also determined according to the thickness of the positive electrode 11, and is preferably in the range of 180°C to 200°C, for example.
[0031] In addition, in the present embodiment, the heating treatment of the central region 11c is not limited. Since the stiffness value of the entire positive electrode 11 is easily controlled to be in the range of 0.018N / mm to 0.040N / mm, it is preferred that the central region 11c is not subjected to the heating treatment. However, in the case where the heating treatment is performed by bringing a part or the entire central region 11c into contact with the heated roller, the heating temperature of the roller is preferably set to a temperature lower than the heating treatment temperature of the first end region 11a and the second end region 11b. In addition, if a part or the entire central region 11c is heated under the same conditions as the heating treatment of the end regions, the stiffness value of the entire positive electrode 11 is sometimes lower than 0.018N / mm. In such a case, it is conceivable that the binder material that is filmed by the heating treatment is present in the entire positive electrode 11, and the charge and discharge cycle characteristics of the battery are greatly reduced.
[0032] In any case, by making the stiffness values of the first end region 11a and the second end region 11b of the positive electrode 11 lower than the stiffness value of the central region 11c of the positive electrode 11, and by making the stiffness value of the positive electrode 11 as a whole in the range of 0.018N / mm to 0.040N / mm (preferably in the range of 0.020N / mm to 0.030N / mm), it is possible to suppress foil breakage when the positive electrode 11 is wound and a decrease in charge and discharge cycle characteristics.
[0033] The rigidity values of the first end region 11a and the second end region 11b of the positive electrode 11 are preferably in the range of 0.025 N / mm or less, for example, from the perspective of suppressing foil breakage when winding the positive electrode 11. In addition, the rigidity value of the central region 11c of the positive electrode 11 is preferably in the range of 0.020 N / mm or more, for example, from the perspective of suppressing a decrease in the charge and discharge cycle characteristics of the battery.
[0034] Figure 3 This is a diagram for explaining the method of measuring the stiffness value based on the ring stiffness method. Figure 3 As shown, the ring stiffness method is a method for evaluating the flexibility of a test piece by measuring the stress when a test piece rolled into a ring shape is pressed at a given speed. In detail, first, each region of the positive electrode 11 (the first end region 11a, the second end region 11b, and the central region 11c) is cut into each region with a width × length of 80 mm, and the two ends are butted together to roll into a ring shape to make a test piece 30 with an outer circumference of 80 mm. Next, the butted portion of the test piece 30 is fixed to the lower flat plate 32 and clamped between the upper flat plate 34 and the lower flat plate 32. Next, the upper flat plate 34 is moved downward at a speed of 1.6 mm / sec to press the outer circumference of the test piece 30, and the rebound force of the test piece 30 when the gap L of the test piece 30 becomes 11 mm is measured by the dynamometer 36. In this way, the rebound force of at least three test pieces 30 is measured, and the obtained rebound forces are converted according to the unit width of the test piece, and their average value is used as the stiffness value of each region. In addition, when measuring the stiffness value of the positive electrode 11 as a whole, the positive electrode 11 is cut into a width (W) × length of 80 mm, and its two ends are butt-jointed and rolled into a ring to make a test piece 30 with an outer circumference of 80 mm. As described above, the rebound force of at least 3 test pieces 30 is measured, and the obtained rebound forces are converted according to the unit width of the test pieces, and their average value is used as the stiffness value of the positive electrode 11 as a whole.
[0035] [negative electrode]
[0036] The negative electrode 12 has a negative electrode current collector and a negative electrode composite material layer disposed on the negative electrode current collector. The negative electrode current collector may be, for example, a foil of a metal such as copper that is stable within the potential range of the negative electrode, or a film that arranges the metal on the surface. The negative electrode composite material layer may include, for example, a negative electrode active material and a binding material. For example, a negative electrode composite material slurry including a negative electrode active material and a binding agent is applied to the negative electrode current collector, and after the coating is dried, the negative electrode composite material layer is formed on the negative electrode current collector by compression, thereby making it possible to manufacture the negative electrode 12.
[0037] The negative electrode active material is a material that can reversibly store and release lithium ions, and examples thereof include carbon materials such as natural graphite and artificial graphite, metals that alloy with lithium such as silicon (Si) and tin (Sn), alloys containing these metal elements, and composite oxides.
[0038] Examples of the binder include the same binders as those for the positive electrode 11. The content of the binder in the negative electrode composite material layer is, for example, preferably 0.5% by mass to 10% by mass, and more preferably 1% by mass to 5% by mass.
[0039] [Isolator]
[0040] For the separator 13, for example, a porous sheet having ion permeability and insulation can be used. Specific examples of the porous sheet include microporous films, woven fabrics, non-woven fabrics, etc. As the material of the separator, olefin resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 can also be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it can also be a multilayer separator including a polyethylene layer and a polypropylene layer, and it can also be used that the surface of the separator is coated with a material such as an aromatic polyamide resin, ceramics, etc.
[0041] [Non-aqueous electrolyte]
[0042] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For the non-aqueous solvent, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof can be used. The non-aqueous solvent can contain a halogen substitution body in which at least a part of the hydrogen atoms of these solvents are replaced by halogen atoms such as fluorine. In addition, the non-aqueous electrolyte is not limited to a liquid electrolyte, and can also be a solid electrolyte using a gel-like polymer. For the electrolyte salt, a lithium salt such as LiPF6 can be used.
[0043] Example 1
[0044] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.
[0045] <Example 1>
[0046] [Production of positive electrode]
[0047] 95 parts by mass of LiNi 0.7 Co 0.25 Al 0.05O2 and 5 parts by mass of graphite as a conductive material are mixed. 95 parts by mass of the mixture and 5 parts by mass of polyvinylidene fluoride (PVDF) as a binding material are dispersed in N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode composite material slurry. The positive electrode composite material slurry is applied to both sides of a strip-shaped positive electrode collector composed of an aluminum foil with a thickness of 16 μm, and the coating is heated and dried. A roller press is used to press the dried coating so that the density becomes 3.6 g / cc, thereby producing a positive electrode with a positive electrode composite material layer formed on both sides of the positive electrode collector. The two ends of the positive electrode in the width direction are heated by a roller heated to 180°C. The width of the two ends of the positive electrode in contact with the heated roller is set to 3% relative to the full width of the positive electrode.
[0048] The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured. As a result, the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the positive electrode as a whole was 0.040 N / mm. The stiffness value was measured as described above.
[0049] [Production of negative electrode]
[0050] 96 parts by mass of artificial graphite as a negative electrode active material, 2 parts by mass of carboxymethyl cellulose (CMC), and 2 parts by mass of styrene butadiene rubber were dispersed in water to prepare a negative electrode composite material slurry. The negative electrode composite material slurry was applied to both sides of a strip-shaped negative electrode collector composed of a copper foil with a thickness of 12 μm, the coating was heated and dried, and the dried coating was pressed using a roller press to a density of 1.55 g / cc, thereby producing a negative electrode having a negative electrode composite material layer formed on both sides of the negative electrode collector.
[0051] [Preparation of non-aqueous electrolyte]
[0052] LiPF6 was dissolved at a ratio of 1.2 mol / L in a non-aqueous solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 20:20:60 (converted at 1 atmosphere and 25°C) to prepare a non-aqueous electrolyte.
[0053] [Fabrication of non-aqueous electrolyte secondary battery]
[0054] (1) A positive electrode and a negative electrode are wound with a separator made of an olefin-based resin interposed therebetween to produce a wound electrode body.
[0055] (2) Place insulating plates above and below the electrode body and insert them into the outer can. Weld the negative electrode lead attached to the negative electrode to the bottom of the outer can, and weld the positive electrode lead attached to the positive electrode to the sealing body.
[0056] (3) After the nonaqueous electrolyte is injected into the outer can, the open end of the outer can is rivet-joined to the sealing body via a gasket to prepare a nonaqueous electrolyte secondary battery.
[0057] <Example 2>
[0058] A positive electrode was produced in the same manner as in Example 1 except that the width of both ends of the positive electrode in contact with the heated roller was set to 5% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results showed that the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.030 N / mm.
[0059] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0060] <Example 3>
[0061] The positive electrode was produced in the same manner as in Example 1 except that the width of both ends of the positive electrode in contact with the heated roller was set to 25% of the total width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured. As a result, the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.025 N / mm.
[0062] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0063] <Example 4>
[0064] A positive electrode was produced in the same manner as in Example 1 except that the width of both ends of the positive electrode in contact with the heated roller was set to 30% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured. As a result, the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.020 N / mm.
[0065] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0066] <Example 5>
[0067] A positive electrode was produced in the same manner as in Example 1 except that the width of both ends of the positive electrode in contact with the heated roller was set to 33% of the total width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured. As a result, the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.018 N / mm.
[0068] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0069] <Example 6>
[0070] A positive electrode was produced in the same manner as in Example 1 except that the width of one end of the positive electrode among the widths of the two ends of the positive electrode in contact with the heated roller was set to 5% relative to the full width of the positive electrode, and the width of the other end of the positive electrode was set to 33% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results showed that the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the positive electrode as a whole was 0.028 N / mm.
[0071] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0072] <Example 7>
[0073] The positive electrode was produced in the same manner as in Example 1 except that the width of one end of the positive electrode among the widths of the two ends of the positive electrode in contact with the heated roller was set to 33% relative to the full width of the positive electrode, and the width of the other end of the positive electrode was set to 5% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results showed that the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.028 N / mm.
[0074] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0075] <Comparative Example 1>
[0076] A positive electrode was produced in the same manner as in Example 1 except that the heat treatment using the roller heated to 180° C. was not performed. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results were all the same. In addition, the stiffness value of the entire positive electrode was 0.045 N / mm.
[0077] Furthermore, a wound electrode body was produced using the positive electrode. However, the foil of the positive electrode was broken, so the production of the nonaqueous electrolyte secondary battery was stopped at that point.
[0078] <Comparative Example 2>
[0079] The positive electrode was produced in the same manner as in Example 1 except that the positive electrode was heated by passing the entire positive electrode through a roller heated to 180° C. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results were all the same. In addition, the stiffness value of the entire positive electrode was 0.013 N / mm.
[0080] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0081] <Comparative Example 3>
[0082] A positive electrode was produced in the same manner as in Example 1 except that the width of both ends of the positive electrode in contact with the heated roller was set to 35% of the total width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured. As a result, the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.016 N / mm.
[0083] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0084] <Comparative Example 4>
[0085] A positive electrode was produced in the same manner as in Example 1 except that the width of both ends of the positive electrode in contact with the heated roller was set to 40% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured. As a result, the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the entire positive electrode was 0.015 N / mm.
[0086] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0087] <Comparative Example 5>
[0088] The positive electrode was produced in the same manner as in Example 1 except that the width of one end of the positive electrode among the widths of the two ends of the positive electrode in contact with the heated roller was set to 30% relative to the full width of the positive electrode, and the width of the other end of the positive electrode was set to 40% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results showed that the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the positive electrode as a whole was 0.016 N / mm.
[0089] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0090] <Comparative Example 6>
[0091] A positive electrode was produced in the same manner as in Example 1 except that the width of one end of the positive electrode among the widths of the two ends of the positive electrode in contact with the heated roller was set to 40% relative to the full width of the positive electrode, and the width of the other end of the positive electrode was set to 30% relative to the full width of the positive electrode. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results showed that the stiffness values of the first end region and the second end region were lower than the stiffness value of the central region. In addition, the stiffness value of the positive electrode as a whole was 0.016 N / mm.
[0092] Then, a nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1 except that the above-mentioned positive electrode was used.
[0093] <Comparative Example 7>
[0094] The heat treatment was not performed on both ends of the positive electrode in the width direction, but the central part of the positive electrode in the width direction was passed through a roller heated to 180°C and subjected to heat treatment. The width of the central part of the positive electrode in contact with the heated roller was set to 34% relative to the full width of the positive electrode. In addition, the positive electrode was produced in the same manner as in Example 1. The stiffness values of the first end region, the second end region, and the central region of the positive electrode were measured, and the results showed that the stiffness values of the first end region and the second end region were higher than the stiffness value of the central region. In addition, the stiffness value of the positive electrode as a whole was 0.033N / mm.
[0095] Furthermore, a wound electrode body was produced using the positive electrode. However, the foil of the positive electrode was broken, so the production of the nonaqueous electrolyte secondary battery was stopped at that point.
[0096] [Evaluation of charge and discharge cycle characteristics]
[0097] For the non-aqueous electrolyte secondary batteries of Examples 1 to 7 and Comparative Examples 2 to 6, at a temperature of 25°C, constant current charging was performed at a current of 0.5C until the voltage became 4.2V, and then constant voltage charging was performed at a voltage of 4.2V until the current became 1 / 50C. Then, constant current discharge was performed at a current of 0.2C until the voltage became 2.5V. The discharge capacity at this time was set as the initial discharge capacity. Next, for each non-aqueous electrolyte secondary battery, at a temperature of 25°C, constant current charging was performed at a current of 0.5C until the voltage became 4.2V, and then constant voltage charging was performed at a voltage of 4.2V until the current became 1 / 50C. Then, constant current discharge was performed at a current of 1C until the voltage became 2.5V. The charge and discharge cycle was performed for 500 cycles, and the capacity retention rate was calculated by the following formula.
[0098] Capacity retention rate (%) = (discharge capacity at the 500th cycle / initial discharge capacity) × 100
[0099] Table 1 summarizes the results of each example and each comparative example.
[0100] [Table 1]
[0101]
[0102] In Comparative Examples 1 and 7, in which the stiffness value of the central region is higher than that of the first end region and the second end region, foil breakage occurred in the positive electrode when the wound electrode body was produced. In addition, in Comparative Examples 2 to 6, in which the stiffness value of the central region is lower than that of the first end region and the second end region but the stiffness value of the positive electrode as a whole is less than 0.018 N / mm, no positive electrode foil breakage occurred, but the capacity retention rate during the charge and discharge cycle was a low value of less than 70%.
[0103] On the other hand, in Examples 1 to 7 in which the stiffness value of the central region is lower than the stiffness values of the first end region and the second end region and the stiffness value of the positive electrode as a whole is in the range of 0.018 N / mm to 0.040 N / mm, no positive electrode foil breakage occurs. In addition, the capacity retention rate during the charge and discharge cycle is higher than that of Comparative Examples 2 to 6, which can suppress the decline in charge and discharge cycle characteristics.
[0104] Explanation of symbols
[0105] 10 non-aqueous electrolyte secondary battery; 11 positive electrode; 11a first end region; 11b second end region; 11c central region; 12 negative electrode; 13 separator; 14 electrode body; 15 battery case; 16 outer can; 17 sealing body; 18, 19 insulating plate; 20 positive electrode lead; 21 negative electrode lead; 22 extension; 23 filter; 24 lower valve body; 25 insulating member; 26 upper valve body; 27 cover; 28 gasket; 30 test piece; 32 lower plate; 34 upper plate; 36 dynamometer.
Claims
1. A non-aqueous electrolyte secondary battery comprising a wound electrode body and a non-aqueous electrolyte, wherein the electrode body is formed by winding a positive electrode and a negative electrode with a separator interposed therebetween, The positive electrode has: a positive electrode current collector; and The positive electrode composite material layer is formed on the positive electrode current collector and contains a positive electrode active material and a binding material. When the positive electrode is divided into a first end region having a width of 1 / 3 relative to the full width of the positive electrode from one end of the positive electrode toward the center, a second end region having a width of 1 / 3 relative to the full width of the positive electrode from the other end of the positive electrode toward the center, and a central region sandwiched between the first end region and the second end region, The stiffness values of the first end region and the second end region are lower than the stiffness value of the central region. The stiffness value of the positive electrode as a whole is in the range of 0.018 N / mm to 0.040 N / mm.
2. The nonaqueous electrolyte secondary battery according to claim 1, wherein The first end region and the second end region of the positive electrode each have a rigidity value of 0.025 N / mm or less.
3. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: The central region of the positive electrode has a rigidity value of 0.020 N / mm or more.